Nonwoven fabric structure and method of manufacture thereof

The nonwoven fabric structure combines long and short fibers with specific thermal fusion and lamination techniques to address the balance of moldability and rigidity, enhancing mechanical strength and reducing delamination for automotive applications.

JP7567289B2Active Publication Date: 2024-10-16TOYOBO MC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020143698
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-27
Publication Date
2024-10-16
Estimated Expiration
2040-08-27

AI Technical Summary

Technical Problem

Existing nonwoven fabrics face challenges in achieving a balance between high moldability, mechanical strength, and rigidity, with issues such as delamination, poor formability, and high cost, particularly when used in automotive applications.

Method used

A nonwoven fabric structure composed of long and short fiber nonwoven fabrics, where long fibers are core-sheath type with polyester cores and thermoplastic resin sheaths, and short fibers are mixed with inorganic fibers, thermally fused and laminated under controlled conditions to enhance rigidity and moldability.

Benefits of technology

The structure achieves high moldability and mechanical strength characteristics, with improved bending rigidity and reduced delamination, suitable for automotive components and other applications requiring lightweight yet rigid materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567289000002
    Figure 0007567289000002
  • Figure 0007567289000001
    Figure 0007567289000001
Patent Text Reader

Abstract

To provide a nonwoven fabric structure excellent in mechanical strength, having a high formability.SOLUTION: A nonwoven fabric structure is made of a nonwoven fabric of continuous fiber and a nonwoven fabric of staple fiber made of mixture of inorganic fiber and thermoplastic resin fiber, which are thermally fused, having a basis weight of 100 to 4000 g / m2, and an apparent density of 0.4 to 1.3 g / cm3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to nonwoven structures and methods for making the same. [Background technology]

[0002] Nonwoven fabrics with excellent moldability and mechanical strength properties are suitable for use in industrial materials, building materials, automobiles, etc. In particular, when used as molded nonwoven fabrics that are lightweight and have excellent rigidity after molding, such as automobile undercovers and dash silencers, they are lightweight and easily conform to the shape of a molding die, such as sound absorption performance, cushioning performance, and uneven protrusions, and can significantly improve energy conservation and workability by reducing the weight of automobiles. In addition, nonwoven fabrics containing a mixture of inorganic fibers and thermoplastic resin fibers are expected to have particularly high bending rigidity, and can also replace part of metal materials.

[0003] Conventionally known high basis weight moldable nonwoven fabrics are mainly made of short fibers and require the use of a large amount of thermal adhesive fibers, which poses problems in terms of heat resistance and cost. In addition, nonwoven fabrics with high mechanical strength such as tensile strength and tear strength have poor moldability (elongation when heated) due to excessive fiber entanglement, while nonwoven fabrics with high moldability generally have poor rigidity.

[0004] Patent Document 1 discloses a nonwoven fabric made of sheath-core composite long fibers that has excellent stretchability and moldability despite its low basis weight and thin thickness. Patent Document 2 proposes a method for producing a dense semi-finished product for automotive trim in which a web of sheath-core composite long fibers is needle-punched to three-dimensionally entangle the fabric, and discloses that the heating temperature range is widened during heating and compression molding. Patent Document 3 discloses a prepreg sheet containing carbon fibers and thermoformable resin fibers. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-241054 [Patent Document 2] JP 2018-9256 A [Patent Document 3] JP 2017-95662 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the technology of Patent Document 1, it is difficult to obtain a nonwoven fabric with high rigidity, and long preheating is required to prevent delamination. In Patent Document 2, the specific rigidity is not specified, and special components are required, which is inferior in cost performance, and it is not easy to bond to polypropylene and the like used as a general-purpose product in automobiles. In Patent Document 3, it is difficult to manufacture a single-layer sheet with a high basis weight, and it is necessary to laminate nonwoven fabrics with low basis weight, and nonwoven fabrics containing highly rigid carbon fibers have problems with fiber dropout and fiber breakage during handling, making the workability poor. As can be seen from this, no high-density nonwoven fabric structure that combines light weight, excellent rigidity, and high moldability has been proposed in the past.

[0007] In view of the above problems, an object of the present invention is to provide a nonwoven fabric structure having high moldability and excellent mechanical strength properties, and a method for producing the same. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems and have completed the present invention having the following configuration. 1. A nonwoven fabric structure in which a long fiber nonwoven fabric and a short fiber nonwoven fabric containing a mixture of inorganic fibers and thermoplastic resin fibers are thermally bonded, and the basis weight is 100 to 4000 g / m 2 and the apparent density is 0.4 to 1.3 g / cm 3 A nonwoven fabric structure comprising: 2. The nonwoven fabric structure according to 1, wherein the long fibers constituting the long-fiber nonwoven fabric are core-sheath fibers, the core component being made of polyester and the sheath component being made of the thermoplastic resin. 3. The nonwoven fabric structure according to 1 or 2, wherein the inorganic fibers are carbon fibers. 4. The nonwoven fabric structure according to any one of 1 to 3, wherein the weight ratio of the long-fiber nonwoven fabric to the entire nonwoven fabric structure is 30% to 85%. 5. A method for producing a nonwoven fabric structure, comprising: entangling a long-fiber nonwoven fabric by a needle punching method; laminating a short-fiber nonwoven fabric containing a mixture of inorganic fibers and thermoplastic resin fibers on the entangled long-fiber nonwoven fabric; and heat-treating the resulting laminate at 140 to 255°C and a pressure of 0.1 to 5 MPa. Effect of the Invention

[0009] Due to the above-mentioned configuration, the nonwoven fabric structure of the present invention has high moldability and excellent mechanical strength properties. [Brief description of the drawings]

[0010] [Figure 1] 1 is a photograph of a three-point bending test measuring device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The nonwoven fabric structure of the present invention is a nonwoven fabric structure in which a long-fiber nonwoven fabric and a short-fiber nonwoven fabric in which inorganic fibers and thermoplastic resin fibers are mixed are thermally fused together, and has a basis weight of 100 to 4000 g / m 2 and the apparent density is 0.4 to 1.3 g / cm 3 It is.

[0012] The total basis weight of the nonwoven fabric structure of the present invention can be appropriately set in consideration of the mechanical strength properties required for the final product, but is preferably 100 to 4000 g / m 2 If the basis weight is too low, the material will be lighter, but it will be difficult to expect high rigidity. The higher the basis weight, the higher the rigidity will be, but the larger the installation space required, so it is necessary to set it appropriately.

[0013] The weight fraction of the long fiber nonwoven fabric relative to the entire nonwoven fabric structure is 30% or more, preferably 50% or more, and more preferably 70% or more. The weight fraction is preferably 85% or less. If it exceeds 85%, the effect of improving the rigidity, which is the object of the present invention, may be reduced. The long fiber nonwoven fabric may be made of long fibers with good thermal formability, and it is preferable that at least a part of the constituent fibers of the long fiber nonwoven fabric is a core-sheath type fiber. Furthermore, crimp-free long fibers are often arranged in the nonwoven fabric without slack or bending with few bending points, and as a result, the strength of each fiber directly contributes to the strength of the nonwoven fabric, so that high rigidity can be expected. It is considered that the long fiber nonwoven fabric has fibers arranged mainly in the two-dimensional in-plane direction rather than in the thickness direction, which makes it easier to increase the bending rigidity and initial modulus.

[0014] Next, the long fiber nonwoven fabric may be used as a single layer, or two or more layers of nonwoven fabric may be laminated. When using a long fiber nonwoven fabric as a single layer, it is necessary to have many fibers aligned in the thickness direction to prevent delamination within the layer. Also, care must be taken when using a single layer, as the number of fiber restraint points increases and moldability may decrease. The nonwoven fabric laminated to the long fiber nonwoven fabric may be a long fiber nonwoven fabric or a short fiber nonwoven fabric.

[0015] When nonwoven fabrics are laminated, single-component nonwoven fabrics may be laminated, but as an example, two or more layers of single-component nonwoven fabrics and core-sheath type fibrous nonwoven fabrics may be laminated. Three layers, in which a core-sheath type fibrous nonwoven fabric is sandwiched between single-component nonwoven fabrics, are also preferred. The laminated nonwoven fabrics are preferably entangled by penetrating a water flow or needles from the core-sheath type fibrous nonwoven fabric using a water punching method or a needle punching method. Since the degree of freedom of the fibers in the long fiber nonwoven fabric is small, problems such as peeling may occur even after needle punching. The needle density (penetration number) and needle depth need to be appropriately set depending on the type of needle used, the desired mechanical strength characteristics, and the basis weight of each layer, and are not limited. If a core-sheath type fibrous nonwoven fabric is used on at least one side and a single-component nonwoven fabric is present in the middle layer, a composite structure with a high rigidity surface layer and a flexible fiber structure in the inner layer can be formed in one thermoforming, and the inner layer can reduce tapping sounds while the surface layer can suppress wear and the like. It is also expected to have excellent sound absorbing properties. A preferred lamination method is to loosely intertwine the fibers of multiple layers in advance using a needle punching method or the like, and then finish the laminate into a single layer using a needle punching method. This makes it easy to obtain high moldability while preventing delamination by providing appropriate fiber restraint. The smaller the basis weight per layer, the higher the bending stiffness can be achieved by arranging the fibers in the in-plane direction.

[0016] Resins used for the long fibers constituting the long fiber nonwoven fabric are preferably polyester, polyolefin, or polyamide, and generally inexpensive polyester or polyolefin is particularly preferred. Examples of polyester include homopolyesters such as polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polybutylene naphthalate (PBN), polyethylene naphthalate (PEN), polycyclohexane dimethyl terephthalate (PCHT), and polytrimethylene terephthalate (PTT), and copolymerized polyesters thereof. Examples of polyolefins include polyethylene (PB), polypropylene (PP), and polyethylene (PE). Polyamide fibers such as nylon 6 (NY6) and nylon 66 can also be used. In addition, additives that are commonly used, such as paints, pigments, matting agents, antistatic agents, flame retardants, and reinforcing particles, may be included. In addition, it is also possible to mix a small amount of other polymers, such as nylon and olefin, within a range that does not impair the object of the present invention. In addition, it is preferable to use core-sheath or side-by-side composite fibers. In particular, combinations of PP / PET, copolymerized PET / PET, PBT / PET, and PE / PP are preferred. In automotive applications, the use of composite fibers such as PP / PET, NY6 / PET, and copolymerized PET / PET is particularly suitable.

[0017] The fineness of the long fibers constituting the long fiber nonwoven fabric is not particularly limited, but is preferably 1 dtex to 10 dtex, more preferably 2.5 dtex to 7 dtex, in view of ease of productivity and mechanical strength properties.

[0018] Next, the short fiber nonwoven fabric in the nonwoven fabric structure of the present invention will be described. The short fiber nonwoven fabric is made of a mixed fiber in which inorganic fibers and thermoplastic resin fibers are mixed. As the inorganic fibers, carbon fibers, glass fibers, basalt fibers, etc. can be used, and fibers with a length of 2 to 10 cm are preferably used. Inorganic fibers are mainly used to improve rigidity, and the longer the fiber, the higher the rigidity can be expected, but if the fiber length exceeds 10 cm, the improvement effect is small and it becomes difficult to manufacture the short fiber nonwoven fabric. Even if long fibers are used, they often break during the manufacturing process of the short fiber nonwoven fabric (especially the fiber mixing process).

[0019] As the thermoplastic resin fiber, polypropylene, polyester, polyamide, polyphenylene sulfide, PTFE, etc. can be used. The fiber length of the thermoplastic resin fiber is, for example, 2 to 10 cm, but is not limited thereto. In order to increase the composite strength of the short fiber nonwoven fabric and the long fiber nonwoven fabric, it is particularly preferable from the viewpoint of preventing delamination (interlayer peeling) that the thermoplastic resin fiber is the same or similar to the material component of the long fiber constituting the long fiber nonwoven fabric. Being the same or similar is understood as common knowledge that it can be discussed in the same chemical classification such as polyester, and that there are few molecular functional groups that repel each other. This makes it possible to thermally bond the long fiber nonwoven fabric and the short fiber nonwoven fabric without using a special adhesive, and solves the problem of peeling at the interface.

[0020] In the nonwoven fabric structure of the present invention, by using composite fibers in which inorganic fibers and thermoplastic resin fibers are mixed with a short fiber nonwoven fabric, it is possible to prevent problems such as abrasion and cracks caused by pebbles kicked up by tires, etc., when the nonwoven fabric structure is used for, for example, an automobile fender cover or undercover. In addition, the nonwoven fabric structure can be used as a structure replacing metals, engineering plastics, etc.

[0021] Next, a method for producing the nonwoven fabric structure of the present invention will be described. The long fiber nonwoven fabric can be produced by a normal production method, but the spunbond method is preferably used from the viewpoint that the fibers are arranged in the in-plane direction (two-dimensional surface direction), the bending rigidity can be easily increased, and mechanical strength properties can be easily obtained. The short fiber nonwoven fabric can be produced by mixing fibers using a carding method, an air-laid method, or the like. If necessary, an integration process may be performed using a needle punch method, a water flow entanglement method, or the like. The short fiber nonwoven fabric can be used as a reinforcing layer, and recycled carbon fibers, for example, may be used as the inorganic fibers. In this case, when the carding method is used in the production of the short fiber nonwoven fabric, it is necessary to take care to set the processing speed low so that the carbon fibers do not break.

[0022] Next, a method for thermally bonding a long-fiber nonwoven fabric and a short-fiber nonwoven fabric will be described. Any of the usual hot press processes can be used for bonding. For example, it may be a press process of a veneer sheet, or it may be processed by passing through a heated metal press roll capable of manufacturing a long roll (for example, a calendar processing facility of Yuri Roll Co., Ltd.), or it may be processed using a high-temperature metal belt press machine. The conditions are set according to the thermoplastic resin contained in the short-fiber nonwoven fabric, and the apparent density of the nonwoven fabric structure can be controlled by pressing under conditions of 140 to 330°C and a pressure of 0.1 to 5 MPa. It is also preferable to once prepare a nonwoven fabric structure in a flat plate shape, and then to again three-dimensionally mold it using a press machine to form a three-dimensional structure. EXAMPLES

[0023] Examples of the present invention will be described below. The present invention is not limited to these examples. First, methods for measuring physical properties of samples prepared in the following examples and comparative examples will be described.

[0024] <Metsuke> The sample was cut into 20 cm squares, its weight was measured, and 2 Converted to mass per unit area (g / m 2 ) was decided.

[0025] <Apparent density> The thickness of the sample was set to 20 g / cm in accordance with JIS L1913 (2010). 2 The apparent density (g / cm 3 ) was obtained by dividing the basis weight measured above by the thickness measured above.

[0026] <Peeling> A sample was cut to a size of 5 cm wide x 30 cm long, and the sample was manually folded lengthwise to approximately 90 degrees 20 times, after which it was visually evaluated whether peeling occurred.

[0027] <Bending stiffness> JIS K7 0 A three-point bending test was carried out in accordance with the standard 17 (see Fig. 1). The specimen was collected in a size of 6 cm x 32 mm, with a support width of 32 mm, an indenter radius of 5 mm, and a speed of 1 mm / min. When the short fiber nonwoven fabric was laminated on only one side, the short fiber nonwoven fabric was on the bottom. The measurement was carried out by setting up the meter as shown in the figure.

[0028] Example 1 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 250 g / m 2 Four layers of long fiber nonwoven fabric (Volance (registered trademark) manufactured by Toyobo Co., Ltd.) were laminated and needle punched twice using an Organ FPD220 (40SM) with a penetration number of 32 and a needle depth of 11 mm to obtain a long fiber web. The converted apparent density of the obtained long fiber web was about 0.09 g / cm. 3 It was. Next, carbon fibers (average fiber length 5 cm, average diameter approximately 5 μm), copolymer polyester staple fibers (fineness 3.3 dTex), and polyethylene terephthalate staple fibers (fineness 4.4 dTex) were mixed at weight ratios of 50%, 25%, and 25% by carding to obtain a fabric with a basis weight of 250 g / m 2 Two pieces of short fiber nonwoven fabric were created. Thereafter, short fiber nonwoven fabrics were laminated on both sides of the long fiber web, and pressed at 220°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Then, a moldability test was conducted.

[0029] Example 2 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 180 g / m 2 A long-fiber nonwoven fabric (Volance (registered trademark) manufactured by Toyobo Co., Ltd.) was needle-punched using an Organ FPD220 (40SM) with a penetration number of 50 and a needle depth of 11 mm to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was 0.91 g / cm. 3 It was. Next, carbon fibers (average fiber length 5 cm, average diameter approximately 5 μm), copolymer polyester staple fibers (fineness 3.3 dTex), and polyethylene terephthalate staple fibers (fineness 4.4 dTex) were mixed at weight ratios of 50%, 25%, and 25% by carding to obtain a fabric with a basis weight of 180 g / m 2 Two pieces of short fiber nonwoven fabric were created. Thereafter, short fiber nonwoven fabrics were laminated on both sides of the long fiber web, and pressed at 220°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Then, a moldability test was conducted.

[0030] Example 3 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 250 g / m 2 Six sheets of long-fiber nonwoven fabric (Volance (registered trademark) manufactured by Toyobo Co., Ltd.) were laminated and needle-punched twice using an Organ FPD220 (40SM) with a penetration number of 70 and a needle depth of 11 mm to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was approximately 0.10 g / cm. 3 It was. Next, carbon fibers (average fiber length 5 cm, average diameter approximately 5 μm), copolymer polyester staple fibers (fineness 3.3 dTex), and polyethylene terephthalate staple fibers (fineness 4.4 dTex) were mixed at weight ratios of 50%, 25%, and 25% by carding to obtain a fiber with a basis weight of 250 g / m 2 Two pieces of short fiber nonwoven fabric were created. Thereafter, short fiber nonwoven fabrics were laminated on both sides of the long fiber web, and pressed at 220°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Then, a moldability test was conducted.

[0031] Example 4 The core is made of polyethylene terephthalate and the sheath is made of polypropylene (weight ratio of the long fibers is 50 / 50) with a fineness of 5.5 dtex and a basis weight of 250 g / m 2 Five sheets of long-fiber nonwoven fabric (manufactured by Toyobo Co., Ltd.) were laminated and needle-punched twice using an Organ FPD220 (40SM) with a penetration number of 32 and a needle depth of 11 mm to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was 0.09 g / cm. 3 It was. Next, carbon fibers (average fiber length 5 cm, average diameter about 5 μm) and polypropylene short fibers (average diameter 20 μm) were mixed at a weight ratio of 50% and 50% by carding to obtain a fiber weight of 250 g / m 2 A single piece of short fiber nonwoven fabric was created. Thereafter, a short fiber nonwoven fabric was laminated on the long fiber web and pressed at 190°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Thereafter, a moldability test was conducted. In Example 4, the IR heat treatment in the moldability test was conducted at 200°C for 90 seconds.

[0032] Comparative Example 1 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 250 g / m 2Six sheets of long-fiber nonwoven fabric (Volance (registered trademark) manufactured by Toyobo Co., Ltd.) were laminated and needle-punched twice using an Organ FPD220 (40SM) with a penetration number of 38 and a needle depth of 12 mm to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was 0.09 g / cm. 3 It was. The long fiber web was then pressed at 190°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. A moldability test was then conducted. In Comparative Example 1, the IR heat treatment in the moldability test was conducted at 250°C for 45 seconds.

[0033] Comparative Example 2 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 80 g / m 2 A long-fiber nonwoven fabric (Volance, manufactured by Toyobo Co., Ltd.) was needle-punched using an Organ FPD220 (40SM) with a penetration number of 38 and a needle depth of 11 mm to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was 0.10 g / cm. 3 It was. The long fiber web was then pressed at 190°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Then, a moldability test was conducted. In Comparative Example 2, the IR heat treatment in the molding test was conducted at 250°C for 45 seconds.

[0034] Comparative Example 3 Made of polyethylene terephthalate long fibers with a fineness of 5.0 dtex and a basis weight of 250 g / m 2 A long-fiber nonwoven fabric (Volance (registered trademark) manufactured by Toyobo Co., Ltd.) was needle-punched once using an Organ FPD220 (40SM) with a penetration number of 38 and a needle depth of 11 mm, and eight sheets of this needle-punched long-fiber nonwoven fabric were stacked and needle-punched a second time under the same conditions as the first time to obtain a long-fiber web. The converted apparent density of the obtained long-fiber web was 0.10 g / cm. 3 It was. Next, carbon fibers (average fiber length 5 cm, diameter approximately 5 μm) and polypropylene short fibers (diameter approximately 20 μm) were mixed at a weight ratio of 50% and 50% by carding to obtain a fiber weight of 250 g / m 2 A single piece of short fiber nonwoven fabric was created. Thereafter, a short fiber nonwoven fabric was laminated on the long fiber web, and pressed at 190°C and a pressure of 0.1 MPa using a metal belt press (manufactured by KBK Steel Products Co., Ltd.) to obtain a nonwoven fabric structure. The physical properties of the obtained nonwoven fabric structure are shown in Table 1. Thereafter, a moldability test was conducted. In Comparative Example 3, the IR heat treatment in the moldability test was conducted at 250°C for 45 seconds.

[0035] [Table 1]

[0036] From the above, it is understood that the examples have higher bending rigidity and better moldability than the comparative examples. [Industrial Applicability]

[0037] The nonwoven fabric structure obtained by the present invention is lightweight and has high rigidity, and therefore can be effectively used as building materials, industrial materials, automobile parts such as automobile undercovers, fender liners, hood silencers, and tonneau boards, sound absorbing materials, and sound insulating materials. In addition, when the inorganic fibers are carbon fibers or glass fibers with high tensile rigidity, they can be used in structural members that require strength. Furthermore, the present invention can effectively utilize recycled carbon fibers extracted from CFRP using thermosetting resins. From the above, the present invention is considered to be a great contribution to industry.

Claims

1. A long-fiber nonwoven fabric composed of polyester and / or olefin resin; A nonwoven fabric structure in which a short fiber nonwoven fabric containing a mixture of inorganic fibers and thermoplastic resin fibers is thermally fused to the nonwoven fabric, A nonwoven fabric structure having a basis weight of 100 to 4000 g / m2 and an apparent density of 0.4 to 1.3 g / cm3.

2. 2. The nonwoven fabric structure according to claim 1, wherein the long fibers constituting the long-fiber nonwoven fabric are core-sheath fibers and have one of the following characteristics (1) or (2). (1) The resin of the thermoplastic resin fiber is polyester, and the sheath component of the long fiber is polyester, or (2) The resin of the thermoplastic resin fiber is polyolefin, and the sheath component of the long fiber is polyolefin.

3. 3. The nonwoven fabric structure according to claim 1, wherein the inorganic fibers are carbon fibers.

4. The nonwoven fabric structure according to any one of claims 1 to 3, characterized in that a weight ratio of the long fiber nonwoven fabric to the entire nonwoven fabric structure is 30% to 85%.

5. A step of entangling the long fiber nonwoven fabric by a needle punch method; a step of laminating a short-fiber nonwoven fabric containing a mixture of inorganic fibers and thermoplastic resin fibers on the entangled long-fiber nonwoven fabric, and heat-treating the laminate at 140 to 255° C. and a pressure of 0.1 to 5 MPa.

Citation Information

Patent Citations

  • Nonwoven fabric having high elongation

    JP1991241054A

  • Interior base material for automobile and its manufacturing method

    JP2006160237A

  • Sound absorption material

    JP2014232281A

  • Sound absorbing material structure

    JP2015196933A

  • Prepreg sheet

    JP2017095662A