Organometallic complex coating liquid and near-infrared absorbing film
A catalyst-free organometallic complex coating liquid with phosphorus-containing dispersants and optical resins addresses degradation issues, enabling efficient, cost-effective, and high-performance near-infrared blocking filters for electronic devices.
Patent Information
- Application Number
- JP2022178591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-19
- Filing Date
- 2022-11-08
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-08
AI Technical Summary
Existing near-infrared blocking filters using organometallic complex coating liquids face issues with degradation due to catalysts at high temperatures, leading to reduced visible light transmittance and inefficient production processes unsuitable for mass production.
A catalyst-free organometallic complex coating liquid comprising a phosphorus-containing dispersant and optical resin, such as thermoplastic or photocurable resins, is used to form a near-infrared absorbing film at lower temperatures and shorter times, maintaining optical performance.
The solution enhances production efficiency, reduces costs, and improves quality while achieving high visible light transmittance and low near-infrared transmittance, suitable for mass production and stringent environmental certifications.
Smart Images

Figure 0007573584000018 
Figure 0007573584000019 
Figure 0007573584000020
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an organometallic complex coating liquid, and in particular to a near-infrared absorbing film comprising the organometallic complex coating liquid. [Background technology]
[0002] With the trend of development that emphasizes the portability of electronic devices, the demands for lighter, thinner, shorter, and smaller components of electronic devices are becoming stricter. As an absorption type near infrared blocking filter, a glass substrate has a problem in the balance between thinning and infrared absorption, and therefore, as an absorption type near infrared blocking filter, a resin type absorption type near infrared blocking filter is developing vigorously. The resin type absorption type near infrared blocking filter is formed by mixing a dispersion of an organic metal complex with a resin component to form a coating liquid, which is then applied onto a substrate to form a near infrared absorbing film. By a specific blending, the optical performance of the near infrared absorbing film can be significantly improved, for example, it can strongly absorb near infrared rays with a wavelength between 800 nm and 1100 nm, and particularly absorb near infrared rays with a wavelength of 940 nm well, so that a near infrared blocking filter with excellent blocking effect can be obtained. Summary of the Invention [Problem to be solved by the invention]
[0003] In the process of applying an organometallic complex coating liquid to a substrate, it is known that a titanium catalyst is usually added and the coating is cured at 85°C and 140°C. However, the added catalyst may deteriorate the near-infrared absorbing film when baked at high temperatures, for example, the visible light transmittance decreases due to blushing. On the other hand, even if the curing reaction is performed at high temperatures, the required time is still several hours or more, and the production efficiency is poor, so it is not suitable for mass production and the cost is high. Therefore, it is desired to further improve the temperature and time of coating film formation without adding a catalyst while maintaining the excellent optical performance of the near-infrared absorbing film. [Means for solving the problem]
[0004] Regarding the problem to be solved, the present disclosure: Organometallic complexes, Phosphorus-containing dispersants, and optical resin The present invention provides an organometallic complex coating solution comprising:
[0005] The optical resin is a thermoplastic resin, a photocurable resin, or a mixture of both. The thermoplastic resin is at least one selected from polycarbonate, polyester, and polycycloolefin. Specifically, the polycarbonate is It has the structure TIFF0007573584000001.tif34169, The polyester is TIFF0007573584000002.tif has the structure 18168, The polycycloolefin is TIFF0007573584000003.tif has the structure 19168, where R is an alkylene or arylene group; The alkylene may be linear, branched, cyclic, or a combination thereof, and a and b are independently integers from 4 to 9, and n and m are each 20 to 30.
[0006] The photocurable resin is at least one selected from an acrylic resin, a siloxane resin, and an imide resin. In one embodiment, the siloxane resin is [R 1 SiO 3 / 2 ] x where R 1 teeth TIFF0007573584000004.tif14168, and x is an integer from 3 to 40.
[0007] The present disclosure also provides a near infrared ray absorbing film made of the organometallic complex coating liquid described in the present disclosure, i.e., the near infrared ray absorbing film comprises an organometallic complex, a phosphorus-containing dispersant, and an optical resin. Effect of the Invention
[0008] The organometallic complex coating solution of the present disclosure can be applied to a substrate and baked to form a film without the need for a separate catalyst, and the temperature and time of the film formation process are significantly reduced compared to the conventional technology. This has the beneficial effects of improving production volume, saving energy and reducing carbon, reducing costs, improving profits, and improving quality, and contributes to passing increasingly strict environmental certifications in related industries and expanding the market.
[0009] The near-infrared absorbing film made of the organometallic complex coating liquid has excellent optical performance, and even if it is thin, it has high transmittance in the visible light range and also has very low transmittance in the near-infrared range, and has an excellent near-infrared blocking effect. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a curve diagram of the transmittance of light of different wavelengths when the thermoplastic resin content is different in the near infrared absorbing film of Example 1 of the present disclosure.
[0011] [Diagram 2]FIG. 11 is a curve diagram of transmittance for light of different wavelengths when the film thickness is different in the near-infrared absorbing film (containing a photocurable resin) of Example 2 of the present disclosure.
[0012] [Diagram 3] FIG. 11 is a curve diagram of transmittance for light of different wavelengths when the content of the photocurable resin in the near infrared absorbing film of Example 2 of the present disclosure is different. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the implementation method of the present disclosure will be described by specific specific examples, and those skilled in the art of the present disclosure can easily understand the scope and effects of the present disclosure by the description of the present disclosure. However, the specific examples described in this specification do not limit the present disclosure, and each of the listed technical features or ideas can be combined with each other. In addition, the present disclosure can be realized or applied by other different implementation methods. Each detail described in this specification can be variously changed or modified according to different viewpoints and applications without departing from the present disclosure.
[0014] In this specification, when a particular feature is described as "comprising," "including," or "having," unless otherwise specified, the feature may include other elements, compositional components, structures, regions, parts, devices, systems, steps, or connections, and does not exclude other features.
[0015] As used herein, the singular forms "a" and "the" include the plural forms, unless stated otherwise, and the terms "or" and "and / or" are used interchangeably herein.
[0016] The numerical ranges described herein are inclusive and combinable, and any value within a numerical range described herein can be used to derive a subrange as a maximum or minimum value. For example, the numerical range "1.5 / 8.5 to 0.5 / 9.5" is understood to include all subranges between the endpoints 1.5 / 8.5 and 0.5 / 9.5, such as 1.4 / 8.6 to 0.5 / 9.5, 1.5 / 8.5 to 0.6 / 9.4, and 1.4 / 8.6 to 0.6 / 9.4. Also, a numerical value should be considered to be within the scope of the present disclosure if it is within each range described herein (e.g., between the maximum and minimum values).
[0017] A first aspect of the present disclosure is a method for producing a composition comprising: The present invention relates to an organometallic complex coating solution comprising:
[0018] The organometallic complex may be, for example, a copper compound and a phosphonic acid compound In one embodiment, the copper compound is a copper salt, such as an anhydride or hydrate of copper acetate, copper chloride, copper formate, copper stearate, copper benzoate, copper pyrophosphate, copper naphthenate, or copper citrate. In one embodiment, the copper compound is a phosphonic acid. compound The structure of can be represented by RPO(OH)2, where R is an alkyl group, a haloalkyl group, a phenyl group, a halophenyl group, a nitrophenyl group, a hydroxylphenyl group, an alkylphenyl group, a haloalkylphenyl group, a nitroalkylphenyl group, or a hydroxylalkylphenyl group. In another embodiment, the copper compound is copper acetate and the phosphonic acid compound is butylphosphonic acid. The above organometallic complex is a type of near infrared absorbing agent.
[0019] The phosphorus-containing dispersant may be at least one selected from phosphoric acid derivatives, phosphorous acid derivatives and hypophosphorous acid derivatives. In one embodiment, the phosphorus-containing dispersant has an alkyl group and / or a polyoxyalkyl group. In another specific embodiment, examples of the phosphorus-containing dispersant include Plysurf A208N (polyoxyethylene alkyl C12, C13 ether phosphate), Plysurf A208F (polyoxyethylene alkyl (C8, 2-ethylhexyl) ether phosphate), Plysurf A208B (polyoxyethylene lauryl ether phosphate), Plysurf A219B (polyoxyethylene lauryl ether phosphate), Plysurf AL (polyoxyethylene styrenated phenyl ether phosphate), Plysurf A212C (polyoxyethylene tridecyl ether phosphate), and Plysurf A215C (polyoxyethylene tridecyl ether phosphate), all of which are manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; NIKKOL DDP-2 (di C12-C15 linear alkanol polyether-2 phosphate), NIKKOL DDP-4 (di C12-C15 linear alkanol polyether-4 phosphate), and NIKKOL DDP-6 (di C12-C15 linear alkanol polyether-6 phosphate ester), and bis(2,4,4-trimethylpentyl)phosphinic acid. The phosphorus-containing dispersant is used to properly disperse the near-infrared absorbing agent and improve its near-infrared absorbing effect. Since the phosphorus-containing dispersant is added at the stage of synthesizing the organometallic complex and is involved in the reaction, in this disclosure, the phosphorus-containing dispersant and the organometallic complex are regarded as one organometallic complex, that is, the total content of the phosphorus-containing dispersant and the organometallic complex represents the total weight of the entire organometallic complex.
[0020] Specifically, the present disclosure forms an organometallic complex coating solution by mixing an organometallic complex dispersion, which includes the organometallic complex described above and a phosphorus-containing dispersant, with an optical resin.
[0021] In one embodiment, the dispersion of the organometallic complex further includes a solvent, which is selected from commonly known solvents, including, but not limited to, water, alcohols, ketones, ethers, esters, aromatic hydrocarbons, halogenated hydrocarbons, dimethylcarboxamide, dimethylacetamide, dimethylsulfoxide, sulfolane, etc. Specific examples of the alcohols include methanol, ethanol, propanol, etc. Examples of the esters include alkyl formates, alkyl acetates, alkyl propionates, alkyl butyrates, alkyl lactates, alkyl alkoxyacetates, alkyl 3-alkoxypropionates, alkyl 2-alkoxypropionates, alkyl 2-alkoxy-2-methylpropionates, alkyl pyruvates, alkyl acetylacetates, and alkyl 2-oxobutyrates. Examples of the ethers include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate. Examples of the ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, and 3-heptanone. Examples of the aromatic hydrocarbons include toluene and xylene.
[0022] The optical resin of the present disclosure, in one embodiment, is a thermoplastic resin, a photocurable resin, or a mixture of both.
[0023] In one embodiment, the thermoplastic resin is at least one selected from polycarbonate, polyester, and polycycloolefin.
[0024] The polycarbonate has a dicarboxylic acid structural unit and a diol structural unit. In one embodiment, the dicarboxylic acid structural unit may have a 9,9-diphenylfluorenyl group, and the benzene ring of the 9,9-diphenylfluorenyl may have a substituent, including but not limited to C1-C10 alkyl groups and halogens. The diol structural unit may have a bisphenol A group (2,2-di(4-hydroxyphenyl)propane), and the benzene ring of the bisphenol A group may have a substituent, including but not limited to C1-C4 alkyl groups, halogens and phenyl groups. In one embodiment, the polycarbonate has the following structure: TIFF0007573584000005.tif34168Here, a and b are each independently an integer from 4 to 9.
[0025] In one specific embodiment, the polyester has the following structure: TIFF0007573584000006.tif21168Here, R is an alkylene group having 4 to 8 carbon atoms or an arylene group having 6 to 30 carbon atoms, and the alkylene may be linear, branched, cyclic, or a combination thereof. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a butylene group, and a cyclopropylene group, and examples of the arylene group include a phenylene group, a phenylenevinylene group, a naphthylene group, a biphenylene group, a bisphenylene A group, and a 9,9-diphenylfluorylene group. In the structure, n is an integer of 20 to 30.
[0026] The polycycloolefin includes a cycloolefin-derived structure (e.g., tetracyclododecene), and may further include an olefin-derived structure (e.g., ethylene, propylene, butene, etc.). In one embodiment, the polycycloolefin has the following structure: TIFF0007573584000007.tif22168Here, n and m are integers from 20 to 30.
[0027] In one specific embodiment, the photocurable resin of the present disclosure is at least one selected from acrylic (acrylic resin), siloxane resin, and imide resin. The monomer of the acrylic resin is, for example, methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, ethylene glycol dimethacrylate, ethyl acrylate, ethyl methacrylate, bisphenol A dimethacrylate, bisphenol A-glycidyl dimethacrylate, and bisphenol A-ethoxylated glycidyl dimethacrylate, and may contain one type of monomer or multiple types of monomers. In one specific embodiment, the siloxane resin is a siloxane containing an acrylic acid ester group or a methacrylic acid ester group, and specifically has the following structure: [R 1 SiO 3 / 2 ] x , Here, R 1 teeth TIFF0007573584000008.tif15168, and x is an integer of 3 to 40. In still another embodiment, the siloxane resin has a half cage structure. TIFF0007573584000009.tif36168 where R is TIFF0007573584000010.tif12168. In one embodiment, the imide resin is, for example, low-temperature photosensitive polyimide photoresist of model number ETERFLEX(TM) EPD-3500 from ETERNAL CHEMICLA CO., LTD.
[0028] When a photocurable resin is used, a photocuring agent may be further added to the organometallic complex coating liquid in order to facilitate photocuring film formation.
[0029] The optical resin used may be in powder, particle or liquid form, for example, a thermoplastic resin in particle form can be added to the dispersion of the organometallic complex, and for example, a photocurable resin in liquid form can be mixed with the dispersion of the organometallic complex.
[0030] In one embodiment, the weight ratio of the total organometallic complex (i.e., the total content of both the organometallic complex and the phosphorus-containing dispersant) to the thermoplastic resin is 0.5 / 9.5 to 7.5 / 2.5, 0.5 / 9.5 to 6.0 / 4.0, or 0.5 / 9.5 to 5.0 / 5.0, for example, the weight ratio of the total organometallic complex to the thermoplastic resin is 0.5 / 9.5, 1.0 / 9.0, 1.5 / 8.5, 2.0 / 8.0, 2.5 / 7.5, 3.0 / 7.0, 3.5 / 6.5, 4.0 / 6.0, 4.5 / 5.5, 5.0 / 5.0, 5.5 / 4.5, 6.0 / 4.0, 6.5 / 3.5, 7.0 / 3.0, or 7.5 / 2.5.
[0031] In one specific embodiment, the weight ratio of the whole organometallic complex (the total content of both the organometallic complex and the phosphorus-containing dispersant) to the photocurable resin is 1.0 / 9.0 to 6.5 / 3.5, 1.0 / 9.0 to 6.0 / 4.0, or 1.0 / 9.0 to 5.0 / 5.0, for example, the weight ratio of the whole organometallic complex to the photocurable resin is 1.0 / 9.0, 1.5 / 8.5, 2.0 / 8.0, 2.5 / 7.5, 3.0 / 7.0, 3.5 / 6.5, 4.0 / 6.0, 4.5 / 5.5, 5.0 / 5.0, 5.5 / 4.5, 6.0 / 4.0, or 6.5 / 3.5. In the present disclosure, the organometallic complex can effectively exert the infrared absorbing effect with a smaller amount of use.
[0032] A second aspect of the present disclosure provides a near infrared absorbing film comprising an organometallic complex, a phosphorus-containing dispersant, and an optical resin.
[0033] The near-infrared absorbing film is formed from the organometallic complex coating liquid of the first embodiment. For example, the near-infrared absorbing film is formed by applying the organometallic complex coating liquid onto a substrate and then heating and baking to remove the solvent.
[0034] Generally, when the thickness of the near-infrared absorbing film increases, the near-infrared blocking ability also increases, but this does not meet the requirement for thinning. On the other hand, when the thickness of the near-infrared absorbing film is reduced, the near-infrared blocking ability also decreases. The near-infrared absorbing film of the present disclosure can achieve excellent near-infrared blocking ability and has excellent optical performance even when the thickness is relatively small. When the thickness is relatively small, it means that the thickness is between 10 μm and 100 μm, or between 20 μm and 90 μm, or between 50 μm and 100 μm, and for example, the thickness can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, or 100 μm. Both the thickness and the components affect the optical performance of the film, and an increase or decrease in the thickness may require the mixing ratio of the components to be adjusted accordingly; for example, a thinner thickness may require an increased content of the organometallic complex as the near-infrared absorbing agent, and this can be adjusted according to the application conditions.
[0035] The near infrared absorbing film of the present disclosure has an average transmittance of 60% to 90% for light in the wavelength range of 400 nm to 700 nm, and may preferably have an average transmittance of 70% to 90%, or 75% to 90%, for example, 60%, 65%, 70%, 75%, 80%, 85%, or 90%. On the other hand, the near infrared absorbing film also has an average transmittance of 40% or less for light in the wavelength range of 800 nm to 1100 nm, and may preferably have an average transmittance of 35% or less, or 30% or less, for example, 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, 2.5%, or 2% or less.
[0036] The near-infrared absorbing film of the present disclosure has a half-transmission wavelength close to the near-infrared region, so that the average transmittance in the visible light region is maintained at a high level. The above half-transmission wavelength indicates the incident light wavelength when the transmittance of the incident light through the near-infrared absorbing film is 50%. When having multiple half-transmission wavelengths, the half-transmission wavelength of the present disclosure indicates a half-transmission wavelength particularly close to the near-infrared region, and more specifically, indicates a half-transmission wavelength between the visible light region and the near-infrared region. Specifically, the half-transmission wavelength can be 700nm or more, or 710nm, 720nm or more, for example, the half-transmission wavelength can be 700nm, 705nm, 710nm, 715nm, 720nm, 725nm, 730nm.
[0037] On the other hand, the near-infrared absorbing film of the present disclosure can also exhibit an extremely excellent blocking ability against the currently widely used 940 nm wavelength light source for biometric authentication. Specifically, the near-infrared absorbing film has a transmittance of 40% or less against light of 940 nm wavelength, more preferably a transmittance of 35% or less, 30% or less, and may have a transmittance of, for example, 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, 2.5%, 2% or less.
[0038] Hereinafter, the present disclosure will be described in detail with reference to the following examples, but the scope of the present disclosure is not limited to these examples.
[0039] Example 1
[0040] First, copper acetate and ethanol were mixed in a ratio of 1g / 100g, and then stirred at room temperature for 1.5 hours to form a first mixed liquid. Separately, 0.5g of Plysurf A208F (Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene-2-ethylhexyl ether phosphate ester), 0.25g of Plysurf A212C (Daiichi Kogyo Seiyaku Co., Ltd., polyoxyethylene tridecyl ether phosphate ester), 0.2g of NIKKOL DDP-6 (Nikko Kagaku Co., Ltd., dipolyoxyethylene (C12-C15) alkyl ether phosphate ester), and 0.2g of bis(2,4,4-trimethylpentyl)phosphinic acid were mixed with 10g of ethanol to form a second mixed liquid. The first mixed liquid and the second mixed liquid were mixed and stirred at room temperature for 1 hour, and 0.6g of butylphosphonic acid was added and stirred at room temperature for 3 hours, and then placed in an oven at 85°C for 12 hours to obtain the entire organometallic complex, which was then placed in toluene to form a dispersion. Next, thermoplastic resin polycarbonate (purchased from Mitsui Chemicals, APEL 401C) was used as the optical resin, and the optical resin and the dispersion were mixed in six ratios as shown in Table 1 to form an organometallic complex coating solution, which was then applied onto a transparent glass substrate and baked at a temperature of 70°C for 30 minutes. It was observed that all six organometallic complex coating solutions obtained from the thermoplastic resin and the dispersion were cured to form near-infrared absorbing films. In addition, the haze of the manufactured near-infrared absorbing films was measured, and the results are shown in Table 1 below.
[0041] [Table 1]
[0042] As is clear from the above table, the organometallic complex coating solution of the present disclosure can form a film under the severe conditions of low temperature and short time without adding a catalyst. However, the haze value is affected by the weight ratio of the organometallic complex and phosphorus-containing dispersant to the thermoplastic resin particles, so it can be adjusted as necessary when applied. In general, a haze value of 60% or less is acceptable. In the best case, the haze value can be lowered to increase the overall light transmittance.
[0043] FIG. 1 shows the transmittance curves of near-infrared absorbing films of the same thickness made of the organometallic complex coating liquids with weight ratios of the total organometallic complex (i.e., the total content of both the organometallic complex and the phosphorus-containing dispersant) to the thermoplastic resin polycarbonate APEL 401C of 7.5 / 2.5, 6.5 / 3.5, 5.0 / 5.0, and 2.5 / 7.5. The results of FIG. 1 show that the average transmittance of the near-infrared absorbing film with a weight ratio of 2.5 / 7.5 to light in the wavelength range of 800nm to 1100nm is about 32%, which can reach 40% or less, thereby satisfying the requirements for the product. When the total amount of the organometallic complex is increased, the average transmittance of the near-infrared absorbing film to light in the wavelength range of 800nm to 1100nm can be further reduced to 10% or less, 5% or less, and can even be about 3% or 2%, so that it is applicable to products with higher requirements for infrared filtration. The organometallic complex is used to absorb infrared rays, but when the amount of the complex increases, the transmittance of the visible light region is also affected, and in practical applications, the required transmittance can be controlled by adjusting the blending ratio of the composition components and the thickness of the film. In addition, although polycarbonate (purchased from Mitsui Chemicals, APEL 401C) is used as the thermoplastic resin here, other examples may use polyester (purchased from Teijin Chemicals, P-3810), polycycloolefin (purchased from ZEON, ZEONEX K22R), or a mixture of any two or three of the above three types of thermoplastic resins, without affecting the optical properties of the film.
[0044] Example 2
[0045] A dispersion was prepared in the same manner as in Example 1, and a photocurable resin: TIFF0007573584000012.tif36168 was added to the dispersion, and 0.2wt%~10wt% of the photocuring agent omnirad 1173 (purchased from IGM Resins company) was added to form an organometallic complex coating solution. It was then coated on a transparent glass substrate, baked at a temperature of 70℃ for 5 minutes, and irradiated with ultraviolet light for 60 seconds to observe the possibility of film formation.
[0046] [Table 2]
[0047] The results show that when a photocurable resin is used in the organometallic complex coating liquid of the present disclosure, the required film formation time is relatively short.
[0048] FIG. 3 shows the transmittance curves of near-infrared absorbing films of the same thickness made of an organometallic complex coating liquid having a weight ratio of the whole organometallic complex (i.e., the total weight of the contents of both the organometallic complex and the phosphorus-containing dispersant) to the photocurable resin of 6.5 / 3.5 and 5.0 / 5.0. The results of FIG. 3 show that the near-infrared absorbing film having a weight ratio of 5.0 / 5.0 has a fairly high average transmittance (reaching 85% or more) for light in the wavelength range of 400nm to 700nm. On the other hand, it has a fairly low average transmittance (reaching up to about 2%) for light in the wavelength range of 800nm to 1100nm. In the example with a weight ratio of 6.5 / 3.5, the average transmittance for light in the wavelength range of 800nm to 1100nm was further reduced, but the average transmittance for light in the wavelength range of 400nm to 700nm was also affected and reduced. In practical applications, the required transmittance can be controlled by adjusting the blending ratio of the composition components and the thickness of the film, as in Example 1.
[0049] In particular, the near-infrared absorbing film of the present disclosure has excellent optical performance even when it is thin. As shown in FIG. 2, the near-infrared absorbing film containing the whole organometallic complex and the photocurable resin (weight ratio is 5.0 / 5.0) has a very excellent near-infrared blocking ability when it is only 90 μm thick, and the average transmittance for light in the 400 nm to 700 nm wavelength range can reach 88% or more, and the average transmittance for light in the 800 nm to 1100 nm wavelength range can reach about 2%. When the thickness is further reduced to, for example, 50 μm, the near-infrared blocking ability tends to decrease, but the average transmittance for light in the 800 nm to 1100 nm wavelength range is 10% or less, so that it can be applied to a wide variety of products. In addition, even when the thickness is further reduced to, for example, 25 μm, the average transmittance for light in the 800 nm to 1100 nm wavelength range is 40% or less. Furthermore, when the thickness is small, the near-infrared absorbing effect can be further enhanced by adjusting the compounding ratio of the organometallic complex (as a whole) and the photocurable resin.
[0050] In the conventional organometallic complex coating liquid, the ratio of organometallic complex and dispersant in the coating liquid is usually high, generally 75wt% or 65wt%, in order to enhance near-infrared absorption. In contrast, the present disclosure has found that by improving the coating liquid, an optical resin with a specific composition is adopted, and the effect of effectively absorbing infrared rays can be achieved in a situation where the total amount of organometallic complex used is smaller. For example, in Example 1, the weight ratio of the total organometallic complex to the optical resin component (thermoplastic resin) is only 2.5 / 7.5, but the transmittance of light with a wavelength of 800nm to 1100nm can be reduced by 40% or less, so that infrared absorption is realized and application to products is possible. In addition, if the total amount of organometallic complex used is increased, for example, when the weight ratio is 5.0 / 5.0 or 7.5 / 2.5, the infrared absorption effect is further improved, and it is applicable to products with higher requirements for infrared filtering.
[0051] The optical resin used in the present disclosure only functions as a carrier in the coating liquid, and does not undergo cross-linking polymerization reaction with the organometallic complex (whole) when forming a film, so unlike conventional film-forming reactions, it can be used as an optical resin by mixing a thermoplastic resin and a photocurable resin without affecting film-forming properties. In addition, since no polymerization or cross-linking reaction is involved, there is no loss of the organometallic complex (whole), and therefore the content of the organometallic complex (whole) can be significantly reduced.
[0052] In addition, the optical resin film formation process disclosed in the present disclosure requires only 30 minutes at 70°C, and therefore has the advantages of energy saving and quick production compared to the conventional process requiring multiple baking steps at higher and different temperatures (e.g., baking at 80°C for 30 minutes and then baking at 140°C for 2 hours), making it very suitable for mass production. It is presumed that such excellent effects are due to the fact that lower temperatures and shorter times are sufficient, since the selected optical resin does not polymerize or crosslink with the organometallic complex (as a whole) and functions only as a carrier.
Claims
1. An organometallic complex coating solution comprising an organometallic complex, a phosphorus-containing dispersant and an optical resin, the organometallic complex comprises a copper compound and a phosphonic acid compound; the copper compound is copper acetate, copper formate, or copper stearate; The phosphonic acid compound is represented by RPO(OH) 2 (wherein R is an alkyl group); the optical resin comprises a thermoplastic resin and / or a photocurable resin; the thermoplastic resin is at least one selected from polycarbonate, polyester, and polycycloolefin; the photocurable resin is at least one selected from a siloxane-based resin and an imide-based resin, The polycarbonate is wherein a and b are independently an integer from 4 to 9, The polyester is (wherein R is an alkylene group having 4 to 8 carbon atoms or an arylene group having 6 to 30 carbon atoms, the alkylene group may be linear, branched, cyclic, or a combination thereof, and n is an integer of 20 to 30), The polycycloolefin is (wherein n and m are integers from 20 to 30), The siloxane-based resin is [R 1 SiO 3/2 ] x (In the formula, R 1 teeth, and x is an integer of 3 to 40.
2. The optical resin includes a thermoplastic resin and a photocurable resin. The organometallic complex coating liquid according to claim 1 .
3. The thermoplastic resin is a polyester, and R is at least one selected from the group consisting of methylene, ethylene, propylene, butylene, cyclopropylene, phenylene, phenylenevinylene, naphthylene, biphenylene, bisphenylene A, and 9,9-diphenylfluorene; The organometallic complex coating liquid according to claim 1 .
4. When the optical resin contains only the thermoplastic resin, the weight ratio of the organometallic complex and the phosphorus-containing dispersant to the thermoplastic resin is 0.5 / 9.5 to 7.5 / 2.5; The organometallic complex coating liquid according to claim 1 .
5. When the optical resin contains only the photocurable resin, the weight ratio of the organometallic complex and the phosphorus-containing dispersant to the photocurable resin is 1.0 / 9.0 to 6.5 / 3.5; The organometallic complex coating liquid according to claim 1 .
6. A coating liquid obtained by curing the organometallic complex coating liquid according to claim 1. Near infrared absorbing film.
7. The thickness is between 10 μm and 100 μm, and the average transmittance is 60% to 90% for light in the wavelength range of 400 nm to 700 nm, and the average transmittance is 40% or less for light in the wavelength range of 800 nm to 1100 nm. The near infrared absorbing film according to claim 6 .
8. The half-transmitted wavelength is 700 nm or more. The near infrared absorbing film according to claim 6 .
Citation Information
Patent Citations
Polypropylene resin composition and use thereof
JP1990049048A
Photosensitive resin composition
JP1993127383A
Phosphor material containing rare earth metal, light-emitting composition containing the same, method for producing the same and light-emitting element containing the phosphor material
JP2009046577A
Near-infrared ray absorber, method for producing the same and optical material
JP2011099038A
Near-infrared absorption filter and method for manufacturing the same
JP2011203467A