Method for continuously generating silicon monoxide gas

The method of using lithium silicate and silicon with moisture adsorption prevention and reduced pressure storage/supplying ensures continuous silicon monoxide gas generation by preventing moisture absorption, addressing the issue of increased pressure in the reaction chamber.

JP7564225B2Active Publication Date: 2024-10-08OSAKA TITANIUM TECHNOLOGIES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022550373
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-16
Filing Date
2021-07-13
Publication Date
2024-10-08
Estimated Expiration
2041-07-13

AI Technical Summary

Technical Problem

Existing methods for generating silicon monoxide gas are inhibited by the generation of large amounts of water vapor and hydrogen gas due to moisture absorption, leading to increased internal pressure in the reaction chamber.

Method used

A method involving a moisture adsorption prevention step to maintain a moisture content of 0.6% by weight or less in the silicon monoxide gas generation raw material, using lithium silicate and silicon, and storing and supplying the raw material under reduced pressure to prevent moisture adsorption.

Benefits of technology

This approach allows continuous generation of silicon monoxide gas without inhibiting the reaction, suppressing the generation of water vapor and hydrogen gas, thereby maintaining a stable reaction environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564225000001
    Figure 0007564225000001
  • Figure 0007564225000002
    Figure 0007564225000002
Patent Text Reader

Abstract

The present invention addresses the problem of providing a silicon monoxide gas generating material with which the reaction for generating silicon monoxide (SiO) gas is unlikely to be inhibited. The silicon monoxide gas generating material according to the present invention has a water content of 0.6 wt% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a raw material for generating silicon monoxide (SiO) gas. The present invention also relates to a method for continuously generating silicon monoxide gas.

Background Art

[0002] "Silicon oxide powder having an average composition represented by SiO x (0.5 < x < 1.5), and when subjected to XRD measurement, in the range of diffraction angle 2θ = 10 to 60°, only one broad crystal peak having a half-value width of 2° or more is detected at 10 to 40°. When the intensity of the broad crystal peak is P1, the intensity P2 of other crystal peaks satisfies P2 / P1 < 0.1" has been proposed in the past (see, for example, Japanese Patent Application Laid-Open No. 2019-67644, etc.).

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0004] By the way, a mixed powder of silicon (Si) alone and silicon dioxide (SiO2) or the like is heat-treated to generate silicon monoxide (SiO) gas, the generated silicon monoxide gas is cooled, and the precipitated silicon oxide (SiO x ) is pulverized to obtain silicon oxide powder as described in Patent Document 1. When such a mixed powder is stored for a long time in an environment with a relatively high humidity or the like, it adsorbs moisture in the air. When a heat-treated mixed powder adsorbed with moisture (having a high moisture content (weight%)) is used to generate silicon monoxide gas, a large amount of water vapor (H2O) and a large amount of hydrogen (H2) gas are also generated. When a large amount of water vapor and a large amount of hydrogen gas are generated, the internal pressure in the reaction chamber increases, and the reaction for generating silicon monoxide gas is inhibited.

[0005] An object of the present invention is to provide a silicon monoxide gas generating raw material in which the reaction for generating silicon monoxide gas is not easily inhibited. [Means for solving the problem]

[0006] A method for continuously generating silicon monoxide gas according to a first aspect of the present invention includes a moisture adsorption prevention step of preventing moisture in the air from being adsorbed onto a silicon monoxide gas generating raw material having a moisture content of 0.6% by weight or less, and a raw material introduction step of continuously introducing the silicon monoxide gas generating raw material into a reaction chamber for generating silicon monoxide gas. The silicon monoxide gas generating raw material contains lithium silicate and silicon (Si).

[0007] As described above, in this method for continuously generating silicon monoxide gas, a silicon monoxide gas generating raw material having a moisture content of 0.6% by weight or less is continuously fed into a reaction chamber for generating silicon monoxide gas (i.e., a reaction chamber for heat-treating the silicon monoxide gas generating raw material). Therefore, the amount of water vapor and hydrogen gas generated during the generation of silicon monoxide gas can be suppressed. Therefore, in this method for continuously generating silicon monoxide gas, silicon monoxide gas can be continuously generated without inhibiting the reaction that generates silicon monoxide gas. In addition, as a result of intensive research by the present inventors, it was found that when a silicon monoxide gas generating raw material containing lithium silicate and silicon is mixed with water, molded, and then dried to form granules, the lithium silicate and silicon are firmly bonded together. Therefore, this silicon monoxide gas generating raw material has mechanical strength when it contains silicate (lithium silicate).

[0008] A method for continuously generating silicon monoxide gas according to a second aspect of the present invention is the method for continuously generating silicon monoxide gas according to the first aspect, wherein the moisture adsorption prevention step includes a storage step of storing the silicon monoxide gas generating raw material in a state not exposed to the atmosphere or under reduced pressure.

[0009] A method for continuously generating silicon monoxide gas according to a third aspect of the present invention is the method for continuously generating silicon monoxide gas according to the first aspect, wherein the moisture adsorption prevention step includes a step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber while not being exposed to the atmosphere or under reduced pressure.

[0010] A method for continuously generating silicon monoxide gas according to a fourth aspect of the present invention is the method for continuously generating silicon monoxide gas according to the second aspect, wherein the moisture adsorption prevention step further includes, after the storage step, a supply step of supplying the silicon monoxide gas generating raw material while not exposed to the atmosphere or under reduced pressure to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber.

[0011] A method for continuously generating silicon monoxide gas according to a fifth aspect of the present invention includes a moisture adsorption prevention step of preventing moisture in the air from being adsorbed onto a silicon monoxide gas generating raw material having a moisture content of 0.6% by weight or less, and a raw material introduction step of continuously introducing the silicon monoxide gas generating raw material into a reaction chamber for generating silicon monoxide gas.

[0012] As described above, in this method for continuously generating silicon monoxide gas, a silicon monoxide gas generating raw material having a moisture content of 0.6% by weight or less is continuously fed into a reaction chamber for generating silicon monoxide gas (i.e., a reaction chamber for heat-treating the silicon monoxide gas generating raw material). Therefore, the amount of water vapor and hydrogen gas generated during the generation of silicon monoxide gas can be suppressed. Therefore, in this method for continuously generating silicon monoxide gas, silicon monoxide gas can be continuously generated without inhibiting the reaction that generates silicon monoxide gas.

[0013] A method for continuously generating silicon monoxide gas according to a sixth aspect of the present invention is the method for continuously generating silicon monoxide gas according to the fifth aspect, wherein the moisture adsorption prevention step includes a storage step of storing the silicon monoxide gas generating raw material in a state not exposed to the atmosphere or under reduced pressure.

[0014] A method for continuously generating silicon monoxide gas according to a seventh aspect of the present invention is the method for continuously generating silicon monoxide gas according to the fifth aspect, wherein the moisture adsorption preventing step includes a step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber while not being exposed to the atmosphere or under reduced pressure.

[0015] A method for continuously generating silicon monoxide gas according to an eighth aspect of the present invention is the method for continuously generating silicon monoxide gas according to the sixth aspect, wherein the moisture adsorption prevention step further includes, after the storage step, a supply step of supplying the silicon monoxide gas generating raw material without exposure to the atmosphere or under reduced pressure to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic diagram of an apparatus for producing active material particles using a silicon monoxide gas generating raw material according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the manufacturing apparatus shown in FIG. 1 to which a drying mechanism is added. [Explanation of symbols]

[0017] 100 Vapor deposition equipment 110 Crucible 120 Heater 130 Evaporation drum 141 Scraper 143 Particle Guide 150 Chamber 151 Chamber body 152 Recovery Department 153 Exhaust pipe 160 Raw material supply hopper 170 Raw material introduction pipe 180 Collection Container 190 Recovery tube 200 Drying mechanism 210 Raw material introduction pipe Gg Gas Guide OP Opening RM precipitation chamber Sr Silicon monoxide gas generating material VL1 First valve VL2 Second valve DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The silicon monoxide gas generating raw material Sr according to the embodiment of the present invention is used to generate silicon monoxide (SiO) gas. As the silicon monoxide gas generating raw material Sr, for example, a "mixed powder of silicon (Si) and silicon dioxide (SiO2)" or a "mixed powder of silicon and a silicate such as lithium silicate (Li2Si2O5, etc.)" is used. The "mixed powder of silicon and silicon dioxide" is used when producing silicon oxide granules, and generates silicon monoxide gas by being heated. The "mixed powder of silicon and a silicate such as lithium silicate" is used when producing silicon oxide granules containing a metal element, and generates silicon monoxide gas containing a metal element such as lithium (Li) by being heated. The metal element may be an element capable of reducing silicon monoxide and stabilizing oxygen, such as an alkali metal such as sodium (Na) or an alkaline earth metal such as magnesium (Mg) or calcium (Ca), other than lithium.

[0019] The silicon monoxide gas generating raw material Sr according to the embodiment of the present invention is dried (described later) before being heated. This drying is performed to reduce the amount of moisture in the silicon monoxide gas generating raw material Sr. Examples of the drying method include heat drying and reduced pressure drying.

[0020] The dried silicon monoxide gas generating raw material Sr is heated to a predetermined temperature to generate silicon monoxide gas, from which active material particles are manufactured through the steps described below. Examples of such active material particles include silicon oxide particles and metal element-containing silicon oxide particles used as active materials for electrodes (particularly, negative electrodes) of lithium ion secondary batteries.

[0021] Incidentally, in order to finally produce active material particles using the silicon monoxide gas generating raw material Sr according to the embodiment of the present invention, it is preferable to use a vapor deposition apparatus 100 as shown in Fig. 1. The vapor deposition apparatus 100 is excellent from the viewpoint of suppressing production costs, etc. The vapor deposition apparatus 100 will be described in detail below.

[0022] As shown in FIG. 1, the deposition apparatus 100 is mainly composed of a crucible 110, a heater 120, a deposition drum 130, a scraper 141, a granular guide 143, a chamber 150, a raw material supply hopper 160, a raw material introduction pipe 170, a recovery container 180, a first valve VL1, and a second valve VL2.

[0023] The crucible 110 is a heat-resistant container with an opening at the center of the top wall as shown in Fig. 1, and is installed in the chamber 150. A through hole (not shown) is formed at one location on the periphery of the top wall of the crucible 110, and a raw material introduction pipe 170 is inserted into the through hole. That is, the silicon monoxide gas generating raw material Sr after drying treatment in the raw material supply hopper 160 is supplied to the crucible 110 through the raw material introduction pipe 170. A gas guide Gg is disposed on the upper side of the top wall of the crucible 110. The gas guide Gg is a member that guides the silicon monoxide gas generated in the crucible 110 to the deposition drum 130, and is installed on the upper surface of the top wall so as to surround the central part of the top wall as shown in Fig. 1.

[0024] The heater 120 is for heating the crucible 110 to a high temperature, and is disposed so as to surround the outer periphery of the crucible 110 .

[0025] The deposition drum 130 is, for example, a cylindrical horizontal drum, and is disposed above an opening OP in the top wall of the crucible 110 as shown in FIG. 1, and its lower portion is surrounded by a gas guide Gg. The deposition drum 130 is rotated in one direction by a driving mechanism (not shown). The deposition drum 130 is provided with a temperature regulator (not shown) for keeping the outer peripheral surface at a constant temperature. The temperature regulator cools the outer peripheral surface temperature of the deposition drum 130 to a temperature suitable for deposition of the deposition source gas by a cooling medium supplied from the outside. The outer peripheral surface temperature of the deposition drum 130 may affect the crystallinity of the precipitate deposited on the precipitate remaining on the deposition drum. If the temperature is too low, the texture of the precipitate may become too sparse, and conversely, if the temperature is too high, crystal growth due to disproportionation reaction may proceed. When silicon monoxide gas is deposited, the temperature is preferably 900°C or less, more preferably in the range of 150°C to 800°C, and especially preferably in the range of 150°C to 700°C.

[0026] The scraper 141 is a member that serves to scrape off the thin film formed on the deposition drum from the deposition drum 130. The scraped-off thin film pieces (active material particles) fall onto a particle guide 143. The material of the scraper 141 affects impurity contamination of the active material particles. In order to suppress this effect, the material of the scraper 141 is preferably stainless steel or ceramics, and particularly preferably ceramics. The scraper 141 is preferably not brought into contact with the outer circumferential surface of the deposition drum 130. This is because this can prevent impurity contamination that may occur due to direct contact between the deposition drum 130 and the scraper 141 from being mixed into the recovered active material particles.

[0027] The granular guide 143 is, for example, a vibrating conveying member, and as shown in FIG. 1, is arranged so as to incline downward as it moves from the vicinity of the deposition drum 130 toward the collection section 152 of the chamber 150. The granular guide 143 receives thin film fragments scraped off by the scraper 141 arranged above it and sends them to the collection section 152 of the chamber 150.

[0028] As shown in FIG. 1, the chamber 150 is mainly formed of a chamber main body 151, a recovery section 152, and an exhaust pipe 153. As shown in FIG. 1, the chamber main body 151 is a box-shaped section having a deposition chamber RM therein, and accommodates the crucible 110, the heater 120, the deposition drum 130, the scraper 141, and the particle guide 143. As shown in FIG. 1, the recovery section 152 is a section that protrudes outward from the side wall of the chamber main body 151, and has a space that communicates with the deposition chamber RM of the chamber main body 151. As described above, the tip section of the particle guide 143 is located in the recovery section 152.

[0029] The raw material supply hopper 160 is a silicon monoxide gas generating raw material supply source, and has an outlet connected to a raw material introduction pipe 170 as shown in Fig. 1. That is, the dried silicon monoxide gas generating raw material Sr fed into the raw material supply hopper 160 is continuously supplied to the crucible 110 via the raw material introduction pipe 170 at an appropriate timing. The dried silicon monoxide gas generating raw material Sr supplied to the crucible 110 becomes silicon monoxide gas.

[0030] The raw material introduction pipe 170 is a round-hole nozzle for continuously introducing the dried silicon monoxide gas generating raw material Sr that has been introduced into the raw material supply hopper 160 into the crucible 110, and is disposed in the center of the top plate of the crucible 110 with its mouth facing upward.

[0031] The collection container 180 is a container for collecting the thin film pieces that have passed through the first valve VL1 and the second valve VL2.

[0032] The first valve VL1 and the second valve VL2 are used to adjust the amount of thin film pieces collected in the collection container 180 by opening and closing, and are provided on a collection pipe 190 that connects the collection part 152 of the chamber 150 and the collection container 180.

[0033] Hereinafter, a case will be described in which silicon oxide particles or metal element-containing silicon oxide particles used for negative electrode materials for lithium ion secondary batteries are finally produced from silicon monoxide gas generating raw material Sr using the above-mentioned vapor deposition apparatus 100.

[0034] First, the silicon monoxide gas generating raw material Sr is dried (heat drying, drying under reduced pressure, etc.). Here, when the silicon monoxide gas generating raw material Sr is dried, for example, by heating drying, it is preferably dried for 1 hour or more and 240 hours or less, within a range of 100°C or more and 400°C or less, and more preferably dried for 4 hours or more and 120 hours or less, within a range of 200°C or more and 350°C or less. When the silicon monoxide gas generating raw material Sr is dried, for example, by reduced pressure drying, it is preferably dried under reduced pressure with a vacuum pump controlled to a range of 10 Pa or more and 100 Pa or less, within a range of 12 hours or more and 120 hours or less, and more preferably dried under reduced pressure with a vacuum pump controlled to a range of 0.1 Pa or more and 100 Pa or less, within a range of 12 hours or more and 240 hours or less. When the silicon monoxide gas generating raw material Sr is dried under these conditions, the moisture in the silicon monoxide gas generating raw material Sr can be removed without generating silicon monoxide gas as much as possible. As described above, the moisture content of the silicon monoxide gas generating raw material Sr after drying is 0.6% by weight or less, preferably 0.3% by weight or less, and more preferably 0.1% by weight or less. In addition, the silicon monoxide gas generating raw material Sr after drying is preferably stored in a sealed container or under reduced pressure.

[0035] Next, the silicon monoxide gas generating raw material Sr after the drying process is charged into the raw material supply hopper 160. Then, the silicon monoxide gas generating raw material Sr after the drying process is continuously charged from the raw material supply hopper 160 through the raw material introduction pipe 170 into the crucible 110.

[0036] Next, when the dried silicon monoxide gas generating raw material Sr is put into the crucible 110, the crucible 110 is heated by the heater 120 while reducing the pressure inside the deposition chamber RM. If the silicon monoxide gas generating raw material Sr has a high moisture content (weight %), a large amount of water vapor and a large amount of hydrogen gas, etc. are generated by heating with the heater 120. If a large amount of water vapor and a large amount of hydrogen gas, etc. are generated, the pressure inside the deposition chamber RM increases. If the pressure inside the deposition chamber RM is too high, the reaction of generating silicon monoxide gas from the dried silicon monoxide gas generating raw material Sr becomes difficult to occur. Here, the pressure inside the deposition chamber RM is preferably 100 Pa or less, more preferably 75 Pa or less, and particularly preferably 20 Pa or less. Furthermore, the temperature in the deposition chamber RM affects the reaction rate of silicon monoxide, and if the temperature is too low, the reaction rate slows down, while if the temperature is too high, there are concerns that side reactions may proceed due to melting of the silicon monoxide gas generating raw material Sr after the drying process, and that energy efficiency may decrease. There is also concern that the temperature may damage the crucible 110. From this perspective, the temperature in the deposition chamber RM is preferably within a range of 1000°C to 1600°C, more preferably within a range of 1100°C to 1500°C, and particularly preferably within a range of 1100°C to 1400°C.

[0037] As described above, the silicon monoxide gas generating raw material Sr after drying is subjected to a reduced pressure heating process, whereby silicon monoxide gas is generated from the silicon monoxide gas generating raw material Sr after drying process in the crucible 110, and the silicon monoxide gas is supplied to the deposition drum 130 through the gas guide Gg. At this time, the deposition drum 130 is rotated by the drive source. The temperature of the outer circumferential surface of the deposition drum 130 is set lower than the temperature in the deposition chamber RM. More specifically, the temperature is set lower than the condensation temperature of the silicon monoxide gas. With this setting, the silicon monoxide gas generated from the crucible 110 is evaporated, precipitated, and accumulated on the outer circumferential surface of the rotating deposition drum 130. Then, a thin film is formed on the deposition drum 130. Then, the thin film on the deposition drum 130 comes into contact with the scraper 141, whereby the thin film is scraped off from the deposition drum 130. The scraped off pieces of the thin film (active material particles) fall along the outer circumferential surface of deposition drum 130 into particle guide 143.

[0038] In the deposition apparatus 100 of the present embodiment, as described above, high-quality active material particles are finally produced from the silicon monoxide gas generating raw material Sr.

[0039] When the dried silicon monoxide gas generating raw material Sr is fed into the raw material feeding hopper 160, it is preferable not to expose the dried silicon monoxide gas generating raw material Sr to the atmosphere. This is because moisture in the atmosphere may be adsorbed by the dried silicon monoxide gas generating raw material Sr. In order to prevent the dried silicon monoxide gas generating raw material Sr from being exposed to the atmosphere, for example, a drying mechanism 200 and a raw material feeding pipe 210 may be configured in the deposition device 100 (see FIG. 2). According to this configuration, first, as shown in FIG. 2, the silicon monoxide gas generating raw material Sr before drying is fed into the drying mechanism 200. Then, the silicon monoxide gas generating raw material Sr is dried in the drying mechanism 200, and water vapor is discharged from a steam port (not shown) of the drying mechanism 200. As described above, when the silicon monoxide gas generating raw material Sr is dried, for example, by heating and drying, it is preferably dried for 1 hour or more and 240 hours or less, within the range of 100° C. or more and 400° C. or less, and more preferably dried for 4 hours or more and 120 hours or less, within the range of 200° C. or more and 350° C. or less. When the silicon monoxide gas generating raw material Sr is dried, for example, by reduced pressure drying, it is preferably dried under reduced pressure in which the pressure is controlled by a vacuum pump so as to be within the range of 12 hours or more and 120 hours or less, within the range of 10 Pa or more and 100 Pa or less, and more preferably dried under reduced pressure in which the pressure is controlled by a vacuum pump so as to be within the range of 12 hours or more and 240 hours or less, within the range of 0.1 Pa or more and 100 Pa or less. The silicon monoxide gas generating raw material Sr after drying is then fed from the drying mechanism 200 through the raw material supply pipe 210 into the raw material supply hopper 160. This configuration makes it possible to prevent the silicon monoxide gas generating raw material Sr after drying treatment from being exposed to the atmosphere.

[0040] EXAMPLES In the following, examples and comparative examples are shown in order to explain the present invention in more detail, but the present invention is not limited to these examples. EXAMPLES

[0041] Silicon monoxide (SiO) gas generating raw material Sr containing silicon dioxide (SiO2) and silicon (Si) was dried at 200°C for 4 hours. The weight of this silicon monoxide gas generating raw material Sr was 524g. The moisture content of this silicon monoxide gas generating raw material Sr was measured with a heat drying type moisture meter, and the moisture content was 0.05% by weight. Then, using the deposition device 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature 1300°C) over 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the silicon monoxide gas generating raw material Sr was charged. After that, through the above-mentioned process, silicon oxide particles (weight: 487g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure inside the deposition chamber RM rose to 15 Pa, and the reaction rate (particle weight / feeding amount of raw material×100) was 93%. EXAMPLES

[0042] The silicon monoxide gas generating raw material Sr containing silicon dioxide and silicon was dried at 100°C for 1 hour. The weight of this silicon monoxide gas generating raw material Sr was 507g. The moisture content of this silicon monoxide gas generating raw material Sr was measured with a heat drying type moisture meter, and the moisture content was 0.29% by weight. Then, using the deposition device 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature 1300°C) over 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the completion of charging the silicon monoxide gas generating raw material Sr. After that, through the above-mentioned process, silicon oxide particles (weight: 446g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 38 Pa, and the reaction rate was 88%. EXAMPLES

[0043] Silicon monoxide gas generating raw material Sr containing silicon dioxide and silicon was subjected to reduced pressure drying treatment under a reduced pressure of 100 Pa for 12 hours. The weight of this silicon monoxide gas generating raw material Sr was 520 g. The moisture content of this silicon monoxide gas generating raw material Sr was measured with a heat drying type moisture meter, and the moisture content was 0.33 wt%. Then, using the deposition device 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature 1300°C) over a period of 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the completion of charging the silicon monoxide gas generating raw material Sr. After that, through the above-mentioned process, silicon oxide particles (weight: 447 g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 44 Pa, and the reaction rate was 86%. EXAMPLES

[0044] Silicon monoxide gas generating raw material Sr containing lithium silicate (Li2Si2O5) and silicon was dried at 200°C for 4 hours. The weight of this silicon monoxide gas generating raw material Sr was 508g. The moisture content of this silicon monoxide gas generating raw material Sr was measured with a heat drying type moisture meter, and the moisture content was 0.05% by weight. Then, using the deposition device 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature 1300°C) over 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the completion of charging the silicon monoxide gas generating raw material Sr. After that, through the above-mentioned process, metal element-containing silicon oxide particles (weight: 477g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 16 Pa, and the reaction rate was 94%.

[0045] Comparative Example 1 The moisture content of silicon monoxide gas generating raw material Sr (without drying treatment) (weight: 530 g) containing silicon dioxide and silicon was measured by a heat drying type moisture meter, and the moisture content was 0.96 wt%. Then, using the deposition apparatus 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature: 1300°C) over a period of 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the completion of charging the silicon monoxide gas generating raw material Sr. After that, through the above-mentioned process, silicon oxide particles (weight: 360 g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 123 Pa, and the reaction rate was 68%.

[0046] Comparative Example 2 The silicon monoxide gas generating raw material Sr containing silicon dioxide and silicon was dried at 100°C for 1 hour. The weight of this silicon monoxide gas generating raw material Sr was 511g. This silicon monoxide gas generating raw material Sr was exposed to the atmosphere for 24 hours. The weight of the silicon monoxide gas generating raw material Sr after exposure to the atmosphere was 513g. The moisture content of this silicon monoxide gas generating raw material Sr was measured with a heat drying type moisture meter, and the moisture content was 0.68% by weight. Then, using the deposition device 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature: 1300°C) over 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the silicon monoxide gas generating raw material Sr was charged. After that, through the above-mentioned process, silicon oxide particles (weight: 393 g) to be used as a negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 80 Pa, and the reaction rate was 74%.

[0047] Comparative Example 3 The moisture content of silicon monoxide gas generating raw material Sr (without drying treatment) (weight: 503 g) containing lithium silicate (Li2Si2O5) and silicon was measured by a heat drying type moisture meter, and the moisture content was 0.81% by weight. Then, using the deposition apparatus 100 shown in FIG. 1, this silicon monoxide gas generating raw material Sr was continuously charged into the crucible 110 in the deposition chamber RM (pressure: 10 Pa, temperature: 1300°C) over a period of 2 hours. Then, silicon monoxide gas was generated, and the furnace was stopped 30 minutes after the completion of charging the silicon monoxide gas generating raw material Sr. After that, through the above-mentioned process, metal element-containing silicon oxide particles (weight: 312 g) used for the negative electrode material for lithium ion secondary batteries were finally produced. At this time, the pressure in the deposition chamber RM increased to 104 Pa, and the reaction rate was 62%.

Claims

1. A moisture adsorption prevention step of preventing moisture in the atmosphere from being adsorbed on a silicon monoxide (SiO) gas generating raw material having a moisture content of 0.6% by weight or less; and a raw material introduction step of continuously introducing the silicon monoxide gas generating raw material into a reaction chamber for generating silicon monoxide gas, The silicon monoxide gas generating raw material contains lithium silicate and silicon (Si). A method for continuously generating silicon monoxide gas.

2. The moisture adsorption prevention step includes a storage step of storing the silicon monoxide gas generating raw material without exposure to the atmosphere or under reduced pressure.

2. The method for continuously generating silicon monoxide gas according to claim 1.

3. The moisture adsorption prevention step includes a step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber while the raw material is not exposed to the atmosphere or is under reduced pressure.

2. The method for continuously generating silicon monoxide gas according to claim 1.

4. The moisture adsorption prevention step further includes a supply step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber without exposure to the atmosphere or under reduced pressure after the storage step.

3. The method for continuously generating silicon monoxide gas according to claim 2.

5. A moisture adsorption prevention step for preventing moisture in the air from being adsorbed onto a silicon monoxide (SiO) gas generating raw material having a moisture content of 0.6% by weight or less; and a raw material introduction step of continuously introducing the silicon monoxide gas generating raw material into a reaction chamber for generating silicon monoxide gas. A method for continuously generating silicon monoxide gas.

6. The moisture adsorption prevention step includes a storage step of storing the silicon monoxide gas generating raw material in a state not exposed to the atmosphere or under reduced pressure.

6. The method for continuously generating silicon monoxide gas according to claim 5.

7. The moisture adsorption prevention step includes a step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber while the raw material is not exposed to the atmosphere or is under reduced pressure.

6. The method for continuously generating silicon monoxide gas according to claim 5.

8. The moisture adsorption prevention step further includes a supply step of supplying the silicon monoxide gas generating raw material to a raw material supply hopper that supplies the silicon monoxide gas generating raw material to the reaction chamber after the storage step, while the raw material is not exposed to the atmosphere or under reduced pressure.

7. The method for continuously generating silicon monoxide gas according to claim 6.

Citation Information

Patent Citations

  • Method for manufacturing silicon oxide powder

    JP2001220122A

  • Continuous manufacturing method and continuous manufacturing device of silicon oxide powder

    JP2001220123A

  • Method for producing silicon oxide powder

    JP2007290890A

  • Raw material for producing silicon oxide, method for producing the same, silicon oxide and method for producing the same

    JP2010150049A

  • Method for manufacturing silicon oxide powder

    JP2012197207A