High-weather-resistance polymer cement waterproof coating and preparation method thereof
By adding rutile titanium dioxide to polyurethane cement waterproof coatings and optimizing the stirring process, the problem of insufficient weather resistance of polymer cement waterproof coatings is solved, significantly improving the weather resistance and waterproof performance of the coating, meeting the national standard requirements.
Patent Information
- Application Number
- CN202411072193.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-05
AI Technical Summary
Under the influence of sunlight exposure, alkaline-superior coatings on the coating itself, and temperature difference, their appearance, mechanical properties and waterproof properties have decreased, and their weather resistance are insufficient, especially the weather resistance of polyurethane cement waterproof coatings needs to be improved.
Add appropriate amount of rutile titanium dioxide as filler and ultraviolet shielding agent to the polyurethane cement waterproof coating formula. The particle size is small and fully filled in the coating through ultrasonic dispersion, improving the density of the pore structure, and optimizing the stirring parameters during the preparation process To improve the tensile properties and weather resistance of the coating.
It significantly improves the weather resistance of the coating, including ultraviolet light resistance, alkali resistance and high and low temperature resistance, and at the same time improves the tensile strength and waterproof performance of the coating, meeting the national standard requirements.
Smart Images

Figure BDA0004981178250000071 
Figure BDA0004981178250000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coatings, and in particular to a highly weather-resistant polymer cement waterproof coating and a preparation method thereof. Background Art
[0002] Polymer cement waterproof coating is a two-component water-based waterproof coating composed of liquid (polymer emulsion and additives) and powder (cement and inorganic filler). It not only has the flexibility brought by polymer emulsion, but also has the rigid strength given by cement. In addition, polymer cement waterproof coating has good adhesion and can be directly constructed on a variety of wet or dry substrates, and can adapt to the deformation of the base. This series of advantages makes it a relatively popular waterproof coating, widely used in waterproofing of industrial and civil projects such as balconies, building exterior walls, kitchens, and bathrooms. However, under the combined effects of factors such as sunlight exposure, alkali efflorescence of the coating itself, and temperature differences, the appearance, mechanical properties, and waterproof properties of the coating will decline, and it is prone to cracking during long-term use. The weather resistance of polymer cement waterproof coating needs to be improved.
[0003] As the main film-forming substance of polymer cement waterproof coating, the type of polymer emulsion has a very important influence on the performance of the prepared coating. There are many emulsions that can be used to prepare polymer cement waterproof coating, and the common types are acrylic emulsion, EVA emulsion, chloroprene emulsion and polyurethane emulsion. Among them, the coating made of polyurethane emulsion has good mechanical properties, wear resistance and low temperature resistance, but the weather resistance of polyurethane cement waterproof coating still needs to be improved. Summary of the invention
[0004] Based on previous research and existing problems, the present invention proposes a highly weather-resistant polymer cement waterproof coating and a preparation method after further research and analysis. On the basis of optimizing the formula of the polyurethane cement waterproof coating, by adding an appropriate amount of TiO2 as a filler, the coating has strong tensile properties and significantly improved UV aging resistance. The coating has better low-temperature flexibility, excellent waterproof performance, and better weather resistance.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a highly weather-resistant polymer cement waterproof coating, comprising a liquid material and a powder material, wherein the liquid material comprises, by weight, 90 to 95 parts of a polyurethane emulsion, 3 to 5 parts of a film-forming aid, 0.1 to 1 part of a defoaming agent, 0.05 to 0.15 parts of a coupling agent, 0.5 to 1.5 parts of titanium dioxide, and 0 to 5 parts of water; the powder material comprises, 60 to 65 parts of cement, 20 to 25 parts of quartz sand, 10 to 15 parts of calcium carbonate, and 0.5 to 1 part of a dispersant.
[0006] Preferably, the mass ratio of liquid material to powder material is 0.6-0.8, and the aggregate-ash ratio is 0.8-1.
[0007] Preferably, the titanium dioxide crystal form is rutile, and the particle size is 30 to 50 nm.
[0008] Preferably, the polymer emulsion is an aqueous polyurethane emulsion with a solid content of 30% to 40%.
[0009] Preferably, the cement is ordinary Portland cement PO 42.5.
[0010] Preferably, the quartz sand particle size is 200 mesh and the calcium carbonate particle size is 350 mesh.
[0011] Preferably, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate.
[0012] Preferably, the defoaming agent is polydimethylsiloxane.
[0013] Preferably, the coupling agent is 3-glycidyloxypropyltrimethoxysilane.
[0014] The present invention also proposes a method for preparing the above-mentioned high weather resistance polymer cement waterproof coating, and the specific method steps are as follows:
[0015] 1) Weigh the powder components according to the measured portion and mix them, keep the speed at 600r / min~800r / min, and stir for 5min~8min to make the powder mix evenly;
[0016] 2) adding the weighed film-forming aid, defoaming agent and coupling agent to the weighed aqueous polyurethane emulsion, rotating at a speed of 500 r / min to 600 r / min, stirring for 10 min to 15 min, and stirring evenly to obtain a liquid material;
[0017] 3) adding weighed titanium dioxide to weighed water, dispersing the mixture of titanium dioxide and water with an ultrasonic cleaner for 30 minutes, and then adding it to the stirred liquid material for stirring at a stirring speed of 800 r / min to 1000 r / min for 10 min to 20 min to obtain a mixed liquid material;
[0018] 4) Add the obtained powder to the mixed liquid while stirring at a speed of 600 r / min to 900 r / min and a stirring time of 5 min to 15 min to obtain the product.
[0019] Compared with the existing technology, the present invention provides a highly weather-resistant polymer cement waterproof coating and a preparation method thereof, which has the following beneficial effects:
[0020] (1) Compared with polyurethane cement waterproof coating, the high weather resistance polymer cement waterproof coating proposed in the present invention has significantly improved weather resistance under the premise that the tensile performance meets the national standard requirements. Rutile titanium dioxide is used as a filler and UV shielding agent for the coating. TiO2 has a small particle size and can be fully filled in the tiny pores of the coating to improve the pore structure of the coating and the compactness of the coating, thereby improving the tensile strength, alkali resistance and high and low temperature resistance of the coating.
[0021] (2) Rutile TiO2 has good light scattering effect and ability to absorb ultraviolet light. It can absorb ultraviolet light entering the coating, protect the chemical bonds of the coating polymer components from being destroyed by ultraviolet light, and improve the stability of the coating's own structure during ultraviolet light irradiation, thereby effectively improving the coating's ultraviolet light resistance. DETAILED DESCRIPTION
[0022] The present invention provides a highly weather-resistant polymer cement waterproof coating and a preparation method. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar replacements and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0023] Example 1
[0024] A highly weather-resistant polymer cement waterproof coating, comprising liquid and powder; in terms of weight, the liquid contains 94 parts of polyurethane emulsion, 4.6 parts of film-forming aid, 0.45 parts of defoaming agent, 0.15 parts of coupling agent, 0.4 parts of titanium dioxide, and 0.4 parts of water; in terms of weight, the powder comprises: 65 parts of cement, 22.2 parts of quartz sand, 11.8 parts of calcium carbonate, and 1 part of dispersant. Among them, the cement uses PO 42.5, the quartz sand particle size is 200 mesh, the calcium carbonate particle size is 350 mesh, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, the defoaming agent is polydimethylsiloxane, the coupling agent is 3-glycidyloxypropyl trimethoxysilane, and the dispersant is sodium hexametaphosphate.
[0025] The preparation process is as follows: first, weighed cement, quartz sand, calcium carbonate and dispersant are mixed at a speed of 600r / min to 800r / min for 5min to 8min, and the powder is obtained by stirring evenly; then, weighed water-based polyurethane emulsion is taken, and film-forming aid, defoamer and coupling agent are added thereto, and the mixture is stirred evenly at a speed of 500r / min to 600r / min for 10min to 15min to obtain liquid; then, titanium dioxide is added to water and ultrasonically stirred. The mixture of titanium dioxide and water is dispersed in a wave cleaning machine for 30 minutes, and then added to the uniformly stirred liquid material, and stirred rapidly at a speed of 800r / min to 1000r / min for 5min to 15min to obtain a mixed liquid material; finally, the prepared powder is added to the above mixed liquid material while stirring at a speed of 600r / min to 900r / min for 5min to 15min. After the stirring is completed, a highly weather-resistant polymer cement waterproof coating is obtained.
[0026] Example 2
[0027] A highly weather-resistant polymer cement waterproof coating, comprising liquid and powder; in terms of weight, the liquid contains 93.8 parts of polyurethane emulsion, 4.6 parts of film-forming aid, 0.45 parts of defoaming agent, 0.15 parts of coupling agent, 0.6 parts of titanium dioxide, and 0.4 parts of water; in terms of weight, the powder comprises: 65 parts of cement, 22.2 parts of quartz sand, 11.8 parts of calcium carbonate, and 1 part of dispersant. Among them, the cement uses PO 42.5, the quartz sand particle size is 200 mesh, the calcium carbonate particle size is 350 mesh, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, the defoaming agent is polydimethylsiloxane, the coupling agent is 3-glycidyloxypropyl trimethoxysilane, and the dispersant is sodium hexametaphosphate.
[0028] The preparation process of the highly weather-resistant polymer cement waterproof coating proposed in this embodiment is the same as that in Example 1.
[0029] Example 3
[0030] A highly weather-resistant polymer cement waterproof coating includes liquid and powder; the liquid contains 93.4 parts of polyurethane emulsion, 4.6 parts of film-forming aid, 0.45 parts of defoamer, 0.15 parts of coupling agent, 0.8 parts of titanium dioxide, and 0.6 parts of water by weight; the powder includes 65 parts of cement, 22.2 parts of quartz sand, 11.8 parts of calcium carbonate, and 1 part of dispersant by weight. Among them, the cement uses PO 42.5, the quartz sand particle size is 200 mesh, the calcium carbonate particle size is 350 mesh, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, the defoamer is polydimethylsiloxane, the coupling agent is 3-glycidyloxypropyl trimethoxysilane, and the dispersant is sodium hexametaphosphate.
[0031] The preparation process of the highly weather-resistant polymer cement waterproof coating proposed in this embodiment is the same as that in Example 1.
[0032] Comparative Example 1
[0033] This comparative example provides a polyurethane cement waterproof coating, the formula and preparation method of which are basically the same as those of Example 1, except that titanium dioxide is not added. In terms of mass fractions, the liquid material contains 94 parts of polyurethane emulsion, 4.6 parts of film-forming aid, 0.45 parts of defoaming agent, 0.15 parts of coupling agent, and 0.4 parts of water; in terms of mass fractions, the powder material includes: 65 parts of cement, 22.2 parts of quartz sand, 11.8 parts of calcium carbonate, and 1 part of dispersant. Among them, the cement uses PO 42.5, the quartz sand particle size is 200 mesh, the calcium carbonate particle size is 350 mesh, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, the defoaming agent is polydimethylsiloxane, the coupling agent is 3-glycidyloxypropyltrimethoxysilane, and the dispersant is sodium hexametaphosphate.
[0034] The preparation process of the polyurethane cement waterproof coating is as follows: first, weighed cement, quartz sand, calcium carbonate and dispersant are mixed at a rotation speed of 600r / min-800r / min and a stirring time of 5min-8min, and the powder is obtained by stirring evenly; then, weighed water-based polyurethane emulsion is taken, a film-forming aid, a defoaming agent and a coupling agent are added thereto, and the mixture is mixed and stirred evenly at a rotation speed of 500r / min-600r / min and a stirring time of 10min-15min to obtain a liquid; finally, the obtained powder is added to the liquid while stirring at a stirring speed of 600r / min-900r / min and a stirring time of 5min-15min. After the stirring is completed, the polyurethane cement waterproof coating is obtained.
[0035] Comparative Example 2
[0036] This example provides a highly weather-resistant polymer cement waterproof coating, the formula and preparation method of which are basically the same as those of Example 1, except that the titanium dioxide is not ultrasonically dispersed. In terms of mass fractions, the liquid contains 94 parts of polyurethane emulsion, 4.6 parts of film-forming aid, 0.45 parts of defoaming agent, 0.15 parts of coupling agent, 0.4 parts of titanium dioxide, and 0.4 parts of water; in terms of mass fractions, the powder includes: 65 parts of cement, 22.2 parts of quartz sand, 11.8 parts of calcium carbonate, and 1 part of dispersant. Among them, the cement uses P.O42.5, the quartz sand particle size is 200 mesh, the calcium carbonate particle size is 350 mesh, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, the defoaming agent is polydimethylsiloxane, the coupling agent is 3-glycidyloxypropyltrimethoxysilane, and the dispersant is sodium hexametaphosphate.
[0037] The preparation process is as follows: first, weighed cement, quartz sand, calcium carbonate and dispersant are mixed at a speed of 600r / min to 800r / min and a stirring time of 5min to 8min, and the powder is obtained by stirring evenly; then, a weighed aqueous polyurethane emulsion is taken, and a film-forming aid, a defoaming agent and a coupling agent are added thereto, and the mixture is stirred evenly at a speed of 500r / min to 600r / min and a stirring time of 10min to 15min to obtain a liquid; then, titanium dioxide is added to water, and then added to the stirred liquid, and the mixture is stirred rapidly at a stirring speed of 800r / min to 1000r / min and a stirring time of 5min to 15min to obtain a mixed liquid; finally, the prepared powder is added to the mixed liquid while stirring at a stirring speed of 600r / min to 900r / min and a stirring time of 5min to 15min. After the stirring is completed, a highly weather-resistant polymer cement waterproof coating is obtained.
[0038] The following performance tests were performed on the polymer cement waterproof coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 2:
[0039] 1. Solid content: According to the fixed test solid content of the sample in Chapter 5 of GB / T6777-2008 "Test Methods for Building Waterproof Coatings", the drying temperature is (105±0.5)℃;
[0040] 2. Untreated tensile properties: The test was carried out in accordance with the provisions of 9.2.1 of GB / T6777-2008 "Test methods for building waterproof coatings", with a tensile speed of 200 mm / min, and the tensile strength and elongation at break of the test samples were tested;
[0041] 3. Tensile properties after heat treatment: Treat the sample and conduct the test in accordance with the provisions of 9.2.2 of GB / T6777-2008 "Test Methods for Building Waterproof Coatings". The heat treatment temperature is (80±2)℃ and the time is (168±1)h. After heat treatment, the tensile strength and elongation at break of the sample are tested in accordance with the provisions of 7.4.3.
[0042] 4. Tensile properties after alkali treatment: treat the sample and conduct the test in accordance with the provisions of 9.2.3 of GB / T6777-2008 "Test methods for building waterproof coatings". The alkali immersion time is (168±1)h. After alkali treatment, the tensile strength and elongation at break of the sample are tested in accordance with the provisions of 7.4.3;
[0043] 5. Tensile properties after UV treatment: Treat the sample and conduct the test in accordance with the provisions of 9.2.5 of GB / T6777-2008 "Test Methods for Building Waterproof Coatings". The UV irradiation time is 240h. After UV treatment, the tensile strength and elongation at break of the sample are tested in accordance with the provisions of 7.4.3.
[0044] 6. Low temperature flexibility: Prepare the coating sample according to the method specified in 7.4.2 Sample preparation in GB / T23445-2009 "Polymer cement waterproof coating", and conduct the test according to 13.2.1 in GB / T16777-2008 "Test methods for building waterproof coatings", with a round rod diameter of 10 mm;
[0045] The test results are shown in Table 1:
[0046] Table 1
[0047]
[0048]
[0049] As can be seen from Table 1, the comparison of the performance results of Examples 1 to 3 and Comparative Example 1 shows that the tensile strength and elongation at break of the highly weather-resistant polymer cement waterproof coating of the present invention after alkali treatment, ultraviolet light irradiation and heat treatment are highly stable, and the weather resistance is better than that of the polyurethane cement waterproof coating, and its water absorption is also better than that of the polyurethane cement waterproof coating. The comparison of the performance results of Example 1 and Comparative Example 2 shows that the dispersion of titanium dioxide during the preparation of the highly weather-resistant polymer cement waterproof coating has a certain influence on the weather resistance of the coating. The addition of titanium dioxide needs to take into account its own small particle size and easy agglomeration properties. In order to fully play its role, it should be fully dispersed in an ultrasonic cleaning machine and stirred rapidly during the coating preparation process.
[0050] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein with equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.
Claims
1. A highly weather-resistant polymer cement waterproof coating, comprising a liquid material and a powder material, characterized in that: Calculated by mass, the liquid material includes: 90-95 parts of polyurethane emulsion, 3-5 parts of film-forming aid, 0.1-1 part of defoaming agent, 0.05-0.15 part of coupling agent, 0.5-1.5 parts of titanium dioxide, and 0-5 parts of water; the powder material includes: 60-65 parts of cement, 20-25 parts of quartz sand, 10-15 parts of calcium carbonate, and 0.5-1 part of dispersant.
2. A highly weather-resistant polymer cement waterproof coating according to claim 1, characterized in that: The mass ratio of liquid to powder is 0.6-0.8, and the aggregate-ash ratio is 0.8-1.
3. According to the highly weather-resistant polymer cement waterproof coating described in claim 2, the titanium dioxide crystal form is rutile and the particle size is 30 to 50 nm.
4. A highly weather-resistant polymer cement waterproof coating according to claim 2 or 3, characterized in that: The polymer emulsion is an aqueous polyurethane emulsion with a solid content of 30% to 40%.
5. The highly weather-resistant polymer cement composite waterproof coating according to claim 1 is characterized in that: The cement is ordinary Portland cement PO 42.
5.
6. A highly weather-resistant polymer cement waterproof coating according to claim 1, characterized in that: The particle size of quartz sand is 200 mesh and the particle size of calcium carbonate is 350 mesh.
7. The highly weather-resistant polymer cement waterproof coating according to claim 1, characterized in that: The film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate.
8. The highly weather-resistant polymer cement waterproof coating according to claim 1, characterized in that: The defoaming agent is polydimethylsiloxane.
9. The highly weather-resistant polymer cement waterproof coating according to claim 1, characterized in that: The coupling agent is 3-glycidyloxypropyltrimethoxysilane.
10. A method for preparing a highly weather-resistant polymer cement waterproof coating as claimed in any one of claims 1 to 9, characterized in that: The steps are as follows: 1) Weigh the powder components according to the measured portion and mix them, keep the speed at 600r / min~800r / min, and stir for 5min~8min to make the powder mix evenly; 2) adding the weighed film-forming aid, defoaming agent and coupling agent to the weighed aqueous polyurethane emulsion, rotating at a speed of 500 r / min to 600 r / min, stirring for 10 min to 15 min, and stirring evenly to obtain a liquid material; 3) adding weighed titanium dioxide to weighed water, dispersing the mixture of titanium dioxide and water with an ultrasonic cleaner for 30 minutes, and then adding it to the stirred liquid material for stirring at a stirring speed of 800 r / min to 1000 r / min for 10 min to 20 min to obtain a mixed liquid material; 4) Add the obtained powder to the mixed liquid while stirring at a speed of 600 r / min to 900 r / min and a stirring time of 5 min to 15 min to obtain the product.
Citation Information
Cited By
Impermeable durable prefabricated assembly type concrete reverse ridge and processing technology thereof
CN121132887A
Anti-permeability durable prefabricated assembled concrete reverse ridge and processing technology thereof
CN121132887B