Nonwoven
Patent Information
- Application Number
- JP2020070612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-04-09
AI Technical Summary
【0009】 本発明の不織布は、厚み回復性に優れ、ふっくらとした風合いが維持される。
Smart Images

Figure 0007570773000002 
Figure 0007570773000003 
Figure 0007570773000004
Abstract
Description
[Technical field]
[0001] The present invention relates to nonwoven fabrics. [Background technology]
[0002] Nonwoven fabrics are often used in absorbent articles such as diapers, and techniques have been developed to impart various functions to these nonwoven fabrics.
[0003] For example, Patent Document 1 describes the incorporation of a resin-bonded nonwoven fabric impregnated or coated with an adhesive into an absorbent article in order to improve the thickness recovery of the absorbent article. Specifically, the resin-bonded nonwoven fabric is disposed as a member of the absorbent article that does not come into contact with the skin. Patent Documents 2 to 4 describe uneven nonwoven fabrics in which a fiber web is previously shaped into an uneven shape and then made into a nonwoven fabric, thereby improving compression recovery rate, cushioning properties, and the like. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-187088 A [Patent Document 3] JP 2012-136791 A [Patent Document 4] JP 2019-44320 A Summary of the Invention [Problem to be solved by the invention]
[0005] For example, when a nonwoven fabric is incorporated into a product such as an absorbent article and enclosed in a packaging bag, it is subjected to compression pressure, and is required to have excellent thickness recovery properties when removed from the packaging bag. However, when attempting to increase the thickness without increasing the basis weight, the thickness recovery is still insufficient compared to the thickness before encapsulation, and there is room for improvement. In this regard, the resin-bonded nonwoven fabric described in Patent Document 1 is formed by impregnating or applying an adhesive to the entire fiber assembly, and therefore has room for improvement in terms of feel compared to an air-through nonwoven fabric. Therefore, with a resin-bonded nonwoven fabric, it is difficult to further improve the thickness recovery while maintaining the fluffy texture of the nonwoven fabric.
[0006] In view of the above problems, the present invention relates to a nonwoven fabric that has excellent thickness recovery properties and maintains a fluffy texture. [Means for solving the problem]
[0007] The present invention is a nonwoven fabric that contains thermoplastic fibers and has fusion points between the fibers. The nonwoven fabric of the present invention preferably has an apparent thickness of 4 mm or more under a load of 50 Pa. The nonwoven fabric of the present invention preferably has an apparent thickness when pressed at 2.5 kPa that is not more than half of the apparent thickness of the nonwoven fabric when pressed at 50 Pa. The nonwoven fabric of the present invention preferably has (1) a recovery rate of the apparent thickness of the nonwoven fabric after being released from compression of 40% or more. The nonwoven fabric of the present invention preferably has an apparent thickness (2) of 2 mm or more and 8 mm or less after being released from compression. The nonwoven fabric of the present invention preferably satisfies either one or both of the above requirements (1) and (2). The nonwoven fabric apparent thickness and thickness recovery rate after release from compression in the above (1) and (2) are values obtained by the following (Method for measuring nonwoven fabric apparent thickness and thickness recovery rate after release from compression). (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample, and the apparent thickness is measured. (b) Next, the nonwoven fabric sample is compressed to 0.7 mm with a load of 20 kPa. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100
[0008] These and other features and advantages of the present invention will become more apparent from the appended claims and the following description, taken in conjunction with the accompanying drawings, where appropriate. Effect of the Invention
[0009] The nonwoven fabric of the present invention has excellent thickness recovery properties and maintains a fluffy feel. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing a part of an observation screen used in a method for measuring the longitudinal orientation degree of fibers, together with a square reference line. [Diagram 2] FIG. 2 is a schematic diagram showing a portion of an observation image, together with a reference circle, used in a method for confirming the presence or absence of a binder on a fiber intersection at the center of the thickness of a nonwoven fabric. [Diagram 3] 1A is a side view of a flat nonwoven fabric, showing the position (line AA) at which cross section A passes through the center of the thickness and is perpendicular to the fiber layer that forms the nonwoven fabric surface (plane), and FIG. 1B is a side view showing the position (line BB) at which cross section B passes through the center of the thickness and is perpendicular to cross section A. [Figure 4]1A is a side view of a nonwoven fabric with a concave-convex shape, showing the position (line AA) at which cross section A is cut, which passes through the center of the thickness and is perpendicular to the fiber layer that forms the nonwoven fabric surface (the concave-convex surface connecting the tops of the convex portions and the bottoms of the concave portions), and FIG. 1B is a side view showing the position (line BB) at which cross section B is cut, which passes through the center of the thickness and is perpendicular to cross section A. [Diagram 5] FIG. 2 is a partially sectional perspective view that illustrates a specific example 1 of the uneven shape of a nonwoven fabric. [Figure 6] 1 is a photograph in lieu of a drawing showing a plane of one side of specific example 2 of a nonwoven fabric having a concave-convex shape. [Figure 7] 7 is a partial cross-sectional view of the nonwoven fabric shown in FIG. 6 taken along the line CC. [Figure 8] 7 is a partial cross-sectional view of the nonwoven fabric shown in FIG. 6 taken along the line DD. [Figure 9] 7 is a photograph showing a plan view of the opposite surface of the nonwoven fabric shown in FIG. 6. [Figure 10] 10 is a partial cross-sectional view taken along the line EE of the nonwoven fabric shown in FIG. 9. [Figure 11] 10 is a partial cross-sectional view of the nonwoven fabric shown in FIG. 9 taken along the line FF. [Figure 12] 1 is a schematic diagram illustrating the manufacturing process of a nonwoven fabric sample in Example 8, in which (A) is an explanatory diagram illustrating the process of placing a fiber web on a male support material and pressing a female support material into the male support material from above the fiber web, (B) is an explanatory diagram illustrating the process of directing a first hot air stream from above the female support material to shape the fiber web, and (C) is an explanatory diagram illustrating the process of removing the female support material and blowing a second hot air stream from above the shaped fiber web to fuse the fibers together. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Preferred embodiments of the nonwoven fabric of the present invention will now be described. The nonwoven fabric of the present invention contains thermoplastic fibers and has fusion points between the fibers. The fusion points are the portions where the fibers are bonded to each other at the contact points between the intersecting fibers. More specifically, the fusion points are formed when the surfaces of the thermoplastic fibers are partially melted by heat treatment during the manufacturing process of the nonwoven fabric, and the fibers are bonded to each other by the melting. For example, an air-through nonwoven fabric is used as the nonwoven fabric of the present invention.
[0012] As the thermoplastic fiber, various types of fibers used in this type of article can be used without any particular restriction. For example, polyester resins such as polyethylene terephthalate (hereinafter referred to as PET), polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, polylactic acid, polybutylene succinate, and their copolymers; various PE resins such as low-density polyethylene (hereinafter referred to as PE), medium-density PE, high-density PE, linear low-density PE, and ultra-high molecular weight PE; various polypropylene resins such as isotactic, atactic, and syndiotactic polypropylene (hereinafter referred to as PP) resins polymerized using a normal Ziegler-Natta catalyst or a metallocene catalyst; various polymethylpentene resins; various polyolefin resins such as ethylene-vinyl alcohol copolymer resin and ethylene-propylene copolymer resin; polyamide resins such as nylon 6, nylon 66, nylon 11, and nylon 12; and engineering plastics such as polycarbonate, polyacetal, polystyrene, and cyclic polyolefin can be used.
[0013] The nonwoven fabric of the present invention has an apparent thickness of 4 mm or more when subjected to a load of 50 Pa. Here, a load of 50 Pa means a load sufficient to suppress fluffing on the surface of the nonwoven fabric, and is a load necessary for properly measuring the apparent thickness of the nonwoven fabric. A load of 50 Pa is applied to the nonwoven fabric, for example, by placing a circular plate having a diameter of 2.5 cm and a mass of 2.45 g on the nonwoven fabric. The aforementioned apparent thickness means the vertical distance between a horizontal plane and an imaginary plane that is in contact with the outermost part of the side of the nonwoven fabric opposite to the one side that is in contact with the horizontal plane when the nonwoven fabric is placed on the horizontal plane (hereinafter, the vertical direction to the horizontal plane may be simply referred to as the "vertical direction"). The above "one side" and "opposite side" refer to the front and back sides of the nonwoven fabric, and are the side that is furthest from the horizontal plane in the vertical direction to the horizontal plane and the side that is closest to the horizontal plane. For example, when the nonwoven fabric of the present invention has an uneven shape on both sides, the apparent thickness is the vertical distance between the position of the apex of the convexity on one side and the position of the apex of the convexity on the other side. In this specification, the one surface side is also referred to as the first surface side and may be designated with the symbol 1A. The opposite surface side is also referred to as the second surface side and may be designated with the symbol 1B. In the nonwoven fabric of this embodiment, the opposite surface (second surface) is the surface side that does not come into contact with the skin during use (non-skin surface side).
[0014] (Method for measuring the apparent thickness of nonwoven fabric under a load of 50 Pa) The nonwoven fabric to be measured is cut into 10 cm x 10 cm pieces to prepare a measurement sample. A laser thickness gauge (high-precision displacement sensor ZS-LD80 (product name) manufactured by Omron Corporation. All laser thickness gauges used in this specification are of this type) is used to measure the thickness of the measurement sample under a load of 50 Pa. Measurements are taken at three locations, and the average value is regarded as the apparent thickness of the nonwoven fabric to be measured. In addition, when the nonwoven fabric to be measured is incorporated into a product, the adhesive strength of the adhesive or the like is weakened by a cooling means such as a cold spray, and the nonwoven fabric is removed from the product and the above measurement is performed. This method of removing the nonwoven fabric is similarly applied to other measurements in this specification. If it is not possible to take out a piece of nonwoven fabric measuring 10 cm x 10 cm, take out as large a piece as possible.
[0015] The nonwoven fabric of the present invention preferably has the above-mentioned apparent thickness at a load of 50 Pa (vertical load), which gives it a fluffy texture. This is due to the degree of longitudinal orientation of the fibers, and a high degree of longitudinal orientation improves the bulk of the nonwoven fabric. Furthermore, the presence of longitudinally oriented fibers makes it possible to achieve high bulk despite a low basis weight. As a result, anyone who touches the nonwoven fabric of the present invention can feel the bulkiness due to the thickness and the soft feel. From this viewpoint, the nonwoven fabric of the present invention more preferably has an apparent thickness of 5 mm or more under a load of 50 Pa, further preferably 6 mm or more, and particularly preferably 7 mm or more. From the viewpoint of ensuring the strength of the nonwoven fabric, the nonwoven fabric of the present invention preferably has an apparent thickness of 9 mm or less, and more preferably 8.5 mm or less, under the above-mentioned load of 50 Pa.
[0016] In addition, the nonwoven fabric of the present invention preferably has an apparent thickness of 50% or less of the apparent thickness of the nonwoven fabric when pressurized at 2.5 kPa (pressurized in the vertical direction) at the load of 50 Pa. The above-mentioned pressurization at 2.5 kPa means a load that is usually assumed when the nonwoven fabric of the present invention is incorporated as a component of a nonwoven fabric product such as an absorbent article, and the nonwoven fabric product is sealed in a packaging bag as a package for sale. That is, when the apparent thickness of the nonwoven fabric when pressurized at 2.5 kPa is below this upper limit, it becomes possible to compactly store a nonwoven fabric product having the nonwoven fabric of the present invention as a component in a packaging bag. Since the nonwoven fabric is usually compressed and sealed in a packaging bag, when a consumer opens and uses it, the nonwoven fabric has been in a compressed storage state due to sealing. Therefore, it is important to evaluate the nonwoven fabric under the assumption of a compressed storage state. The apparent thickness of the nonwoven fabric when pressurized at 2.5 kPa can be measured by setting the load to 2.5 kPa in the above-mentioned (method of measuring the apparent thickness of a nonwoven fabric at a load of 50 Pa).
[0017] As a result, the nonwoven fabric of the present invention has a fluffy feel due to its sufficient thickness, while also having high compression properties that enable it to be enclosed in a package. From this viewpoint, the apparent thickness of the nonwoven fabric of the present invention when pressed at the above-mentioned 2.5 kPa is more preferably 33.3% or less, and even more preferably 25% or less, of the apparent thickness of the nonwoven fabric when pressed at a load of 50 Pa. Furthermore, from the viewpoint of maintaining the fusion state of the fusion points between the fibers and maintaining the shape recovery of the fibers after the load is applied, the nonwoven fabric of the present invention preferably has an apparent thickness when pressed at the above-mentioned 2.5 kPa of the apparent thickness of the nonwoven fabric when a load of 50 Pa is applied, which is 10% or more, more preferably 12.5% or more, and even more preferably 16.7% or more.
[0018] At the same time, it is preferable that the nonwoven fabric of the present invention satisfies either or both of the following requirements (1) and (2) in terms of the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of nonwoven fabric after releasing from compression). (1) The recovery rate of the apparent thickness of the nonwoven fabric after release from compression is 40% or more. (2) The apparent thickness of the nonwoven fabric after release from compression is 2 mm or more and 8 mm or less.
[0019] (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample to measure its apparent thickness. This measurement is performed based on the above-mentioned (Method for measuring the apparent thickness of nonwoven fabric under a load of 50 Pa). (b) Next, the following "pressure treatment" is performed. The nonwoven fabric of the measurement sample is compressed to 0.7 mm with a load of 20 kPa. At this time, the nonwoven fabric is compressed to 0.7 mm, for example by inserting a spacer. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100
[0020] As a result, the nonwoven fabric of the present invention has a sufficient thickness while also having high compression properties and a fluffy feel, i.e., high cushioning properties, and also has high thickness recovery after being released from compression. Such effects are further enhanced when the nonwoven fabric of invention 1 has a longitudinal orientation of fibers and / or a binder structure present on fiber intersections, which will be described later. More specifically, a low basis weight, bulky nonwoven fabric can be formed by using fibers with a high degree of longitudinal orientation, and the increased amount of compressive deformation due to buckling of the longitudinally oriented fibers can result in bulky and highly compressible fabric. In addition, the presence of a binder at the fiber intersections suppresses crushing due to plastic deformation at the fiber fusion intersections, and the use of high core ratio fibers improves the relaxation modulus, making it possible to effectively achieve thickness recovery after release from compression. This allows the nonwoven fabric of the present invention to maintain the fluffy texture even after compression. That is, the nonwoven fabric of the present invention allows the fabric to be enclosed in a highly compressed package while providing a sense of bulk due to its thickness and a soft feel due to compression, and allows the fabric to provide a sense of its original fluffy texture after opening the package. The nonwoven fabric of the present invention also achieves and maintains both sufficient thickness and excellent cushioning properties before and after compression.
[0021] From this viewpoint, the nonwoven fabric of the present invention more preferably has a recovery rate of the apparent thickness of 45% or more after the above-mentioned compression and release, and further preferably has a recovery rate of 50% or more. From the same viewpoint, the nonwoven fabric of the present invention more preferably has an apparent thickness of 2.3 mm or more, and further preferably 2.5 mm or more, after being released from the compression. The greater the "recovery rate [%] of apparent thickness of nonwoven fabric after release from compression," the better the thickness recovery after release from compression.
[0022] In order to provide a soft feel to the nonwoven fabric of the present invention, the recovery rate of the apparent thickness of the nonwoven fabric after the above-mentioned compression and release is preferably 80% or less, more preferably 70% or less, and even more preferably 60% or less. From the same viewpoint, the nonwoven fabric of the present invention more preferably has an apparent thickness of 4 mm or less, and further preferably 3.8 mm or less, after the above-mentioned compression and release.
[0023] The nonwoven fabric of the present invention has a deformation stroke of preferably 1 mm or more, more preferably 1.5 mm or more, and even more preferably 2 mm or more after being released from compression. Furthermore, from the viewpoint of ensuring the strength of the nonwoven fabric in the thickness direction, the nonwoven fabric deformation stroke after the above-mentioned compression and release is preferably 6 mm or less, more preferably 5.5 mm or less, and even more preferably 5 mm or less. As a result, the nonwoven fabric of the present invention, in addition to the above-mentioned properties, is able to better retain the amount of deformation that gives it a feeling of softness even after being sealed in a package. The nonwoven fabric deformation stroke after compression and release is an index that indicates the cushioning properties of a nonwoven fabric after long-term compression, and is a quantification of the amount of deformation in the compression direction of the nonwoven fabric when compressed. The larger this value is, the fluffier the texture of the nonwoven fabric is. This makes it possible to quantitatively express the fluffiness and cushioning properties when a person touches the nonwoven fabric. By creating a nonwoven fabric configuration that increases the compression deformation stroke, it is possible to produce a nonwoven fabric that achieves a fluffier texture. This nonwoven fabric deformation stroke can be obtained by the following measurement method.
[0024] (Method for measuring deformation stroke of nonwoven fabric after releasing compression) The nonwoven fabric to be measured is cut to 10cm x 10cm to prepare a measurement sample. If it is not possible to take out a 10cm x 10cm piece of nonwoven fabric to be measured, take out a piece as large as possible. The pressure treatment described above (Method of measuring nonwoven fabric apparent thickness and thickness recovery rate after release from compression) is applied. Then, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is used as the measurement data. This apparent thickness of the nonwoven fabric after release from compression is called A. Next, the thickness of the measurement sample after the pressure treatment is measured in the same manner when a pressure of 2.5 kPa is applied, and this thickness is designated as B. Finally, the deformation stroke of the nonwoven fabric is calculated using the following formula. "Nonwoven fabric deformation stroke after compression and release [mm]" = AB
[0025] Such a nonwoven fabric of the present invention can be realized by various structures in the nonwoven fabric, for example, the nonwoven fabric may have the following layers a to i. a. Natural fiber layer b. A layer of hollow fibers having a partially embossed crimped portion c. A composite fiber of a core-sheath type, in which the core ratio is greater than the sheath ratio by mass. d. Elastomer fiber layer e. Low elongation fiber layer f. Unfused fiber layer g. A layer of multiple uneven nonwoven fabrics h. Layer having longitudinal fiber orientation i. Layer with binder at fiber intersections
[0026] These layers may be present in the entire nonwoven fabric of the present invention, or may be present in a part of it. When present in a part of it, these layers are preferably in the middle layer of the thickness of the nonwoven fabric. Also, it is preferable that they are present on the side opposite to the surface receiving the compressive force. For example, when the nonwoven fabric of the present invention is used as a top sheet of an absorbent article, the opposite side is the non-skin side. In addition, the nonwoven fabric of the present invention may have any one of the layers shown below, or may have more than one of them. When the nonwoven fabric of the present invention has more than one of the layers shown below, the layers may be separate layers, or each of the layers may have a mixed structure within one layer. The "middle layer of thickness" of the nonwoven fabric mentioned above means the "middle layer 50%" portion when the apparent thickness of the nonwoven fabric under a load of 50 Pa is defined as the upper layer 25%, the middle layer 50%, and the lower layer 25%.
[0027] In particular, the layers a, d, f, and h are preferably intermediate layers within the above-mentioned thickness range. It is preferable that the layers b, c, e and g constitute the entire nonwoven fabric. The layer i preferably constitutes 70% of one side of the nonwoven fabric.
[0028] The above items a to i will be described in detail below. a. Natural fiber layer This layer is a layer using natural fibers, unlike thermoplastic fibers. The natural fibers referred to here are not particularly limited, but are preferably cellulose fibers, cotton, etc. For example, cellulose fibers are not thermally fused at the intersections between the fibers, and the fibers are relatively free to deform. It is preferable that the cellulose fibers are curled by being crimped or spirally formed. The nonwoven fabric of the present invention has a high thickness recovery after compression due to the presence of a natural fiber layer. As such cellulose fibers, those commonly used in this type of product can be used without any particular limitation. For example, those described in paragraphs
[0098] and
[0291] of JP2017-526473A can be mentioned. The method for constructing this layer as a nonwoven fabric is not particularly limited, but for example, natural fibers are mixed with thermoplastic fibers, or sandwiched between layers of thermoplastic fibers, and then the layers are made into a nonwoven fabric using a thermal bonding method such as fixing with an embossing roll or an air-through method, or a needle punch method or a spun lace method.
[0029] b. A layer of hollow fibers having a partially embossed crimped portion The hollow fiber contains air inside, and has a structure in which the air is trapped in the hollow by the embossed and compressed parts, which gives the hollow fiber the ability to recover from bending like a tubular balloon. The nonwoven fabric of the present invention has a layer of hollow fibers partially having such embossed and compressed portions, and thus has high thickness recovery after compression. The method for forming this layer as a nonwoven fabric is not particularly limited, but for example, hollow fibers using a thermoplastic resin are used, and the fibers are compressed with an embossing roll or the like to form a nonwoven fabric.
[0030] c. A composite fiber of a core-sheath type, in which the core ratio is greater than the sheath ratio by mass. Specifically, the core-sheath type composite fiber is a fiber containing two or more different resin components as constituent components. With respect to this melting point, when the resin component of the sheath has a lower glass transition temperature than the resin component of the core (for example, the resin component of the core is PET and the resin component of the sheath is PE), the thickness recovery of the nonwoven fabric can be improved by reducing the mass ratio of the resin component with the lower glass transition temperature. The following factors are considered to be the cause of this. It is known that resins with low glass transition temperatures have a low relaxation modulus. It is also known that a low relaxation modulus makes it difficult to recover from deformation. Therefore, it is considered that a higher thickness recovery can be imparted to the nonwoven fabric by reducing the resin component with a low glass transition temperature as much as possible. The core-sheath type composite fiber preferably has a configuration in which a core component and a sheath component are concentrically arranged. "The core ratio is greater than the sheath ratio of the core-sheath mass ratio of the composite fiber" means that the mass ratio of the core component in the mass of the composite fiber is greater than the mass ratio of the sheath component in the mass of the composite fiber. As such a core-sheath type composite fiber, any fiber that is commonly used in this type of article can be used without any particular restrictions. For example, the fiber described in paragraph
[0051] of JP 2019-44321 A can be used. The above-mentioned core-sheath type composite fiber is a thermoplastic fiber, and is thermally fused to other fibers at their intersections to form fusion points. The nonwoven fabric of the present invention has high thickness recovery after compression due to the inclusion of layers of the core-sheath type composite fibers as described above. The method for forming this layer as a nonwoven fabric is not particularly limited, but it is preferable to use a thermal bonding method such as an air-through method.
[0031] (Method for identifying different resin components in core-sheath composite fibers) Whether or not the composite fiber contains two or more types of resin components is judged from the melting point peak measured by the following method. When counting endothermic peaks, if peaks appear at intervals of 5°C or more, it is judged that the resin components are different types. (1) Prepare a 0.01 g nonwoven fabric sample as a measurement sample. (2) Using a differential scanning calorimeter "DSC7000X" (product name, manufactured by Hitachi High-Tech Science Corporation), 0.01 g of a nonwoven fabric sample is weighed into an aluminum pan, heated to 200°C, and then cooled to 0°C at a rate of 10°C / min. (3) Raise the temperature to 300°C at a rate of 10°C / min and measure the endothermic peak.
[0032] (Method for measuring the mass ratio of the core component and the sheath component to the mass of core-sheath type composite fiber) The nonwoven fabric to be measured is cut to a size of 10 cm x 10 cm to prepare a measurement sample. If it is not possible to take out a piece of nonwoven fabric measuring 10 cm x 10 cm, take out a piece as large as possible. The measurement sample is frozen with liquid nitrogen, and then the thickness cross section of the nonwoven fabric is cut with a razor blade so as to be perpendicular to the flow direction of the fibers when the nonwoven fabric is viewed in plan, to obtain a cross section of the core-sheath type composite fiber. The cross section of the composite fiber is observed at a magnification of 2000 times using a tabletop scanning electron microscope (SEM) JCM-6000Plus (manufactured by JEOL Ltd., product name. All SEMs used in this specification are of this type). The size of the observation screen is enlarged to 43 μm vertically and 60 μm horizontally. The cross-sectional areas of the core and sheath components are measured, the volume per unit length is calculated, and the core-sheath ratio (mass ratio) is calculated from the density of each resin component. The average value of the measurement results for 10 fibers is used as the measurement data for the core-sheath ratio. The density of the resin component is the value from the Plastic Materials Directory (Processing Technology Research Association).
[0033] d. Elastomer fiber layer The nonwoven fabric of the present invention has a layer of elastic elastomer fibers, which enhances the thickness recovery after compression. The term "elastomer" as used herein is defined as a material that does not break brittle when stretched and has elasticity. The elastomer fibers may be any commonly used fiber, and examples of such fibers include thermoplastic elastomer fibers described in paragraphs
[0010] to
[0060] of JP2007-321293A. The method for constructing this layer as a nonwoven fabric is not particularly limited, but for example, an elastomer fiber using a thermoplastic resin is used, or a thermoplastic elastomer fiber is mixed with a thermoplastic fiber, or the layer is sandwiched between layers of thermoplastic fiber, and then the nonwoven fabric is formed using a thermal bonding method such as fixing with an embossing roll or an air-through method, or a needle punch method or a spun lace method.
[0034] e. Low elongation fiber layer The low elongation fiber refers to a fiber whose elongation (breaking elongation) measured according to JIS L1015 7.7.1 is 100% or less. The thickness recovery of the nonwoven fabric of the present invention is further improved by the presence of the low elongation fiber in the aforementioned "c. A layer of fibers that are sheath-core composite fibers and have a core ratio greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers." Also, in the nonwoven fabric of the present invention, the "e. A layer of low elongation fibers" is more dominant in terms of thickness recovery than the aforementioned "c. A layer of fibers that are sheath-core composite fibers and have a core ratio greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers." Such low elongation fibers are difficult to elongate and therefore undergo little change in shape. Therefore, the nonwoven fabric of the present invention has high thickness recovery after compression by including a layer of low elongation fibers. From this viewpoint, the elongation of the low elongation fibers is more preferably 90% or less, and even more preferably 85% or less. The elongation of the low elongation fiber is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more, from the viewpoint of strengthening the fusion between the fibers and increasing the strength of the nonwoven fabric. The method for forming this layer into a nonwoven fabric is not particularly limited, but for example, the nonwoven fabric may be formed by a thermal bonding method such as fixing with an embossing roll or an air-through method, or by a needle punch method or a spun lace method.
[0035] f. Unfused fiber layer An unfused fiber layer is a layer in which the intersections of fibers are not bonded together. Specifically, it is a layer that is not thermally fused by thermoplastic fibers. It is also a layer that is not bonded or mechanically bonded by a binder. The fibers of such layers are preferably made of a high melting point resin. In the unfused fibrous layer, the fibers are relatively free to deform, and therefore, the nonwoven fabric of the present invention has high thickness recovery after compression by including the unfused fibrous layer. From this viewpoint, it is preferable that the unfused fiber layer is particularly the above-mentioned intermediate thickness layer. The method for constructing this layer as a nonwoven fabric is not particularly limited, but for example, fibers made of a high melting point resin are mixed with thermoplastic fibers and the nonwoven fabric is formed using a needle punching method or a spun lace method, or a thermal bonding method in which the fibers made of a high melting point resin are sandwiched between layers of thermoplastic fibers and fixed using an embossing roll or an air-through method, or a needle punching method or a spun lace method is used to form a nonwoven fabric.
[0036] g. A layer of multiple uneven nonwoven fabrics The convex portions of one uneven nonwoven fabric face one side, and the convex portions of the other uneven nonwoven fabric face the opposite side, and the bottoms of the concave portions of the nonwoven fabrics are joined together, so that the concave portions support each other's uneven structures while maintaining thickness. This improves the shape retention of the layer in which the uneven nonwoven fabrics are stacked. In addition, the spaces in the concave portions of the uneven nonwoven fabrics increase the flexibility of the layer in which the uneven nonwoven fabrics are stacked, improving softness to the touch and cushioning. A specific example of a layer in which such uneven nonwoven fabrics are stacked is shown in FIG. 1 of JP 2013-194333 A. In addition, as a method for laminating the uneven nonwoven fabrics together, various methods that can be usually used can be adopted without any particular restrictions. For example, embossing, heat fusion by hot air treatment, and bonding by hot melt adhesive can be mentioned. From the viewpoint of maintaining a soft texture, heat fusion by hot air treatment and bonding by hot melt adhesive are preferable to embossing. The number of layers of the uneven nonwoven fabric is not limited to two, but may be three or more. In the case of three or more layers, an additional layer may be laminated between one side and the opposite side. The nonwoven fabric of the present invention has a layer in which a plurality of such uneven nonwoven fabrics are laminated, and thus has excellent shape retention, flexibility, softness to the touch and cushioning properties, and has high thickness recovery after compression.
[0037] h. Layer having longitudinal fiber orientation The longitudinal orientation of fibers means that the fibers are oriented in the thickness direction of the nonwoven fabric. As described above, the thickness direction means the vertical direction to the horizontal plane when one side of the nonwoven fabric is placed on the horizontal plane. Examples of layers having such longitudinal fiber orientation are described in JP-A-5-263345, paragraphs
[0005] to
[0026] . A layer having longitudinally oriented fibers is less likely to collapse even when subjected to a compressive force in the thickness direction, and has high shape recovery properties. Therefore, the nonwoven fabric of the present invention has a layer having such longitudinal fiber orientation, and thus has high thickness recovery after compression. In particular, the deformation stroke of the nonwoven fabric after release from compression can be improved. From this viewpoint, it is preferable that the layer having longitudinally oriented fibers is present at least in the intermediate thickness layer portion of the nonwoven fabric of the present invention. The method for forming this layer into a nonwoven fabric is not particularly limited, but it is preferable to form the nonwoven fabric using a thermal bonding method in which thermoplastic fibers are fixed using an embossing roll or air-through method, or a needle punch method or a spun lace method.
[0038] The longitudinal orientation of the fibers is indicated by the degree of longitudinal orientation of the fibers. The "degree of longitudinal orientation" is a value measured by the method described below (Method for measuring the degree of longitudinal orientation of fibers), and indicates the degree to which the orientation of fibers having a thickness direction component is uniform. The term "fibers having a thickness direction component" refers to fibers that have a vertical component as a vector relative to a horizontal plane when the nonwoven fabric of the present invention is placed on a horizontal plane with one of the front and back sides facing up. In this specification, "thickness direction" means that the vertical component is greater than zero. Also, "fibers having a thickness direction component" is synonymous with "longitudinal oriented fibers."
[0039] From the viewpoint of improving the thickness recovery property of the nonwoven fabric after compression, the degree of longitudinal orientation is preferably 55% or more, more preferably 60% or more, and even more preferably 65% or more. From the viewpoint of increasing the strength of the nonwoven fabric, the degree of longitudinal orientation is preferably 95% or less, more preferably 90% or less, and even more preferably 80% or less.
[0040] (Method for measuring the degree of longitudinal orientation of fibers) (1) A nonwoven fabric sample is frozen with liquid nitrogen and placed on a horizontal plane. Then, a thickness cross section (cross section in the vertical direction) of the nonwoven fabric sample at a position that is 50% of the thickness in the vertical direction relative to the horizontal plane (the center of the thickness) is prepared by cutting with a razor blade. (2) The thickness cross section is observed at 35x magnification using a SEM, and an observed image is taken. (3) A reference line L forming a square of 0.5 mm x 0.5 mm (dimensions within the observed image) is added to the observed image. Here, the reference line L is composed of an upper side L1 and a lower side L2 that are aligned with the direction along the horizontal plane, and a left side L3 and a right side L4 that are aligned with the vertical direction. (4) Count the total number of fibers passing through the reference line formed by each side of the square. The total number of fibers passing through the reference line L of the top and bottom sides L1 and L2 of the square is the "top and bottom fiber count," and the total number of fibers passing through the reference line L of the left and right sides L3 and L4 of the square is the "left and right fiber count." (5) The degree of longitudinal orientation Q of fibers in a nonwoven fabric is calculated as (number of up-down fibers) / (number of up-down fibers + number of left-right fibers)×100. Three observation images of each of these were prepared and measured for the same nonwoven fabric sample, and the average was used as the measurement data. 1 shows an observation screen with a square reference line L. In the figure, black dots 71 are positions where the fiber 7 passes through the reference line L (L1 to L4).
[0041] The "thickness center" refers to a portion between a horizontal plane and an imaginary plane in the "apparent thickness" of the nonwoven fabric defined above, the portion being 50% of the distance in the vertical direction to the horizontal plane. The thickness of the nonwoven fabric here is measured based on the above-mentioned (method of measuring the apparent thickness of a nonwoven fabric under a load of 50 Pa).
[0042] i. Layer with binder at fiber intersections The fiber intersection refers to a portion where two or more fibers cross. The binder present at the fiber intersection preferably covers the outer surface of the portion where the fibers cross and overlap. In addition, the binder preferably extends to the fiber surface other than the fiber intersection while being present at the fiber intersection. It is also preferred that the binder is present at fiber intersections in the thickness center of the nonwoven fabric of the present invention, i.e., the layer in which the binder is present at the fiber intersections is preferably located in the thickness center of the nonwoven fabric of the present invention.
[0043] In the nonwoven fabric of the present invention, which contains thermoplastic fibers and has fusion points between fibers, the binder acts to restore the three-dimensional intersections between fibers by providing a layer having a binder at the fiber intersections. That is, when a compressive force (pressing force) is applied to the nonwoven fabric of the present invention from one side, the three-dimensional intersections of the fibers at the fiber intersections are crushed by the compressive force. However, when the compressive force is removed, the binder restores the arrangement of the three-dimensional intersections of the fibers at the fiber intersections. The nonwoven fabric of the present invention has high thickness recovery after compression due to the above-mentioned effect in the layer in which the binder is present at the fiber intersections.
[0044] Such a binder has a viscosity or adhesiveness that allows it to adhere to the surface of the fiber intersections and not run off. The binder also has a softness that ensures the mobility of the fibers at the fiber intersections necessary for the cushioning properties of the nonwoven fabric, while having a viscosity or adhesiveness that allows the positional relationship between the fibers to be restored to their original position after the movement. Furthermore, it is preferable that the binder has elasticity in view of the above-mentioned action.
[0045] Various binders can be used, including, for example, acrylic resins, ester resins, vinyl acetate resins, styrene resins, vinyl acetate-ethylene resins, and styrene-butadiene rubber. In particular, acrylic resins, styrene-butadiene rubber, etc. are preferred as they have the viscosity, adhesiveness, and softness to restore the three-dimensional intersection arrangement of fibers at the fiber intersections.
[0046] (Method for checking the presence or absence of binder at fiber intersections in the center of nonwoven fabric thickness) (1) Prepare a 0.3 g nonwoven fabric sample as a measurement sample. Next, place the nonwoven fabric sample in a beaker containing 100 mL of ethyl acetate and stir for 30 minutes. Remove the nonwoven fabric sample and dry it. This washes away any ingredients that were attached to the nonwoven fabric sample, such as skin care agents and hot melt adhesives. (2) The nonwoven fabric sample is dyed using an identification reagent (Bouken Stain II fiber identification reagent, manufactured by Boken Quality Evaluation Organization, a general incorporated foundation) that dyes the binder adhered to the fiber surface a color different from the fiber to distinguish between the two. (3) After freezing the nonwoven fabric sample with liquid nitrogen, two cross sections passing through the center of the thickness of the nonwoven fabric sample are prepared by cutting with a razor blade. One is cross section A passing through the center of the thickness of the nonwoven fabric sample (a cross section passing through the center of the thickness and perpendicular to the fiber layer that forms the nonwoven fabric surface). The other is cross section B passing through the center of the thickness of the nonwoven fabric sample and perpendicular to cross section A. The cross section may be any of a cross section along the MD (machine direction) direction (machine flow direction in the manufacturing process) in the plane of the nonwoven fabric, a cross section along the CD (cross direction) direction (direction perpendicular to the machine flow direction), and any cross section therebetween. It is sufficient that a cross section passing through the thickness center along at least one of the planar directions satisfies the predetermined requirements. (4) The sample prepared in (3) above is placed on a horizontal surface with the cross section facing upward. In this state, an observation image is taken at 100x magnification using a digital microscope VHX-900 (product name, manufactured by Keyence Corporation). (5) For the observation images of the above two cross sections, a reference circle C with a diameter of 1.0 mm (dimensions within the observation image) is drawn within the observation image. The number of fiber intersections (N) within the reference circle C and the number of dyed fiber intersections (Nb) among the number of fiber intersections (N) are counted. As a result of the counting, the cross section with the larger number of dyed fiber intersections (Nb) is the measurement object. (The range in focus in the observation image is the measurement object.) Fiber intersections are counted both where the fibers are fused and where they are not fused. When obtaining an observation image of the thickness center portion of cross section A, the cross section sample is adjusted to the center of the observation screen starting from a low magnification, and the thickness center portion is identified by increasing the magnification. (6) Next, the presence rate of the binder on fiber intersections per unit area at the center of the thickness of the nonwoven fabric is calculated based on the following formula (S1). H(%)=Nb÷N×100 (S1) H: Presence rate of binder on fiber intersections per unit area Nb: Number of dyed fiber intersections within reference circle C N: Number of fiber intersections within reference circle C (including Nb) For each of these, three points are observed on the same nonwoven fabric sample, and two observation images are prepared and measured. The larger value of the measurement result for the binder presence rate on the fiber intersections of cross sections A and B is adopted, and the average is used as the measurement data. FIG. 2 shows that a plurality of fiber intersections 6 where fibers 7 intersect with each other, and dyed fiber intersections 61, are present within a reference circle C marked on the observation screen.
[0047] The two cross sections A and B in (3) above are, for example, as follows. When the nonwoven fabric has a flat shape with no unevenness in the fiber layers in both the planar and thickness directions, cross section A is a cross section that passes through the thickness center and is perpendicular to the fiber layers that form the nonwoven fabric surface (plane). In this case, cross section B is a cross section that passes through the thickness center and is along the nonwoven fabric plane. Specifically, cross section A is a cross section along the vertical line AA that passes through the thickness center 105 of the nonwoven fabric 100S as shown in Figure 3(A). Cross section B is a cross section along the horizontal line BB at the thickness center 105 of the nonwoven fabric 100S as shown in Figure 3(B). In addition, when the fiber layer of the nonwoven fabric meanders in the thickness direction to have an uneven shape with alternating convex and concave portions, the cross section A is a cross section that passes through the thickness center and is perpendicular to the fiber layer that forms the nonwoven fabric surface (the wall surface connecting the top of the convex portion and the bottom of the concave portion). In this case, the cross section B is a cross section along the fiber layer that passes through the thickness center and forms the nonwoven fabric surface (the wall surface connecting the top of the convex portion and the bottom of the concave portion). Specifically, the cross section A is a cross section along the line AA that passes through the thickness center 105 of the nonwoven fabric 100W as shown in FIG. 4(A). The cross section B is a cross section along the line BB (a line perpendicular to the line AA) at the position of the thickness center 105 of the nonwoven fabric 100W as shown in FIG. 4(B).
[0048] The details of the dyeing process (2) above will now be described. (2-1) Shake the container of Bouken Stain II well to mix thoroughly. (2-2) Place 1.5 mL of the mixed Bowen Stain nII in a beaker of approximately 200 mL in size, add deionized water, and make the total volume 30 mL to create a dye solution. (2-3) Heat the dye solution and add the nonwoven fabric sample when it reaches about 90°C before boiling, and boil at 95°C for 2 minutes. (2-4) Take out the nonwoven fabric sample, rinse it thoroughly with water, and then dry it. (2-5) The color is compared with the identification color. For example, a binder containing acrylic resin or styrene-butadiene rubber will be dyed red and the fiber will remain white (however, the dyeing of the binder will vary depending on the binder components).
[0049] The binder is a resin component different from the constituent fibers of the nonwoven fabric, and is fixed to the surface of the constituent fibers after the nonwoven fabric is formed. For example, the binder is sprayed onto one side of the nonwoven fabric by a spray or the like to adhere to the fiber intersections. The binder is preferably sprayed from the side of the nonwoven fabric opposite to the side that comes into contact with the skin, from the viewpoint of suppressing a sticky feeling when the nonwoven fabric comes into contact with the skin. From the same viewpoint, the spraying mass of the binder is 5 g / m per unit area of the nonwoven fabric. 2 The following is preferred: In order to effectively exert the action of the binder on the fiber intersections, the mass of the binder to be sprayed is set to 0.3 g / m per unit area of the nonwoven fabric. 2 The above is preferred.
[0050] In the nonwoven fabric of the present invention, from the viewpoint of effectively exerting the action of the binder, the proportion of the mass of the binder in the mass of the nonwoven fabric is preferably 1% or more. In the nonwoven fabric of the present invention, from the viewpoint of realizing a fluffy feel, the proportion of the mass of the binder in the mass of the nonwoven fabric is preferably 15% or less.
[0051] (Method for measuring the ratio of binder mass to nonwoven fabric mass) (1) Prepare a total of 1.0 g of a nonwoven fabric sample that has been treated in the same manner as in (1) above (Method for confirming the presence or absence of binder at fiber intersections in the center of the nonwoven fabric). (2) Cut the nonwoven fabric sample into small pieces of 0.1 mm square. Place 1.0 g of the sample into a beaker and add hexafluoroisopropanol (hereinafter referred to as HFIP) to separate it into HFIP-insoluble and HFIP-soluble parts. This dissolves the PET components of the fibers. (3) Add heated xylene at 130°C to the HFIP insoluble fraction obtained in (2) above, thoroughly stir, and filter to separate into heated xylene insoluble fraction and heated xylene soluble fraction, thereby dissolving the PP and PE components of the fibers. (4) The HFIP insoluble and heated xylene insoluble fractions obtained in (3) above are weighed and subjected to TG / DTA measurement. The amount burned in the TG / DTA measurement is defined as the binder mass (the fibers may contain additives such as titanium oxide. If the fibers contain titanium oxide, this allows the binder and titanium oxide to be separated). (5) The binder mass obtained in (4) above is divided by 1.0 g of the nonwoven fabric sample prepared in (1) above to calculate the binder mass percentage (%).
[0052] In the above method (method for measuring the proportion of binder mass in a nonwoven fabric sample), the amount of binder adhered to the entire nonwoven fabric can be grasped as a mass proportion of the nonwoven fabric mass, relative to the fibers, regardless of the surface to which the binder is sprayed.
[0053] The binder may be present at other fiber intersections as well, so long as it is present at the fiber intersections in the thickness center of the nonwoven fabric. The fiber intersections where the binder is present may be fused fibers or may be intersections of non-fused fibers. Since the binder has adhesiveness, a small amount of the binder can exert the above-mentioned effect. Therefore, the fiber intersection where the binder is present is preferably a fusion point between fibers. Compared to the intersection of non-fused fibers, the fusion point already forms a bonded intersection, so it is not necessary to form an intersection by the binder. As a result, a small amount of binder is required for thickness recovery at the fusion point between fibers compared to the non-fused fiber intersection, and the thickness recovery effect due to the elasticity of the binder can be prevented from being reduced by the adhesiveness of the binder. When the binder is present at the fusion points between the fibers, the positional relationship (stereoscopic crossing relationship) between the fixed fibers can be more firmly maintained. Furthermore, when the binder is present at the intersections between non-fused fibers, the positional relationship between the fibers (three-dimensional intersection relationship) can be restored while maintaining soft deformability when pressed. From the viewpoint of achieving both thickness recovery and soft cushioning of the nonwoven fabric, it is preferable that the binder is present at both the fusion points between fibers and the intersections between non-fused fibers. In this case, it is preferable that the number of fiber intersections at the center of the thickness of the nonwoven fabric where the binder is present is greater than the number of fused fiber intersections.
[0054] The nonwoven fabric of the present invention is preferably made of thermoplastic fibers. For example, it is preferably composed of the layers b to i described above. This facilitates the restoration of the original shape from the fusion points between the fibers, and can further improve the recovery and cushioning properties.
[0055] Furthermore, the nonwoven fabric of the present invention is preferably made of the composite fiber described above in "c. A layer of fibers that is a sheath-core composite fiber and has a core-sheath mass ratio greater than the sheath mass ratio" among thermoplastic fibers. Specifically, the nonwoven fabric of the present invention is preferably made of composite fibers that contain two or more different resin components, and the core-sheath mass ratio of the composite fiber is preferably such that the core ratio is greater than the sheath ratio.
[0056] Furthermore, in the nonwoven fabric of the present invention, the above-mentioned composite fiber is preferably a low elongation fiber as described in "e. Low elongation fiber layer" rather than an elastomeric fiber as described in "d. Elastomer fiber layer" above. In other words, the elongation of the composite fiber is preferably 100% or less, and more preferably within the range described in "e. Low elongation fiber layer" above. This suppresses deformation caused by the weight and minute pressure generated by the elastomeric fiber, making the recovery effect more likely to be exhibited.
[0057] In addition, the nonwoven fabric of the present invention preferably has fusion points between fibers in the thickness center. For example, it is preferable that the nonwoven fabric has the above-mentioned layers b to e and g to i in the thickness center. This prevents the fibers from being biased due to compression in the thickness center, and allows the restoring force originating from the fusion points between the fibers to be exerted uniformly within the layers, preventing unevenness in recovery and cushioning properties.
[0058] The definition of the "thickness center portion" and the method for measuring the thickness are as described above. The fusion point can be confirmed by the following method.
[0059] (Method for checking the presence or absence of fusion points between fibers in the center of the thickness of a nonwoven fabric) (1) Cut the nonwoven fabric to be measured into a piece of 10 cm x 10 cm to prepare a nonwoven fabric sample. If it is not possible to cut out a piece of 10 cm x 10 cm to be used as the nonwoven fabric to be measured, cut out a piece of the largest possible size. (2) Obtain an observation image of the thickness center of the nonwoven fabric sample by carrying out the same processes as (1) and (2) in the above (Method of measuring the longitudinal orientation of fibers). At that time, adjust the cross-sectional sample to the center of the observation screen from a low magnification, and then increase the magnification to identify the thickness center. (3) A reference circle with a diameter of 0.5 mm (dimensions within the observed image) is drawn within the observed image, and the number of fusions between fibers within the circle is counted to determine whether or not fusions exist (the range in focus in the observed image is the measurement target). The number of fusions is also counted, and these are measured by preparing and measuring three observation images of the same sample, and the average is used as the measurement data for the number of fusions per unit area.
[0060] In the nonwoven fabric of the present invention, the number of fusion points at the center of the thickness per unit area is set to 100 / mm from the viewpoint of the strength of the nonwoven fabric. 2 More than 120 pieces / mm is preferable. 2 More preferably, 150 pieces / mm 2 The above is more preferable. The number of fusion points per unit area at the center of the thickness is set to 300 / mm in order to give the nonwoven fabric a soft feel. 2 Less than 250 pieces / mm is preferable. 2 Less than 220 pieces / mm is more preferable. 2 The following is even more preferred:
[0061] In addition, in the nonwoven fabric of the present invention, from the viewpoint of fluffy texture, the smaller the area of the embossed part (hereinafter also referred to as embossed part) as shown in the above "g. Layer in which multiple uneven nonwoven fabrics are laminated" is, the better. Therefore, the embossing rate measured by the following method is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. The lower limit of the embossing rate is not particularly set, but is 0% or more.
[0062] (Method of measuring embossing rate) (1) Select the part of the nonwoven fabric sample with the highest embossing rate, cut the nonwoven fabric to be measured into a 10 cm x 10 cm sample to prepare a measurement sample. If it is not possible to take out a sample of 10 cm x 10 cm to be measured, take out the largest possible size. (2) With the nonwoven fabric placed horizontally, an observation image is taken. The area ratio of the film-like portion in a 50 mm x 50 mm square of the observation image is measured as the embossing ratio. Three observation images are prepared and measured for each sample, and the average is used as the measurement data. The film-like portion refers to a surface that has no irregularities larger than the fiber diameter, a surface formed with irregularities equal to or smaller than the fiber diameter, or a flat surface that has no irregularities equal to or smaller than the fiber diameter.
[0063] The nonwoven fabric of the present invention preferably has an uneven shape at the above embossing ratio. The uneven shape is preferably on at least one side of the nonwoven fabric of the present invention and the opposite side, and more preferably on both sides. This makes it easier for the embossed part to retain space, and can further improve recovery and cushioning properties.
[0064] Furthermore, the nonwoven fabric of the present invention preferably has a degree of longitudinal orientation of fibers in the range of values shown in the above-mentioned "h. Layer having longitudinal orientation of fibers". It is preferable that the nonwoven fabric of the present invention has such a degree of longitudinal orientation of fibers at least in the intermediate layer. In the nonwoven fabric of the present invention, as described above in "i. Layer in which a binder is present at fiber intersections", it is preferable that the binder is present at fiber intersections in the thickness center. It is also preferable that the proportion of the mass of the binder in the mass of the nonwoven fabric of the present invention is within the range described above in "i. Layer in which a binder is present at fiber intersections".
[0065] The nonwoven fabric of the present invention has a basis weight of 100 g / m2 in order to have excellent compressibility and a fluffy feel while having the bulk due to the apparent thickness of the nonwoven fabric under a load of 50 Pa. 2Less than 60 g / m 2 Less than 40 g / m is more preferable. 2 The following is even more preferred: The lower limit of the basis weight is not particularly limited, but from the viewpoint of improving the texture of the nonwoven fabric, it is set to 8 g / m 2 More than 10 g / m is preferable. 2 More preferably, 15 g / m 2 The above is more preferable.
[0066] The nonwoven fabric of the present invention, while having the above-mentioned configuration, preferably has an uneven shape having convex parts, concave parts, and walls connecting the convex parts and the concave parts in the thickness direction of the nonwoven fabric. By making the uneven shape, the nonwoven fabric of the present invention becomes bulkier (thicker) and has a good texture while suppressing the basis weight. As a result, the nonwoven fabric of the present invention can have a fluffy texture due to the above-mentioned compression characteristics, i.e., a high cushioning property.
[0067] When the nonwoven fabric of the present invention 1 has an uneven shape, various uneven shapes can be used. In addition, various materials that are usually used as materials that come into contact with the skin can be used. For example, the uneven shape of the nonwoven fabric may be of various types, such as those with solid convexities, those with hollow convexities, those with a single fiber layer, those with a two-layer fiber layer, those with convexities arranged in a scattered manner in the planar direction, those with convexities and concaves arranged in a ridge-like pattern, etc. In addition, the uneven shape is not limited to being on one side, and may be on both sides. Among these, preferred is a nonwoven fabric having a single layer structure in which the convex portions of the concave-convex shape are hollow and the concave-convex shape is present on both sides of the nonwoven fabric, for example the following nonwoven fabric 80 (specific example 1) and nonwoven fabric 90 (specific example 2). These are explained below.
[0068] Nonwoven fabric 80 (Specific Example 1) has a layer structure containing thermoplastic fibers and has the following uneven shape. In addition, nonwoven fabric 80 satisfies the above-mentioned requirements of (h. Layer having longitudinal fiber orientation) and (i. Layer having binder at fiber intersections). That is, it has outer fiber layers 81, 82 on the first surface (one surface) 1A side and the second surface (opposite surface) 1B side, and a plurality of connecting portions 83 disposed between the outer fiber layer 1 on the first surface 1A side and the outer fiber layer 2 on the second surface 1B side. The outer fiber layer 81 on the first surface 1A side and the outer fiber layer 82 on the second surface 1B side and the connecting portions 83 are partially fused to each other. Furthermore, in the outer fiber layer 82 and the connecting portions 83 on the second surface 1B side, the binder is present at the intertwined fiber points, and is attached so as to cover the intertwined fiber points. The outer fiber layers 81, 82 and the connecting portion 83 form an uneven shape in the thickness direction of the nonwoven fabric 80, which includes hollow convex portions, concave portions, and walls connecting the convex portions and the concave portions. The uneven shape is formed on both the first surface 1A side and the second surface 1B side. Specifically, on the first surface 1A side, the convex portions 81 formed by the outer fiber layer 81 and the concave portions 88 between the outer fiber layers 81 have an uneven shape. On the second surface 1B side, the convex portions 82 formed by the outer fiber layer 82 and the concave portions 89 between the outer fiber layers 82 have an uneven shape. Both the convex portions 81 formed by the outer fiber layer 81 and the convex portions 82 formed by the outer fiber layer 82 are hollow. The connecting portion 83 forms a wall portion 83 connecting the convex portions 81 and the concave portions 88 (the convex portions 82 and the concave portions 89). The nonwoven fabric 80 may have various configurations described in paragraphs
[0010] to
[0048] of JP 2019-44319 A. For example, the uneven shape of the nonwoven fabric 80 may be a shape in which the convex portions 81 formed by the outer surface fiber layer 81 and the concave portions 88 between them are arranged in a ridge-like shape on the first surface 1A side. Similarly, the convex portions 82 formed by the outer surface fiber layer 82 and the concave portions 89 between them may be arranged in a ridge-like shape on the second surface 1B side. In addition, the outer surface fiber layers 81 and 82 may have fibers oriented in the planar direction. The wall portion 83 formed by the connecting portion 83 may have fibers oriented vertically. The outer surface fiber layer 1 that becomes the convex portion on the first surface 1A side may have two types (a first outer surface fiber layer 81A and a second outer surface fiber layer 81B) having lengths extending along different directions that intersect in a plan view of the nonwoven fabric. The multiple connecting portions 83 may be arranged along different directions that intersect in a plan view of the nonwoven fabric, and may have two types (first connecting portions 83A and second connecting portions 83B) with different wall surface orientations of the connecting portions 83. In this case, the first connecting portions 83A and the second connecting portions 83B may have wall surface orientations that are different from each other, or the fibers may be oriented vertically. This nonwoven fabric 80 typically has the shape shown in FIG. Such a nonwoven fabric 80 can be produced by the method described in paragraphs
[0049] to
[0057] of JP 2019-44319 A.
[0069] The nonwoven fabric 90 (Specific Example 2) has a layer structure containing thermoplastic fibers and has the following uneven shape. The nonwoven fabric 90 satisfies the above-mentioned requirements of (h. Layer having longitudinal fiber orientation) and (i. Layer having binder at fiber intersections). That is, on the first surface (one surface) 1A side, a plurality of vertical ridges 911 protruding toward the first surface 1A side in the thickness direction of the nonwoven fabric are arranged extending in one direction on the first surface 1A side in a plan view. The vertical ridges 911 are arranged side by side at intervals in another direction on the first surface 1A side in a plan view different from the one direction on the first surface 1A side. In addition, horizontal ridges 921 extending in the other direction on the first surface 1A side are arranged connecting the vertical ridges 911. The vertical ridges 911 and horizontal ridges 921 each form a hollow convex portion. The nonwoven fabric 90 has an uneven shape in its thickness direction, which includes convex portions, concave portions, and wall portions 911W connecting the convex portions and the concave portions, by the vertical ridges 911 and horizontal ridges 921 and the concave portions 922 between them. On the first surface 1A side, the convex portions formed by the vertical rib portions 911 and the horizontal rib portions 921 have lengths extending along different directions that intersect in a plan view of the nonwoven fabric 90. In this case, the uneven shape on the first surface side of the nonwoven fabric 90 may be a shape in which the convex portions formed by the vertical rib portions 911 and the horizontal rib portions 921 and the concave portions therebetween are arranged in a ridge-groove shape. In addition, on the second surface (opposite surface) 1B side, a plurality of hollow convex ridges 931 are arranged, which extend in one direction on the second surface 1B side in plan view and are arranged in another direction on the second surface 1B side different from the one direction on the second surface 1B side. In addition, a concave ridge 936 sandwiched between the plurality of convex ridges 931 extends in one direction on the second surface 1B side. The uneven shape on the second surface 1B side of the nonwoven fabric 90 has a shape in which the convex ridges 931 and the concave ridges 936 are arranged in a ridge-like shape. The convex ridges 931 are formed by a plurality of convex portions 934 connected in a ridge-like shape, and narrow and wide portions are alternately connected and arranged in a plan view. Between the convex portions 934 connected in a ridge-like shape, there is a slightly low depression 935. Nonwoven fabric 90 has an uneven shape in its thickness direction, which includes protrusions, recesses, and walls 931W connecting the protrusions and recesses, formed by protrusions 931 and recesses 936. Furthermore, in the convex rib portion 931, the concave rib portion 936, and the wall portion 931W, the binder is present at the fiber entanglement points, and is attached so as to cover the fiber entanglement points. The nonwoven fabric 90 may have various configurations described in paragraphs
[0012] to
[0058] of JP 2019-44320 A. For example, the orientation direction of the fibers constituting the vertical ridge portion 911 and the fibers constituting the horizontal ridge portion 921 may be different. The height of the vertical ridge portion 911 and the height of the horizontal ridge portion 912 may be different, and the horizontal ridge portion 921 may be curved in the thickness direction of the nonwoven fabric 90 or may have an equal height. In addition, each of the two lines constituting the widthwise outline of the convex strip portion 931 when viewed in plan from the second surface 1B side may be a curve having multiple arcs. Fuzz may be arranged on the side of the convex strip portion 931. This nonwoven fabric 90 typically has the shapes shown in FIGS. Such a nonwoven fabric 90 can be produced by the method described in paragraphs
[0059] to
[0065] of JP 2019-44320 A.
[0070] Such a nonwoven fabric of the present invention can be used for various purposes. For example, the nonwoven fabric of the present invention can be used in absorbent articles such as diapers, sanitary napkins, panty liners, and urine pads. Absorbent articles typically have a liquid-permeable top sheet, a back sheet, and an absorbent sandwiched between them. The nonwoven fabric of the present invention can be particularly suitably used as a top sheet. Furthermore, the nonwoven fabric can also be used as a sheet in the gather part, an exterior sheet, or a sheet in the wing part of an absorbent article. The nonwoven fabric of the present invention can also be used as a component of an eye mask or a mask.
[0071] In relation to the above-mentioned embodiments, the present invention further discloses the following nonwoven fabric and absorbent article.
[0072] <1> A nonwoven fabric containing thermoplastic fibers and having fusion points between the fibers, The apparent thickness of the nonwoven fabric under a load of 50 Pa is 4 mm or more, The apparent thickness of the nonwoven fabric when pressed at 2.5 kPa is half or less of the apparent thickness of the nonwoven fabric when pressed at 50 Pa, A nonwoven fabric, the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of a nonwoven fabric after releasing from compression) satisfy either or both of the following requirements (1) and (2). (1) The recovery rate of the apparent thickness of the nonwoven fabric after release from compression is 40% or more. (2) The apparent thickness of the nonwoven fabric after release from compression is 2 mm or more and 8 mm or less. (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample, and the apparent thickness is measured. (b) Next, the nonwoven fabric sample is compressed to 0.7 mm with a load of 20 kPa. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100
[0073] <2> A nonwoven fabric containing thermoplastic fibers and having fusion points between the fibers, The apparent thickness of the nonwoven fabric under a load of 50 Pa is 4 mm or more, The apparent thickness of the nonwoven fabric when pressed at 2.5 kPa is half or less of the apparent thickness of the nonwoven fabric when pressed at 50 Pa, A nonwoven fabric, the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of a nonwoven fabric after release from compression) satisfy the following requirement (1). (1) The recovery rate of the apparent thickness of the nonwoven fabric after release from compression is 40% or more. (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample, and the apparent thickness is measured. (b) Next, the nonwoven fabric sample is compressed to 0.7 mm with a load of 20 kPa. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100
[0074] <3> A nonwoven fabric containing thermoplastic fibers and having fusion points between the fibers, The apparent thickness of the nonwoven fabric under a load of 50 Pa is 4 mm or more, The apparent thickness of the nonwoven fabric when pressed at 2.5 kPa is half or less of the apparent thickness of the nonwoven fabric when pressed at 50 Pa, A nonwoven fabric, the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of a nonwoven fabric after release from compression) satisfy the following requirement (2). (2) The apparent thickness of the nonwoven fabric after release from compression is 2 mm or more and 8 mm or less. (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample, and the apparent thickness is measured. (b) Next, the nonwoven fabric sample is compressed to 0.7 mm with a load of 20 kPa. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100 <4> A nonwoven fabric containing thermoplastic fibers and having fusion points between the fibers, The apparent thickness of the nonwoven fabric under a load of 50 Pa is 4 mm or more and 9 mm or less, The apparent thickness of the nonwoven fabric when pressed at 2.5 kPa is half or less of the apparent thickness of the nonwoven fabric when pressed at 50 Pa, A nonwoven fabric, the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of a nonwoven fabric after releasing from compression) satisfy both of the following requirements (1) and (2). (1) The recovery rate of the apparent thickness of the nonwoven fabric after release from compression is 40% or more and 80% or less. (2) The apparent thickness of the nonwoven fabric after release from compression is 2 mm or more and 8 mm or less. (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing compression) (a) For the "apparent thickness of nonwoven fabric before compression," a load of 50 Pa is applied to the nonwoven fabric sample, and the apparent thickness is measured. (b) Next, the nonwoven fabric sample is compressed to 0.7 mm with a load of 20 kPa. This compressed state is maintained in an atmosphere of 50°C for 24 hours, and then released from the compressed state and left in an atmosphere of 25°C for 30 minutes. (c) After that, a laser thickness gauge is used to measure the thickness at a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, calculate the recovery rate of the nonwoven fabric apparent thickness using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" x 100
[0075] <5> The apparent thickness of the nonwoven fabric under a load of 50 Pa is 5 mm or more, preferably 6 mm or more, and more preferably 7 mm or more. <1> ~ <4> 13. The nonwoven fabric according to any one of claims 1 to 12. <6> The apparent thickness of the nonwoven fabric under a load of 50 Pa is 9 mm or less, and preferably 8.5 mm or less. <1> ~ <5> 13. The nonwoven fabric according to any one of claims 1 to 12. <7> The recovery rate of the apparent thickness of the nonwoven fabric after the compression and release is 45% or more, and preferably 50% or more. <1> ~ <6> 13. The nonwoven fabric according to any one of claims 1 to 12. <8> The recovery rate of the apparent thickness of the nonwoven fabric after the compression and release is 80% or less, preferably 70% or less, and more preferably 60% or less. <1> ~ <7> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0076] <9> The deformation stroke of the nonwoven fabric after the compression and release is 1 mm or more and 6 mm or less. <1> ~ <8> 13. The nonwoven fabric according to any one of claims 1 to 12. <10> The deformation stroke of the nonwoven fabric after compression and release is 1.5 mm or more, and preferably 2 mm or more. <1> ~ <9> 13. The nonwoven fabric according to any one of claims 1 to 12. <11> The deformation stroke of the nonwoven fabric after compression and release is 5.5 mm or less, and preferably 5 mm or less. <1> ~ <10> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0077] <12> The thermoplastic fiber is <1> ~ <11> 13. The nonwoven fabric according to any one of claims 1 to 12. <13> The composite fiber is a core-sheath type composite fiber containing two or more different resin components, and the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fiber. <1> ~ <12> 13. The nonwoven fabric according to any one of claims 1 to 12. <14> The endothermic peaks of the two or more different resin components are separated by 5° C. or more. <13> The nonwoven fabric described in <15> The elongation of the composite fiber is 100% or less, preferably 90% or less, and more preferably 85% or less. <1> ~ <14> 13. The nonwoven fabric according to any one of claims 1 to 12. <16> The elongation of the composite fiber is 40% or more, preferably 50% or more, and more preferably 60% or more. <1> ~ <15> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0078] <17> The above-mentioned fiber has a fusion point at the center of the thickness. <1> ~ <16> 13. The nonwoven fabric according to any one of claims 1 to 12. <18> The number of fusion points per unit area at the center of thickness is 100 / mm 2 More than 300 pieces / mm 2 The above <17> The nonwoven fabric described in <19> The embossing ratio is 15% or less and has an uneven shape, and the embossing ratio is preferably 10% or less, more preferably 5% or less, and more preferably 0% or more. <1> ~ <18> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0079] <20> The degree of longitudinal orientation of the fibers is 55% or more, preferably 60% or more, and more preferably 65% or more. <1> ~ <19> 13. The nonwoven fabric according to any one of claims 1 to 12. <21> The degree of longitudinal orientation of the fibers is 95% or less, preferably 90% or less, and more preferably 80% or less. <1> ~ <20> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0080] <22> The binder is present at the fiber intersections in the center of the thickness. <1> ~ <21> 13. The nonwoven fabric according to any one of claims 1 to 12. <23> The fiber intersections where the binder is present are the fusion points between the fibers. <22> Written on non-woven fabric. <24> The mass of the binder is 1% or more and 15% or less of the mass of the nonwoven fabric. <23> The nonwoven fabric described in
[0081] <25> The nonwoven fabric has an uneven shape having a protrusion, a recess, and a wall portion connecting the protrusion and the recess in the thickness direction of the nonwoven fabric. <1> ~ <24> 13. The nonwoven fabric according to any one of claims 1 to 12. <26> The uneven shape has one structure selected from the group consisting of a solid protrusion, a hollow protrusion, a single-layer fiber layer, a two-layer fiber layer, protrusions arranged in a scattered manner in a planar direction, and protrusions and recesses arranged in a ridge-groove pattern, or a combination of multiple structures. <25> The nonwoven fabric described in <27> The above-mentioned having uneven shapes on both sides <1> ~ <26> 13. The nonwoven fabric according to any one of claims 1 to 12. <28> A nonwoven fabric having one surface and an opposite surface opposite to the one surface, The sheet has outer fiber layers on the one surface side and the opposite surface side, and a plurality of connecting portions disposed between the outer fiber layer on the one surface side and the outer fiber layer on the opposite surface side, The outer fiber layer on one side and the outer fiber layer on the opposite side are partially fused to each other at the connecting portion. <1> ~ <27> 13. The nonwoven fabric according to any one of claims 1 to 12. <29> A nonwoven fabric having one surface and an opposite surface opposite to the one surface, On the one surface side, A plurality of vertical ridge portions protruding toward the one surface side in the thickness direction of the nonwoven fabric extend in one direction on the one surface side in a plan view, and are arranged side by side at a distance from each other in another direction on the one surface side in a plan view different from the one direction on the one surface side, A horizontal ridge portion extending in another direction on the one surface side is arranged to connect the vertical ridge portions. <1> ~ <28> 13. The nonwoven fabric according to any one of claims 1 to 12. <30> The vertical ridges and horizontal ridges on one surface have convex portions and concave portions between the convex portions, and the concave portions are arranged in a ridge-groove shape. <29> The nonwoven fabric described in <31> The present invention has a convex ridge portion extending in one direction, the convex ridge portion being formed by connecting a plurality of convex portions in a ridge shape, and having a shape in which narrow portions and wide portions are alternately connected in a plan view. <1> ~ <30> 13. The nonwoven fabric according to any one of claims 1 to 12.
[0082] <32> The above <1> ~ <31> 13. An absorbent article comprising the nonwoven fabric according to any one of claims 1 to 12. <33> The absorbent article has a top sheet disposed on the skin contact side, a back sheet disposed on the non-skin contact side, and an absorbent body sandwiched between the top sheet and the back sheet, The above <1> ~ <31> 13. An absorbent article having the nonwoven fabric according to claim 1 as a top sheet. EXAMPLES
[0083] The present invention will be described in more detail below based on examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are all based on mass unless otherwise specified. In Table 1 below, "-" means that the item does not have a corresponding value, etc.
[0084] The "apparent thickness of nonwoven fabric under a load of 50 Pa" and the "apparent thickness of nonwoven fabric when compressed at 2.5 kPa" in Table 1 were measured in accordance with the above-mentioned (Method for measuring apparent thickness of nonwoven fabric under a load of 50 Pa). The "apparent thickness of nonwoven fabric after release from compression", "recovery rate of apparent thickness of nonwoven fabric after release from compression" and "deformation stroke of nonwoven fabric after release from compression" in Table 1 were measured based on the above-mentioned (Method for measuring apparent thickness and thickness recovery rate of nonwoven fabric after release from compression) and (Method for measuring deformation stroke of nonwoven fabric after release from compression). In addition, the "core-sheath mass ratio" in Table 1 was measured based on the above-mentioned (method of measuring the mass ratio of the core component and sheath component to the mass of a core-sheath composite fiber), and the "elongation" was measured in accordance with JIS L1015 7.7.1. Furthermore, in Table 1, "presence or absence of fusion points between fibers in the thickness center," "embossing rate," "lengthwise orientation of fibers," and "presence or absence of binder at fiber intersections in the thickness center" were measured based on the above-mentioned (method for confirming the presence or absence of fusion points between fibers in the thickness center of a nonwoven fabric), (method for measuring the embossing rate), (method for measuring the lengthwise orientation of fibers), and (method for confirming the presence or absence of binder at fiber intersections in the thickness center of a nonwoven fabric).
[0085] Example 1 (1) Preparation of raw nonwoven fabric A raw nonwoven fabric having the uneven shape shown in Figures 6 to 11 was produced by the air-through method using core-sheath type thermoplastic composite fibers having the fiber diameters shown in Table 1. The size of the raw nonwoven fabric was 100 mm x 100 mm. Specifically, it was produced based on the manufacturing method described in paragraphs
[0059] to
[0065] of Patent Document 4. The first hot air blowing treatment was performed under conditions of a temperature of 160°C, a wind speed of 54 m / sec, and a blowing time of 6 seconds. The second hot air blowing treatment was performed under conditions of a temperature of 160°C, a wind speed of 6 m / sec, and a blowing time of 6 seconds. (2) Preparation of binder coating solution A binder solution with a solid content of about 50% was mixed with deionized water to make a total of 90% by mass to prepare a binder coating solution. A commercially available acrylic emulsion with high elasticity was used as the binder. (3) Spraying the binder coating liquid Next, the binder coating liquid was evenly applied by spraying to the second surface (opposite surface) 1B of the raw nonwoven fabric on which the convex streak portion 931 and the concave streak portion 936 were arranged. The amount of the binder coating liquid applied was 3.5 g / m 2 This was measured by the change in mass of the nonwoven fabric before and after the binder was applied. This produced nonwoven fabric sample A1 of Example 1 having the basis weight shown in Table 1. The binder was attached to the center of the nonwoven fabric in the thickness direction, and was present in large amounts at the fiber intersections in particular. This nonwoven fabric sample A1 satisfies the above-mentioned requirements (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), (h. a layer having fibers with longitudinal orientation), and (i. a layer in which a binder is present at fiber intersections).
[0086] Example 2 Nonwoven fabric sample A2 of Example 2 was produced in the same manner as in Example 1, except that the basis weight was as shown in Table 1. The binder was adhered to the center of the nonwoven fabric in the thickness direction, and was present in a particularly large amount at the fiber intersections. This nonwoven fabric sample A2 satisfies the above-mentioned requirements of (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), (h. a layer having fibers with longitudinal orientation), and (i. a layer in which a binder is present at fiber intersections).
[0087] Example 3 Nonwoven fabric sample A3 of Example 3 was produced in the same manner as in Example 1, except that the fiber diameter and basis weight were as shown in Table 1. This nonwoven fabric sample A3 satisfies the above-mentioned requirements of (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), (h. a layer having fibers with longitudinal orientation), and (i. a layer in which a binder is present at fiber intersections).
[0088] Example 4 Nonwoven fabric sample A4 of Example 4 was prepared in the same manner as in Example 1, except that in the preparation method described in paragraphs
[0059] to
[0065] of Patent Document 4, the height of the protrusions of the support was changed to 6.0 mm, thereby making the apparent thickness and basis weight of the nonwoven fabric under a load of 50 Pa as shown in Table 1, and the bulk was made lower than that of Example 1. This nonwoven fabric sample A4 satisfies the above-mentioned requirements of (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), (h. a layer having fibers with longitudinal orientation), and (i. a layer in which a binder is present at fiber intersections).
[0089] Example 5 Nonwoven fabric sample A5 of Example 5 was produced in the same manner as in Example 4, except that the core-sheath ratio and basis weight of the thermoplastic conjugate fiber were set as shown in Table 1. As shown in Table 1, the elongation of the thermoplastic conjugate fiber was lower than that of Example 1 due to the core-sheath ratio. This nonwoven fabric sample A5 satisfies the above-mentioned requirements (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), and (h. a layer having longitudinal fiber orientation).
[0090] Example 6 Nonwoven fabric sample A6 of Example 6 was produced in the same manner as in Example 4, except that the core-sheath ratio, elongation, basis weight, and fiber diameter of the thermoplastic conjugate fiber were as shown in Table 1, and elastic elastomer fiber was used instead of the thermoplastic conjugate fiber. This nonwoven fabric sample A6 satisfies the above-mentioned requirements of (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (d. a layer of elastomeric fibers), and (h. a layer having longitudinal fiber orientation).
[0091] Example 7 Nonwoven fabric sample A7 of Example 7 was produced in the same manner as in Example 4, except that the constituent components of the composite fibers were as shown in Table 1, the fiber intersections in the thickness center were not fused (no fused intersections), and the basis weight was as shown in Table 1. Specifically, it was prepared by the method described in paragraphs
[0059] to
[0065] of Patent Document 4. The fiber web used to manufacture the nonwoven fabric was prepared in the following manner. That is, a core-sheath type (PET (core): PE (sheath) = 5:5 (mass ratio)) thermoplastic fiber with a fineness of 3.5 dtex was used to make a fiber web with a basis weight of 10 g / m2. 2 Next, two sheets of fiber web A were prepared using single fiber (PET: 100%) with a fineness of 3.5 dtex and a basis weight of 10 g / m 2 The fiber web B was sandwiched between the fiber webs A from above and below to be used as the fiber web. This nonwoven fabric sample A7 satisfies the above-mentioned requirements (e. layer of low elongation fiber) and (f. unfused fiber layer).
[0092] Example 8 A nonwoven fabric sample A8 of Example 8 was produced in the same manner as in Example 1, except that the raw nonwoven fabric was produced by the manufacturing method described in paragraphs
[0049] to
[0057] of JP 2019-44319 A and the support shown in Figure 12 was used. The nonwoven fabric sample A8 had the uneven shape shown in Figure 5. In the above manufacturing method, the support male member 120 shown in FIG. 12 was a rectangular column shape with a height of 8 mm for the protrusion 121, and a square shape of 2 mm x 2 mm when viewed from above. The pitch of the rectangular column was 5 mm in both the MD and CD directions. The support female member 130 shown in FIG. 12 was a metal member having a lattice-shaped protrusion 131 corresponding to the recess 122 of the support male member 120, and was pressed between the protrusions 121 of the support male member 120. The adjacent protrusions 121, 121 of the support female member 130 were arranged at a pitch of 5 mm, and the space into which the fibers were inserted when the support male member 120 and the support female member 130 were pressed was 0.5 mm on one side, and 1 mm on both sides of the protrusion 120 of the support male member 120. The hot air blowing treatment was performed under conditions of a temperature of 160°C, a wind speed of 6 m / sec, and a blowing time of 6 seconds. This nonwoven fabric sample A8 satisfies the above-mentioned requirements of (c. a layer of fibers that are core-sheath type composite fibers, in which the core ratio is greater than the sheath ratio in terms of the core-sheath mass ratio of the composite fibers), (e. a layer of low-elongation fibers), (h. a layer having fibers with longitudinal orientation), and (i. a layer in which a binder is present at fiber intersections).
[0093] Comparative Example 1 A nonwoven fabric with an uneven shape as described in Example 1 of Patent Document 3 was produced by the air-through method using core-sheath type thermoplastic conjugate fibers having the fiber diameters shown in Table 1. The basis weight was as shown in Table 1. The nonwoven fabric was used as it was, without being coated with a binder coating liquid, as nonwoven fabric sample C1 of Comparative Example 1. This nonwoven fabric sample C1 satisfies the above-mentioned requirements (c. a layer of fibers that are sheath-core composite fibers, in which the core ratio is greater than the sheath ratio by mass) and (e. a layer of low-elongation fibers).
[0094] Comparative Example 2 A flat nonwoven fabric without irregularities was produced by the air-through method using core-sheath type thermoplastic composite fibers having the fiber diameters shown in Table 1. The basis weight was as shown in Table 1. The nonwoven fabric was used as nonwoven fabric sample C2 of Comparative Example 2 without being coated with a binder coating liquid. This nonwoven fabric sample C2 satisfies the above-mentioned requirements (c. a layer of fibers that are sheath-core composite fibers, in which the core ratio is greater than the sheath ratio by mass) and (e. a layer of low-elongation fibers).
[0095] Comparative Example 3 The resin-bonded nonwoven fabric described in Example 1 of Patent Document 1 was produced using fibers (PET) having the fiber diameters shown in Table 1. The resin-bonded coating solution used in Example 1 was spray-coated to produce the nonwoven fabric. The coating amount was 16.6 g / m 2 This resin-bonded nonwoven fabric was designated as nonwoven fabric sample C3 of Comparative Example 3. The nonwoven fabric sample C3 had no irregularities and was flat. In addition, this nonwoven fabric sample C3 satisfies the above-mentioned requirements of (e. layer of low elongation fiber), (f. unfused fiber layer), and (i. layer having binder at fiber intersections).
[0096] Comparative Example 4 The nonwoven fabric located on the back of the surface material was removed from a medium-sized tape diaper of Pampers Ultra Thin Dry Fresh (obtained in May 2018) manufactured by The Procter & Gamble Company that was sold in China, and the nonwoven fabric sample was placed in a beaker containing 100 mL of ethyl acetate and stirred for 30 minutes, after which the nonwoven fabric sample was removed and dried. The nonwoven fabric thus obtained was designated as nonwoven fabric sample C4 of Comparative Example 4. The nonwoven fabric sample C4 had no irregularities and was flat. In addition, this nonwoven fabric sample C4 satisfies the above-mentioned requirements of (e. layer of low elongation fiber), (f. unfused fiber layer), and (i. layer having binder at fiber intersections).
[0097] Comparative Example 5 Nonwoven fabric sample C5 of Comparative Example 5 was produced based on Example 1 described in JP 2012-136803 A. This nonwoven fabric sample C5 satisfies the above-mentioned requirements (c. a layer of fibers that are sheath-core composite fibers, in which the core ratio is greater than the sheath ratio by mass) and (e. a layer of low-elongation fibers).
[0098] The following measurements and tests were carried out for the above examples and comparative examples. (1) Measurement of items 6 to 11 and 13 to 15 in Table 1 below Each nonwoven fabric sample was measured based on the above-mentioned respective measuring methods corresponding to each item. (2) Measurement of item 12 in Table 1 below The above-mentioned method (method for confirming the presence or absence of binder at fiber intersections in the center of the thickness of the nonwoven fabric) was applied mutatis mutandis to measure the presence or absence of dyed fiber intersections in the observation images of each of the front and back sides (first side and second side) of the nonwoven fabric. (3) Test for item 16 in Table 1 below (feel: MMD (mean coefficient of friction variation) test) The variation in the average coefficient of friction (MMD) of the nonwoven fabric surface was measured using an automatic surface tester (KESFB4-A-SE: manufactured by Kato Tech Co., Ltd.). A test piece measuring 20 cm x 20 cm was prepared and attached to a test table with a smooth metal surface. The contact surface of the contactor was pressed against the test piece with a force of 49 cN, and the test piece was moved horizontally 2 cm at a constant speed of 0.1 cm / sec. A uniaxial tension of 19.6 cN / cm was applied to the test piece. The contactor was made of 20 piano wires with a diameter of 0.5 mm arranged and bent into a U-shape with a width of 10 mm, and the contact surface was pressed against the test piece with a force of 49 cN using a weight. The measured value of the average deviation of the coefficient of friction is expressed as the MMD value. This measurement was performed in both MD and CD, and the average value was calculated using the following formula (S2), which was used as the average deviation of the coefficient of friction. Friction coefficient mean deviation = {(MMD MD 2 +MMDCD 2 ) / 2} 1 / 2 (S2) The average deviation of the friction coefficient indicates the degree of variation in friction, with a smaller value indicating a smoother feel when touched by hand.
[0099] [Table 1]
[0100] As shown in Table 1, the nonwoven fabric samples A1 to A8 of Examples 1 to 8 had an apparent thickness of 4 mm or more under a load of 50 Pa, which was thicker than the nonwoven fabric samples C2 to C5 of Comparative Examples 2 to 5, and either or both of the apparent thickness and recovery rate of the nonwoven fabric after compression and release were larger than those of the nonwoven fabric samples C1 to C5 of Comparative Examples 1 to 5, showing excellent thickness recovery. In addition, the compressibility from the apparent thickness under a load of 50 Pa to the apparent thickness when pressurized at 2.5 kPa was also sufficiently high. As a result, the nonwoven fabric samples A1 to A8 of Examples 1 to 8 could be felt to be sufficiently thick under a light load (load of 50 Pa) such that the skin touched the surface of the nonwoven fabric, and when a heavy load (load of 2.5 kPa) was applied to strongly press the nonwoven fabric, the thickness was sufficiently crushed, and soft deformability and cushioning could be felt. This changing tactile sensation was maintained even after compression and release. In other words, it was found that the nonwoven fabric of the present invention has high cushioning properties and a fluffy texture can be felt both before and after compression and release. Furthermore, the nonwoven fabric samples A1 to A8 of Examples 1 to 3 had sufficiently smaller MMD and better texture than the binder-containing nonwoven fabrics C3 to C5 of Comparative Examples 3 to 5. This is because the nonwoven fabric samples A1 to A8 of Examples 1 to 3 had a larger apparent thickness at a load of 50 Pa and a larger apparent thickness after compression and release than the nonwoven fabrics C3 to C5 of Comparative Examples 3 to 5. In addition, the nonwoven fabric samples A1 to A8 of Examples 1 to 3 suppressed the effects of the unevenness and adhesiveness of the binder itself due to the thickness characteristics, thereby realizing a high level of smoothness when touched by hand. In measuring MMD (variation of mean coefficient of friction), which indicates texture, the terminal that measures friction is subjected to the irregular adhesive force from the binder on the fiber surface, resulting in a large variation in the mean coefficient of friction. In addition, if the fibers are strongly bonded together by the binder and harden, when the terminal picks up the frictional force of the nonwoven fabric surface, it cannot flexibly deform, and the frictional force on the terminal fluctuates. These microscopic phenomena, such as hardening and stickiness of the fibers, create a large difference in texture. The difference in MMD values shown in Table 1, even if small numerically, means a significant difference in texture as felt on the delicate skin surface.
[0101] Any numerical limit or range set forth herein includes the recited end values of that numerical limit or range, and all values and subranges within that numerical limit or range are expressly included as if expressly stated. As used herein, the words "a," "an," and "the like" mean "one or more." Obviously, numerous modifications and variations of the present invention are possible in light of the above teachings. It is therefore to be understood that, within the scope of the appended claims, the invention may be practiced otherwise than as specifically described herein. All patents and other references cited above are incorporated herein by reference in their entirety as if fully set forth above. [Explanation of symbols]
[0102] 6 Fiber intersection 61 Dyed fiber intersections 7. Fiber 71 Sunspot 80, 90 Uneven nonwoven fabric 100S, 100W non-woven fabric 105 Nonwoven fabric thickness center C Reference circle L, L1, L2, L3, L4 reference line
Claims
1. A nonwoven fabric containing thermoplastic fibers and having fusion points between the fibers, The thermoplastic fiber is a core-sheath type composite fiber containing two or more different resin components, and the core ratio of the composite fiber is greater than the sheath ratio. A binder is present at the fusion points between the fibers in the thickness center portion, The apparent thickness of the nonwoven fabric under a load of 50 Pa is 4 mm or more, The apparent thickness of the nonwoven fabric when pressed at 2.5 kPa is half or less of the apparent thickness of the nonwoven fabric when pressed at 50 Pa, A nonwoven fabric, the values obtained by the following (method of measuring the apparent thickness and thickness recovery rate of a nonwoven fabric after releasing from compression) satisfy either or both of the following requirements (1) and (2). (1) The recovery rate of the apparent thickness of the nonwoven fabric after release from compression is 40% or more. (2) The apparent thickness of the nonwoven fabric after compression and release is 2 mm or more and 8 mm or less. (Method of measuring apparent thickness and thickness recovery rate of nonwoven fabric after releasing from compression) (a) "Nonwoven fabric apparent thickness before compression": a load of 50 Pa is applied to a nonwoven fabric sample to measure its apparent thickness. (b) Next, the nonwoven fabric of the measurement sample is compressed to 0.7 mm under a load of 20 kPa. This compressed state is maintained in an atmosphere at 50° C. for 24 hours, and then the compressed state is released and the sample is left in an atmosphere at 25° C. for 30 minutes. (c) Then, a laser thickness gauge is used to measure the thickness under a load of 50 Pa. Measurements are taken at three locations, and the average value is taken as the measurement data to obtain the "apparent thickness of the nonwoven fabric after release from compression." (d) Finally, the recovery rate of the nonwoven fabric apparent thickness is calculated using the following formula. "Recovery rate of apparent thickness of nonwoven fabric after release from compression [%]" = "apparent thickness of nonwoven fabric after compression and release" ÷ "apparent thickness of nonwoven fabric before compression" × 100
2. 2. The nonwoven fabric according to claim 1, wherein the deformation stroke of the nonwoven fabric after the compression and release is 1 mm or more and 6 mm or less.
3. 3. The nonwoven fabric according to claim 1 or 2, which is made of thermoplastic fibers.
4. The nonwoven fabric according to any one of claims 1 to 3, wherein the conjugated fibers have an elongation of 100% or less.
5. The nonwoven fabric according to any one of claims 1 to 4, wherein the degree of longitudinal orientation of the fibers is 55% or more.
6. The nonwoven fabric according to any one of claims 1 to 5, wherein the mass of the binder is 1% or more and 15% or less of the mass of the nonwoven fabric.
7. An absorbent article comprising the nonwoven fabric according to any one of claims 1 to 6.
Citation Information
Patent Citations
Absorptive article
JP2001187088A
Bulky composite sheet and manufacturing method
JP2005520704A
Nonwoven fabric and method for producing the same
JP2008255525A
Nonwoven fabric and absorbent article including the same
JP2012136791A
Bulky conjugate filament nonwoven fabric
JP2016041858A