Metal paste for bonding and method for manufacturing bonded body

A metal paste with metal powder, copper salt, and amine forms a self-aligning, heat-resistant bonding layer by generating a liquid phase during temperature rise, addressing low thermal conductivity and alignment issues in solder-based bonding methods.

JP7568068B2Active Publication Date: 2024-10-16MITSUBISHI MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023511696
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-01
Filing Date
2022-03-31
Publication Date
2024-10-16
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

Existing bonding methods using solder materials face issues with low thermal conductivity, generation of intermetallic compounds leading to reduced bonding reliability, and difficulty in self-aligning member positions during joining, especially in high-temperature environments.

Method used

A metal paste comprising metal powder, copper salt, amine, and alcohol is used, with a specific weight ratio of copper to metal powder, allowing a liquid phase to form during temperature rise, enabling self-alignment and forming a metal sintered body with high bonding strength and heat resistance.

Benefits of technology

The metal paste enables self-alignment of members during bonding, forms a strong and heat-resistant bonding layer, maintaining reliability even in high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568068000006
    Figure 0007568068000006
  • Figure 0007568068000007
    Figure 0007568068000007
  • Figure 0007568068000008
    Figure 0007568068000008
Patent Text Reader

Abstract

This metal paste for joining includes a metal powder, a copper salt, an amine, and an alcohol, the ratio A / B of the weight A of Cu in the copper salt and the weight B of the metal powder is placed in the range of 0.02 to 0.25, the metal paste is in the form of a paste in the temperature range of 15-35°C, a liquid phase occurs over the course of increasing the temperature from 35°C, the liquid phase dissipates over the course of increasing the temperature above the liquid phase generation temperature, and a metal sintered compact is formed at or above the liquid phase dissipation temperature.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal bonding paste used for bonding members together, and to a method for manufacturing a bonded body using this metal bonding paste. This application claims priority based on Japanese Patent Application No. 2021-062770, filed on April 1, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] For example, semiconductor devices such as LEDs and power modules have a structure in which a semiconductor element is bonded onto a circuit layer made of a metal member. Here, when electronic components such as semiconductor elements are bonded onto a circuit layer, a method using a solder material is widely used, as shown in Patent Document 1, for example. Furthermore, Patent Document 2 proposes a technique in which a plating film and a Sn-based solder layer are formed, and then alloyed by heat treatment to form an alloy layer, and electronic components are mounted on a substrate.

[0003] Furthermore, Patent Document 3 proposes a technique for bonding electronic components such as semiconductor elements onto a circuit using a metal paste containing metal powder. In this metal paste, a bonding layer made of a conductive sintered body is formed, and electronic components such as semiconductor elements are bonded onto a circuit via this bonding layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-271782 A [Patent Document 2] Patent No. 6459656 [Patent Document 3] Patent No. 6428339 Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, as described in Patent Documents 1 and 2, when components are joined together using a solder material, a liquid phase is generated during the temperature rise process during joining. At this time, the relative positions of the components are adjusted by the surface tension of the liquid phase. In other words, the relative positions of the components are self-aligned. However, when solder is used for bonding, the bonding layer formed between the components contains intermetallic compounds, which may result in a relatively low thermal conductivity.Furthermore, cracks may easily occur in the bonding layer when subjected to a temperature cycle, which may result in a decrease in bonding reliability.

[0006] Furthermore, when an electronic component such as a semiconductor element is joined to a circuit layer via a solder material, there is a risk that part of the solder will melt when used in a high-temperature environment, resulting in a decrease in the reliability of the joint between the electronic component such as a semiconductor element and the circuit layer. In particular, in recent years, the heat resistance of semiconductor elements themselves has improved, and semiconductor devices are sometimes used in high-temperature environments such as the engine compartments of automobiles, making it difficult to meet these demands with the conventional structure in which components are joined with solder.

[0007] On the other hand, in the metal paste described in Patent Document 3, the bonding layer is made of a sintered metal body, and therefore has excellent thermal conductivity and bonding reliability. Furthermore, when the bonding layer is formed from a sintered metal, the bonding layer can be formed under relatively low temperature conditions and the melting point of the bonding layer itself is high, so that the bonding strength does not decrease significantly even in a high temperature environment. However, when components are bonded together using a metal paste, no liquid phase is generated during the heating process during bonding, making it impossible to self-align the relative positions of the components.

[0008] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a metal paste for bonding that produces a liquid phase during the heating process during bonding, enables adjustment of the relative positions of components by self-alignment, and is capable of forming a bonding layer made of a metal sintered body having excellent heat resistance and bonding strength, and a method for manufacturing a bonded body using this metal paste for bonding. [Means for solving the problem]

[0009] In order to solve the above problems, the metal paste for joining of the present invention contains a metal powder, a copper salt, an amine, and an alcohol, and has a ratio A / B of the weight A of Cu in the copper salt to the weight B of the metal powder in the range of 0.02 or more and 0.25 or less. The metal paste is in a paste form within a temperature range of 15°C or more and 35°C or less, and is characterized in that a liquid phase is generated during the heating process from 35°C and disappears during the heating process above the liquid phase generation temperature, and a metal sintered body is formed at or above the liquid phase disappearance temperature.

[0010] According to the bonding metal paste of this configuration, it contains metal powder, copper salt, amine, and alcohol, is in a paste state within a temperature range of 15°C to 35°C, and generates a liquid phase during the temperature rise process from 35°C, so that printing, dispense application, or pin transfer is possible in a room temperature working environment. Meanwhile, a liquid phase is generated during the temperature rise process during bonding, and the relative positions of the bonding members can be self-aligned. In addition, since it contains metal powder, even if a liquid phase is generated, a distance can be secured between the members, and a bonding layer can be sufficiently formed. Furthermore, since the liquid phase disappears above the liquid phase formation temperature and a metal sintered body is formed above the liquid phase disappearance temperature, the bonding strength does not decrease even in a high temperature environment, and a bonding layer with excellent heat resistance and bonding strength can be formed. In addition, since the ratio A / B of the weight A of Cu in the copper salt to the weight B of the metal powder is set within the range of 0.02 to 0.25, a liquid phase can be sufficiently formed during the temperature rise process, and the density of the metal sintered body after sintering is sufficiently high, thereby achieving strong bonding strength. Furthermore, because it contains alcohol, the copper ions of the copper salt that has become liquid during the temperature rise process during bonding can be reduced to generate nano-sized copper particles, and the organic components that have formed a complex with the copper ions volatilize, making it possible to reliably eliminate the liquid phase.

[0011] In the bonding metal paste of the present invention, the metal powder is preferably one or both of silver and copper. In this case, since the metal powder is one or both of silver and copper, it is possible to form a bonding layer having particularly excellent thermal conductivity.

[0012] Furthermore, in the bonding metal paste of the present invention, the copper salt preferably includes an organic carboxylate copper salt. In this case, since the copper salt contains an organic carboxylate copper salt, a metal complex can be reliably formed by adding it together with an amine, and a liquid phase can be reliably produced during the temperature rise process during bonding.

[0013] Furthermore, the metal bonding paste of the present invention may contain two or more types of copper salts. In this case, even if a single copper salt does not form a paste-like mixture in the temperature range of 15° C. to 35° C., by combining two or more types, it is possible to form a paste-like mixture in the temperature range of 15° C. to 35° C. In addition, the liquid phase generation temperature and liquid phase disappearance temperature can be adjusted by the combination.

[0014] In the bonding metal paste of the present invention, the amine preferably contains a linear alkylamine. In this case, since the amine contains a linear alkylamine, a metal complex can be reliably formed by adding it together with a copper salt, and a liquid phase can be reliably produced during the temperature rise process during bonding.

[0015] In the bonding metal paste of the present invention, the amine may be composed of two or more kinds of amines. In this case, even if a single amine does not form a paste-like mixture in the temperature range of 15° C. to 35° C., by combining two or more types, it is possible to form a paste-like mixture in the temperature range of 15° C. to 35° C. In addition, the liquid phase generation temperature and liquid phase disappearance temperature can be adjusted by the combination.

[0016] In the bonding metal paste of the present invention, the alcohol may be composed of two or more kinds of alcohol. In this case, even if the paste viscosity of a single alcohol is not optimal depending on the method of use, by combining two or more types, it is possible to adjust the paste viscosity to an appropriate value.

[0017] The bonding metal paste of the present invention preferably further contains a silver salt in addition to the metal powder, copper salt, amine and alcohol. In this case, the silver salt reacts with the amine to form a silver complex, and the silver complex is reduced by the alcohol to produce nano-sized silver particles, making it possible to further improve the bonding strength.

[0018] The manufacturing method of a joined body of the present invention is a manufacturing method of a joined body in which a first member and a second member are joined, and is characterized in that the above-mentioned joining metal paste is placed between the first member and the second member at a temperature range of 15°C or more and 35°C or less, the temperature is raised while the joining metal paste is placed between the first member and the second member to generate a liquid phase between the first member and the second member, the temperature is further raised to above the liquid phase generation temperature to eliminate the liquid phase, and the temperature is further raised to above the liquid phase disappearance temperature to form a metal sintered body, thereby joining the first member and the second member.

[0019] According to the manufacturing method of the bonded body having this configuration, the above-mentioned bonding metal paste is placed between the first member and the second member at a temperature range of 15°C or more and 35°C or less, and then the temperature is raised to generate a liquid phase, so that the relative positions of the first member and the second member can be self-aligned by the surface tension of the liquid phase. In addition, the temperature is raised to above the liquid phase formation temperature to eliminate the liquid phase, and then the temperature is raised further to above the liquid phase disappearance temperature to form a metal sintered body, so that a bonding layer made of a metal sintered body can be formed and a bonded body having excellent heat resistance and bonding strength can be manufactured. Effect of the Invention

[0020] According to the present invention, it is possible to provide a metal paste for bonding that can generate a liquid phase during the heating process during bonding, adjust the relative positions of components by self-alignment, and form a bonding layer made of a metal sintered body that has excellent heat resistance and bonding strength, and a method for manufacturing a bonded body using this metal paste for bonding. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a flow diagram showing a method for joining bodies using a joining metal paste according to an embodiment of the present invention. [Diagram 2] 1A to 1C are explanatory diagrams of a method for joining bodies using a joining metal paste according to an embodiment of the present invention. [Diagram 3] 1 is an explanatory diagram of a mounting position of a Si chip and a method of checking self-alignment in an embodiment. FIG. [Figure 4] FIG. 2 is an explanatory diagram of a method for evaluating a liquid phase generation temperature in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, a bonding metal paste and a method for producing a bonded body according to one embodiment of the present invention will be described. The bonding metal paste of the present embodiment is used when manufacturing a bonded body by bonding a first member and a second member, for example, when bonding a semiconductor element (second member) as an electronic component to a circuit layer (first member) of an insulating circuit board.

[0023] The bonding metal paste of the present embodiment contains a metal powder, a copper salt, an amine, and an alcohol, and may further contain a silver salt. In the bonding metal paste of this embodiment, the ratio A / B of the weight A of Cu in the copper salt to the weight B of the metal powder is set within the range of 0.02 to 0.25.

[0024] The joining metal paste of this embodiment is in a paste form within a temperature range of 15°C or higher and 35°C or lower, a liquid phase is generated during the temperature rise from 35°C, the liquid phase disappears at temperatures above the liquid phase generation temperature, and a metal sintered body is formed at temperatures above the liquid phase disappearance temperature.

[0025] In this embodiment, as described above, the bonding metal paste contains copper salt and amine, and thus a metal complex (copper complex) is formed by mixing them. This metal complex becomes paste-like within a temperature range of 15° C. to 35° C., and a liquid phase is generated by further heating.

[0026] Here, if the ratio A / B of the Cu weight A in the copper salt to the metal powder weight B is less than 0.02, the copper salt content will be insufficient, and the liquid phase will not be sufficiently formed during the temperature rise process during bonding, which may impair self-alignment. On the other hand, if the weight ratio A / B exceeds 0.25, the liquid phase will be excessively generated, the amount of volatilized organic matter will increase, and the density of the metal sintered body after firing will decrease, which may result in a decrease in bonding strength. For this reason, in this embodiment, the ratio A / B of the weight A of Cu in the copper salt to the weight B of the metal powder is set within the range of 0.02 to 0.25. The weight ratio A / B is preferably 0.04 or more, more preferably 0.06 or more, and is preferably 0.20 or less, more preferably 0.15 or less.

[0027] In this embodiment, the metal powder is preferably one or both of silver and copper. Moreover, it is preferable that the metal powder has an average particle size within the range of 100 nm to 3 μm.

[0028] The copper salt may be any salt that forms a copper complex when added together with an amine. In this embodiment, it is preferable to use an organic carboxylate copper salt as the copper salt. Specifically, copper acetate (II) monohydrate, copper citrate 2.5 hydrate, copper 2-ethylhexanoate, etc. can be used as the copper salt, and it is preferable to use copper acetate (II) monohydrate as the copper salt. In this embodiment, two or more types of copper salts may be contained as the copper salt.

[0029] The amine may be any amine that forms a copper complex when added together with the copper salt. In this embodiment, the amine preferably contains a linear alkylamine. Specifically, dodecylamine, tetradecylamine, stearinamine, aminodecane, etc. can be used, and dodecylamine is preferably used as the amine. In this embodiment, the amine may contain two or more types of amines.

[0030] As the alcohol, glycerin, α-terpineol, diethylene glycol (DEG), 2-ethyl-1,3-hexanediol (EHD), etc. can be used. In particular, it is preferable to use glycerin. In this embodiment, the alcohol may contain two or more types of alcohol.

[0031] If necessary, a silver salt may be contained. The silver salt may be any silver salt that forms a silver complex when added together with an amine. In this embodiment, examples of the silver salt include silver acetate, silver oxalate, silver propionate, silver myristate, and silver butyrate. In particular, it is preferable to use silver acetate.

[0032] Here, the content of the metal powder is preferably within the range of 25 mass % to 75 mass %. The content of the copper salt is preferably within the range of 4 mass % to 16 mass %. Furthermore, the amine content is preferably within the range of 16 mass % to 54 mass %. The alcohol content is preferably within the range of 1 mass % to 10 mass %. Furthermore, when a silver salt is contained, the content of the silver salt is preferably within the range of 0.1 mass % to 12 mass %. The contents of each component are based on the bonding metal paste being 100 mass %.

[0033] The bonding metal paste of this embodiment can be produced by weighing out the above-mentioned metal powder, copper salt, amine, alcohol, and, if necessary, silver salt in a predetermined ratio, and mixing them.

[0034] Next, a method for producing a bonded body using the bonding metal paste of this embodiment will be described with reference to FIGS. In this embodiment, a bonded body 10 (semiconductor device) in which a first member 11 (circuit layer of an insulating circuit board) and a second member 12 (semiconductor element) are bonded via a bonding layer 15 is manufactured.

[0035] (Paste application process S01) First, as shown in FIG. 2(a), the bonding metal paste 20 of this embodiment is disposed between the first member 11 and the second member 12. In this embodiment, the bonding metal paste 20 is printed by screen printing on the bonding surface of the first member 11. The applied thickness is preferably within a range of 20 μm to 500 μm.

[0036] (Liquid phase formation step S02) Next, the first member 11 and the second member 12 are laminated with the bonding metal paste 20 interposed therebetween, and are heated to a liquid phase generating temperature or higher. At this time, in the process of increasing the temperature from 35° C., a copper complex formed by a copper salt and an amine contained in the bonding metal paste 20 is liquefied, and a liquid phase 21 is generated between the first member 11 and the second member 12. As a result, as shown in FIG. 2(b), the relative positions of the first member 11 and the second member 12 are self-aligned due to the surface tension of the liquid phase 21. Here, the formation temperature of the liquid phase 21 is preferably within a range of more than 35° C. and not more than 100° C. The formation temperature of the liquid phase 21 is more preferably less than 100° C. Furthermore, when the bonding metal paste 20 contains a silver salt, a silver complex is formed by the silver salt and an amine.

[0037] (Liquid phase volatilization process S03) After the relative positions of the first member 11 and the second member 12 are self-aligned, the material is further heated and held at a constant temperature. The holding temperature is preferably in the range of 100° C. or more and 200° C. or less, and the holding time at the holding temperature is preferably in the range of 5 minutes or more and 180 minutes or less. The holding temperature is more preferably less than 200° C. In addition, it is preferable to set the temperature so that the liquid phase does not volatilize all at once. 2(c), the alcohol reduces the copper complex to generate nano-sized copper particles, and the organic components (acid component of the copper salt, amine, and alcohol) volatilize, causing most of the liquid phase 21 to disappear. In addition, when the bonding metal paste 20 contains a silver salt, the silver complex formed by the silver salt and the amine is reduced by the alcohol to generate nano-sized silver particles.

[0038] (Sintering process S04) After the organic components have evaporated, the mixture is further heated to a temperature higher than the liquid phase disappearance temperature. The heating temperature is preferably in the range of 200°C to 400°C, and the holding time at the heating temperature is preferably in the range of 1 minute to 90 minutes. At this time, the sintering of the metal powder progresses, and a bonding layer 15 made of a sintered metal body is formed, as shown in FIG. 2(d). When the bonding metal paste 20 contains silver salt, nano-sized silver particles are generated, which allows sintering to proceed sufficiently and improves the bonding strength.

[0039] According to the bonding metal paste of the present embodiment configured as described above, it contains metal powder, copper salt, amine, and alcohol, is in a paste state within a temperature range of 15°C to 35°C, and is configured to generate a liquid phase during the temperature rise process from 35°C. Therefore, when the bonding metal paste 20 is disposed between the first member 11 and the second member 12 and bonded, a liquid phase is generated between the first member 11 and the second member 12 during the temperature rise process during bonding, and the relative positions of the first member 11 and the second member 12 can be self-aligned due to the surface tension of this liquid phase. In addition, since it contains metal powder, even if a liquid phase is generated, a distance can be secured between the first member 11 and the second member 12, and the bonding layer 15 can be sufficiently formed.

[0040] Furthermore, in this embodiment, the temperature is raised to above the liquid phase formation temperature to eliminate the liquid phase, and then the temperature is raised again to above the liquid phase disappearance temperature to form a metal sintered body. Therefore, even if the material is placed in a high temperature environment again after sintering, no liquid phase is generated, and a bonding layer having excellent heat resistance and bonding strength can be formed. In this embodiment, the ratio A / B of the Cu weight A in the copper salt to the metal powder weight B is set to a range of 0.02 or more, so that the copper salt content is ensured, and the liquid phase is sufficiently formed during the temperature rise process during bonding, allowing self-alignment. Furthermore, the ratio A / B of the Cu weight A in the copper salt to the metal powder weight B is set to a range of 0.25 or less, so that the amount of liquid phase generated is not excessive and the amount of volatilized organic matter is suppressed, so that the density of the metal sintered body after firing is sufficiently high, and strong bonding strength can be achieved. Furthermore, since this embodiment contains alcohol, nano-sized copper particles can be generated by reducing the copper ions of the copper salt that has become liquid during the temperature rise process during bonding, and the organic components that have formed a complex with the copper ions volatilize, making it possible to reliably eliminate the liquid phase.

[0041] Furthermore, in the bonding metal paste of this embodiment, when the metal powder is one or both of silver and copper, a bonding layer 15 made of a sintered body of these metals can be formed, making it possible to form a bonding layer 15 having particularly excellent thermal conductivity.

[0042] Furthermore, in the bonding metal paste of this embodiment, when the copper salt contains an organic carboxylate copper salt, adding it together with an amine can reliably form a metal complex, and can reliably cause a liquid phase to appear during the temperature rise process during bonding.

[0043] Furthermore, in the bonding metal paste of this embodiment, when the copper salt contains two or more kinds of copper salts, even if a single copper salt does not form a paste-like mixture in a temperature range of 15° C. to 35° C., by combining two or more kinds, the mixture can be made into a paste-like mixture in a temperature range of 15° C. to 35° C. In addition, the liquid phase generation temperature and the liquid phase disappearance temperature can be adjusted by the combination.

[0044] Furthermore, in the bonding metal paste of this embodiment, when the amine contains a linear alkylamine, adding it together with the copper salt can reliably form a metal complex, and can reliably cause a liquid phase to appear during the temperature rise process during bonding.

[0045] Furthermore, in the bonding metal paste of this embodiment, when two or more kinds of amines are contained as the amines, even if a single amine does not turn the mixture into a paste-like state in the temperature range of 15° C. to 35° C., by combining two or more kinds, the mixture can be turned into a paste-like state in the temperature range of 15° C. to 35° C. In addition, the liquid phase generation temperature and the liquid phase disappearance temperature can be adjusted by the combination.

[0046] Furthermore, in the joining metal paste of this embodiment, when the alcohol contains two or more types of alcohol, even if the paste viscosity of a single alcohol is not optimal depending on the method of use, it is possible to adjust the paste viscosity to an appropriate value by combining two or more types.

[0047] Furthermore, when the bonding metal paste of this embodiment contains a silver salt in addition to the metal powder, copper salt, amine, and alcohol, the silver salt reacts with the amine to form a silver complex, and the alcohol reduces this silver complex to produce nano-sized silver particles, thereby making it possible to further improve the bonding strength.

[0048] According to the manufacturing method of the bonded body 10 of this embodiment, the above-mentioned bonding metal paste 20 is disposed between the first member 11 and the second member 12 at a temperature range of 15°C or more and 35°C or less, and then the temperature is raised to generate the liquid phase 21. Therefore, the relative positions of the first member 11 and the second member 12 can be self-aligned by the surface tension of the liquid phase 21. In addition, in this embodiment, the temperature is raised to above the liquid phase generation temperature to eliminate the liquid phase, and then the temperature is raised further to above the liquid phase disappearance temperature to form a metal sintered body. This makes it possible to form a bonding layer 15 made of a metal sintered body, and to manufacture a bonded body 10 having excellent heat resistance and bonding strength.

[0049] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in the present embodiment, a semiconductor element (second component) is joined as an electronic component to a circuit layer (first component) of an insulating circuit board, but this is not limited thereto, and it is sufficient that the first component and the second component are joined using the joining metal paste of the present invention. EXAMPLES

[0050] The results of an evaluation test performed to evaluate the effects of the bonding metal paste and the method for producing a bonded body according to the present invention will be described below.

[0051] Example 1 First, a copper salt-amine mixture was obtained by mixing the copper salt and amine shown in Tables 1 and 2 in the ratios shown in Tables 1 and 2. Then, the copper salt-amine mixture was mixed with a metal powder and alcohol shown in Tables 1 and 2 to obtain various mixtures according to Examples 1 to 19 of the present invention and Comparative Examples 1 to 15. In Tables 1 and 2, the metal particle size of the metal powder used is shown in parentheses. In Comparative Example 11, Sn-3.0% Ag-0.5% Cu cream solder (manufactured by Senju Metal Industry Co., Ltd.) was used (shown as SnAg3Cu0.5 in Table 2). In Comparative Example 12, the Cu core Sn shell paste described in Example 1 of Japanese Patent No. 6645317 was used.

[0052] Next, the above mixture was placed on an oxygen-free copper plate 2 mm thick metallized with Ag (thickness: 50 μm, area: 3 mm square). A square Si chip (with Au metallized surface) 400 μm thick and 2.5 mm on each side was mounted on the mixture. The mounting position was adjusted so that the surface on which the mixture was placed and two sides of the element surface were aligned, as shown in Figure 3(a). This was heated to form a bonding layer, and the oxygen-free copper plate and the Si chip were bonded. The resulting mixture and bonding condition were evaluated for the following items.

[0053] In Examples 1-19 of the present invention and Comparative Examples 9, 10, 13, and 14, the temperature was raised from room temperature, held for 60 minutes at the liquid phase volatilization step temperature shown in Tables 3 and 4, further raised and held for 15 minutes at the baking step temperature shown in Tables 3 and 4, and then lowered to room temperature. The temperature rise rate and temperature fall rate were 2° C. / min.

[0054] In Comparative Example 11, in which SnAgCu was used as the metal powder, the temperature was raised from room temperature, held at the liquid phase volatilization step temperature shown in Table 4 for 3 minutes, further raised and held at the firing step temperature shown in Table 4 for 10 seconds, and then lowered to room temperature. The temperature rise rate and temperature fall rate were 30°C / min. The liquid phase generation temperature was the melting temperature of SnAgCu, and the liquid phase disappearance temperature was the volatilization temperature of the flux.

[0055] In Comparative Example 12, in which a Cu core Sn shell was used as the metal powder, the temperature was raised from room temperature, held at the liquid phase volatilization step temperature shown in Table 4 for 3 minutes, further raised and held at the firing step temperature shown in Table 4 for 10 seconds, and then lowered to room temperature. The temperature rise rate and temperature fall rate were 30°C / min. The liquid phase generation temperature was the melting point of Sn, and the liquid phase disappearance temperature was the volatilization temperature of the flux.

[0056] (Properties at 15℃-35℃) The resulting mixtures were visually inspected, and those that contained powdery residues (i.e., crumbly) were deemed to be "powder-like." For all mixtures other than those that were "powder-like," the viscosity was measured using a rheometer (TA Instruments, DHR-3) at temperatures of 15°C and 35°C and a shear rate of 10 (1 / s). Mixtures with a viscosity of 10 Pa s or more and 500 Pa s or less at both 15°C and 35°C were deemed to be "paste-like," and those with a viscosity of less than 10 Pa s measured at either temperature were deemed to be "liquid."

[0057] (Whether or not liquid phase occurs / liquid phase formation temperature) Measurements were performed using a thermogravimetric differential thermal analysis (TG-DTA) (NETZSCH, STA-2500 Regulus). Differential thermal analysis was performed on each of the resulting mixtures in a nitrogen atmosphere at a heating rate of 10°C / min from 25°C to 500°C. When no weight loss was observed in the TG curve and an endothermic peak was observed in the DTA curve, it was determined that a liquid phase had formed. In Tables 3 and 4, samples that were judged to have produced a liquid phase are marked as "Yes," samples that did not produce a liquid phase and maintained a liquid state are marked as "Remains liquid," and samples that did not produce a liquid phase are marked as "No." The liquid phase formation temperature was determined as the temperature at the point where a tangent drawn from the peak of the DTA curve toward the low temperature part (low temperature side) intersects with an extension of the flat part of the DTA curve, as shown in FIG.

[0058] (Disappearance of liquid phase / liquid phase disappearance temperature) Measurements were performed up to 500°C using the same measuring equipment and conditions as when determining whether or not a liquid phase was generated. If a weight loss equal to or greater than the amount of alcohol or flux added was confirmed by 300°C in the TG curve, the liquid phase had disappeared and was marked as "A." If the weight loss was less than the amount of alcohol or flux added, the liquid phase remained and was marked as "B." The liquid phase disappearance temperature was determined as the temperature at which the tangent line during the weight loss in the TG curve intersects with the extension of the straight line at which the weight loss has ended and the steady state.

[0059] (Self-alignment) After firing, the distance between adjacent sides of the bonding material and the chip was measured. If the distance on all four sides was 0.2 mm or more, as shown in Figure 3(b), the alignment was judged to be "A." If the distance on even one side was less than 0.2 mm, the alignment was judged to be "B."

[0060] (Share Strength) The bonding strength was measured using a shear strength evaluation tester (MFM 1500HF manufactured by TRY PRESICION). Specifically, the bonding strength was measured by fixing the oxygen-free copper plate of the bonded body horizontally, pushing the Si chip of the bonded body horizontally from the side with a shear tool at a position 50 μm above the surface (top surface) of the bonding layer, and measuring the strength when the Si chip breaks. The shear tool moving speed was 0.1 mm / sec. The strength test was performed three times per condition, and the arithmetic average value was used as the measured value of the bonding strength.

[0061] (Heat resistance evaluation) The fired samples were subjected to 100 thermal shock cycles using a thermal shock tester (TSE-11-A manufactured by Espec Corporation) in which the samples were heated to 175°C for 15 minutes, cooled to -40°C for 15 minutes, and then heated again to 175°C. An ultrasonic imaging device (FSP8V manufactured by Hitachi Power Solutions) was used to capture images to confirm the area where the oxygen-free copper plate and the Si chip were bonded with the bonding layer. The transducer (probe) used had a frequency of 140MHz. The peeled area was calculated from the captured image, and an area where the peeled area was less than 10% of the chip area was rated "A", and an area where it was 10% or more was rated "B". In the image taken with the ultrasonic imaging device, the areas where the Si chip and oxygen-free copper plate had peeled off appear white, and the bonded areas appear grey.

[0062] [Table 1]

[0063] [Table 2]

[0064] [Table 3]

[0065] [Table 4]

[0066] In Comparative Examples 1, 2, and 4-6, the mixture was in a powder form in the temperature range of 15° C. to 35° C., and it was not possible to print the mixture on an oxygen-free copper plate. Therefore, self-alignment, heat resistance, and shear strength were not evaluated. In Comparative Examples 3, 7, 8, and 15, the mixture was in a liquid state in the temperature range of 15° C. to 35° C., and it was not possible to print the mixture on the oxygen-free copper plate. Therefore, self-alignment, heat resistance, and shear strength were not evaluated.

[0067] In Comparative Example 9, the ratio A / B of the Cu weight A in the copper salt to the metal powder weight B was 0.01, and the copper salt content was insufficient, so the liquid phase was not sufficiently formed and the self-alignment was "B". In Comparative Example 10, the ratio A / B of the Cu weight A in the copper salt to the metal powder weight B was 0.27, and the amount of volatilized organic matter was large, resulting in a low metal sintered density in the bonding layer and a low bonding strength (shear strength).

[0068] In Comparative Examples 11 and 12, a Cu-Sn based solder material was used, and the heat resistance was insufficient. In Comparative Example 13, an Ag paste not containing copper salt was used, and no liquid phase was generated during the temperature rise process, resulting in a self-alignment grade of "B." In Comparative Example 14, the firing temperature was lower than the liquid phase disappearance temperature, and organic components remained inside the bonding layer made of the metal sintered body, resulting in a low bonding strength.

[0069] In contrast, Example 1-19 of the present invention contains metal powder, copper salt, and an amine, is in a paste-like state within a temperature range of 15°C or higher and 35°C or lower, a liquid phase is generated during the heating process from 35°C, the liquid phase disappears during the heating process above the liquid phase generation temperature, and a metal sintered body is formed at or above the liquid phase disappearance temperature, and the self-alignment was rated "A" and the heat resistance and bonding strength were excellent.

[0070] From the above, it has been confirmed that the present invention can provide a metal paste for bonding that can generate a liquid phase during the heating process during bonding, adjust the relative positions of the components by self-alignment, and form a bonding layer with excellent heat resistance and bonding strength, as well as a method for manufacturing a bonded body.

[0071] Example 2 Example 20 of the present invention was prepared by adding 4 mass % of silver salt (silver acetate) to the bonding metal paste of Example 2 of the present invention shown in Table 1. Next, an oxygen-free copper plate having a thickness of 2 mm and an outermost surface metallized with Ag (hereinafter, Ag-metallized copper plate) was prepared.

[0072] On this Ag metallized layer, the bonding metal pastes of invention examples 2 and 20 were applied (thickness: 100 μm, area: 3 mm square). A square Si chip (with Au metallized surface) 2.5 mm thick and 2.5 mm on each side was mounted on the applied mixture. This was heated to form a bonding layer, and the oxygen-free copper plate and the Si chip were bonded. The heating temperature and holding time of the liquid phase volatilization step and the heating temperature and holding time of the firing step were set as shown in Table 5. Then, the shear strength was measured in the same manner as in Example 1. The measurement results are shown in Table 5.

[0073] [Table 5]

[0074] As shown in Table 5, it was confirmed that the joining metal paste of Example 20 of the present invention, in which silver salt was added, had improved shear strength compared to the joining metal paste of Example 2 of the present invention, in which no silver salt was added.

Claims

1. The composition comprises a metal powder, a copper salt, an amine, and an alcohol, and a ratio (A / B) of a weight (A) of Cu in the copper salt to a weight (B) of the metal powder is within a range of 0.02 or more and 0.25 or less, A metal paste for joining, which is in a paste form within a temperature range of 15°C or higher and 35°C or lower, which generates a liquid phase during heating from 35°C, which disappears during heating above the liquid phase generation temperature, and which forms a metal sintered body at or above the liquid phase disappearance temperature.

2. 2. The bonding metal paste according to claim 1, wherein the metal powder is one or two of silver and copper.

3. 3. The bonding metal paste according to claim 1, wherein the copper salt includes an organic carboxylate copper salt.

4. The bonding metal paste according to any one of claims 1 to 3, characterized in that the copper salt comprises two or more kinds of copper salts.

5. The metal bonding paste according to claim 1 , wherein the amine comprises a linear alkylamine.

6. The metal bonding paste according to any one of claims 1 to 5, characterized in that the amine comprises two or more types of amine.

7. The bonding metal paste according to any one of claims 1 to 6, characterized in that the alcohol comprises two or more types of alcohol.

8. The bonding metal paste according to any one of claims 1 to 7, further comprising a silver salt.

9. A method for manufacturing a bonded body in which a first member and a second member are bonded, comprising the steps of: The joining metal paste according to any one of claims 1 to 8 is disposed between the first member and the second member in a temperature range of 15°C to 35°C, The joining metal paste is disposed between the first member and the second member, and a temperature is raised to generate a liquid phase between the first member and the second member; The method for producing a joined body comprises further increasing the temperature to above the liquid phase generation temperature to eliminate the liquid phase, and then increasing the temperature to above the liquid phase disappearance temperature to form a metal sintered body, thereby joining the first member and the second member.

Citation Information

Patent Citations

  • Aluminum casting alloy for intake manifold

    JP1989028339A

  • Optical head for magneto-optical recording carrier

    JP1989059656A

  • Metal paste for soldering and soldering method

    JP2000271782A

  • Production method of conductive film

    JP2014186902A

  • Bonding paste and semiconductor device using same

    JP2019070174A