Test piece for rolling fatigue test, rolling fatigue test method using said test piece, and manufacturing method of test piece

The test piece and method address the challenge of non-spherical inclusions in rolling fatigue tests by embedding non-spherical inclusions with a gap and marker member, enabling precise verification of their impact on bearing lifespan and fatigue behavior.

JP7560392B2Active Publication Date: 2024-10-02SANYO SPECIAL STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021043727
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-02
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Existing rolling fatigue tests do not adequately consider the properties, arrangement, and effects of non-spherical inclusions in steel, which contribute to premature bearing failure due to short-life flaking, making it difficult to clarify the relationship between inclusion characteristics and bearing lifespan.

Method used

A test piece and method are developed to include non-spherical inclusions with a gap between the inclusion and matrix, using a marker member to identify their position, allowing for a thrust-type rolling fatigue test that specifies the inclusion's surface position and trajectory, and utilizes ultrasonic flaw detection to correct the test results.

Benefits of technology

This approach enables precise verification of the harmful effects of non-spherical inclusions on rolling fatigue by maintaining a controlled interface state, allowing for advanced analysis of inclusion-matrix interactions and improved bearing reliability by identifying and analyzing the fatigue state around inclusions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560392000001
    Figure 0007560392000001
  • Figure 0007560392000002
    Figure 0007560392000002
  • Figure 0007560392000003
    Figure 0007560392000003
Patent Text Reader

Abstract

To provide a rolling test method considering the properties and arrangement of an inclusion different from a spherical shape.SOLUTION: The test piece is a test piece used for a rolling fatigue test, which includes: a test piece body; and inclusion that is generated in a steel manufacturing process, and which is embedded at a depth predetermined from the surface of the body. The inclusion may include an A-type inclusion, a B-type inclusion, a C-type inclusion, or a D-type inclusion classified by JIS standards. A gap is formed between the inclusion and the mother phase of the test piece main body.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a test piece used in a rolling fatigue test. [Background technology]

[0002] Flaking that occurs before the bearings are expected to break down even when used under proper lubrication conditions has been reported, hindering the realization of smaller and lighter bearing designs. Flaking is known to be caused by nonmetallic inclusions in steel. Nonmetallic inclusions are inevitably generated during the refining, casting, and solidification processes of steel, and those that cannot be completely removed during these processes are contained in the steel. Nonmetallic inclusions remain and are contained in the bearing material after further downstream processes such as rolling and forging. Flaking that originates from nonmetallic inclusions usually occurs not on the surface of the part but somewhat inside. This is due to high shear stress occurring somewhat inside the bearing race when the bearing race and rolling elements (balls, rollers, etc.) come into rolling contact.

[0003] Direct observation of rolling fatigue is difficult because fatigue progresses inside the component before it causes flaking. In addition, it is rare to find the inclusions that caused the flaking on the fracture surface after flaking has occurred. Therefore, although there is no doubt that inclusions affect bearing life, the direct relationship between the size, shape, dispersion, chemical composition, etc. of inclusions (hereinafter referred to as "properties of inclusions") and life has not yet been clarified.

[0004] The life index of rolling bearings is L 10 Life expectancy is important. 10 The lifespan refers to the lifespan when 90% of the test pieces do not flake when multiple samples are subjected to life tests under the same conditions. In this way, it is customary for bearing lifespans to be evaluated probabilistically. Rather than relying on probability theory, it is necessary to directly verify the relationship between the properties of inclusions and lifespan / rolling fatigue, and to clarify the quantitative relationship between the two, in order to realize steel that does not cause short-life flaking.

[0005] On the other hand, Non-Patent Document 1 discloses that SUJ2 steel was artificially prepared with a large number of residual / dispersed voids in the steel, the behavior of rolling fatigue cracks in these voids was observed, and the behavior was compared with stress simulations for voids or general inclusions, indicating that harmfulness is aggravated when there are gaps (voids) between the inclusions and the matrix.

[0006] In relation to this, Non-Patent Document 2 discloses a technology for significantly improving the rolling fatigue life by subjecting a steel material to hot isostatic pressing (HIP) processing in order to close the gaps between inclusions and the parent phase.

[0007] According to Non-Patent Document 2, it is clear that the state of the inclusion-matrix interface is a factor in changing the life. However, after spalling occurs, it is practically difficult to verify whether there was a gap around the inclusion beforehand, and it was not possible to estimate the contribution of the gap to the length of the life.

[0008] Therefore, in order to understand the relationship between the properties of inclusions and life or rolling fatigue, it is essential to align the state of the inclusion-matrix interface, which has a strong influence on life, in a constant state, i.e., to fix the interface conditions, prior to rolling fatigue testing. It is also assumed that it is relatively large inclusions that cause short-life spalling in bearings, and it is also necessary to consider that there is a low possibility that such inclusions exist in the very small stress-loaded volume in the limited number of evaluation rolling fatigue test pieces.

[0009] In recent years, there has been a demand for bearing steels that not only pursue longer life, but also suppress the sudden occurrence of short-life flaking to improve the reliability of parts. Therefore, in order to realize such bearing products, it is necessary to clarify the relationship between the properties of inclusions and life, and to know the properties of inclusions that are the starting point of short-life flaking.

[0010] However, to do this, it is necessary to understand in advance the properties of the inclusions, which are factors that affect rolling fatigue, the state of the interface between the parent phase and the inclusion, and their location in the steel, and then to conduct rolling fatigue tests on the inclusions and verify the properties and lifespan of the inclusion, or, if there is no spalling, the properties of the inclusion and the fatigue state around it, in a one-to-one comparison.

[0011] This is because, although the various factors listed above are highly likely to affect the life, it is difficult to isolate and verify the effects after the test.Patent Document 1 is known as a technique for conducting rolling fatigue tests with the properties of target inclusions known in advance, and verifying the effects on life and rolling fatigue by one-to-one comparison.

[0012] In this patent, a test piece is prepared in which an artificial inclusion is included by artificial means, and after creating a state in which a gap is provided between the inclusion and the surrounding matrix, the position of the inclusion is adjusted and a rolling fatigue test is performed. In the embodiment, a method for preparing a test piece using spherical Al2O3 and a rolling fatigue test method are shown, which assumes spherical inclusions among the inclusions in actual steel materials (spherical inclusions among D-type inclusions classified in the JIS standard JIS G 0555). [Prior art documents] [Patent documents]

[0013] [Patent Document 1] JP 2020-63922 A [Non-patent literature]

[0014] [Non-Patent Document 1] Takeshi Fujimatsu, Kazuhiko Hiraoka, and Atsuyuki Yamamoto, "Crack Initiation Behavior from Internal Defects in Rolling Contact Fatigue of High Carbon Chromium Bearing Steel," Iron and Steel Institute of Japan, Vol. 1.94, No. 1 (2008), pp. 13-20 [Non-Patent Document 2] K. Hashimoto, T. Fujimatsu, N. Tsunekage, K. Hiraoka, K. Kida, and EC Santos, "Effect of inclusion / matrix interface cavities on internal-fracture-type rolling contact fatigue life," Materials & Design, Elsevier BV, (Netherlands), Vol. 32, Issue 10, December 2011, pp. 4980-4985 Summary of the Invention [Problem to be solved by the invention]

[0015] However, Patent Document 1 discloses findings related to test specimens containing spherical inclusions, which have a simple shape, and does not specifically consider a rolling fatigue test method that takes into account the properties and arrangement of inclusions that are different from spherical shapes.

[0016] An object of the present invention is to provide a rolling test method that takes into account the properties and arrangement of inclusions that are not spherical. [Means for solving the problem]

[0017] (1) A test piece used in the rolling fatigue test according to the present invention comprises: (1) a test piece main body; and at least one inclusion selected from the group consisting of A-type inclusions, B-type inclusions, C-type inclusions and D-type inclusions as defined in JIS G 0555, embedded to a predetermined depth from the surface of the test piece main body, and having a shape other than spherical, wherein there is a gap between the inclusion and the matrix of the test piece main body.

[0018] (2) The test piece described in (1) above, characterized in that a marker member that can be distinguished from the parent phase of the test piece main body is embedded in a position in the test piece main body different from the inclusions.

[0019] (3) The test piece according to (2) above, wherein the marker member is formed in a cylindrical shape and has a composition different from that of the parent phase of the test piece main body.

[0020] (4) The test piece according to any one of (1) to (3) above, characterized in that the hardness of the test piece is 55 HRC or more.

[0021] (5) A rolling fatigue testing method, comprising carrying out a thrust type rolling fatigue test using a test piece according to any one of (1) to (4) above.

[0022] (6) A rolling fatigue test method for performing a thrust type rolling fatigue test using the test piece described in (2) or (3) above, characterized in that the surface position of the test piece main body directly above the inclusion is identified from the position of the marker member, and a track is set so that a rolling element passes through this identified surface position, thereby performing the thrust type rolling fatigue test.

[0023] (7) The rolling fatigue testing method according to (6) above, characterized in that the specified surface position is corrected based on the test results of an ultrasonic flaw detection test.

[0024] (8) A method for manufacturing a test piece as described in (1) above, comprising the steps of: rolling or forging a steel material as the inclusion extraction step; taking a test piece for inclusion extraction for axial fatigue from the rolled material obtained in the rolling step or the forged material obtained in the forging step, and subjecting the test piece for inclusion extraction to a fatigue test using axial ultrasonic vibration to fracture the test piece for inclusion extraction; and an inclusion removal step for obtaining information regarding the properties of the inclusions manifested on the fracture surface of the test piece for inclusion extraction and removing the inclusions together with the fracture surface of the test piece for inclusion extraction.

[0025] (9) A method for producing a test piece according to the above (8), characterized in that, before conducting the fatigue test using ultrasonic vibration, a steel embrittlement step is carried out by charging the test piece for inclusion extraction with hydrogen.

[0026] (10) A method for manufacturing a test piece used in a rolling fatigue test, the method including the steps of: preparing a first intermediate material having a predetermined outer shape; forming a hole of a predetermined diameter and depth in a surface of the first intermediate material; embedding at least one of A-type inclusions, B-type inclusions, C-type inclusions and D-type inclusions defined in JIS G 0555, in the hole, the inclusion having a shape other than spherical, and performing hot isostatic pressing on the first intermediate material in which the inclusion is embedded; processing the first intermediate material into a second intermediate material suitable for tensile processing; and tensile processing the second intermediate material in a predetermined direction to form a gap between the parent phase of the second intermediate material and the inclusion.

[0027] (11) In the method for manufacturing a test piece described in (10) above, the tensile processing is performed by applying a stress of 0.85 to 0.95 times the tensile strength of the second intermediate material to a predetermined position of the second intermediate material, where the tensile strength of the second intermediate material at the time of the tensile processing is taken as 1. Effect of the Invention

[0028] According to the present invention, non-spherical inclusions (non-metallic inclusions) that are generated during the steel manufacturing process and remain distributed in the steel even after it has undergone subsequent rolling, forging, etc. are extracted, their properties are identified, and then the extracted inclusions are placed in a very small stress-loaded volume in a rolling fatigue test piece with a gap provided between the inclusion and the surrounding parent phase, and a rolling fatigue test can be performed. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is a structural diagram of a test piece according to an embodiment. [Diagram 2]4 is a flowchart showing a manufacturing process of a test piece according to an embodiment. [Diagram 3] FIG. 2 is a diagram showing the configuration of an intermediate material A. [Figure 4] FIG. 2 is a diagram showing an example of the shape of a test piece for inclusion extraction. [Diagram 5] 1 is an optical microscope image showing the fracture surface of a test piece that broke after ultrasonic fatigue testing. [Figure 6] This is an enlarged secondary electron image of a portion of Figure 5 taken by an SEM of the inclusion that emerged as the fracture initiation point. [Figure 7] FIG. 13 is a diagram showing the configuration of an intermediate material B to which a tensile process is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, a test specimen and a rolling fatigue test method according to an embodiment of the present invention will be described in detail with reference to the drawings.

[0031] FIG. 1 is a structural diagram of the test piece of this embodiment. FIG. 1(a) is a front view, and FIG. 1(b) is a view seen from the arrow X of the test piece of FIG. 1(a) cut along the XX cross section. FIG. 1(c) is a view seen from the arrow Y of the test piece of FIG. 1(a) cut along the YY cross section. For ease of explanation, some dimensional relationships are exaggerated in FIG. 1. Also, FIG. 1(b) and (c) show enlarged views of a cylindrical sample.

[0032] The test piece 100 of this embodiment includes a hollow disk-shaped test piece body 100A having an inner diameter hole 101 at the center, and is formed into an elliptical shape with a minor axis in the XX direction and a major axis in the YY direction, as can be seen from the front view of Fig. 1(a). An inclusion 105 is embedded below a position corresponding to a raceway in a thrust type rolling fatigue test described later on the mirror polished surface of the test piece body 100A. Inclusions 105 are nonmetallic inclusions that are generated in steels specified by the JIS standard or various steels that deviate from the JIS standard due to the manufacturing process of the steel. The JIS standard (JIS G 0555: Microscopic test method for nonmetallic inclusions in steel) presents a method for evaluating the distribution state of nonmetallic inclusions that appear on the polished surface of a sample taken from a steel bar by mirror polishing the cross section parallel to the rolling direction of the steel. These are used as a means of confirming the quality of steel. Nonmetallic inclusions are roughly classified into A type (sulfide type), B type (alumina type, particle group consisting of single particles aligned in the deformation direction of the steel), C type (silicate type, elongated individual particles with an aspect ratio (length / thickness) generally exceeding 3), and D type (granular oxide type, single particles that do not deform and have a low aspect ratio of less than 3 with a square or circular shape). Of these, in the present invention, any type of nonmetallic inclusions except for spherical inclusions can be used. Also, only one type of inclusion among the A to D types may be embedded, or a mixture of multiple types of inclusions (for example, a mixture of D type inclusions and A type inclusions) may be embedded.

[0033] The XX line extends in the minor axis direction of the test piece 100, and a pair of cylindrical marking members 107 are embedded at a position on the XX line at a predetermined distance from the center of a hole 103 with a flat bottom. The marking members 107 are disposed to clearly identify the position of the hole 103 relative to the matrix of the test piece main body 100A. Specifically, the marking members 107 and the matrix of the test piece main body 100A are made of materials with different compositions, so that the interface can be clearly identified. Although details will be described later, the interface between the matrix of the test piece main body 100A and the marking members 107 can be clearly identified by making the test piece main body 100A from SUJ2 steel (see JIS G 4805) and the marking members 107 from stainless steel.

[0034] The marker member 107 can be formed into a cylindrical shape with a diameter of 0.5 mm and a height of 3 mm, for example. In FIG. 1, for convenience of explanation, the cylindrical sample 104 (the preparation method will be described later) with the inclusion 105 appearing on the bottom surface, the hole 103 with the bottom surface machined to be flat, the marker member 107, and the small drill hole 106 are shown by solid lines, but by performing the hot isostatic pressing process described later, the interfaces of the inclusion 105, the cylindrical sample 104, and the hole 103 with the bottom surface machined to be flat are in close contact with each other, and the interfaces of the marker member 107 and the small drill hole 106 are also in close contact with each other. Then, by performing the tensile process described later, a gap 108 is formed between the inclusion 105 present below the polished surface of the test piece 100 and the parent phase of the test piece main body 100A in the tensile processing direction YY (see FIG. 1(c)). On the other hand, in the XX direction perpendicular to the tensile processing direction YY, no gap 108 is formed between the inclusions 105 and the parent phase of the test piece body 100A (see FIG. 1(b)).

[0035] 2 is a flow chart showing the manufacturing process of the test piece of this embodiment. The manufacturing process will be described in detail with reference to the specific conditions under which the test piece 100 was manufactured as an example. The intermediate material 100A1 and the intermediate material 100A2 are intermediate materials of the test piece main body 100A, and the intermediate material 100A2 is manufactured after the intermediate material 100A1 is manufactured. (Step S1) In step S1, an intermediate material 100A1 shown in FIG. 3 is prepared. A cylindrical specimen 104, an inclusion 105, and a mark member 107 are embedded in the intermediate material 100A1 at predetermined positions. The intermediate material 100A1 and the cylindrical specimen 104 (in which the inclusion 105 is exposed on the bottom surface by a fatigue test described later) may be made of, for example, SUJ2 steel (see JIS G 4805), which is widely known as a material for bearing steel. However, the present invention is not limited to this, and any type of steel for which fatigue characteristics are to be obtained may be appropriately selected. The process of preparing the intermediate material 100A1 includes a rolling process of rolling SUJ2 steel, a normalizing process of normalizing the rolled material, a spheroidizing annealing process of spheroidizing the normalized rolled material, and a shaping process of processing the material into a test piece shape (i.e., a hollow disk shape with both sides parallel to each other). When using hypereutectoid steel such as SUJ2, a spheroidizing annealing process is carried out as a pretreatment to obtain an appropriate quenched structure in the quenching process described below. On the other hand, when using hypoeutectoid steel, a carburizing quenching process is carried out instead of quenching, so there is no need to carry out the spheroidizing annealing process. In the shaping process, it is desirable to polish one side 102 smoothly. This is because, as will be described later, one side 102 will be drilled (holes 103, etc.). However, there is no need to carry out a buffing finish process.

[0036] In the rolling process in the examples, SUJ2 steel was rolled to a diameter of 65 mm. In the normalizing process in the examples, the rolled material was held at a heating temperature of 865°C for 1 hour, followed by air cooling. In the spheroidizing annealing process in the examples, a heat treatment was performed with a maximum heating temperature of 800°C, and the material was held at that temperature for a predetermined time, followed by slow cooling.

[0037] In this embodiment, SUJ2 steel is used as an example, but the present invention is not limited to this, and other steels can be used. In this case, the normalizing treatment and spheroidizing annealing treatment in step S1 and the normalizing treatment and spheroidizing annealing treatment when reprocessing the test piece described later can be performed under conditions suitable for the selected steel type, or can be omitted depending on the steel type.

[0038] Next, in the shaping process of the embodiment, a hollow disk-shaped intermediate material 100A1 was produced with an outer diameter of 60 mm (corresponding to dimension A in FIG. 3), an inner diameter of 20 mm (corresponding to dimension B in FIG. 3), and a thickness of 8 mm (corresponding to dimension C in FIG. 3). Both sides of the intermediate material 100A1 were processed to be parallel. One side 102 was polished smoothly. Needless to say, the outer diameter, inner diameter, and thickness of the intermediate material 100A1 are not limited to the above values, and can be changed as appropriate depending on the test conditions.

[0039] (Step S2) In step S2, a hole 103 (which can be machined, for example, by an end mill) with a flat bottom (i.e., cylindrical with a bottom) and a pair of small drill holes 106 are formed in the intermediate material 100A1. The hole 103 can be machined at a position corresponding to the track on the polished surface 102 of the intermediate material 100A1. In this embodiment, the dimensions of the hole 103 are 2.6 mm in diameter and 2 mm in depth. The small drilled holes 106 are formed in the intermediate material 100A1 in a cylindrical shape with a bottom at positions on either side of the hole 103 in the radial direction of the intermediate material 100A1. In the embodiment, the dimensions of the small drilled holes 106 were 0.6 mm in diameter and 3 mm in depth. Needless to say, the diameter and depth of the holes 103 and 106 can be appropriately changed depending on the test conditions and the shape of the cylindrical sample 104 and the size of the marker member 107 described later. The hole 103 is formed on the upper surface side in the structural diagram of the test piece of this embodiment illustrated in FIG. 1, but it may be formed after the lower surface side is polished smoothly in the same manner as the above-mentioned one side 102. In this case, the pair of small drill holes 106 are also machined on the upper surface side. In this case, the length of the cylindrical sample 104 including the inclusion 105 and the depth of the hole 103 are set to be within the depth range of the marker member 107 from the surface of the one side 102. The distance (the above-mentioned specified distance) from the outer diameter portion of the cylindrical sample 104 to the marker member 107 is set to, for example, 1 mm or more, so that when the cylindrical sample 104 and the marker member 107, which is made of a material with a different composition, are brought into close contact with each other by the hot isostatic pressing process described below, the chemical composition of the marker member 107 does not affect the fatigue properties of the cylindrical sample 104.

[0040] (Step S3) In step S3, a test piece for inclusion extraction is prepared to obtain the inclusion 105 to be introduced into the test piece body 100A. This inclusion 105 is used as a defect to be introduced into the test piece body 100A. For this purpose, a test piece for inclusion extraction is prepared from the steel material to be evaluated, a fatigue test is performed, and an inclusion (extracted inclusion) that appears at the origin of the fracture surface after the test can be used as the inclusion 105 to be introduced into the test piece body 100A. In this case, the inclusion is an inclusion that was accidentally included in a steel test piece randomly collected. The method of the fatigue test is not particularly limited, but if it is desired to shorten the test time, ultrasonic fatigue testing may be selected. In addition, a defect that is expected to be an inclusion may be detected for the steel material to be evaluated by a method such as ultrasonic flaw detection testing, a test piece is prepared to include the defect, and the steel material is fractured by a fatigue test. If an inclusion appears at the origin of the fracture surface after the test, the inclusion may be used.

[0041] FIG. 4 is a cross-sectional view of the test piece for inclusion extraction cut along its longitudinal direction. Here, dimensional information of the test piece for inclusion extraction is also shown as an example. However, the dimensions are not limited to these and can be adjusted as appropriate. The test piece for inclusion extraction can be manufactured by first preparing a base material test piece that will be the base material of the test piece to be used in the inclusion extraction test (base material test piece preparation process), and then subjecting the base material test piece to a shape processing process (shape processing process). Each process included in step S3 will be described in detail below.

[0042] (Regarding the process of preparing the base material test piece in step S3) The manufacturing process of the base material test piece will be described by taking SUJ2 steel as an example. This process includes a rolling process in which SUJ2 steel is rolled, a normalizing process in which the rolled material is normalized, and a spheroidizing annealing process in which the normalized rolled material is spheroidized. Note that a forging process may be performed instead of the rolling process. In the rolling process in the example, SUJ2 steel was processed to a diameter of 65 mm by hot rolling. In the normalizing process in the example, a normalizing process was performed in which the steel was held at a heating temperature of 865°C for 1 hour and then air-cooled. In the spheroidizing annealing process in the example, a heating process was performed with a maximum heating temperature of 800°C, and a spheroidizing annealing process was performed in which the steel was held at that temperature for a predetermined time and then slowly cooled. When using steel other than SUJ2 steel, the base material test piece may be manufactured by a method suitable for each steel type, taking into account the processing method after this step.

[0043] (Regarding the shape processing process in step S3) Based on the above-mentioned classification of inclusions, the following explanation will be given. When D-type inclusions are extracted and used through fatigue testing, for example, when the evaluation volume is 300 mm 3 It is desirable to carry out an axial fatigue test (the direction of repeated stress loading on the test piece is the axial direction, and in this case the fracture surface is perpendicular to the axial direction) as described above. Furthermore, it is preferable to take the test piece for inclusion extraction so that its long axis direction is roughly parallel to the rolling direction of the rolled material. When it is desired to extract and use inclusions that are elongated in the rolling direction or aligned in the rolling direction, such as A-type, B-type, and C-type inclusions, it is preferable to take the test piece for inclusion extraction so that the long axis direction is the direction in which the cross-sectional area of ​​the inclusion is maximum, that is, the direction perpendicular to the rolling direction. In the case of forged material, the test piece for inclusion extraction may be taken according to the above-described method for rolled material, with the forging direction as the reference. In this case, in the case of a base material in which the extracted inclusions are D-type despite multiple tests being carried out, it may be easier to detect A-type, B-type, and C-type inclusions by reducing the evaluation volume of the test piece for inclusion extraction. Since the present invention is concerned with extracting and utilizing inclusions contained in steel material, the type and size of the inclusions will be derived from the history of the steel material to be evaluated (the manufacturing process of the steel material). In the examples, as an example, the aim was to extract inclusions elongated in the rolling direction (other than the D-type inclusions classified as above), and ultrasonic fatigue testing was used as a means to achieve this. When processing the base material test piece into the shape of the test piece for inclusion extraction shown in Figure 3, rough processing (in other words, coarse processing) was performed so that the longitudinal direction of the ultrasonic fatigue test piece was perpendicular to the rolling direction of the rolled material, and this roughly processed test piece for inclusion extraction was subjected to a quenching and tempering treatment, after which it was subjected to finish processing.

[0044] (Step S4) In step S4, a fatigue test is performed on the test piece for inclusion extraction to obtain inclusions. Here, an ultrasonic fatigue test is taken as an example to explain the method. The ultrasonic fatigue test piece for inclusion extraction needs to satisfy a predetermined resonance frequency. Therefore, before carrying out the ultrasonic fatigue test, the resonance frequency of the processed test piece for inclusion extraction is confirmed. The resonance frequency of the ultrasonic fatigue tester used in this example is 20,000Hz ± 500Hz, but the resonance frequency of the test piece is preferably within 20000Hz ± 200Hz, more preferably within 20,000Hz ± 30Hz. If the resonance frequency of the test piece for inclusion extraction does not satisfy these preferred ranges, the resonance frequency can be adjusted to the range by adjusting the length of the test piece for inclusion extraction. The resonance frequency of the test piece for inclusion extraction used in the examples is 19,980Hz, which satisfies the above-mentioned conditions. However, if the size of the test piece for inclusion extraction is increased to increase the risk volume within the output range of the ultrasonic fatigue testing machine, the maximum stress that can be applied to the test piece for inclusion extraction decreases with the size of the risk volume. Therefore, it is possible to promote fracture by embrittling the steel material using hydrogen charging as described below.

[0045] After the resonance frequency is confirmed, the test piece for inclusion extraction can be hydrogen-charged prior to the ultrasonic fatigue test in order to break the test piece for inclusion extraction more quickly. This causes hydrogen embrittlement of the steel material, and the breaking stress of the test piece for inclusion extraction can be reduced. In addition, the embrittlement fracture of the test piece for inclusion extraction makes the fracture surface more likely to be flat, and when the test piece for inclusion extraction is inserted into the drill hole 103 with a flat bottom, the interface between the fracture surface and the bottom of the drill hole 103 is more consistent. The hydrogen charging method is not particularly limited, but may be, for example, a method of immersing the test piece in various electrolytes, a method of exposing the test piece to high-pressure hydrogen gas, or a method of performing electrolysis in an electrolyte with the test piece as the cathode.

[0046] In the examples, hydrogen charging was carried out by a cathode charging method in which electrolysis was carried out in an electrolyte with the test piece for inclusion extraction as the cathode. An electrolyte prepared by adding sodium chloride and ammonium thiocyanate to pure water was used. When the electrolyte was taken as 100 mass%, the concentration of sodium chloride was 3 mass% and the concentration of ammonium thiocyanate was 0.3 mass%. The hydrogen charging time was 6 continuous hours. The average current density flowing through the inclusion test piece was 1.0 mA / cm. 2 The test temperature was 50°C.

[0047] Since the hydrogen diffusion coefficient into steel is temperature dependent, the efficiency of hydrogen charging can be improved by increasing the temperature of the electrolyte. Therefore, hydrogen charging may be performed efficiently by adjusting the temperature of the electrolyte to, for example, a temperature higher than room temperature.

[0048] In addition, since the hydrogen charged into the test specimen for inclusion extraction is gradually released after the test specimen for inclusion extraction is taken out into the atmosphere, it is desirable to subject the specimen to ultrasonic fatigue testing promptly after hydrogen charging.

[0049] The ultrasonic fatigue test is a test in which a test piece is subjected to repeated axial loads of tension and compression by ultrasonic vibration. It is known that when a test piece is continuously vibrated by ultrasonic waves, the test piece heats up due to internal friction caused by repeated tension and compression at high speed. This heat increases the ductility of the test piece, thereby hindering fracture from the inclusions. Therefore, in order to perform an appropriate test, it is necessary to suppress the heat generation of the test piece for inclusion extraction, for example, by blowing compressed air cooled by a chiller onto the test piece for inclusion extraction as necessary, or by performing intermittent operation in which ultrasonic oscillation is repeated and stopped. In the embodiment, as a means of suppressing the heat generation of the test piece for inclusion extraction, both the blowing of compressed air and intermittent operation in which ultrasonic oscillation is repeated for 0.11 sec and stopped for 0.40 sec were performed.

[0050] Furthermore, materials with low hardness have greater internal friction within the test piece under the same load stress than steel materials with high hardness, and are more likely to generate heat. In other words, if the output of the ultrasonic fatigue tester is simply increased to speed up the test, materials with low hardness will generate significant heat, making it impossible to perform an appropriate fatigue test. Therefore, it is desirable to select the output of the ultrasonic fatigue tester appropriately depending on the hardness of the test piece for inclusion extraction in the quenched and tempered state or the carburized, quenched and tempered state (these vary depending on the type of steel). In the embodiment, ultrasonic fatigue testing was performed at a test stress of 900 MPa, and the fracture life was 5 x 10 5 It has been determined that this cycle is sufficient to break the test specimen within a reasonable time.

[0051] (Step S5) In step S5, information regarding the properties of the inclusions appearing on the fracture surface of the inclusion extraction test piece is obtained. As mentioned above, the properties of the inclusions include the size, shape, dispersion state, and chemical composition of the inclusions. This information can be obtained, for example, by observation and analysis using an EDS-equipped scanning electron microscope (SEM-EDS). For example, by acquiring an SEM image of the fracture surface of the inclusion test piece using an EDS-equipped scanning electron microscope and analyzing the acquired SEM image, the size of the inclusion can be determined as the square root of the projected area of ​​the inclusion (√area). Similarly, the size of the inclusion can be determined as the circle equivalent diameter by image analysis. Furthermore, the chemical composition of the inclusion can be grasped by detecting the characteristic X-rays of the inclusion excited by the electron beam. Information on the shape and dispersion state can also be obtained by observation using a scanning electron microscope. By carrying out this step S5, the classification of the extracted inclusions (classification of A, B, C, and D, or classification of whether they are combined) can be determined.

[0052] Figure 5 shows an example of an optical microscope image taken by photographing the fracture surface of a test piece for inclusion extraction after an ultrasonic fatigue test. The area near the origin of the fracture surface exhibits a fish-eye pattern as shown by the dashed area in the figure, and the inclusion (non-metallic inclusion) that was the origin of the fracture is extracted near the center.

[0053] Figure 6 is an enlarged SEM image of the inclusion shown in Figure 5, and in this example, it is confirmed that it is a B-type inclusion. If the required inclusion is not obtained, the above inclusion extraction steps can be repeated until the required inclusion is obtained.

[0054] (Step S6) In step S6, the inclusions on the fracture surface of the test piece for inclusion extraction extracted as described above are cut so as to include the inclusions, to prepare a cylindrical sample 104 including the inclusions 105. At this time, since the position of the inclusions 105 on the fracture surface of the test piece for inclusion extraction is not necessarily located at the center of the cylindrical sample 104, it is advisable to obtain position information and use the information when arranging the inclusions later. Note that, when the major axis and minor axis of the inclusions are clearly different, it is advisable to obtain information on the orientation of the inclusions. Then, the cylindrical sample 104 is placed inside the hole 103 so that the fracture surface side on which the inclusions 105 are present in the cylindrical sample 104 faces the bottom surface of the hole 103 whose bottom surface has been machined to be flat. Here, the arrangement direction of the inclusions 105 on the bottom surface of the hole 103 whose bottom surface has been machined to be flat can be changed according to the purpose of the fatigue test. In the embodiment, the inclusions 105 are disposed so that the extension direction of the inclusions 105 coincides with the XX direction in Fig. 3 (the radial direction of the intermediate material 100A1 passing through the pair of marker members 107). At this time, a part of the interface between the cylindrical sample 104 and the hole 103 may be spot welded so that the storage position of the cylindrical sample 104 does not shift before the hot isostatic pressing process performed thereafter.

[0055] Also, a stainless steel marker member 107 is embedded in the small drill hole 106. After embedding, the parent phase of the intermediate material 100A1 and the marker member 107 are joined by hot isostatic pressing, and the interface between the parent phase and the marker member 107 is in a distinguishable state, which can be used to identify the embedded position of the inclusion 105. That is, when a plane along the polished surface 102 side of the test piece 100 is defined as a coordinate plane consisting of an X-axis and a Y-axis perpendicular to each other, the position where the inclusion 105 exists can be identified based on the identified coordinate position of the marker member 107. This makes it possible to place the inclusion 105 under the track of the rolling element during a thrust type rolling fatigue test described later.

[0056] (Step S7) In step S7, hot isostatic pressing (HIP) is performed on the intermediate material 100A1. As a pretreatment for the hot isostatic pressing, the intermediate material 100A1 is placed in a separately prepared low carbon steel case (not shown), a core bar (not shown) is inserted into the inner diameter hole 101 of the intermediate material 100A1, and the case is then sealed. After the case is sealed, the inside of the case is evacuated and hot isostatic pressing is performed, and then the case is cooled. The heating temperature in the hot isostatic pressing is 1150°C or higher, preferably 1160°C or higher. The pressure in the hot isostatic pressing is preferably 110MPa or higher, more preferably 140MPa or higher. In the embodiment, the pressure is set to 147MPa, the heating temperature is set to 1170°C, and the holding time at the heating temperature is 5h.

[0057] By applying hot isostatic pressing, the cylindrical sample 104 and the inclusions 105 can be brought into close contact with the holes 103, and the marker members 107 can be brought into close contact with the small drill holes 106.

[0058] (Step S8) In step S8, the intermediate material 100A1 is subjected to a normalizing process and a spheroidizing annealing process, and a re-processing process is performed in which the portion made of SUJ2 is processed into the intermediate material 100A2. As shown in FIG. 7, the intermediate material 100A2 of the embodiment has a shape suitable for the tensile process (step S9 described later) for artificially forming a gap around the inclusion 105. The intermediate material 100A2 is a hollow disk-shaped member having an inner diameter hole 109 at the center. The inner diameter hole 109 has an arc-shaped recess 109a and an arc-shaped recess 109b at symmetric positions with the inner diameter hole 109 as the center in a direction parallel to the subsequent tensile direction YY. These arc-shaped recesses 109a and 109b are formed in an arc shape with a smaller radius of curvature than the inner diameter hole 109, and protrude in a direction away from the center of the inner diameter hole 109. In addition, the inner diameter hole 109 has an arc-shaped recess 109c and an arc-shaped recess 109d at symmetric positions with the inner diameter hole 109 as the center in a direction XX perpendicular to the tensile direction YY of the tensile process. These arc-shaped recesses 109c and 109d are formed in an arc shape with a smaller radius of curvature than the inner diameter hole 109, and protrude in a direction away from the center of the inner diameter hole 109. The inclusions 105 embedded in the intermediate material 100A2 in a state of close contact with the surrounding parent phase are positioned so that they pass near the center line and are located near the middle circumference in a direction XX perpendicular to the direction YY in which the tensile processing is applied, as shown in Figure 7. This position adjustment can be performed by utilizing the mark member 107.

[0059] In the normalizing step in the embodiment, a normalizing treatment was performed in which the material was held at a heating temperature of 865°C for 1 hour and then air-cooled. In the spheroidizing annealing step in the embodiment, a heat treatment was performed with a maximum heating temperature of 800°C, and the material was held at that temperature for a predetermined time and then slowly cooled. In the reworking step in the embodiment, the outer diameter (corresponding to dimension A in FIG. 3) of the intermediate material 100A2 was 54 mm, the thickness (corresponding to dimension C in FIG. 3) of the intermediate material 100A2 was 6.2 mm, the radius of the inner diameter hole 109 was 10 mm, the radius of curvature of the arc-shaped recesses 109a and 109b was 6.5 mm, and the radius of curvature of the arc-shaped recesses 109c and 109d was 7 mm. The thickness of the intermediate material 100A2 may be set to an appropriate size that does not cause plastic deformation of the pin in the tensile processing in step S9 described later.

[0060] (Step S9) In step S9, the intermediate material 100A2 is subjected to a tensile process in order to form a gap around the inclusion 105. The tensile process can be performed by providing pins made of high hardness steel in the arc-shaped recesses 109a and 109b, respectively, and fixing these pins to a cold die steel jig for tensile process (the jig has holes machined to match the cross-sectional shape of the pins) attached to a servo tester, and then pulling the intermediate material 100A2 in the YY direction through the pins fixed to the die. The tensile process can be performed in a cold state. In the embodiment, the pins were manufactured by grinding a part of a SUJ2 round bar having a diameter of 12 mm in the longitudinal direction, and then adjusting it to about 60HRC by quenching and tempering. In order to form a gap between the inclusion 105 and the parent phase by applying tension to the intermediate material 100A2 in a spheroidized annealed state made of SUJ2 as in this embodiment, it is desirable to perform tension so that, assuming that the tensile strength of the intermediate material 100A2, which is a spheroidized annealed material, is 1, a stress of at least 0.85 times the tensile strength is applied to the vicinity of the portion where the inclusion 105 is embedded. To achieve this, for example, when the shape of the intermediate material 100A2 in FIG. 7 is used, the stroke amount of the tension process may be at least 5.3 mm. Note that, assuming that the tensile strength of the intermediate material 100A2 is 1, a stress of at least 0.85 times the tensile strength is required, but the stress concentration effect caused by the presence of the inclusion 105 is not taken into consideration with respect to the magnitude of this stress. However, in reality, with the assistance of the stress concentration effect of the inclusion 105, a stress exceeding the tensile strength acts around the inclusion 105, so that it is possible to form the gap 108 only around the inclusion 105. If it is desired to increase the size of the gap 108, the stroke amount described above can be further increased. In that case, the stress applied to the vicinity of the inclusion 105 is preferably at most 0.95 times or less, and more preferably 0.93 times or less. The reason for setting an upper limit on the stress applied by the tensile processing is to prevent voids from being formed in places other than the periphery of the embedded inclusion 105 and from affecting the rolling fatigue behavior and lifespan. In the embodiment, the stroke amount of the tension process was set to 7 mm. After the tension process, the inner diameter hole 101 can be machined to a circular shape again. This makes it easier to adjust the position in the thrust test described later. However, the process of machining the inner diameter hole 101 to a circular shape again can be omitted. 7, the intermediate material 100A2 may be changed to an appropriate shape that can impart the stress required for forming the gap 108 around the inclusion 105. As described above, the thickness of the intermediate material 100A2 may be set to an appropriate size that does not cause plastic deformation of the pin during the tensile processing.

[0061] (Step S10) In step S10, the intermediate material 100A2 is quenched and tempered to adjust the hardness of the intermediate material 100A2. The hardness (Rockwell hardness) of the intermediate material 100A2 after quenching and tempering is preferably 55HRC or more, more preferably 58HRC or more. If the hardness is lower than this, rolling fatigue will progress not only in the defects and their surroundings but also in the parent phase itself, making it difficult to distinguish and verify the harmfulness of the defects themselves. In the embodiment, the heating temperature for quenching was 835°C, the heating time was 0.5h, and oil quenching was used as a rapid cooling means for quenching. In addition, the tempering temperature was 180°C, the tempering time was 1.5h, and air cooling was used as a cooling means after the tempering temperature was reached. The hardness of the intermediate material 100A2 after quenching and tempering was about 62HRC.

[0062] (Step S11) After removing the oxide scale of the intermediate material 100A2 generated by the heat treatment by surface grinding, the depth of the inclusion 105 in the intermediate material 100A2 is identified by ultrasonic testing at a frequency of 50 MHz, and the intermediate material 100A2 is buffed based on the depth information, and adjusted so that the inclusion 105 is located in the high shear stress depth region under the thrust type rolling fatigue test conditions described below. During the ultrasonic testing, in addition to the depth of the inclusion 105, the coordinate position directly above the embedded portion of the inclusion 105 can also be identified. In the buffing finishing process, the surface is polished by rotating a buff coated with an abrasive and bringing it into contact with the surface. Cotton, felt, etc. can be used for the buff. If the position cannot be identified by the 50 MHz ultrasonic testing, the depth of the inclusion 105 may be identified by using ultrasonic testing at a higher frequency.

[0063] The test piece 100 used in the thrust rolling fatigue test is completed by the process described in steps S1 to S11 above. Then, the thrust rolling fatigue test can be performed taking into account the inclusions with properties different from those of a sphere. This allows precise verification of the harmfulness of the inclusions (their effects on life and rolling fatigue).

[0064] The thrust type rolling fatigue test will be described in detail with reference to an example. As a preparation before the thrust type rolling fatigue test, the position of the mark member 107, which serves as a precise mark embedded in the small drill hole 106, was identified by visually inspecting the buffed surface. Then, a track was arranged so that the rolling element would pass between the pair of mark members 107. A single thrust bearing race (model number 51305) made of SUJ2 was used as the upper plate to be combined with the test piece 100. A rolling element was arranged between the test piece 100 and the upper plate. SUJ2 steel balls with a diameter of 3 / 8 inches were used as the rolling element. Three of these rolling elements were arranged equally spaced at 120° intervals. As described above, the position directly above the embedded portion of the inclusion 105 can be identified by utilizing the coordinate position of the mark member 107. At this time, if the coordinate position information of the inclusion 105 in the ultrasonic flaw detection test is also utilized, the track position can be determined more precisely. That is, the position directly above the embedded portion of the inclusion 105, which is identified by utilizing the coordinate position of the marker member 107, can be corrected based on the test results of the ultrasonic flaw detection test. Regarding the layout of the track, taking into consideration that the behavior of rolling fatigue may change depending on the layout of the inclusion within the track width, the track may be set so that the center of the track width passes directly above the embedded portion, or may be purposely shifted appropriately from the center of the track width, and can be set appropriately according to the purpose of the test.

[0065] Next, a load is applied so that a maximum Hertzian contact stress of 4.5 GPa is applied to the contact portion between the rolling element and the test piece 100. The load cycle speed is, for example, 1800 cycles / min, lubrication is by immersion in an ISO VG68 oil bath, and a thrust type rolling fatigue test is performed at room temperature, thereby making it possible to evaluate the rolling fatigue behavior of the inclusion 105. These conditions for the thrust type rolling fatigue test may be adjusted according to the environment to be evaluated.

[0066] As described above, by using the method of rolling fatigue testing by introducing defects according to this embodiment, it is possible to introduce inclusion 105, the properties of which are known in advance, into a target position in test piece body 100A, create a state in which a gap is provided between inclusion 105 and the surrounding parent phase, perform a rolling fatigue test on it, and reliably observe the rolling fatigue behavior such as cracks around the inclusion embedding position after the test based on the position information known in advance. Regarding inclusion 105, it is possible to test inclusions that are not elongated but granular in shape using the method of the present invention.

[0067] Furthermore, if it is possible to induce spalling from the inclusions 105, it will also be possible to verify the relationship between the size of the inclusions 105 and the lifespan. Furthermore, with this method, tests are performed under conditions in which the composition and shape of the inclusions 105 that impart rolling fatigue and the state of the inclusion-matrix interface are determined in advance, so it is easy to reflect these conditions in analysis using the finite element method, making it possible to perform more advanced verification than ever before.

[0068] As described above, this embodiment is a method in which non-metallic inclusions that have been generated and contained in steel during the manufacturing process are extracted, and the size, composition, and shape of these inclusions are determined in advance and then introduced into a rolling fatigue test piece made of bearing steel.The inclusion and the parent phase are then brought into close contact with each other, and a gap is created between the inclusion and the surrounding parent phase.A rolling fatigue test is then performed on the inclusion to precisely verify its harmfulness to rolling fatigue (its effect on life and fatigue).

[0069] Furthermore, with this method, even if the test is interrupted before spalling occurs, the location of the inclusion in the steel is precisely identified in advance, making it possible to carry out cross-sectional observation of the fatigue condition around the inclusion.

[0070] The rolling fatigue testing method using inclusions, the properties of which have been determined in this embodiment, is performed from a state in which various information about the inclusions that affect the lifespan, such as their size, shape, composition, the state of the gap between the inclusions and the parent phase, and their location in the steel, is known in advance, making it possible to precisely verify the harmfulness of the inclusions (their effect on lifespan and rolling fatigue).

[0071] When using this test method, the precise location of the inclusion is known in advance, so the fatigue state around the inclusion can be easily observed. By using the conventional cross-sectional observation method or a non-destructive observation method, it is expected that the fatigue behavior around the inclusion can be verified more precisely than ever before.

[0072] Although the embodiment has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This new embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0073] 100 test pieces 100A Test piece body 100A1 100A2 Intermediate material 101 Inner diameter hole 102 Polished surface 103 Hole with flat bottom 104 Cylindrical sample 105 Inclusions 106 Small Drill Hole

Claims

1. A test piece used in a rolling fatigue test, A test piece main body portion, and at least one of A-type inclusions, B-type inclusions, C-type inclusions and D-type inclusions as defined in JIS G 0555, embedded to a predetermined depth from the surface of the test piece body, the inclusions having a shape other than spherical, A gap is provided between the inclusion and the parent phase of the test piece body portion, a marking member capable of being distinguished from the parent phase of the test piece main body is embedded on a side of the inclusion, avoiding a gap between the surface of the test piece main body and the inclusion; Test specimen.

2. 2. The test piece according to claim 1, wherein the marker member is formed in a cylindrical shape and has a composition different from that of the parent phase of the test piece body.

3. 3. The test piece according to claim 1, wherein the hardness of the test piece is 55 HRC or more.

4. A method for testing rolling fatigue, comprising the step of carrying out a thrust type rolling fatigue test using the test piece according to any one of claims 1 to 3.

5. A rolling fatigue testing method for performing a thrust type rolling fatigue test using the test piece according to claim 1 or 2, comprising the steps of: A rolling fatigue testing method characterized in that the surface position of the test piece main body directly above the inclusion is identified from the position of the marker member, and a track is set so that a rolling element passes through this identified surface position, thereby performing the thrust type rolling fatigue test.

6. The specified surface position is corrected based on the test results of the ultrasonic flaw detection test. The rolling fatigue testing method according to claim 5,

7. A method for manufacturing a test piece used in a rolling fatigue test, comprising the steps of: Producing a first intermediate member having a predetermined outer shape; forming a first hole having a predetermined diameter and a predetermined depth in a surface of the first intermediate material; a step of embedding at least one of type A inclusions, type B inclusions, type C inclusions and type D inclusions as defined in JIS G 0555, and having a shape other than a sphere, into the first hole; forming a second hole at a position different from the first hole on the surface of the first intermediate material; A step of embedding a mark member in the second hole so that the mark member can be distinguished from the parent phase of the first intermediate material; a step of performing hot isostatic pressing on the first intermediate material in which the inclusions and the mark members are embedded; A step of processing the first intermediate material into a second intermediate material having a shape suitable for stretch processing; and a step of stretching the second intermediate material in a predetermined direction to form gaps between the parent phase of the second intermediate material and the inclusions.

8. The stretching process is performed by applying a stretching force to a predetermined position of the second intermediate material.

8. The method for manufacturing a test piece according to claim 7, wherein a stress is applied that is 0.85 to 0.95 times the tensile strength of the second intermediate material, assuming that the tensile strength of the first intermediate material is 1.

Citation Information

Patent Citations

  • Inspection device for nonmetallic inclusion

    JP1990052251A

  • Steel for machine structure

    JP2002194484A

  • Bearing ring with artificial defect, roller bearing with an artificial defect, and lifetime testing method for roller bearing

    JP2004340808A

  • Method for predicting maximum inclusion diameter in steel product by ultrasonic fatigue test

    JP2020034292A

  • Test piece, test piece manufacturing method, and rolling fatigue test method using the test piece

    JP2020063922A