Filler and filling method thereof
A dual-compound filler system with separate containers for a curable compound and curing agent, releasing ions to form calcium carbonate, addresses the durability and workability issues of conventional fillers, ensuring long-term structural reinforcement.
Patent Information
- Application Number
- JP2020154703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-15
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-15
AI Technical Summary
Conventional fillers using epoxy resins deteriorate due to moisture, leading to strength loss over time, and mortar fillers are difficult to inject into small gaps, while existing methods struggle with efficient filling of large voids.
A filler system comprising a first composition with a curable compound and a second composition with a curing agent, both contained in separate containers, where at least one of them releases carbonate or calcium ions, allowing for efficient mixing and curing post-injection, forming a calcium carbonate layer for enhanced strength and durability.
The system provides excellent workability, maintains high strength over time, and prevents premature curing, effectively reinforcing structures and ground areas with improved resistance to moisture and structural integrity.
Smart Images

Figure 0007560029000002 
Figure 0007560029000003 
Figure 0007560029000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a filler that can be used in structures, ground, etc. The present invention also relates to a method for filling said filler. [Background technology]
[0002] In bridges, tunnels and other structures, cracks and debris may occur due to poor construction during construction or if a long period of time has passed since construction. Structures with cracks and debris will have a reduced strength. Many of these structures support social infrastructure such as traffic and transportation, and therefore cannot be easily rebuilt or demolished. Furthermore, large-scale repairs or reinforcement is difficult when infrastructure functions are suspended.
[0003] For this reason, a method is sometimes used in which a filler containing a curable resin such as an epoxy resin is injected into cracked or cracked parts of a structure, and the curable resin is then cured (eg, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-031661 A [Patent Document 2] JP 2018-104996 A [Patent Document 3] JP 2015-030987 A Summary of the Invention [Problem to be solved by the invention]
[0005] When cracks or cracked parts of a structure are repaired using a conventional filler, the strength of the repaired part can be increased until a certain period of time has passed since the repair. However, in the case of conventional fillers containing epoxy resins, the hardened epoxy resin gradually deteriorates due to rainwater and moisture attached to the concrete, and peeling may occur at the interface between the filler and the surface of the structure. In addition, peeling may occur at the interface between the filler and the surface of the structure due to seasonal fluctuations and repeated vibration and expansion and contraction. For this reason, with conventional fillers, the strength of the repaired part gradually decreases, and after a long period of time has passed since the repair (for example, 20 to 50 years after the repair), repairs will be required again.
[0006] If mortar is used as a filler, the strength of the repaired area can be maintained for a long period of time. However, since mortar has a high viscosity, it is difficult to efficiently inject the mortar into small gaps such as cracks and junk, and the workability is poor.
[0007] In addition, fillers are sometimes used to pack boreholes in the ground after excavating the ground for oil mining, storing and burying carbon dioxide, etc., or to reinforce the boundary surface between the ground and a structure for burying and disposing of high-level radioactive waste. However, when the distance from the injection port to the filling point is long as described above, or when the void volume is large, it can be difficult to efficiently inject conventional fillers into the voids.
[0008] An object of the present invention is to provide a filler which is easy to work with, can increase the strength of the filled area, and can maintain high strength for a long period of time. Another object of the present invention is to provide a method for filling with the filler. [Means for solving the problem]
[0009] According to a broad aspect of the present invention, there is provided a filler comprising a first composition, a second composition, a first container, and a second container, the first container encapsulating the first composition, the second container encapsulating the second composition, the first composition comprising a hardenable compound, the second composition comprising a hardener, and at least one of the first composition and the second composition comprising a compound capable of releasing carbonate ions or calcium ions.
[0010] In a particular aspect of the filler according to the present invention, the compound capable of releasing carbonate ions or calcium ions is tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium sulfate, calcium carbonate, calcium bicarbonate, sodium carbonate, or sodium bicarbonate.
[0011] In a specific aspect of the packing material according to the present invention, the wall thickness of the first container and the wall thickness of the second container are each 50 μm or more and 2000 μm or less.
[0012] In a particular aspect of the filling material according to the present invention, the wall material of the first container and the wall material of the second container are each water-soluble.
[0013] In a specific aspect of the filler according to the present invention, the internal volume of the first container and the internal volume of the second container are each 1 cc or more and 10,000 cc or less.
[0014] According to a broad aspect of the present invention, there is provided a method for filling a filling material, comprising the steps of injecting the above-mentioned filling material into a filling location, and destroying the first container and the second container to mix and harden the first composition and the second composition.
[0015] In a specific aspect of the method for filling a filler according to the present invention, the first composition and the second composition are mixed by destroying the first container and the second container.
[0016] In a specific aspect of the method for filling a filler according to the present invention, the filling location is a filling location of a structure or a filling location of the ground. Effect of the Invention
[0017] The filler according to the present invention comprises a first composition, a second composition, a first container, and a second container. In the filler according to the present invention, the first composition is enclosed in the first container, and the second composition is enclosed in the second container. In the filler according to the present invention, the first composition contains a hardening compound, and the second composition contains a hardening agent. In the filler according to the present invention, at least one of the first composition and the second composition contains a compound capable of releasing carbonate ions or calcium ions. Since the filler according to the present invention has the above-mentioned configuration, it is easy to work with, can increase the strength of the filled area, and can maintain high strength for a long period of time. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a cross-sectional view of a filler according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a filler according to a second embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view for explaining the filling method of the filler according to the first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below.
[0020] (filling material) The filler according to the present invention comprises a first composition, a second composition, a first container, and a second container. In the filler according to the present invention, the first composition is enclosed in the first container, and the second composition is enclosed in the second container. In the filler according to the present invention, the first composition contains a hardening compound, and the second composition contains a hardener. In the filler according to the present invention, at least one of the first composition and the second composition contains a compound capable of releasing carbonate ions or calcium ions (hereinafter, may be referred to as "compound X").
[0021] Since the filler according to the present invention has the above-mentioned configuration, it is easy to work with, can increase the strength of the filled area, and can maintain high strength for a long period of time.
[0022] In the filler according to the present invention, after the filler is filled into cracked or junkered parts of a structure, or into a borehole in the ground, the hardening compound hardens, and the strength of the filled part can be increased. In addition, when the part filled with the filler comes into contact with rainwater and moisture attached to the concrete, the carbonate ions or calcium ions contained in the moisture react chemically with the carbonate ions or calcium ions released from the compound X contained in the filler, and calcium carbonate (cement) is generated at the contact surface between the moisture and the hardened filler. That is, a calcium carbonate layer is generated on the surface of the hardened filler. The generated calcium carbonate further increases the strength of the filled part. In addition, the generated calcium carbonate effectively prevents the filler from further contacting with moisture, and can effectively prevent deterioration of the hardened product of the hardening compound and deterioration of the structure. Therefore, the filler according to the present invention can maintain the strength of the filled part and the strength of the structure at a high level for a long period of time. It is considered that calcium carbonate is usually generated over several months to several years.
[0023] In addition, the filler according to the present invention can be used whether the filling location is dry or wet. Furthermore, the filler according to the present invention can be used even when water is flowing out from the filling location. Therefore, the filler according to the present invention can be quickly filled into structures and ground for various purposes.
[0024] The above-mentioned structure includes a concrete structure, an RC viaduct structure, a mountain tunnel, an underground tunnel structure, etc. Since the effect of the present invention is more effectively exerted, it is preferable that the above-mentioned structure is a concrete structure.
[0025] The ground may be a bedrock, diluvial deposits, alluvial deposits, artificial ground, etc. The ground is preferably a bedrock, since the effects of the present invention are more effectively exhibited.
[0026] In addition, in order to further increase the strength of the filled area, it is effective to use a filler containing an inorganic salt such as sodium bicarbonate. However, when a filler containing a large amount of inorganic salt is mixed in advance or immediately before filling through an opening, the filler may thicken due to a hardening reaction or may separate. Furthermore, the above filler has the problem that pressure is required during injection due to the thickening.
[0027] In addition, in the above-mentioned filler, the first composition containing the curable compound and the second composition containing the curing agent are sealed in separate containers, and are in a state before being mixed, and can be mixed after filling, so that unintended hardening of the filler before use can be prevented. In the filler according to the present invention, the thickening of the curable compound and the curing agent due to the curing reaction can be suppressed before filling, so that it can be filled at low pressure. In the filler according to the present invention, the hardening reaction of the filler can be advanced after the filler is sufficiently filled in the filling portion. Therefore, it is easy to work with and the strength of the entire filling portion can be increased.
[0028] The filler according to the present invention can suppress separation of the filler before filling. Furthermore, since the filler according to the present invention has excellent workability, it can be efficiently injected into the void even when the distance from the injection port to the filling location is large or the void volume is large.
[0029] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings. In the following embodiments, different parts can be replaced with each other.
[0030] FIG. 1 is a cross-sectional view of a filler according to a first embodiment of the present invention.
[0031] The filler 1 includes a first composition 11, a second composition 12, a first container 13, and a second container 14. The first composition 11 is enclosed in the first container 13. The second composition 12 is enclosed in the second container 14. In the filler 1, the first composition 11 includes a hardenable compound, and the second composition 12 includes a hardener. In the filler 1, at least one of the first composition 11 and the second composition 12 includes a compound (compound X) capable of releasing carbonate ions or calcium ions.
[0032] The first container 13 has a wall. The first container 13 has an internal space within the wall. A first composition 11 is enclosed throughout the internal space of the first container 13. The second container 14 has a wall. The second container 14 has an internal space within the wall. A second composition 12 is enclosed throughout the internal space of the first container 14.
[0033] A first container 13 in which the first composition 11 is enclosed and a second container 14 in which the second composition 12 is enclosed are directly connected.
[0034] FIG. 2 is a cross-sectional view of a filler according to a second embodiment of the present invention.
[0035] The filler 1A includes a first composition 11A, a second composition 12A, a first container 13A, and a second container 14A. The first composition 11A is enclosed in the first container 13A. The second composition 12A is enclosed in the second container 14A. In the filler 1A, the first composition 11A includes a curable compound, and the second composition 12A includes a curing agent. In the filler 1A, at least one of the first composition 11A and the second composition 12A includes a compound (compound X) capable of releasing carbonate ions or calcium ions.
[0036] The first container 13A has a wall. The first container 13A has an internal space within the wall. The first composition 11A is enclosed in a part of the internal space of the first container 13A. The first container 13A has a space in which the first composition 11A is not accommodated. The second container 14A has a wall. The second container 14A has an internal space within the wall. The second composition 12A is enclosed in a part of the internal space of the second container 14A. The second container 14A has a space in which the second composition 12A is not accommodated.
[0037] The first container 13A has a first container body 13Aa having an opening, and a lid 13Ab. After the first composition 11A is placed in the first container body 13Aa, the opening of the first container body 13Aa is sealed with the lid 13Ab.
[0038] The second container 14A has a first container body 14Aa having an opening and a lid 14Ab. After the second composition 12A is poured into the second container body 14Aa, the opening of the second container body 14Aa is sealed with the lid 14Ab.
[0039] A first container 13A in which a first composition 11A is enclosed and a second container 14A in which a second composition 12A is enclosed are indirectly connected via a joining member 15A.
[0040] The first container in which the first composition is enclosed and the second container in which the second composition is enclosed may be connected. The first container in which the first composition is enclosed and the second container in which the second composition is enclosed may be separate. The filling material may be a set product including the first container in which the first composition is enclosed and the second container in which the second composition is enclosed.
[0041] The walls of the first container and the second container may be integral. The first container and the second container may share a wall. The first composition and the second composition may be separated by only one wall.
[0042] Hereinafter, the details of each component used in the filler according to the present invention will be described.
[0043] <First composition> The first composition includes a curable compound. The first composition may include only the curable compound. The first composition may be the curable compound. The content of the curing agent in 100% by weight of the first composition is preferably less than the content of the curing agent in 100% by weight of the second composition, and the first composition preferably does not include a curing agent.
[0044] The curable compound includes a curable compound that can be cured by mixing with a curing agent, a thermosetting compound that can be cured by heating, and a photocurable compound that can be cured by irradiation with light. From the viewpoint of filling the voids and then curing the filler and from the viewpoint of increasing the storage stability of the filler, the curable compound is preferably a curable compound that can be cured by mixing with the curing agent. The curable compound that can be cured by mixing with the curing agent may be a thermosetting compound or may not be a thermosetting compound. The curable compound that can be cured by mixing with the curing agent may be, for example, a curable compound that can be cured at 0°C or lower by mixing with the curing agent.
[0045] Examples of the curable compound include an epoxy compound, a polyol compound, a silicone compound, a phenol compound, a vinyl ester compound, and a naphthoxazine compound. From the viewpoint of more effectively increasing the strength of the filled portion after curing, the curable compound is preferably an epoxy compound.
[0046] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, water-added bisphenol A type epoxy compounds, dimer acid modified bisphenol A type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, naphthalene type epoxy compounds, biphenyl type epoxy compounds, dimer acid type epoxy compounds, triepoxypropyl isocyanurate (triglycidyl isocyanurate), hydantoin epoxy compounds, aliphatic epoxy compounds, dicyclocyclic type epoxy compounds, glycidyl ether type epoxy compounds, glycidyl ester type epoxy compounds, and glycidyl amine type epoxy compounds.
[0047] In order to more effectively exert the effects of the present invention, the epoxy compound is preferably a bisphenol A type epoxy compound or a bisphenol F type epoxy compound.
[0048] Examples of the polyol compound include bisphenol A, bisphenol F, phenol novolac, cresol novolac, cyclohexanediol, methylcyclohexanediol, isophoronediol, dicyclohexylmethanediol, dimethyldicyclohexylmethanediol, ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, polyester polyol, polyether polyol, a polymer obtained by dehydration condensation of a polybasic acid and a polyhydric alcohol, and a polymer obtained by ring-opening polymerization of a lactone such as ε-caprolactone or α-methyl-ε-caprolactone.
[0049] In order to more effectively exert the effects of the present invention, the polyol compound is preferably a polyester polyol or a polyether polyol.
[0050] The silicone compound may be an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms. The main chain of the organopolysiloxane is generally a diorganosiloxane polymer structure, but may have a partially branched structure or a cyclic structure. The alkenyl group of the organopolysiloxane may be a vinyl group, a 1-propenyl group, a 2-propenyl group, an isopropenyl group, a butenyl group, a 1-methyl-2-propenyl group, a petenyl group, a hexenyl group, an octenyl group, and a cyclohexenyl group.
[0051] Examples of the phenol compound include novolac type phenols, biphenol type phenols, naphthalene type phenols, dicyclopentadiene type phenols, aralkyl type phenols, and dicyclopentadiene type phenols.
[0052] Examples of the vinyl ester compound include a reaction product of an epoxy compound and an unsaturated monobasic acid. Examples of the epoxy compound include aliphatic glycidyl ethers such as bisphenol A diglycidyl ether and its high molecular weight homologues, novolac-type polyglycidyl ether and its high molecular weight homologues, and 1,6-hexanediol diglycidyl ether. Examples of the unsaturated monobasic acid include acrylic acid and methacrylic acid. Examples of the reaction product of the epoxy compound with the acrylic acid and the methacrylic acid include epoxy (meth)acrylate.
[0053] When the first composition contains the vinyl ester compound, the first composition may contain a radical polymerizable unsaturated monomer. The radical polymerizable unsaturated monomer may be a styrene monomer, an α-, o-, m-, p-alkyl, nitro, cyano, amide, or ester derivative of styrene, a styrene-based monomer such as chlorostyrene, vinyltoluene, or divinylbenzene, a diene such as butadiene, 2,3-dimethylbutadiene, isoprene, or chloroprene; an ethyl (meth)acrylate, a methyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, or a methacrylate-based monomer such as methyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, or a methacrylate-based monomer such as methyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, or a methacrylate-based monomer such as methyl (meth)acrylate, ethyl (meth)acrylate, ... (meth)acrylic acid esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofuryl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate; (meth)acrylic acid amides such as (meth)acrylic acid amide and (meth)acrylic acid N,N-dimethylamide; vinyl compounds such as (meth)acrylic acid anilide; unsaturated dicarboxylic acid diesters such as diethyl citraconic acid; monomaleimide compounds such as N-phenylmaleimide; and N-(meth)acryloylphthalimide.
[0054] In addition, when the first composition contains the vinyl ester compound, it is preferable that the first composition contains the vinyl ester compound and the radically polymerizable unsaturated monomer.
[0055] In 100% by weight of the first composition, the content of the curable compound is preferably 1% by weight or more, more preferably 10% by weight or more, even more preferably 50% by weight or more, and preferably 100% by weight or less, more preferably 90% by weight or less, even more preferably 75% by weight or less. When the content of the curable compound is equal to or more than the lower limit and equal to or less than the upper limit, the initial strength of the filled portion can be further increased. In addition, when the first composition contains the compound X, the content of the curable compound in 100% by weight of the first composition is less than 100% by weight.
[0056] In the total weight of the first composition and the first container (100% by weight), the content of the first composition is preferably 10% by weight or more, more preferably 30% by weight or more, and even more preferably 50% by weight or more, and is preferably 95% by weight or less, more preferably 90% by weight or less, and even more preferably 85% by weight or less. When the content of the first composition is equal to or more than the lower limit and equal to or less than the upper limit, the first composition and the second composition can be mixed well.
[0057] The first composition may contain components other than the curable compound as necessary. The components other than the curable compound contained in the first composition include antioxidants, low shrinkage agents, viscosity adjusters, and colorants. Only one type of component other than the curable compound may be used, or two or more types may be used in combination.
[0058] <Second Composition> The second composition includes a curing agent. The second composition may include only the curing agent. The second composition may be the curing agent. The content of the curable compound in 100% by weight of the second composition is preferably less than the content of the curable compound in 100% by weight of the first composition, and the second composition preferably does not include a curable compound.
[0059] When the first composition contains an epoxy compound, the second composition preferably contains an epoxy curing agent. A cured product of the epoxy resin can be obtained by reacting the epoxy compound with the epoxy curing agent.
[0060] The curing agent for the epoxy compound (epoxy curing agent) may include an amine compound, an imidazole compound, an amide compound, a cyano compound, an acid anhydride, etc. The amine compound may include ethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine, amine adducts thereof, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, etc. Examples of the imidazole compound include methylimidazole, 2-ethyl-4-methylimidazole, 1-isobutyl-2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, ethylimidazole, isopropylimidazole, 2,4-dimethylimidazole, phenylimidazole, undecylimidazole, heptadecylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Examples of the amide compound include polyamide. Examples of the cyano compound include dicyandiamide. Examples of the acid anhydride include maleic anhydride and its compounds, phthalic anhydride and its compounds, and the like.
[0061] In order to more effectively exert the effects of the present invention, the epoxy curing agent is preferably an amine-based curing agent (amine compound) or an acid-based curing agent.
[0062] The compounding ratio of the epoxy compound and the epoxy curing agent can be appropriately changed depending on the combination of the types of epoxy compound and epoxy curing agent. The compounding ratio of the epoxy compound and the epoxy curing agent can be set, for example, based on the epoxy equivalent (active hydrogen equivalent). The content of the epoxy curing agent relative to 100 parts by weight of the epoxy compound is preferably 10 parts by weight or more, more preferably 20 parts by weight or more, preferably 120 parts by weight or less, more preferably 100 parts by weight or less.
[0063] When the first composition contains a polyol compound, it is preferred that the second composition contains a curing agent for the polyol compound.
[0064] The curing agent for the polyol compound includes a polyisocyanate compound. The polyol compound and the polyisocyanate compound are cured to obtain a urethane resin. The polyisocyanate compound includes an aromatic polyisocyanate, an alicyclic polyisocyanate, and an aliphatic polyisocyanate. The aromatic polyisocyanate includes phenylene diisocyanate, toluene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate. The alicyclic polyisocyanate includes cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and dimethyldicyclohexylmethane diisocyanate. Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.
[0065] From the viewpoint of exerting the effects of the present invention more effectively, the curing agent for the polyol compound (polyisocyanate compound) is preferably diphenylmethane diisocyanate or toluene diisocyanate.
[0066] The mixing ratio of the polyol compound and the polyisocyanate compound can be appropriately changed depending on the combination of the types of the polyol compound and the polyisocyanate compound. The mixing amount of the polyisocyanate compound is preferably an amount such that the amount of hydroxyl groups of the polyol compound is equal to the amount of isocyanate groups (NCO amount) of the polyisocyanate compound.
[0067] The curing agent (crosslinking agent) for the silicone compound may be, for example, an organohydrogenpolysiloxane having two or more SiH groups. Examples of the organohydrogenpolysiloxane include phenylmethylhydrogenpolysiloxane, 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, methylhydrogenpolysiloxane blocked at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with trimethylsiloxy groups, dimethylpolysiloxane blocked at both ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with dimethylhydrogensiloxane, methylhydrogensiloxane-diphenylsiloxane copolymer blocked at both ends with trimethylsiloxy groups, and methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer blocked at both ends with trimethylsiloxy groups.
[0068] Examples of the phenol compound hardener include hexamethylenetetramine and paraformaldehyde.
[0069] Examples of the curing agent for the vinyl ester compound include organic peroxides, such as ketone peroxides, perbenzoates, hydroperoxides, diacyl peroxides, peroxyketals, hydroperoxides, diallyl peroxides, peroxyesters, and peroxydicarbonates.
[0070] In 100% by weight of the second composition, the content of the curing agent is preferably 10% by weight or more, more preferably 50% by weight or more, and preferably 100% by weight or less, more preferably 75% by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the initial strength of the filled portion can be further increased. In addition, when the second composition contains the compound X, the content of the curing agent in 100% by weight of the second composition is less than 100% by weight.
[0071] In the total 100% by weight of the second composition and the second container, the content of the second composition is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, and is preferably 95% by weight or less, more preferably 90% by weight or less, even more preferably 85% by weight or less. When the content of the second composition is equal to or more than the lower limit and equal to or less than the upper limit, the first composition and the second composition can be mixed well.
[0072] From the viewpoint of more effectively curing the mixture of the first composition and the second composition, the content of the curing agent in the filler is preferably equal to the reaction part number equivalent.
[0073] The second composition may contain components other than the curing agent as necessary. Examples of the components other than the curing agent contained in the second composition include a crosslinking agent and a water absorbing agent. Only one type of the components other than the curing agent may be used, or two or more types may be used in combination.
[0074] <Compound capable of releasing carbonate ions or calcium ions (Compound X)> In the filler, at least one of the first composition and the second composition contains a compound capable of releasing carbonate ions or calcium ions (compound X). In this case, the compound X may be contained in the first composition, the second composition, or both the first composition and the second composition.
[0075] The compound X may be a compound capable of releasing carbonate ions, a compound capable of releasing calcium ions, a compound capable of releasing both carbonate ions and calcium ions, or a mixture of a compound capable of releasing carbonate ions and a compound capable of releasing calcium ions. The compound X may be in the form of particles. The compound X may be used alone or in combination of two or more kinds.
[0076] Examples of the compound capable of releasing carbonate ions include carbonates and hydrogen carbonates. Examples of the carbonates include ammonium carbonate, potassium carbonate, sodium carbonate, barium carbonate, magnesium carbonate, lithium carbonate, copper (II) carbonate, iron (II) carbonate, and silver (I) carbonate. Examples of the hydrogen carbonates include ammonium hydrogen carbonate, potassium hydrogen carbonate, calcium hydrogen carbonate, and sodium hydrogen carbonate.
[0077] Examples of the compound capable of releasing calcium ions include tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydrogen carbonate, calcium hydroxide, calcium oxide, and calcium sulfate.
[0078] An example of the compound capable of releasing both carbonate ions and calcium ions is calcium hydrogen carbonate.
[0079] The compound X is preferably tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium sulfate, calcium carbonate, calcium hydrogen carbonate, sodium carbonate, or sodium hydrogen carbonate. The compound X is more preferably calcium carbonate, calcium hydrogen carbonate, sodium carbonate, or sodium hydrogen carbonate. In this case, the effect of the present invention can be more effectively exhibited.
[0080] The compound X may be an inclusion of a microcapsule. The filler may include a microcapsule containing the compound X as an inclusion. In the filler, at least one of the first composition and the second composition may include a microcapsule containing the compound X as an inclusion. When the compound X is an inclusion of a microcapsule, the timing and amount of carbonate ions or calcium ions released from the compound X can be controlled.
[0081] The microcapsules are preferably capable of releasing the compound X. Examples of the microcapsules include physically destructible capsules, meltable capsules, and water-soluble capsules. Examples of the material of the physically destructible capsules include glass and plastic. Examples of the material of the meltable capsules include low molecular weight polyethylene wax, styrene-butadiene copolymers, and styrene-isoprene copolymers. When the water-soluble capsules come into contact with moisture, the membrane that constitutes the microcapsules collapses. Examples of the material of the water-soluble capsules include hydrolyzable ethyl cellulose, proteins such as gelatin, alginic acid, starch, polylactic acid, polybutylene succinate, polyvinyl alcohol, and sodium polyacrylate.
[0082] From the viewpoint of better controlling the timing and amount of carbonate ions or calcium ions released from compound X, the microcapsules are preferably water-soluble.
[0083] The content of the compound X is preferably 20 parts by weight or more, more preferably 50 parts by weight or more, and preferably 300 parts by weight or less, more preferably 200 parts by weight or less, based on 100 parts by weight of the curable compound. When the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, carbonate ions or calcium ions are released more effectively, and calcium carbonate is produced well. When the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, the strength of the filled area can be further increased.
[0084] The content of the compound X is preferably 20 parts by weight or more, more preferably 50 parts by weight or more, and preferably 300 parts by weight or less, more preferably 200 parts by weight or less, based on 100 parts by weight of the total of the curable compound and the curing agent. When the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, carbonate ions or calcium ions are released more effectively, and calcium carbonate is produced well. When the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, the strength of the filled area can be further increased.
[0085] In the total of 100% by weight of the first composition and the second composition, the content of the compound X is preferably 20% by weight or more, more preferably 50% by weight or more, and preferably 300% by weight or less, more preferably 200% by weight or less. When the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, carbonate ions or calcium ions are released more effectively, and calcium carbonate is produced well. In addition, when the content of the compound X is equal to or more than the lower limit and equal to or less than the upper limit, the strength of the filled area can be further increased.
[0086] <First container and second container> The packing material according to the present invention includes a first container and a second container. The first composition is sealed in the first container. The second composition is sealed in the second container.
[0087] The material of the first container (wall of the first container, the first container body, the lid of the first container) and the material of the second container (wall of the second container, the second container body, the lid of the second container) may be an organic material or an inorganic material. The materials of the first container and the second container may be the same or different.
[0088] Examples of the material of the first container and the second container include glass and resin. Examples of the resin include thermoplastic resin. The first container and the second container may be containers that can be broken by physical or chemical action.
[0089] The first container and the second container may each be a physically destructible container, a meltable container, a water-soluble container, or the like. The material of the physically destructible container may be glass, plastic, or the like. The material of the meltable container may be low molecular weight polyethylene wax, styrene-butadiene copolymer, styrene-isoprene copolymer, or the like. The wall of the water-soluble container disintegrates when it comes into contact with moisture. The material of the water-soluble container may be hydrolyzable ethyl cellulose, proteins such as gelatin, alginic acid, starch, polylactic acid, polyvinyl alcohol, sodium polyacrylate, or the like.
[0090] From the viewpoint of breaking the containers more easily, the material of the first container and the material of the second container are preferably water-soluble. From the viewpoint of breaking the containers more easily, the material of the wall of the first container and the material of the wall of the second container are preferably water-soluble.
[0091] The shape of the first container is not particularly limited. The outer shape of the first container and the second container may be rectangular, spherical, pyramidal, conical, prismatic, or cylindrical. The shapes of the first container and the second container may be the same or different. From the viewpoint of further improving workability, the outer shape of the first container and the second container is preferably spherical or rectangular.
[0092] The internal volume of the first container and the internal volume of the second container are each preferably 1 cc or more, more preferably 10 cc or more, and even more preferably 50 cc or more, and are preferably 10,000 cc or less, more preferably 5,000 cc or less, and even more preferably 1,000 cc or less. The internal volume of the first container and the internal volume of the second container may be 500 cc or less, or may be 100 cc or less. When the internal volumes of the containers are equal to or more than the lower limit and equal to or less than the upper limit, the workability can be further improved.
[0093] The thickness of the wall of the first container and the thickness of the wall of the second container are preferably 0.01 mm or more, more preferably 0.1 mm or more, and preferably 3 mm or less, more preferably 1 mm or less. When the thickness of the wall is equal to or greater than the lower limit, unintended breakage of the first container and the second container can be suppressed. When the thickness of the wall is equal to or less than the upper limit, the first container and the second container can be easily broken at a desired timing.
[0094] (Method of filling with filler) The filler can be filled into voids in structures, ground, etc. The filler can be used to repair structures, ground, etc. The filler can be suitably used as a repair agent for structures, ground, etc.
[0095] The method for filling the filler preferably includes a step of injecting the filler into the filling location (filling step), and a step of mixing and hardening the first composition and the second composition by destroying the first container and the second container (hardening step).
[0096] In the filling step, the first composition, the second composition, the first container, and the second container are filled into the filling location. Before filling, the first composition and the second composition are not taken out of the first container and the second container, respectively.
[0097] The method of injecting the filler is not particularly limited, and examples thereof include a method of directly injecting the filler into the filling area, a method of drilling from the surface of the structure and ground toward the cracked or junk part to form an injection port and injecting the filler from the injection port, etc. If there is a void inside the structure, or if the cracks reach deep inside the structure, it is preferable to form an injection port in the structure and inject the filler from the injection port. Also, the injection amount of the filler can be appropriately changed depending on the size of the area to be filled, etc.
[0098] The pressure when injecting the filler can be appropriately changed depending on the viscosity of the filler, the size of the portion to be filled, etc. The filler may be injected into the cracked portion or the junk portion at high pressure or low pressure. The pressure when injecting at high pressure is preferably 0.5 MPa or more, preferably 24 MPa or less. The pressure when injecting at low pressure is preferably 0.01 MPa or more, preferably 0.5 MPa or less. The filler can be filled at low pressure because it can suppress the thickening of the curable compound and the curing agent due to the curing reaction before filling. From the viewpoint of shortening the working time and injecting the filler well to the depth of the void, the pressure when injecting the filler is preferably 0.5 MPa or more, preferably 24 MPa or less.
[0099] The above-mentioned filling point is preferably a filling point of a structure or a filling point of the ground.
[0100] In the step of mixing the first composition and the second composition, it is preferable to mix the first composition and the second composition by destroying the first container and the second container by a physical action or a chemical action. Examples of the physical action include impact, etc. Examples of the chemical action include melting the container and dissolving the container in water, etc.
[0101] In the step of mixing the first composition and the second composition, it is preferable to mix the first composition and the second composition by breaking the first container and the second container with a stirrer.
[0102] The first container and the second container do not have to be completely destroyed. The first container and the second container may be burned or may remain after mixing and hardening of the filler. The stirrer may be removed or may remain after mixing and hardening of the filler.
[0103] The conditions for curing the filler can be appropriately changed depending on the type of curable compound, etc.
[0104] FIG. 3 is a cross-sectional view for explaining the filling method of the filler according to the first embodiment of the present invention.
[0105] The structure 100 is a concrete structure. A crack 102 has occurred in a wall surface 101 of the structure 100.
[0106] The filler supplying device 50 includes an injection gun 51 and a tank 52. The tank 52 is filled with the filler.
[0107] First, a hole is drilled at a specified angle from an uncracked portion of the wall surface 101 toward the crack 102 to form an injection port 104. Next, an injection plug 21 with a check valve is attached to the injection port 104. The injection plug 21 is connected to an injection gun 51. Next, a compressor is used to inject a filler into the crack 102, and the filler is left to cure until it hardens. In this manner, the structure can be repaired. The above-mentioned filler can be used as a repair agent.
[0108] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0109] First composition: First base agent (curable compound; epoxy compound): "Infraguard CRJM base agent" manufactured by Sekisui Chemical Co., Ltd. (epoxy compound content: 100% by weight) Second hardener (epoxy hardener) as second composition: "Infraguard CRJM Hardener" manufactured by Sekisui Chemical Co., Ltd. (epoxy hardener content: 100% by weight)
[0110] Compound X: Compound capable of releasing calcium: Calcium chloride Compounds capable of releasing carbonate ions: Sodium bicarbonate
[0111] First container and second container (Takamiya Sangyo "egg-shaped capsule", made of polystyrene, wall thickness approximately 500 μm, internal volume 66 cc)
[0112] Example 1 (1) Preparation of filling material The first main agent and calcium chloride were enclosed in the first container, and the capsule was closed to obtain a first container containing a first composition. The first composition contains the first main agent and calcium chloride.
[0113] The second container was filled with a second hardening agent and sodium bicarbonate, and the capsule was closed to obtain a second container filled with a second composition. The second composition includes the second hardening agent and sodium bicarbonate.
[0114] In this way, a filler having a first container in which the first composition is enclosed and a second container in which the second composition is enclosed as a set was obtained. In the obtained filler, the contents of the curing agent and compound X were as shown in Table 1, when the curable compound was taken as 100 parts by weight.
[0115] (2) Filling with filler A 75 mm diameter through hole was drilled on one side of a sandstone block (200 mm wide x 200 mm deep x 200 mm high), and one of the openings was surface-painted with FRP (fiber-reinforced plastic) to create a filling block with a void and one opening.
[0116] The resulting eight sets of filler were poured into the opening of the filling block, and then the first and second containers were broken with a steel stirring rod, the first composition and the second composition were stirred and mixed, and the mixture was allowed to harden to obtain a repaired block.
[0117] (Examples 2 to 5) (1) Preparation of filling material A filler was obtained in the same manner as in Example 1, except that the types and amounts of the blended components were changed as shown in Table 1.
[0118] (2) Filling with filler In the same manner as in Example 1, the filler was filled to obtain a repaired block.
[0119] Comparative Example 1 (1) Preparation of filling material A filler was obtained in the same manner as in Example 1, except that the types and amounts of the blended components were changed as shown in Table 1.
[0120] In Comparative Example 1, compound X was not used.
[0121] (2) Filling with filler In the same manner as in Example 1, the filler was filled to obtain a repaired block.
[0122] Comparative Example 2 (1) Preparation of filling material The first composition was obtained by blending the first main component and calcium chloride. The first composition contains the first main component and calcium chloride.
[0123] The second hardening agent and sodium bicarbonate were mixed to obtain a second composition. The second composition contains the second hardening agent and sodium bicarbonate.
[0124] In this way, a filler containing the first composition and the second composition as a set was obtained. In the obtained filler, when the curable compound was taken as 100 parts by weight, the contents of the curing agent and compound X were as shown in Table 1.
[0125] In Comparative Example 2, no container was used as the filler (the substance filled into the filling target).
[0126] (2) Filling with filler The same filling block as in Example 1 was prepared.
[0127] The first composition and the second composition were premixed. The filler (mixture) was injected through the opening of the filling block. The mixture was then cured to obtain a repaired block.
[0128] Comparative Example 3 (1) Preparation of filling material The same filler as in Comparative Example 2 was prepared.
[0129] In Comparative Example 3, no container was used as the filler (the substance filled into the filling target).
[0130] (2) Filling with filler The same filling block as in Example 1 was prepared.
[0131] The first and second compositions of the filler obtained were each injected from the opening of the filling block. During the injection, the first and second compositions were mixed. Next, the mixture was hardened to obtain a repaired block.
[0132] (evaluation) (1) Workability In filling the above-mentioned filler, the workability was evaluated according to the following criteria.
[0133] [Workability criteria] ○: Immediately after the start of filling, contact between the curable compound and the curing agent is prevented, curing does not progress, and filling properties are excellent. ×: The curable compound and the curing agent are in contact with each other before or immediately after the start of filling, so curing proceeds and filling properties are poor.
[0134] (2) Immersion test (calcium carbonate formation) The repaired blocks obtained in Examples 1 and 2 and Comparative Examples 1 to 3 were immersed in distilled water. The repaired blocks obtained in Examples 3 and 4 were immersed in a 3000 ppm aqueous solution of sodium bicarbonate. The repaired block obtained in Example 5 was immersed in a 4 wt % aqueous solution of calcium chloride. After 720 hours of immersion, each repaired block was taken out and the surface condition of the filled area was observed to confirm whether calcium carbonate had been generated.
[0135] [Criteria for determining calcium carbonate formation] ○: In the repaired block, calcium carbonate particles are precipitated on the entire surface of the sandstone block. △: In the repaired block, calcium carbonate particles are partially precipitated on the surface of the sandstone block. ×: No calcium carbonate particles were precipitated on the surface of the sandstone block in the repaired block.
[0136] The filler compositions and results are shown in Table 1 below.
[0137] [Table 1]
[0138] In Examples 1 to 5, the surfaces of the test samples were cloudy from the early stage of immersion. When the repaired blocks obtained in Examples 1 to 5 were observed in detail 720 hours after immersion, calcium carbonate particles were found to have precipitated over the entire surface of the sandstone block. Calcium carbonate particles were also found to have precipitated sufficiently in pores away from the filling section. When the surface of this repaired block was observed with a scanning electron microscope, aggregates of calcium carbonate particles with a dense crystal structure (calcite structure of calcium carbonate) were confirmed.
[0139] Detailed observation of the repaired blocks obtained in Comparative Examples 2 and 3 after 720 hours of immersion revealed that calcium carbonate particles had partially precipitated on the surface of the sandstone blocks. In pores away from the filled area, there was very little calcium carbonate particle precipitation. This is thought to be because the hardening compound and the hardener were in contact with each other before the start of filling in Comparative Example 2, and immediately after the start of filling in Comparative Example 3, and the hardening reaction proceeded, causing thickening or separation, preventing the filler from reaching the pores. [Explanation of symbols]
[0140] 1,1A…Filling material 11, 11A...First composition 12, 12A...Second composition 13, 13A...First container 13Aa…First container body 13Ab…Lid 14, 14A...Second container 14Aa...Second container body 14Ab…Lid 15A…Joint material 21…Injection plug 50…Feeding device 51...Injection gun 52…Tank 100...Structure 101...Wall 102...Crack 104…Inlet
Claims
1. A first composition, a second composition, a first container, and a second container, The first composition is enclosed in the first container, The second composition is enclosed in the second container, the first composition comprises a curable compound; the curable compound is an epoxy compound, the second composition comprises a curing agent; A filling material, wherein at least one of the first composition and the second composition comprises a compound capable of releasing carbonate ions or calcium ions.
2. A filling material as described in claim 1, wherein at least one of the first composition and the second composition contains a compound capable of releasing calcium ions.
3. 2. The filler of claim 1, wherein the compound capable of releasing carbonate ions or calcium ions is tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium sulfate, calcium carbonate, calcium bicarbonate, sodium carbonate, or sodium bicarbonate.
4. The filler according to any one of claims 1 to 3, wherein the thickness of the wall of the first container and the thickness of the wall of the second container are each 50 µm or more and 2000 µm or less.
5. The filling material according to any one of claims 1 to 4, wherein the wall material of the first container and the wall material of the second container are each water-soluble.
6. The filler according to any one of claims 1 to 5, wherein the internal volume of the first container and the internal volume of the second container are each 1 cc or more and 10,000 cc or less.
7. A step of injecting the filler according to any one of claims 1 to 6 into a filling location; and a step of mixing and hardening the first composition and the second composition by destroying the first container and the second container.
8. The method for filling a filler according to claim 7, wherein the filling location is a filling location of a structure or a filling location of the ground.
Citation Information
Patent Citations
Hand operated injection device
JP1991081454A
Filler and filling using the same
JP1998060410A
Method for reinforcing concrete structure
JP2003013612A
Injection material injecting method for concrete structure, and injection material used therefor
JP2015030987A
Bio-based restoration method for concrete
JP2016525879A