Particulate material and its manufacturing method, dielectric material, slurry composition and resin composition
By producing spherically shaped titanium dioxide particles with controlled size and surface treatment, the issues of insufficient filling rates and dielectric properties in conventional methods are addressed, resulting in high-performance dielectric materials for thin film capacitors.
Patent Information
- Application Number
- JP2020020838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-02-10
AI Technical Summary
Conventional methods for producing titanium dioxide particles result in aggregates with large particle sizes and irregular shapes, leading to insufficient filling rates and poor dielectric properties when used in thin film capacitors, while smaller particles fail to achieve satisfactory dielectric properties due to aggregation issues.
The production of titanium dioxide particles with controlled sphericity, size, and surface treatment, such as silica coating, to enhance dispersibility and electrical properties, along with a slurry and resin composition for improved application in dielectric materials.
The resulting particles exhibit excellent electrical properties and improved filling rates, enabling high-performance dielectric materials suitable for thin film capacitors.
Smart Images

Figure 0007560254000004 
Figure 0007560254000005 
Figure 0007560254000006
Abstract
Description
[Technical Field]
[0001] The present invention relates to a particulate material made of titanium dioxide, a method for producing the same, a dielectric material, a slurry composition, and a resin composition. [Background technology]
[0002] Conventional particulate materials made of titanium dioxide with high sphericity and close to monodispersion have been produced by a method in which titanium dioxide powder is melted by being introduced into a flame and then rapidly cooled, by a method in which titanium dioxide is produced by subjecting titanium tetrachloride gas to an oxidation reaction or from titanium alkoxide by a sol-gel method, or by calcining titanium dioxide and then pulverizing it.
[0003] An example of a manufacturing method using titanium tetrachloride as a raw material is disclosed in Patent Document 1. According to Example 1 of Patent Document 1, titanium dioxide obtained from titanium tetrachloride gas is an aggregate having a BET-equivalent particle diameter of 300 nm and an average particle diameter of 0.6 μm as measured by laser particle size analysis. The particle material made of titanium dioxide obtained by heating and melting such an aggregate has an average particle diameter far exceeding 10 μm.
[0004] Recently, development of a thin-film capacitor, which uses particulate dielectric materials in thin layers of sealing materials and the like to provide capacitor functionality, has been progressing (see, for example, Patent Documents 2 and 3). Aiming to realize this thin-film capacitor, attempts were made to create a film with a thickness of 20 to 50 μm using a resin composition in which particulate titanium oxide, as described in Patent Document 1, is dispersed in a resin material. However, satisfactory dielectric properties could not be achieved because a sufficient packing density could not be achieved with a particulate material consisting of aggregates of small primary particles with a particle diameter of approximately 300 nm. Other particle size distributions include large particulate materials with particle diameters of 10 μm or more. However, while a sufficient packing density could be achieved with these large particulate materials, it was difficult to process them into a film of this thickness. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2008-273832 [Patent Document 2] International Publication No. 2016 / 158228 [Patent Document 3] Japanese Patent Application Laid-Open No. 2016-111182 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention was completed in view of the above circumstances, and aims to solve the problem of providing a particulate material made of titanium dioxide of submicron to micron order, a method for producing the same, a dielectric material, a slurry composition, and a resin composition. [Means for solving the problem]
[0007] (1) The particulate material of the present invention that solves the above-mentioned problems is a particulate material made of titanium dioxide having a volume average particle diameter of 0.3 to 20 μm, a sphericity of 0.9 or more, a moisture content of 0.5 mass% or less, and a linseed oil absorption of 0.25 mL / g or less. In particular, when the extract is stirred and suspended at a concentration of 3.5 g / 35 mL at 20°C for 30 minutes and then separated into solid and liquid, the EC is 40 μS / cm or less, the chloride ion concentration is 100 ppm or less, and the sodium ion concentration is 30 ppm or less, which enables the material to exhibit excellent electrical properties when used in electronic materials.
[0008] Furthermore, a silica layer is formed on the surface, and the FT-IR spectrum shows a peak at 3730-3770 cm -1 By coating the surface with silica, chemical stability can be improved, and the presence of OH groups makes it easy to perform surface treatments to improve affinity with resin materials and the like.
[0009] The surfaces of the particulate material are preferably treated with a silane compound.
[0010] (2) The method for producing a particulate material of the present invention, which solves the above-mentioned problems, is a method for producing a particulate material as described in (1) above, and includes a deflagration step in which raw particulate material made of metallic titanium is suspended in a carrier and introduced into a high-temperature oxidizing atmosphere to be combusted. In particular, it is preferable to have a silica coating step in which a tetraalkoxysilane compound is attached to the surface and heated after the deflagration step.
[0011] (3) The dielectric material of the present invention, which solves the above problems, comprises the particulate material described in (1) above.
[0012] (4) The slurry composition of the present invention that solves the above problems comprises the particulate material described in (1) and an organic solvent that disperses the particulate material.
[0013] (5) The resin composition of the present invention, which solves the above problems, comprises the particulate material described in (1) and a resin material for dispersing the particulate material. [Effects of the Invention]
[0014] The particulate material of the present invention can be suitably used as a dielectric material by having the particle size, sphericity, moisture content and linseed oil absorption within the above-mentioned ranges. [Brief explanation of the drawings]
[0015] [Figure 1] FIG. 2 is a graph showing the particle size distribution of the particulate material of Example 1. [Figure 2] FIG. 10 is a graph showing the particle size distribution of the particulate material of Example 2. [Figure 3] FIG. 10 is a graph showing the particle size distribution of the particulate material of Example 3. [Figure 4] FIG. 10 is a graph showing the particle size distribution of the particulate material of Example 4. [Figure 5] FIG. 10 is a graph showing the particle size distribution of the particulate material of Example 5. [Figure 6]1 is an XRD spectrum of the particulate material of Example 1. [Figure 7] 1 is an XRD spectrum of the particulate material of Example 2. [Figure 8] 1 is an XRD spectrum of the particulate material of Example 3. [Figure 9] 1 is an XRD spectrum of the particulate material of Example 4. [Figure 10] 1 is an SEM photograph of the particulate material of Example 1. [Figure 11] FIG. 1 is an SEM photograph of the particulate material of Example 2. [Figure 12] FIG. 1 is an SEM photograph of the particulate material of Example 3. [Figure 13] 1 is an SEM photograph of the particulate material of Example 4. [Figure 14] 1 is an SEM photograph of the particulate material of Comparative Example 1. [Figure 15] FIG. 1 is an SEM photograph of the particulate material of Comparative Example 2. [Figure 16] 1 is an FT-IR spectrum of the particulate material of Example 1. DETAILED DESCRIPTION OF THE INVENTION
[0016] The particulate material and its manufacturing method, dielectric material, slurry composition, and resin composition of the present invention will be described in detail below based on the following embodiments.
[0017] (particle material) The particulate material of this embodiment is made of titanium dioxide. "Made of titanium dioxide" means that the titanium dioxide content, based on the mass of each particle constituting the particulate material, is 50% or more, preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, particularly preferably 90% or more, and most preferably 100% or more. Titanium dioxide is a preferred material as a dielectric material, and a relatively high content is preferable. However, even if a small amount of material other than titanium dioxide is mixed, sufficient performance can be achieved, and the mixed material may impart desirable properties. The crystalline structure of titanium dioxide is not particularly limited, but preferably includes an anatase type.
[0018] The particulate material of this embodiment has a volume average particle diameter of 0.3 to 20 μm. Preferred lower limit values include 0.3 μm, 0.5 μm, 0.7 μm, and 1.0 μm, and preferred upper limit values include 20 μm, 10 μm, 7 μm, and 3 μm. These lower and upper limit values can be arbitrarily combined. A larger volume average particle diameter improves the performance as a dielectric material, while a smaller volume average particle diameter makes it easier to incorporate into thin films.
[0019] The particulate material of this embodiment has a sphericity of 0.90 or more, preferably 0.95 or more, more preferably 0.98 or more, and even more preferably 0.99 or more. A higher sphericity reduces the viscosity when dispersed in an organic solvent or resin material, thereby improving fluidity.
[0020] The particulate material of this embodiment has a moisture content of 0.5% by mass or less, preferably 0.4% by mass or less, more preferably 0.3% by mass or less, even more preferably 0.25% by mass or less, and particularly preferably 0.2% by mass or less. By reducing the moisture content, the dielectric loss tangent can be reduced, and as a result, the performance as a dielectric material can be improved.
[0021] The particulate material of this embodiment has a linseed oil absorption of 0.25 mL / g or less, more preferably 0.20 mL / g or less, even more preferably 0.18 mL / g or less, and particularly preferably 0.15 mL / g or less. The lower the linseed oil absorption, the higher the packing rate of the particulate material, improving its performance as a dielectric material. To reduce the linseed oil absorption, adding a particulate material with a relatively small particle size that can enter the gaps between particulate materials with particle sizes close to monodisperse can improve the overall packing rate. In other words, using a particulate material with two particle size peaks can improve packing. For example, the particle size of the smaller of the two peaks is preferably 40% or less, and more preferably 30% or less, of the particle size of the larger peak.
[0022] The particulate material of this embodiment preferably has a silica layer made of silica on its surface. The thickness of the silica layer is preferably 1 nm to 50 nm, with the lower limit preferably being 1 nm or 3 nm and the upper limit preferably being 50 nm or 30 nm. These lower and upper limits can be arbitrarily combined. Furthermore, the mass of the silica layer is preferably about 0.01% to 1% based on the total mass. The lower limit preferably being 0.02% or 0.05%, and the upper limit preferably being 0.80% or 0.70%. These lower and upper limits can be arbitrarily combined. It is preferable that OH groups are present on the surface of the silica layer. In particular, in the FT-IR spectrum, a peak at 3730-3770 cm -1 It is preferable that the silica layer covers the surface without any gaps. For example, it is preferable that the silica layer covers 50% or more of the area of the entire surface, more preferably 70% or more, even more preferably 90% or more, and particularly preferably 100%.
[0023] The particle material of this embodiment is preferably surface-treated with a surface treatment agent. A silane compound is preferred as the surface treatment agent. A compound having an organic functional group is preferred as the silane compound. Alternatively, silazanes having an organic functional group, such as hexamethyldisilazane, can also be used. A silane coupling agent can also be used. Examples of organic functional groups that the silane compound can have include alkyl groups (having 1 to 10 carbon atoms), phenyl groups, vinyl groups, epoxy groups, phenylamino groups, amino groups, acrylic groups, methacrylic groups, and styryl groups. The number of organic functional groups introduced per silane compound molecule is not particularly limited, but it is preferred to introduce organic functional groups into one to three of the four bonds of the Si atom. The amount of the surface treatment agent to be reacted can be 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100% of the number of OH groups present on the surface.
[0024] The particulate material of this embodiment is preferably suspended at a concentration of 3.5 g / 35 mL under stirring at 20°C for 30 minutes, and the resulting extract after solid-liquid separation has an EC of 40 μS / cm or less, a chloride ion concentration of 100 ppm or less, and a sodium ion concentration of 30 ppm or less. The upper limit of the EC value can be 35 μS / cm or less, 30 μS / cm or less, or 20 μS / cm or less. The upper limit of the chloride ion concentration can be 80 ppm or less, 50 ppm or less, 30 ppm or less, 20 ppm or less, or 5 ppm or less. The upper limit of the sodium ion concentration can be 25 ppm or less, 20 ppm or less, 15 ppm or less, 10 ppm or less, or 5 ppm or less. By controlling the EC value, chloride ion concentration, and sodium ion concentration within the above ranges, the material can be suitably used for applications such as semiconductor encapsulation.
[0025] (Method of manufacturing particulate material) The method for producing a particulate material of this embodiment is a method that can suitably produce the particulate material of this embodiment described above. The production method of this embodiment includes a deflagration step in which raw particulate material made of metallic titanium is suspended in a carrier and introduced into a high-temperature oxidizing atmosphere to be combusted. In the deflagration step, the raw particulate material is introduced into an oxidizing atmosphere heated to a high temperature by flame, plasma, arc discharge, laser, or the like, whereby the metallic titanium constituting the raw particulate material is oxidized to form an oxide gas.
[0026] The material is then rapidly cooled to agglomerate it, resulting in spherical particulate material made of titanium dioxide. By controlling the composition, particle size, and input amount of the raw particulate material, the composition of the carrier, the concentration of the raw particulate material in the carrier, the composition and temperature of the oxidizing atmosphere, etc., the particle size distribution, sphericity, moisture content, and EC value of the resulting particulate material can be controlled.
[0027] Increasing the particle size of the particulate material to 0.3 μm or more can be achieved by using titanium powder with an average particle size of 5 μm or more as the raw material and using the deflagration method. Further increasing the particle size of the particulate material can be achieved by increasing the average particle size of the raw titanium powder. Furthermore, increasing the particle size of the particulate material to 20 μm or more can be achieved by reducing the amount of oxygen required for theoretical complete combustion and by increasing the amount of raw material input, thereby promoting particle growth. Further reducing the particle size of the particulate material can be achieved by suppressing particle growth by reducing the amount of raw material powder input per unit time.
[0028] To achieve a sphericity of 0.9 or higher, titanium metal powder is burned in an oxygen atmosphere to form titanium oxide gas. This is then rapidly cooled to form titanium oxide droplets, which become spherical due to surface tension and are then rapidly cooled again to solidify. The sphericity of the particulate material can be further increased by slowing the cooling rate.
[0029] The moisture content of the particulate material can be reduced to 0.5% by mass or less by reducing the amount of moisture attached to or contained in the raw particulate material, reducing the amount of moisture in the carrier (including moisture generated by combustion), or reducing the amount of moisture generated by combustion of the combustion-supporting gas. This can also be achieved by heating and drying the produced particulate material. The heating temperature is preferably a temperature at which adsorbed water is removed or higher, and further preferably a temperature at which bound water can be removed.
[0030] In order to reduce the linseed oil absorption of a particulate material to 0.25 mL / g or less, it is possible to increase the sphericity and also to adjust the particle size distribution of the particulate material so that it has two or more peaks, as mentioned above.
[0031] The EC value of the particulate material can be reduced to 40 μS / cm or less by reducing the content of alkali metals and alkaline earth metals in the raw particulate material. For example, this can be achieved by purifying metallic titanium as the raw particulate material to reduce the amount of impurities contained therein, or by avoiding contact of the produced particulate material with components that improve EC (alkali metals, alkaline earth metals, and compounds containing them).
[0032] The chloride ion concentration of the particulate material can be reduced to 100 ppm or less by reducing the chloride concentration in the raw particulate material, for example, by avoiding the use of titanium dioxide produced from titanium tetrachloride gas or by avoiding treatment with chlorine-containing compounds such as hydrochloric acid.
[0033] The particle diameter of the raw material particle material can have a lower limit of approximately 0.1 μm, 1 μm, 10 μm, or 30 μm, and an upper limit of approximately 300 μm, 200 μm, 150 μm, or 100 μm. These lower and upper limits can be combined arbitrarily. Increasing the lower limit increases the particle diameter of the resulting particle material, while decreasing the upper limit decreases the particle diameter of the resulting particle material.
[0034] The carrier may be a fluid such as a gas or a liquid. Examples of the gas include nitrogen, argon, oxygen, and hydrocarbon gases such as propane and methane, either singly or in mixture, and air may also be used. Examples of the liquid include water, acetone, alkanes, ethers, and alcohols.
[0035] It is particularly preferable to use a carrier with reduced moisture content. In addition to the moisture content, it is also preferable to reduce components (those with hydrogen in the molecule) that generate water upon combustion. It is preferable to control the amount of moisture contained and the amount of moisture generated by combustion to 5% by volume or less in the combustion furnace. In particular, the upper limit of the moisture content can be 3%, 2%, 1%, or 0.5% by volume. Furthermore, the amount of moisture contained in the produced particulate material can be reduced by reducing the amount of moisture contained in the carrier and the amount of moisture generated by combustion. There are no particular limitations on the method for reducing the moisture content in the carrier, but it can be dried by some method, and when air is used as the carrier, the moisture content can be adjusted by selecting a time when the humidity in the air is low. Furthermore, a gas that does not generate moisture upon combustion can also be used.
[0036] The moisture content of the produced particulate material can also be reduced by heating the particulate material. The heating temperature is preferably 200°C or higher, more preferably 400°C or higher, and even more preferably 500°C. The heating time is not particularly limited, but it is preferable to continue heating until the moisture content reaches the aforementioned level. It is also preferable to remove the moisture physically attached to the particulate material as well as the water that is chemically bound to it by heating.
[0037] When the oxidizing atmosphere is formed by a flame, the flame can be formed by burning a mixture of a combustion supporting gas and a combustible gas. Examples of the combustion supporting gas include oxygen and air. Examples of the combustible gas include hydrocarbon gases such as propane, methane, and acetylene, as well as ammonia and hydrogen gas. The mixing ratio of the combustion supporting gas to the combustible gas is not particularly limited, but it is preferable to create an oxidizing flame with a stoichiometric excess of the combustion supporting gas.
[0038] The concentration of the raw material particles in the carrier is not particularly limited, but is preferably 0.2 to 3 kg / Nm 3 The lower limit is 0.2 kg / Nm 3 , 0.6kg / Nm 3 The upper limit is 3.0 kg / Nm 3 , 1.5kg / Nm 3 When the concentration is increased, the particle size of the resulting particulate material increases, and when the concentration is decreased, the particle size of the resulting particulate material decreases.
[0039] The feed rate of the raw material particles can be set to approximately 0.2 kg / h to 5.0 kg / h. Examples of lower limits include 0.2 kg / h and 0.6 kg / h, and examples of upper limits include 5.0 kg / h and 2.0 kg / h. Increasing the feed rate results in a larger particle size of the resulting particle material, while decreasing the feed rate results in a smaller particle size of the resulting particle material.
[0040] In addition to the carrier, a combustion-promoting gas or an inert gas may be supplied. The combustion-promoting gas can be supplied near the oxidizing atmosphere.
[0041] These reactions proceed in a reactor, and the amount of combustion-supporting gas (such as oxygen) supplied to the reactor is preferably in excess of the amount sufficient to oxidize the combustible gas and raw material particles.
[0042] It is also possible to form a silica layer on the surface (silica coating process). The method for forming the silica layer is not particularly limited, but it can be formed by attaching tetraalkoxysilane or trimethoxysilane to the surface and then reacting it. Heating can be used during the reaction. The lower limit of the heating temperature can be 20°C, 30°C, or 40°C. The method for attaching the tetraalkoxysilane to the surface is not particularly limited, but liquid tetraalkoxysilane can be directly sprayed onto the surface, evaporated into a gaseous state, or dissolved in an organic solvent and sprayed onto the surface. The amount of tetraalkoxysilane can be determined depending on the thickness of the silica layer to be formed. The type of tetraalkoxysilane is not particularly limited, but examples include those having an alkoxy group with about 1 to 4 carbon atoms.
[0043] The surface treatment is the same as that described above for the particulate material, and therefore will not be described here.
[0044] (Slurry Composition) The slurry composition of this embodiment is a composition in which the particulate material of this embodiment is dispersed in an organic solvent. The organic solvent is not particularly limited, but examples thereof include methanol, ethanol, isopropanol, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl acetate, ethyl acetate, toluene, hexane, THF, ethyl methyl ketone, methyl isobutyl ketone, cyclohexanone, dimethylacetamide, dimethylformamide, acetic acid, and oleic acid.
[0045] The mixing ratio of the particulate material to the organic solvent is not particularly limited as long as fluidity is maintained, but for example, the mass ratio of (particulate material):(organic solvent) can be about 5:95 to 85:15. The slurry composition of this embodiment can be used to supply the particulate material when mixed with a resin material, other particulate material, etc., or can be used to apply the particulate material by applying it to a target site and then drying the organic solvent.
[0046] (Resin composition) The resin composition of this embodiment is a composition in which the particulate material of this embodiment is dispersed in a resin material. Examples of the resin material that can be used include a polymer compound that can be melted by heating, a polymer compound after hardening, and a polymer precursor that can be hardened by a reaction. Examples of the resin material include, but are not limited to, epoxy resin, urea resin, polyester resin, acrylic resin, polyimide resin, LCP resin (liquid crystal resin), COC resin (cyclic olefin copolymer), and fluororesin.
[0047] The mixing ratio of the particulate material to the resin material is not particularly limited as long as fluidity is maintained, but for example, the mass ratio of (particulate material):(resin material) can be about 5:95 (lower limit) to 90:10 (upper limit), with the lower limit being 10:90, 20:80, 30:70, 40:60, 50:50, 60:40, 70:30, or 80:20. The resin composition of this embodiment can be used as a part or all of a semiconductor encapsulant, as well as a part or all of a substrate material.
[0048] (dielectric materials) The dielectric material of this embodiment is a material that contains the slurry composition or resin composition of this embodiment and can be used as a dielectric. The dielectric material of the present invention preferably contains a large amount of particulate material, for example, preferably 60 mass % or more. As explained in the section on the resin composition above, it can also be used as a part of a substrate material or an encapsulant to exert its effects as a dielectric material. [Example]
[0049] Example 1 The granular material was produced by supplying 10 g / min of raw material granular material made of metallic titanium with a volume average particle diameter of 30 μm, 2.2 L / min of propane gas as a combustible gas, and 1.5 times the amount of oxygen gas as a combustion support gas required for combustion of the raw material granular material and the combustible gas into a combustion furnace (deflagration process). Because the combustion support gas was supplied in excess, nearly complete combustion was achieved.
[0050] The combustion furnace was connected to an exhaust fan to create a negative pressure inside the furnace, and the resulting particulate material was collected through a bag filter. The analytical data for the resulting particulate material are summarized in Table 1.
[0051] 14 g of the obtained particulate material was mixed and dispersed in epoxy resin (4.7 g of ZX1059, 1.3 g of Ethacure 100) to obtain a resin composition (filling rate of particulate material: 70 mass %). This resin composition was heated and cured at 170°C, and a rectangular parallelepiped of 4 mm x 4 mm x 30 mm was cut out from the obtained cured product (resin composition) to prepare a test sample.
[0052] Example 2 Test samples were prepared and evaluated in the same manner as in Example 1, except that the volume average particle diameter of the raw particle material was changed to 100 μm.
[0053] Example 3 Test samples were prepared and evaluated in the same manner as in Example 1, except that the amount of oxygen gas used as the combustion supporting gas was 1.05 times the amount required for combustion of the particulate material and propane gas used as the combustible gas.
[0054] Example 4 Test samples were prepared and evaluated in the same manner as in Example 2, except that the amount of oxygen gas used as the combustion supporting gas was 1.05 times the amount required for combustion of the particulate material and propane gas used as the combustible gas.
[0055] Example 5 Test samples were prepared and evaluated in the same manner as in Example 1, except that the volume average particle diameter of the raw particle material was changed to 20 μm, the supply rate of the raw particle material was changed to 7 g / min, and the amount of oxygen gas used as a combustion-supporting gas was increased to 2.0 times the amount required for combustion of the particle material and propane gas used as a combustible gas.
[0056] Example 6 To 20 g of the particulate material of Example 1, 1.2 g of tetraethoxysilane was slowly added dropwise over 10 minutes, and then 0.2 g of ion-exchanged water was added dropwise over 10 minutes while stirring and mixing. The mixture was then reacted at 60°C for 1 hour, and further heated at 120°C for 2 hours to distill off the volatile components. The obtained particulate material was measured by FT-IR (diffuse reflectance method), and showed a peak at 3750 cm -1 A peak derived from SiO-H was detected in the vicinity, confirming that a silica layer had formed on the surface of the particulate material made of titanium dioxide.
[0057] (Comparative Example 1) A cured resin composition was prepared in the same manner as in Example 1, except that a particulate material made of commercially available titanium dioxide (titanium(IV) oxide, anatase type, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used and the filling rate of the particulate material was set to 20 mass %, and the dielectric constant was measured in the same manner.
[0058] Example 7 20 g of the particulate material obtained in Example 1 was dried at 500° C. for 2 hours and then collected.
[0059] (Comparative Example 2) Test samples were prepared and evaluated in the same manner as in Comparative Example 1, except that a commercially available particulate material made of titanium dioxide (titanium dioxide (IV), rutile type, -5 μm, 99.9%, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the raw particle material.
[0060] Table 1 shows the manufacturing conditions, volume-average particle size, sphericity, true specific gravity, rutile titanium dioxide content calculated from XRD measurement (the remainder is believed to be anatase titanium dioxide), oxygen content, moisture content (Karl Fischer method: before and after moisture absorption), and linseed oil absorption for each example and comparative example. The moisture absorption conditions for measuring moisture content were 40°C, 85% RH, and 24 hours. Linseed oil absorption was measured by adding linseed oil drop by drop to 1 g of the particulate material until fluidization was confirmed visually. The linseed oil absorption was calculated as the amount of linseed oil (ml) added divided by the weight of the particulate material (g).
[0061] The particle size distributions of the particulate materials of Examples 1 to 5 measured by laser particle size analysis are shown in Figures 1 to 5. XRD measurement spectra of the particulate materials of Examples 1 to 4 are shown in Figures 6 to 9. SEM photographs of the particulate materials of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Figures 10 to 15. The FT-IR spectrum of the particulate material of Example 1 is shown in Figure 16. It was found that the peak width of the particle size distribution of the particulate material of each Example was narrow. Furthermore, two narrow peaks were confirmed for the particulate material of Example 1, and the SEM photograph also revealed that particles with smaller particle sizes had entered the gaps between particles with larger particle sizes.
[0062] [Table 1]
[0063] (Filling rate evaluation) For Examples 1 and 2 and Comparative Examples 1 and 2, resin compositions with filling rates (FC) of 20 mass%, 40 mass%, 60 mass%, and 70 mass% were prepared by varying the mixing ratio of each particulate material to the epoxy resin, and test specimens were cut out from the cured products cured under the conditions of Example 1. The dielectric constant of these test specimens was measured (Table 2).
[0064] [Table 2]
[0065] As is clear from Table 2, it was found that the higher the filling rate, the higher the relative dielectric constant. It was also found that the particulate material of Comparative Example 1 could not achieve a filling rate of 40 mass% or more, and the particulate material of Comparative Example 2 could not achieve a filling rate of 60 mass% or more. This is thought to be because the particulate material of Comparative Example 1 had an irregular shape and a small particle diameter, as is clear from the SEM photographs, sphericity, and volume average particle diameter.
[0066] (Evaluation of leachable substances) 3.5 g of each particulate material of Examples 1 to 5 and Comparative Examples 1 and 2 was added to 35 mL of pure water, stirred and suspended at 20°C for 30 minutes, and then subjected to solid-liquid separation to obtain an extract. These extracts were analyzed by ion chromatography to determine the amount of Li in the ionic impurities detected. + , Na + , K. + , F - , Cl - The amount of HCl and the electrical conductivity (EC) were measured and the results are shown in Table 3.
[0067] [Table 3]
[0068] Examples 1 to 5 and 7 are all Li + , Na + , K. + , F - , Cl - It was found that the EC value was 5 ppm or less. Examples 1 to 5 and 7 also showed small values of 20 μS / cm or less.
Claims
1. A particulate material made of titanium dioxide having a volume average particle size of 0.3 to 20 μm, two particle size peaks, a sphericity of 0.9 or more, a moisture content of 0.5 mass% or less, and a linseed oil absorption of 0.25 mL / g or less.
2. 2. The particulate material according to claim 1, wherein the particle size of the smaller of the two peaks is 40% or less of the particle size of the larger of the two peaks.
3. A particulate material as described in claim 1 or 2, wherein the electrical conductivity of the extract after solid-liquid separation after stirring and suspending at a concentration of 3.5 g / 35 mL at 20°C for 30 minutes is 40 μS / cm or less, the chloride ion concentration is 100 ppm or less, and the sodium ion concentration is 30 ppm or less.
4. A silica layer is formed on the surface, In the FT-IR spectrum measured by the diffuse reflectance method, -1 The particulate material according to any one of claims 1 to 3, having a peak at
5. 5. The particulate material according to claim 1, which has been surface-treated with a silane compound.
6. The present invention comprises a particulate material made of titanium dioxide having a volume average particle size of 0.3 to 20 μm, a sphericity of 0.9 or more, a moisture content of 0.5 mass% or less, and a linseed oil absorption of 0.25 mL / g or less, The particulate material may have one or more of the following components (A) to (C): (A) The electric conductivity of the extract after solid-liquid separation after stirring and suspending at a concentration of 3.5 g / 35 mL at 20° C. for 30 minutes is 40 μS / cm or less, the chloride ion concentration is 100 ppm or less, and the sodium ion concentration is 30 ppm or less. (B) a silica layer is formed on the surface; In the FT-IR spectrum measured by the diffuse reflectance method, -1 It has a peak at (C) The surface is treated with a silane compound.
7. A method for producing a particulate material made of titanium dioxide having a volume average particle size of 0.3 to 20 μm, a sphericity of 0.9 or more, a moisture content of 0.5 mass% or less, and a linseed oil absorption of 0.25 mL / g or less, comprising the steps of: The method includes a deflagration step in which raw material particles made of metallic titanium are suspended in a carrier and then introduced into a high-temperature oxidizing atmosphere to be combusted, The particulate material may have one or more of the following components (A) to (C), and when it further has the following component (B), it may have the following component (D). (A) The electric conductivity of the extract after solid-liquid separation after stirring and suspending at a concentration of 3.5 g / 35 mL at 20° C. for 30 minutes is 40 μS / cm or less, the chloride ion concentration is 100 ppm or less, and the sodium ion concentration is 30 ppm or less. (B) a silica layer is formed on the surface; In the FT-IR spectrum measured by the diffuse reflectance method, -1 It has a peak at (C) The surface is treated with a silane compound. (D) A silica coating step of attaching a tetraalkoxysilane compound to the surface and heating the surface after the deflagration step.
8. A slurry composition comprising the particulate material according to any one of claims 1 to 5 and an organic solvent for dispersing the particulate material.
9. A resin composition comprising the particulate material according to any one of claims 1 to 5 and a resin material for dispersing the particulate material.
Citation Information
Patent Citations
Thermoplastic resin foamed sheet having photocatalytic function
JP2000017096A
High purity titanium oxide and method for producing the same
JP2008273832A
Titanium dioxide containing composite particle
JP2012111842A
Method for manufacturing spherical titanium oxide particle
JP2012246203A
Thin film capacitor
JP2016111182A