Preparation method and application of intelligent self-lubricating liner
By conducting conductive treatment and conductivity enhancement on the self-lubricating fabric, combined with the modification of phenolic resin, an intelligent self-lubricating liner capable of monitoring changes in bearing resistance is prepared, which solves the time-consuming and error problems of traditional self-lubricating bearing wear detection and achieves It combines the intelligent monitoring of liner wear and the electrical conductivity of the bearing, and is simple, efficient and environmentally friendly.
Patent Information
- Application Number
- CN202410887338.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
The traditional self-lubricating bearing pad wear detection method requires manual participation, is time-consuming and contains errors, and disassembly and installation may affect the normal operation of other parts of the equipment, making it difficult to achieve intelligent monitoring.
By surface roughening, conductivity treatment and conductivity enhancement of self-lubricating fabrics, combined with conductive modification of phenolic resin, an intelligent self-lubricating liner capable of monitoring changes in bearing resistance is prepared to achieve real-time detection of liner wear.
It realizes intelligent monitoring of liner wear, improves the conductivity and friction and wear performance of the liner, simplifies the process, and does not pollute the environment, so it has strong development potential.
Smart Images

Figure CN118727448A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of self-lubricating bearings, and in particular to a preparation method and application of an intelligent self-lubricating liner. Background Art
[0002] Self-lubricating bearings are bearings that have a small amount of lubricant or no lubricant at all, so that the sliding bearings have their own lubrication. Self-lubricating bearing technology breaks through the limitations of general grease lubrication and achieves oil-free lubrication, eliminating the need for lubrication devices and sealing devices for lubricating oil and grease, thereby greatly simplifying the design of bearings and reducing costs. Self-lubricating material bearing technology is the current development trend of lubrication technology, and the development of self-lubricating composite materials with high mechanical strength and good friction performance has become the focus of the field of tribology.
[0003] Traditional liner-type self-lubricating bearings are made by pasting a layer of self-lubricating liner material on the inner spherical surface of the outer ring of the bearing. The sliding friction of the liner sliding surface on the outer spherical surface of the inner ring replaces the sliding friction of the steel surface, thereby playing a role in reducing wear and resisting wear. They are currently widely used in the fields of aviation and engineering machinery. The main failure form of liner-type self-lubricating bearings is liner wear. Currently, the wear amount of liner-type self-lubricating bearings is usually measured by feeler gauges during shutdown or measured by clearance after disassembly. Both require manual work, which is time-consuming, has certain manual errors, and the disassembly and installation of bearings may affect the normal operation of other parts of the equipment. With the development of intelligent equipment, intelligent requirements are put forward for the wear status monitoring of key motion nodes. Therefore, the present invention proposes a preparation method and application of an intelligent self-lubricating liner. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention proposes a preparation method and application of an intelligent self-lubricating liner, which can intelligently monitor the wear of the liner.
[0005] In order to achieve the above object, the present invention is implemented by the following technical solution: a method for preparing an intelligent self-lubricating liner, comprising the following steps:
[0006] S1: using organic solvent to roughen and remove impurities from the surface of self-lubricating fabric;
[0007] S2: soaking the self-lubricating fabric with roughened and impurity-removed surface in a reaction solution to make it conductive;
[0008] S3: soaking the self-lubricating fabric after the soaking treatment in a conductive enhancement solution;
[0009] S4: Phenolic resin is applied on the surface of the self-lubricating fabric after the conductivity enhancement treatment.
[0010] Furthermore, the self-lubricating fabric is a PTFE-aramid fabric made by mixing and weaving aramid fibers and tetrafluoroethylene fibers.
[0011] Furthermore, the organic solvent is one of methanol, ethanol, acetone, butyl acetate and DMF solution.
[0012] Furthermore, the reaction solution is one or more of a PEDOT-PSS solution, a d-sorbitol solution, a dimethyl sulfoxide solution and a sodium dodecyl sulfate solution.
[0013] Furthermore, the reaction solution is a PEDOT-PSS solution, and a PEDOT-PSS solid powder and a solvent (wherein the PEDOT-PSS solid powder is (3,4-ethylenedioxythiophene)-poly(4-styrenesulfonic acid, and the solvent is one of water, methanol, ethanol or acetone; and the ratio of the mass of the PEDOT-PSS solid powder to the volume of the solvent is 1 g:0.13 L) are stirred, dissolved and evenly mixed to obtain a PEDOT-PSS solution; the self-lubricating fabric is immersed in the PEDOT-PSS solution for multiple times, and the ratio of the mass of the PEDOT-PSS solid powder to the volume of the solvent is 1 g:0.13 L.
[0014] Furthermore, the self-lubricating fabric is immersed in a PEDOT-PSS solution for six times, the temperature of the PEDOT-PSS solution is 20° C., and the immersion times are 30 s, 1 min, 5 min, 10 min, 30 min and 60 min, respectively.
[0015] Furthermore, the conductivity enhancing solution is one of dilute hydrochloric acid, dilute sulfuric acid, ferric chloride solution or DMF solution containing graphite.
[0016] Furthermore, the self-lubricating fabric was immersed in the conductive enhancing solution for three times, the temperature of the conductive enhancing solution was 20° C., and the immersion time was 30 min. After the immersion in the conductive enhancing solution was completed, the self-lubricating fabric was heat treated.
[0017] Furthermore, a conductive modified phenolic resin is applied on one surface of the self-lubricating fabric, and an unmodified phenolic resin is applied on the other surface. The conductive modified phenolic resin is a phenolic resin with conductive filler, and the conductive filler is one or more of graphite, graphene, carbon fiber and carbon nanotubes.
[0018] An application of an intelligent self-lubricating pad is to use an intelligent self-lubricating pad prepared by any of the preparation methods described above, bond the self-lubricating pad to a bearing, and monitor changes in the resistance value of the bearing.
[0019] The beneficial effects of the preparation method and application of the above-mentioned intelligent self-lubricating liner are:
[0020] By soaking the self-lubricating fabric in a reaction solution to make it conductive, and then further improving the conductivity of the self-lubricating fabric with a conductive enhancing solution, and by setting a conductive layer and an insulating layer on both sides of the conductive self-lubricating fabric, the wear degree of the pad can be determined by monitoring the resistance change of the bearing. In addition, the preparation method is simple and efficient, has no pollution to the environment, can significantly improve the conductivity of the pad and effectively apply it to intelligent self-lubricating bearings, improves the friction and wear performance, and makes the bearing as a whole have electrical conductivity, and has great development potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation of the present invention, the following will briefly introduce the drawings required for use in the specific implementation. In all the drawings, each element or part is not necessarily drawn according to the actual scale.
[0022] Figure 1 This is a test diagram of the friction and wear performance and electrical conductivity of the self-lubricating liner in Example 1 of the present invention;
[0023] Figure 2 This is a test diagram of the friction and wear performance and electrical conductivity of the self-lubricating liner in Example 2 of the present invention;
[0024] Figure 3 This is a test chart of the friction and wear performance and electrical conductivity of the self-lubricating pad in Example 3 of the present invention. DETAILED DESCRIPTION
[0025] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.
[0026] The present invention provides a method for preparing an intelligent self-lubricating liner, comprising the following steps:
[0027] S1: using organic solvent to roughen and remove impurities from the surface of self-lubricating fabric;
[0028] S2: soaking the self-lubricating fabric with roughened and impurity-removed surface in a reaction solution to make it conductive;
[0029] S3: soaking the self-lubricating fabric after the soaking treatment in a conductive enhancement solution;
[0030] S4: Phenolic resin is applied on the surface of the self-lubricating fabric after the conductivity enhancement treatment.
[0031] Specifically, the self-lubricating fabric is a PTFE-aramid fabric made by mixing aramid fibers and tetrafluoroethylene fibers, the organic solvent is one of methanol, ethanol, acetone, butyl acetate and DMF solution, the reaction solution is one or more of PEDOT-PSS solution, d-sorbitol solution, dimethyl sulfoxide and sodium dodecyl sulfate solution, and the conductivity enhancing solution is one of dilute hydrochloric acid, dilute sulfuric acid, ferric chloride solution or DMF solution containing graphite.
[0032] An application of an intelligent self-lubricating pad is to use the intelligent self-lubricating pad prepared by the preparation method, bond the self-lubricating pad to a bearing, and monitor the change of the resistance value of the bearing.
[0033] In the following embodiments, the friction and wear properties and electrical conductivity of the self-lubricating gasket material prepared in each embodiment were measured at room temperature. The measurement conditions were a load of 220 MPa, a frequency of 10 times / min, and a swing angle of ±25°. The wear amount and the corresponding electrical conductivity after 100,000 swings were measured.
[0034] Example 1
[0035] This embodiment provides a method for preparing an intelligent self-lubricating liner, comprising the following steps:
[0036] S1: Preparation of PEDOT-PSS solution;
[0037] Prepare 300 ml of 1.3 wt% PEDOT-PSS solution, specifically: prepare the required PEDOT-PSS solid powder and solvent, wherein the PEDOT-PSS solid powder is (3,4-ethylenedioxythiophene)-poly(4-styrenesulfonic acid), the solvent is ethanol, and the mass ratio of the PEDOT-PSS solid powder to the solvent (ethanol) is 1 g:0.13 L.
[0038] More specifically: weigh 3.9g of PEDOT-PSS solid powder, slowly add it to an appropriate amount of solvent, and stir it with a glass rod or magnetic stirrer until the PEDOT-PSS solid powder is completely dissolved. After the solution is fully and evenly mixed, ensure that the PEDOT-PSS solid powder is evenly dispersed in the solvent, check the concentration of the solution to ensure that it reaches the required 1.3wt%; if the volume of the solution is less than 300ml, add an appropriate amount of solvent to dilute it. If the solution exceeds 300ml, heat it to evaporate part of the solvent and reduce the volume of the solution to 300ml;
[0039] S2: Preparation of conductive self-lubricating pad
[0040] First, the PTFE-aramid fabric was cleaned with 0.5wt% butyl acetate to remove surface dirt and impurities and improve wettability; the PTFE-aramid fabric was immersed in a 1.3wt% PEDOT-PSS solution at 20°C for six times, with the immersion time being 30s, 1min, 5min, 10min, 30min and 60min respectively to ensure sufficient solution penetration and absorption; after the immersion, it was heat treated at 100°C for 30min to promote the polymerization of PEDOT-PSS and the volatilization of the solvent, so that the PTFE-aramid fabric has conductivity;
[0041] S3: Preparation of enhanced conductive self-lubricating liner
[0042] Then, the PTFE-aramid fabric obtained in step S2 was immersed in dilute hydrochloric acid (10 wt %) at 20° C. for three times, each time for 30 min, to ensure sufficient solution penetration and absorption, and the PEDOT-PSS-modified PTFE-aramid fabric was subjected to secondary modification to further improve the conductivity of the PTFE-aramid fabric;
[0043] S4: Preparation of smart self-lubricating liner
[0044] Finally, the surface of the self-lubricating fabric obtained in step S3 is dipped in phenolic resin for a second time.
[0045] First, weigh phenolic resin, ethyl acetate, anhydrous ethanol and conductive filler (graphene) in a mass ratio of 3:1:1:1, mix the phenolic resin, ethyl acetate and anhydrous ethanol evenly, and then add the conductive filler (graphene) to obtain a first impregnation liquid; evenly apply the first impregnation liquid on one side of the self-lubricating fabric liner so that the thickness of the phenolic resin on the surface of the self-lubricating fabric is uniform, and dry it to obtain the self-lubricating fabric after the first impregnation;
[0046] A phenolic resin, ethyl acetate and anhydrous ethanol in a mass ratio of 4:1:1 are weighed again for the second time, and mixed evenly to obtain a second impregnation liquid; the second impregnation liquid is evenly applied to the other side of the self-lubricating fabric after the first impregnation, and the self-lubricating fabric after the second impregnation is obtained after drying; after the second impregnation is completed, the self-lubricating fabric is high-temperature cured at 180°C for 1h to obtain an intelligent self-lubricating pad.
[0047] Finally, the intelligent self-lubricating pad sample obtained above was tested. The side coated with conductive phenolic resin (first impregnation liquid) was bonded to the lower specimen, and the tribological properties of the sample were tested using a screen-displayed high-temperature material end face friction and wear tester at room temperature, a load of 500N, and a sliding speed of 0.36m / s. At the same time, a multimeter was used to measure the resistance change of the intelligent self-lubricating pad in real time, and a GFM wear tester was used to measure the wear scar depth of the pad every 1min.
[0048] The curve of the change of the vertical resistance of the intelligent self-lubricating pad with time when the pad is worn is as follows: Figure 1 As shown in the figure, it can be seen that in the early stage of wear, the resistance value increases rapidly. As time goes by, the resistance value drops sharply at a certain moment, and finally decreases to about 100 ohms and tends to be flat. The resistance changes from high to low, which represents the wear from the insulating layer of the pad to the conductive layer of the pad. The real-time monitoring of the pad wear is achieved through the change of resistance value or the accumulation of electrical signals. In the subsequent wear process, the resistance value shows an upward trend because the conductive layer has been worn through.
[0049] Example 2
[0050] This embodiment is basically the same as Example 1, except that the conductive enhancement solution is a 1M ferric chloride solution. Specifically, the PTFE-aramid fabric is immersed in the ferric chloride solution at 20°C for three times for 30 minutes each time to ensure sufficient solution penetration and absorption, and the PEDOT-PSS-modified PTFE-aramid fabric is subjected to secondary modification to further improve the conductivity of the PTFE-aramid fabric.
[0051] Finally, the obtained intelligent self-lubricating pad sample was tested. The side coated with conductive phenolic resin (first impregnation liquid) was bonded to the lower specimen, and the tribological properties of the sample were tested using a screen-displayed high-temperature material end face friction and wear tester at room temperature, a load of 500N, and a sliding speed of 0.36m / s. At the same time, a multimeter was used to measure the resistance change of the intelligent self-lubricating pad in real time, and a GFM wear tester was used to measure the wear scar depth of the pad every 1min.
[0052] The curve of the change of the vertical resistance of the intelligent self-lubricating pad with time when the pad is worn is as follows: Figure 2 As shown in the figure, it can be seen that in the early stage of wear, due to the uneven dispersion of ferric chloride solution, the initial resistance value is very high and keeps floating. As time goes by, the resistance value begins to decrease, and finally decreases to about 5 ohms and tends to be flat. The resistance from high to low represents the wear from the insulating layer of the pad to the conductive layer of the pad. The floating increase in resistance is due to the real-time monitoring of the pad wear through the change of resistance value or the accumulation of electrical signals.
[0053] Example 3
[0054] This embodiment is basically the same as Example 1, except that the conductive enhancement solution is a DMF solution containing graphite (wherein the mass ratio of graphite to DMF is 1:20), specifically: the PTFE-aramid fabric is immersed in the DMF solution containing graphite at 20°C for three times, each time for 30 minutes, to ensure sufficient solution penetration and absorption, and the PEDOT-PSS-modified PTFE-aramid fabric is subjected to secondary modification to further improve the conductivity of the PTFE-aramid fabric.
[0055] Finally, the obtained intelligent self-lubricating pad sample was tested. The side coated with conductive phenolic resin (first impregnation liquid) was bonded to the lower specimen, and the tribological properties of the sample were tested using a screen-displayed high-temperature material end face friction and wear tester at room temperature, a load of 500N, and a sliding speed of 0.36m / s. At the same time, a multimeter was used to measure the resistance change of the intelligent self-lubricating pad in real time, and a GFM wear tester was used to measure the wear scar depth of the pad every 1min.
[0056] The curve of the change of the vertical resistance of the intelligent self-lubricating pad with time when the pad is worn is as follows: Figure 3 As shown in the figure, it can be seen that in the early stage of wear, the resistance value increases in stages. As time goes by, the resistance value begins to decrease and fluctuates continuously, eventually decreasing to about 10 ohms and tends to be flat. The resistance changes from high to low, which represents the wear from the insulating layer of the liner to the conductive layer of the liner. The real-time monitoring of the liner wear can be achieved through the change of resistance value or the accumulation of electrical signals.
[0057] The present application provides a preparation method and application of an intelligent self-lubricating pad, which makes the self-lubricating fabric conductive by immersing it in a reaction solution, and further improves the conductivity of the self-lubricating fabric by using a conductive enhancing solution, and finally sets a conductive layer and an insulating layer on both sides of the conductive self-lubricating fabric, so that the wear degree of the pad can be judged by monitoring the resistance change of the bearing. In addition, the preparation method is simple and efficient, has no pollution to the environment, can significantly improve the conductivity of the pad and effectively apply it to intelligent self-lubricating bearings, improves the friction and wear performance, and makes the bearing as a whole have electrical conductivity, and has great development potential.
[0058] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing an intelligent self-lubricating liner, characterized in that: The following steps are involved: S1: using organic solvent to roughen and remove impurities from the surface of self-lubricating fabric; S2: soaking the self-lubricating fabric with roughened and impurity-removed surface in a reaction solution to make it conductive; S3: soaking the self-lubricating fabric after the soaking treatment in a conductive enhancement solution; S4: Phenolic resin is applied on the surface of the self-lubricating fabric after the conductivity enhancement treatment.
2. The method for preparing an intelligent self-lubricating liner according to claim 1, characterized in that: The self-lubricating fabric is a PTFE-aramid fabric made by mixing and weaving aramid fibers and tetrafluoroethylene fibers.
3. The method for preparing an intelligent self-lubricating liner according to claim 2, characterized in that: The organic solvent is one of methanol, ethanol, acetone, butyl acetate and DMF solution.
4. The method for preparing an intelligent self-lubricating liner according to claim 1, characterized in that: The reaction solution is one or more of a PEDOT-PSS solution, a d-sorbitol solution, a dimethyl sulfoxide solution and a sodium dodecyl sulfate solution.
5. The method for preparing an intelligent self-lubricating liner according to claim 4, characterized in that: The reaction solution is a PEDOT-PSS solution, and the PEDOT-PSS solid powder and the solvent are stirred to dissolve and evenly mix to form a PEDOT-PSS solution; the self-lubricating fabric is immersed in the PEDOT-PSS solution for multiple times, wherein the PEDOT-PSS solid powder is (3,4-ethylenedioxythiophene)-poly(4-styrenesulfonic acid), the solvent is one of water, methanol, ethanol or acetone, and the ratio of the mass of the PEDOT-PSS solid powder to the volume of the solvent is 1g:0.13L.
6. The method for preparing an intelligent self-lubricating liner according to claim 5, characterized in that: The self-lubricating fabric is immersed in a PEDOT-PSS solution for six times, the temperature of the PEDOT-PSS solution is 20° C., and the immersion times are 30 s, 1 min, 5 min, 10 min, 30 min and 60 min, respectively.
7. The method for preparing an intelligent self-lubricating liner according to claim 4, characterized in that: The conductivity enhancing solution is one of dilute hydrochloric acid, dilute sulfuric acid, ferric chloride solution or DMF solution containing graphite.
8. The method for preparing an intelligent self-lubricating liner according to claim 7, characterized in that: The self-lubricating fabric was immersed in the conductive enhancing solution for three times, the temperature of the conductive enhancing solution was 20° C., and the immersion time was 30 minutes. After the immersion in the conductive enhancing solution was completed, the self-lubricating fabric was subjected to heat treatment.
9. The method for preparing an intelligent self-lubricating liner according to claim 1, characterized in that: Conductive modified phenolic resin is applied on one surface of the self-lubricating fabric, and unmodified phenolic resin is applied on the other surface. The conductive modified phenolic resin contains conductive filler, which is one or more of graphite, graphene, carbon fiber and carbon nanotube.
10. An application of an intelligent self-lubricating gasket, the intelligent self-lubricating gasket prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The self-lubricating pad is bonded to the bearing and the change in the resistance value of the bearing is monitored.
Citation Information
Cited By
Polymer material for intelligent self-lubricating joint bearing as well as preparation method and application of polymer material
CN122425947A
Self-lubricating bearing based on electroluminescence service state recognition and manufacturing method
CN122565834A
Novel gasket material for intelligent self-lubricating joint bearing as well as preparation method and application of novel gasket material
CN122584703A
Self-lubricating bearing, device and method based on magnetic response wear state recognition
CN122650101A
Self-lubricating bearing and method based on force-induced luminescence service condition recognition
CN122981242A