Polishing Pad

The polishing pad with a transparent end point detection window having a specific Abbe number range addresses chromatic aberrations, ensuring precise end point detection by minimizing light dispersion effects.

JP7575661B2Active Publication Date: 2024-10-30FUJIBO HLDG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020163732
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-10-30
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Conventional polishing pads with increased transparency for end point detection windows suffer from chromatic aberrations due to light dispersion, leading to potential malfunctions in end point detection during polishing processes.

Method used

The polishing pad incorporates a transparent end point detection window with a specific Abbe number range of 38.1 to 42.2, calculated using the refractive indices of NaD, NaF, and NaC lines, to minimize light dispersion-induced aberrations, allowing precise end point detection.

Benefits of technology

This configuration effectively suppresses aberrations caused by light dispersion, enabling accurate and stable end point detection during polishing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575661000002
    Figure 0007575661000002
  • Figure 0007575661000003
    Figure 0007575661000003
  • Figure 0007575661000001
    Figure 0007575661000001
Patent Text Reader

Abstract

To provide a polishing pad equipped with a window for endpoint detection which can suppress reflected light from an object to be polished from dispersing to improve accuracy in endpoint detection.SOLUTION: A polishing pad 3 is equipped with a polishing layer 3C and a window 3B for endpoint detection provided at a predetermined position thereof. The polishing pad 3 can detect an endpoint in polishing processing on the basis of reflected light L2 from an object 2 to be polished transmitting through the window 3B for endpoint detection, during polishing processing for the object 2 to be polished. As a material of the window 3B for endpoint detection, a material having Abbe number corresponding to values at which chromatic aberration (color deviation) of inspection light L1 and reflected light L transmitting through the window 3B for endpoint detection can be suppressed is employed. This can suppress the reflected light L2 from dispersing, so as to improve accuracy in endpoint detection by a detection mechanism 7.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing pad, and more particularly to a polishing pad having a transparent endpoint detection window at a predetermined location in the polishing layer. [Background technology]

[0002] Conventionally, polishing pads for polishing a wafer as a workpiece have been known, and furthermore, polishing pads equipped with an end point detection window that transmits light reflected from the workpiece in order to detect the end point when polishing a wafer have been known (for example, Patent Document 1). In the polishing pad of Patent Document 1, the light transmittance of the material that serves as the end point detection window is increased compared to conventional techniques, thereby preventing malfunctions in the end point detection and enabling end point detection using visible light without any problems. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-48151 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, even if the transparency of the material used for the end point detection window is increased, as in the polishing pad of Patent Document 1, there is still a possibility that the end point detection will malfunction because aberration (chromatic aberration) occurs as a color shift due to the dispersion of reflected light from the polished object. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a polishing pad having an inspection window that suppresses aberration caused by the dispersion of reflected light and enables endpoint detection with higher accuracy than conventional methods. [Means for solving the problem]

[0005] In view of the above circumstances, the present invention provides a polishing pad comprising a polishing layer for polishing an object to be polished, and an end point detection window provided in the polishing layer for transmitting an inspection light irradiated onto the object to be polished and a light reflected from the object to be polished, the end point of polishing being detectable based on the light reflected from the object to be polished, The Abbe number vD calculated from Equation 1 based on the refractive indices nD, nF, and nC of the NaD line with a wavelength of 589 nm, the NaF line with a wavelength of 486 nm, and the NaC line with a wavelength of 656 nm of the reflected light is 38.1 ~ 42.2 The end point detection window is characterized by using a material that This is what we believe. Abbe number vD=(nD-1) / (nF-nC) Equation 1 Effect of the Invention

[0006] With this configuration, it is possible to suppress aberrations caused by the dispersion of reflected light from the workpiece being polished, thereby providing a polishing pad equipped with an inspection window that enables endpoint detection with greater accuracy than conventional methods. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a perspective view showing an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the main part taken along line II-II in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1 and 2, reference numeral 1 denotes a polishing apparatus that polishes a thin plate-like object to be polished 2 (e.g., a semiconductor wafer) with a polishing pad 3. When performing polishing of the object to be polished 2, the polishing apparatus 1 is capable of detecting the progress of the polishing process and the end point of the process by irradiating a surface 2A of the object to be polished 2 with an inspection light L1 and detecting reflected light L2 from the surface 2A. The polishing apparatus 1 is equipped with a polishing platen 4 located on the lower side and having a polishing pad 3 fixed on its upper surface, a holding platen 5 located on the upper side and holding the workpiece 2 to be polished on its lower surface, a slurry supply mechanism 6 that supplies slurry between the workpiece 2 to be polished and the polishing pad 3, and a detection mechanism 7 that uses an inspection light L1 to detect the progress of polishing of the workpiece 2 and the end point of the processing. The object 2 to be polished by the polishing apparatus 1 is an optical material, a silicon wafer, a glass substrate for liquid crystal, a semiconductor substrate, and a plate-like object such as glass, metal, ceramic, etc. As the slurry to be supplied by the slurry supply mechanism 6, a suitable conventionally known material can be used depending on the object 2 to be polished and the required processing accuracy. The polishing platen 4 and the holding platen 5 are each substantially disk-shaped and are adapted to rotate in the direction of the arrow by a drive mechanism (not shown), and the holding platen 5 is provided so as to be movable up and down. When polishing the object 2, the holding platen 5 presses the polished surface (lower surface) 2A of the object 2 against the polishing surface 3A of the polishing pad 3 at a set pressure while they are rotated relative to one another, and slurry is supplied from a slurry supply mechanism 6 between the polished surface 2A of the object 2 and the polishing surface 3A of the polishing pad 3.

[0009] When polishing the workpiece 2, it is necessary to detect the progress of the polishing of the workpiece 2 and the end point of the polishing. Therefore, the polishing apparatus 1 is provided with a detection mechanism 7 that irradiates an inspection light L1 from below toward above and detects the progress of the polishing process and the end point of the process based on the reflected light L2 reflected from the polished surface 2A of the workpiece 2. In addition, a transparent end point detection window 3B is provided at a predetermined position of the polishing pad 3, which transmits the inspection light L1 and the reflected light L2 from the polished surface 2A of the workpiece 2. 2, the polishing pad 3 includes a disk-shaped polishing layer 3C located on the upper side, and a disk-shaped support layer 3D bonded with an adhesive to the lower surface of the polishing layer 3C. A transparent, substantially cylindrical end point detection window 3B is provided at a predetermined position of the polishing layer 3C, and a through hole 3Da is drilled below the end point detection window 3B at the position of the support layer 3D for passing the inspection light L1 and the reflected light L2 from the workpiece 2. The upper surface 3Ba of the end point detection window 3B and the polishing surface 3A, which is the upper surface of the polishing layer 3C, are flush with each other. The lower surface 3Bb of the end point detection window 3B and the lower surface of the polishing layer 3C are flush with each other, and the upper surface of the support layer 3D is bonded thereto with an adhesive. The polishing pad 3, which is made up of the polishing layer 3C and the support layer 3D integrated vertically, has its lower surface (the lower surface of the support layer 3D) fixed to the upper surface 4A of the polishing table 4 with an adhesive.

[0010] The polishing table 4 is provided with a light-emitting unit 7A that irradiates inspection light L1 vertically upward and a light-receiving unit 7B that receives reflected light L2 from the polished object 2, below the end-point detection window 3B of the polishing pad 3 and the through-hole 3Da of the support layer 3D. The detection mechanism 7 includes the light-emitting unit 7A, the light-receiving unit 7B, and a control unit 7C that controls their operation and detects the progress of polishing and the end point where polishing ends. During polishing of the workpiece 2, the light emitting unit 7A of the detection mechanism 7 irradiates the inspection light L1 upward, which passes through the transparent end point detection window 3B and is irradiated onto the polished surface 2A of the workpiece 2. The inspection light L1 is then reflected downward by the polished surface 2A of the workpiece 2, and the reflected light L2 passes through the transparent end point detection window 3 and is detected by the light receiving unit 7B. The reflected light L2 detected by the light receiving unit 7B is transmitted to the control unit 7C. As the polishing of the workpiece 2 progresses and the polishing surface 2A of the workpiece 2 is gradually polished, the intensity of the reflected light L2 detected by the light-receiving unit 7B changes. When the intensity of the reflected light L2 detected by the light-receiving unit 7B reaches a preregistered intensity, the control unit 7C determines that the polishing surface 2A has reached the end point of polishing, and stops the polishing. Then, the drive mechanism is stopped, so that the rotation of the polishing platen 4 and the holding platen 5 stops, and the supply of slurry from the slurry supply mechanism 6 is also stopped. The detection mechanism 7 detects the end point of the polishing process when the workpiece 2 is polished in this manner. The configuration of the detection mechanism 7 using the inspection light L1 and the reflected light L2 is publicly known from the above-mentioned Patent Document 1 and the like.

[0011] The polishing layer 3C is made of hard urethane. Hard urethane is produced by a prepolymer method in which a urethane prepolymer, which is a reaction intermediate between a polyol component and an isocyanate component, is used to harden a polyurethane polyurea resin obtained by adding and mixing a hardener (chain extender) such as a diamine or diol, a foaming agent, a catalyst, etc. In the following, the polishing layer and the end point detection window are described as being made of a polyurethane polyurea resin, but a polyurethane resin or a polyurea resin may also be used.

[0012] A method for producing the polishing layer 3C may include, for example, a preparation step of preparing at least a polyurethane bond-containing isocyanate compound as a prepolymer, a curing agent, and a hollow body; a mixing step of mixing at least the polyurethane bond-containing isocyanate compound and the curing agent to obtain a mixed liquid for molding a molded body; a molded body molding step of molding a polyurethane polyurea resin molded body from the mixed liquid for molding a molded body; and a polishing layer formation step of forming a polishing layer having the polishing surface from the polyurethane polyurea resin molded body.

[0013] In the preparation process, for example, polyurethane bond-containing isocyanate compound, hardener, and hollow body are used as the raw material of polyurethane polyurea resin molded body in the manufacture of the polishing layer 3C.Furthermore, polyol compound may be used together with the above-mentioned components, and components other than the above-mentioned may be used together within the range that does not impair the effect of the present invention.

[0014] The polyurethane bond-containing isocyanate compound prepared in the preparation step is a compound obtained by reacting the following polyisocyanate compound with a polyol compound under commonly used conditions, and contains a polyurethane bond and an isocyanate group in the molecule. In addition, other components may be contained in the polyurethane bond-containing isocyanate compound within the range that does not impair the effects of the present invention. The polyurethane bond-containing isocyanate compound may be a commercially available product, or may be a product synthesized by reacting a polyisocyanate compound with a polyol compound. The reaction is not particularly limited, and addition polymerization may be performed using a method and conditions known in the art for producing polyurethane resins. For example, the polyisocyanate compound heated to 50°C is added to a polyol compound heated to 40°C while stirring in a nitrogen atmosphere, and the mixture is heated to 80°C after 30 minutes and then reacted at 80°C for 60 minutes.

[0015] First, the polyisocyanate compound means a compound having two or more isocyanate groups in the molecule. The polyisocyanate compound is not particularly limited as long as it has two or more isocyanate groups in the molecule. For example, diisocyanate compounds having two isocyanate groups in the molecule include m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), naphthalene-1,4-diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyl Examples of the diisocyanate include diphenylmethane-4,4-diisocyanate, xylylene-1,4-diisocyanate, 4,4-diphenylpropane diisocyanate, trimethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate. Furthermore, as the polyisocyanate compound, a diisocyanate compound or a diisothiocyanate is preferable, and among them, 2,4-TDI, 2,6-TDI, MDI, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate are more preferable, and 2,4-TDI, 2,6-TDI, p-phenylene diisothiocyanate, and xylylene-1,4-diisothiocyanate are particularly preferable. These polyisocyanate compounds may be used alone, or a plurality of polyisocyanate compounds may be used in combination.

[0016] Next, the above-mentioned polyol compound means a compound having two or more alcoholic hydroxyl groups (OH) in the molecule. Examples of the polyol compound used in the synthesis of the polyurethane bond-containing isocyanate compound include diol compounds, triol compounds, and the like, such as ethylene glycol, diethylene glycol (DEG), butylene glycol, and the like; polyether polyol compounds, such as poly(oxytetramethylene) glycol (or polytetramethylene ether glycol) (PTMG), and the like; polyester polyol compounds, such as the reaction product of ethylene glycol and adipic acid, and the reaction product of butylene glycol and adipic acid, and the like; polycarbonate polyol compounds, polycaprolactone polyol compounds, and the like. Also, trifunctional propylene glycol with ethylene oxide added thereto can be used. Among these, PTMG or a combination of PTMG and DEG is preferred. The above polyol compounds may be used alone or in combination of two or more.

[0017] Here, the NCO equivalent of the prepolymer, which indicates the molecular weight of the prepolymer per NCO group, is preferably 200-800, more preferably 300-700, and further more preferably 400-600. Specifically, the NCO equivalent of the prepolymer can be determined as follows. NCO equivalent of prepolymer = (parts by mass of polyisocyanate compound + parts by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound x parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound) - (number of functional groups per molecule of polyol compound x parts by mass of polyol compound / molecular weight of polyol compound)]

[0018] As the curing agent, for example, a polyamine compound and / or a polyol compound can be used. The polyamine compound means a compound having two or more amino groups in the molecule, and an aliphatic or aromatic polyamine compound, particularly a diamine compound, can be used. Examples of the amine compounds include ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4-diamine, 3,3-dichloro-4,4-diaminodiphenylmethane (methylenebis-o-chloroaniline) (hereinafter abbreviated as MOCA), polyamine compounds having the same structure as MOCA, etc. Also, the polyamine compounds may have a hydroxyl group, and examples of such amine compounds include 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, etc. As the polyamine compound, a diamine compound is preferable, MOCA, diaminodiphenylmethane, and diaminodiphenylsulfone are more preferable, and MOCA is particularly preferable. The polyamine compound may be used alone or in combination of two or more polyamine compounds. In order to facilitate mixing with other components and / or to improve the uniformity of the bubble diameter in the subsequent molding process, the polyamine compound is preferably degassed under reduced pressure while being heated as necessary. As a method for degassing under reduced pressure, a method known in the production of polyurethane may be used, and for example, degassing can be performed at a vacuum of 0.1 MPa or less using a vacuum pump. When a solid compound is used as a curing agent, it can be degassed under reduced pressure while being melted by heating.

[0019] The polyol compound used as the curing agent is not particularly limited as long as it is a diol compound, a triol compound, etc. The polyol compound may be the same as or different from the polyol compound used to form the prepolymer. Specific examples include low molecular weight diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, and high molecular weight polyol compounds such as poly(oxytetramethylene) glycol, polyethylene glycol, and polypropylene glycol. The above polyol compounds may be used alone or in combination of two or more.

[0020] Here, the components are mixed so that the R value, which is the equivalent ratio of the active hydrogen groups (amino groups and hydroxyl groups) present in the curing agent to the isocyanate groups present at the ends of the polyurethane bond-containing isocyanate compound, is 0.60 to 1.40. The R value is preferably 0.65 to 1.30, and more preferably 0.70 to 1.20.

[0021] The hollow body means a microsphere having a void. The microsphere includes those having a spherical shape, an elliptical shape, and shapes similar thereto. Examples of hollow bodies include unfoamed heat-expandable microspheres having an outer shell (polymer shell) made of a thermoplastic resin and a low-boiling point hydrocarbon contained in the outer shell, and those obtained by thermally expanding unfoamed heat-expandable microspheres. As disclosed in JP-A-57-137323, for example, the polymer shell may be a thermoplastic resin such as an acrylonitrile-vinylidene chloride copolymer, an acrylonitrile-methyl methacrylate copolymer, or a vinyl chloride-ethylene copolymer. Similarly, the low-boiling point hydrocarbon contained in the polymer shell may be, for example, isobutane, pentane, isopentane, or petroleum ether. In addition to using the hollow bodies, bubbles may be formed by chemical foaming such as water foaming or foaming due to mechanical agitation, or these methods may be combined.

[0022] Next, the mixing step will be described. In the mixing step, the polyurethane bond-containing isocyanate compound as a prepolymer, the curing agent, and the hollow bodies prepared in the preparation step are fed into a mixer and stirred and mixed. The mixing step is carried out in a state where the components are heated to a temperature at which the fluidity of each component can be ensured. There is no particular restriction on the order of mixing, but it is preferable to prepare a mixed liquid obtained by mixing the polyurethane bond-containing isocyanate compound and the hollow body, and a mixed liquid obtained by mixing the curing agent and other components as necessary, and feed both mixed liquids into a mixer and mix and stir them. In this way, the mixed liquid for molding is prepared.

[0023] Next, in the molded body forming process, the mixed liquid for molding the molded body prepared in the above mixing process is poured into a mold frame at 50 to 100°C, and the prepolymer and the curing agent react to form a polyurethane polyurea resin, whereby the mixed liquid hardens and a polyurethane polyurea resin molded body is formed.

[0024] In the polishing layer forming step, the polyurethane-polyurea resin molded body obtained in the molded body forming step is sliced ​​into sheets, and the sliced ​​resin sheets are cut into a predetermined shape. The resin sheet thus obtained is ground on the front and / or back. One side becomes the polishing surface 3A, and by performing cutting processing or the like on the polishing surface 3A using a required cutter, grooves with any pitch, width, and depth can be formed, and thus the polishing layer 3C is obtained.

[0025] The support layer 3D may be a support base material such as an impregnated nonwoven fabric impregnated with a resin, a foam such as polyethylene foam or polyurethane foam, or polyethylene terephthalate (PET). When the support layer 3D is an impregnated nonwoven fabric, the manufacturing process of the support layer 3D may include at least a step of wet-solidifying the resin impregnated in the nonwoven fabric substrate, and a step of puffing both sides of the wet-solidified fiber assembly. The nonwoven fabric substrate of this embodiment is not particularly limited, and various known ones may be used. Examples of the nonwoven fabric substrate include polyolefin-based, polyamide-based, and polyester-based nonwoven fabrics. The method of entangling fibers when obtaining the nonwoven fabric substrate is not particularly limited, and may be, for example, needle punching or water flow entanglement. The nonwoven fabric substrate may be one of the above-mentioned types alone or a combination of two or more types. The nonwoven fabric substrate has many gaps between fibers and is highly water absorbent, but impregnating the substrate with resin fills the gaps with resin, reducing water absorbency.

[0026] Examples of resins to be impregnated into the nonwoven fabric substrate include polyurethane-based resins such as polyurethane and polyurethane polyurea; acrylic-based resins such as polyacrylate and polyacrylonitrile; vinyl-based resins such as polyvinyl chloride, polyvinyl acetate and polyvinylidene fluoride; polysulfone-based resins such as polysulfone and polyethersulfone; acylated cellulose-based resins such as acetylated cellulose and butyrylated cellulose; polyamide-based resins and polystyrene-based resins.

[0027] The density of the nonwoven fabric before resin impregnation (web state) is preferably 0.3 g / cm 3 More preferably, it is 0.1 to 0.2 g / cm 3 The density of the nonwoven fabric after resin impregnation is preferably 0.5 g / cm. 3 More preferably, it is 0.3 to 0.4 g / cm 3 If the density of the nonwoven fabric is too high, the processing accuracy tends to deteriorate, and if it is too low, it tends to absorb water relatively easily. The adhesion rate of the resin to the nonwoven fabric is expressed as the weight of the attached resin relative to the weight of the nonwoven fabric, and is preferably 50% or more, and more preferably 75 to 200%. If the adhesion rate of the resin is too high, it tends to not exhibit the desired cushioning properties as the support layer 3D, and if it is too low, the support layer 3D will absorb water, which will affect the polishing properties.

[0028] As an example of impregnating a nonwoven fabric substrate with a resin and wet-coagulating it, a case where a polyurethane resin is used will be described. A polyurethane resin is mixed with a solvent capable of dissolving the polyurethane resin and miscible with the coagulation liquid described below, and other additives as necessary, and the mixture is degassed under reduced pressure as necessary to prepare a polyurethane resin solution. The solvent is not particularly limited, but examples thereof include N,N-dimethylformamide (DMF), isopropyl alcohol (IPA), and N,N-dimethylacetamide. For example, the polyurethane resin may be dissolved in the solvent in a range of 5 to 25% by mass, more preferably 8 to 15% by mass, based on the total amount of the polyurethane resin solution. In the above range, the polyurethane resin can be easily distributed throughout the nonwoven fabric substrate.

[0029] Next, a sheet-shaped nonwoven fabric is immersed in the polyurethane resin solution, and then the resin solution is squeezed out by using a mangle roller capable of applying pressure between a pair of rollers to adjust the amount of resin solution to a desired level, so that the nonwoven fabric base is substantially uniformly impregnated with the resin solution. Next, the nonwoven fabric base impregnated with the resin solution is immersed in a coagulation liquid mainly composed of a poor solvent for the resin, such as water, to coagulate and regenerate the polyurethane resin. In order to adjust the regeneration speed of the resin, an organic solvent such as a polar solvent other than the solvent in the resin solution may be added to the coagulation liquid. The temperature of the coagulation liquid is not particularly limited as long as it is a temperature at which the resin can be coagulated, and may be, for example, 15 to 60°C. Thereafter, if necessary, the solvent remaining in the nonwoven fabric impregnated with the resin may be removed using a conventionally known cleaning liquid, and the cleaning liquid may be removed by using a mangle roller or drying. In this way, a fiber aggregate in which the resin has been wet-coagulated can be obtained. Then, both sides of the fiber aggregate are subjected to a puff treatment to adjust the thickness of the fiber aggregate.

[0030] In the fiber assembly whose thickness has been adjusted, through holes are formed in the thickness direction at predetermined positions. The through holes can be formed by a drilling process or the like. In this way, the support layer 3D is obtained.

[0031] For the support layer 3D, a transparent substrate made of, for example, polyethylene terephthalate (PET) can be used. The support layer 3D can be attached and fixed to the polishing layer 3C by using double-sided tape or adhesive on both sides of the polyethylene terephthalate substrate and applying pressure as necessary. There are no particular limitations on the double-sided tape or adhesive used for bonding to the polishing layer 3C, and any double-sided tape or adhesive known in the art can be selected and used.

[0032] The end point detection window 3B can be made of the same material as the polishing layer 3C, for example, hard urethane. The hard urethane of the end point detection window 3B is manufactured by a prepolymer method in which a urethane prepolymer is used and a curing agent (chain extender) such as diamines or diols, additives, catalysts, etc. are added and mixed to obtain a polyurethane polyurea resin, which is then cured.

[0033] The urethane prepolymer used in the end point detection window 3B may be, for example, a polyurethane bond-containing isocyanate compound, which is the same as that used in the polishing layer 3C. The polyurethane bond-containing isocyanate compound may be a commercially available product, or may be a product synthesized by reacting a polyisocyanate compound with a polyol compound. There is no particular restriction on the reaction, and the addition polymerization reaction may be carried out using a method and conditions known in the manufacture of polyurethane resins. In addition, other components may be contained in the polyurethane bond-containing isocyanate compound within a range that does not impair the effects of the present invention. As the polyisocyanate compound, diisocyanate compounds and diisothiocyanates are preferred, and the diisocyanate compounds and diisothiocyanates used in the polishing layer 3C can be used. Among them, 2,4-TDI, 2,6-TDI, MDI, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate are more preferred, and 2,4-TDI, 2,6-TDI, p-phenylene diisothiocyanate, and xylylene-1,4-diisothiocyanate are particularly preferred. These polyisocyanate compounds may be used alone, or multiple polyisocyanate compounds may be used in combination.

[0034] The polyol compound used in the synthesis of the above polyurethane bond-containing isocyanate compound can also be the polyol compound used in the polishing layer. Among the polyol compounds, PTMG or the combination of PTMG and DRG is preferred. The above polyol compound can be used alone or in combination of multiple polyol compounds.

[0035] For the prepolymer used in the end point detection window 3B, the NCO equivalent of the prepolymer, which indicates the molecular weight of the prepolymer per NCO group, is preferably 200-800, more preferably 300-700, and even more preferably 400-600.

[0036] As the curing agent, for example, a polyamine compound and / or a polyol compound can be used. As the polyamine compound, a diamine compound containing a sulfur atom and not containing a halogen is preferable, 2-methyl-4,6-bis(methylthio)-1,3-benzenediamine and dimethylthiotoluenediamine are more preferable, and 2-methyl-4,6-bis(methylthio)-1,3-benzenediamine is particularly preferable. The polyamine compound may be used alone, or a combination of multiple polyamine compounds listed here may be used. The polyamine compound used in the end point detection window 3B is preferably degassed under reduced pressure, if necessary while being heated, in the same manner as in the polishing layer 3C, to facilitate mixing with other components and / or to remove air bubbles.

[0037] In addition, the polyol compound used as the curing agent for the end point detection window 3B can be any compound such as a diol compound or a triol compound without any particular limitation. In addition, the polyol compound may be the same as or different from the polyol compound used to form the prepolymer used for the end point detection window 3B. The polyol compound may be used alone or in combination with a plurality of polyol compounds.

[0038] Here, the components are mixed so that the equivalent ratio R of the active hydrogen groups (amino groups and hydroxyl groups) present in the curing agent used in the end point detection window to the isocyanate groups present at the ends of the polyurethane bond-containing isocyanate compound used in the end point detection window 3B is 0.60 to 1.40. The R value is preferably 0.65 to 1.30, and more preferably 0.70 to 1.20.

[0039] In addition, UV-curable resins can be used as the material for the end point detection window 3B, such as acrylic (methacrylic) esters and their urethane modifications, thiokol-based materials, etc., and reactive diluents and organic solvents can be used as appropriate depending on the application.

[0040] The polishing pad 3 of this embodiment can be manufactured by known methods such as a method of bonding a polishing layer and a base layer together, or a method of forming a polishing layer on a base layer. EXAMPLES

[0041] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. Example 1 First, the polishing pad 3 was produced. 3,3'-dichloro-4,4'-diaminodiphenylmethane was added as a curing agent to a prepolymer containing an adduct of 2,4-tolylene diisocyanate and polyoxytetramethylene glycol, and the prepolymer was cured to form the polishing layer 3C. The base layer was obtained by impregnating a nonwoven fabric made of polyethylene fibers with a polyurethane resin solution, followed by wet solidification and drying. The base layer was attached to the polishing layer with a double-sided tape having a hot-melt adhesive layer, to obtain the polishing pad 3. Next, a window member for detecting the end point was produced by adding 2-methyl-4,6-bis(methylthio)-1,3-benzenediamine (product name: Ethacure 300) as a curing agent to a prepolymer containing an adduct of 2,4-tolylene diisocyanate and polyoxytetramethylene glycol, and curing the mixture to obtain a window member for detecting the end point. Finally, a 6 cm×10 cm through hole was made in part of the polishing pad 3, and an end point detection window member machined to the same shape as the through hole was fitted into the hole to obtain a polishing pad 3 equipped with an end point detection window 3B. Example 2 Except for the fact that the window member for end point detection was made of urethane acrylate (product name: Luxidia V4260 manufactured by DIC Corporation), which is a UV-curable resin, a polishing pad equipped with a window for end point detection was prepared in the same manner as in Example 1. The diluent used for curing was Aronix M-111 (monofunctional nonylphenol acrylate manufactured by Toagosei Co., Ltd.), the photopolymerization initiator was Irgacure 184 (α-hydroxyalkylphenone manufactured by IGM Resins BV), and the mixture ratio (weight ratio) was 3:7:0.5 (resin:diluent:initiator). (Comparative Example) A polishing pad 3 having an end point detection window was prepared in the same manner as in Example 1, except that the curing agent used as the end point detection window member was changed to 3,3'-dichloro-4,4'-diaminodiphenylmethane.

[0042] This embodiment focuses on the Abbe number and the refractive index of three types of light that are the basis for its calculation in relation to the material used for the end point detection window 3B. The end point detection window 3B of this embodiment can suppress the color aberration (color shift) of the reflected light L2 from the workpiece 2, thereby enabling the detection mechanism 7 to detect the end point position with high accuracy. Table 1 shows the values ​​on which the refractive index and Abbe number of three types of light are calculated for the endpoint detection windows of Examples 1 and 2 of the present invention, and the comparative example endpoint detection window used for comparison, as well as the calculated Abbe numbers. In Table 1, Example 1 is an endpoint detection window made from Ethacure 300 and a prepolymer, Example 2 is an endpoint detection window made from only a UV curable resin, and Comparative Example shows an endpoint detection window made from MOCA with a prepolymer added. Then, the refractive indexes of three types of reflected light were measured for Example 1, Example 2, and Comparative Example. Then, the values ​​(the numerator of the Abbe number and the denominator of the Abbe number) that are the basis of the Abbe number calculated based on the three types of refractive index were obtained, and the Abbe number vD was calculated for Example 1, Example 2, and Comparative Example using the formula described below. More specifically, for Examples 1 and 2 and Comparative Example, test pieces having a length of 30 to 40 mm, a width of 8 mm, and a thickness of 1 mm were prepared, and the refractive indices nD, nF, and nC of light of the test pieces at NaD line with a wavelength of 589 nm, NaF line with a wavelength of 486 nm, and NaC line with a wavelength of 656 nm were measured using an Atago Co., Ltd. "Multi-wavelength Abbe refractometer DR-M4" at a temperature of 20°C and monobromonaphthalene as an intermediate liquid, and the Abbe number vD was calculated based on these three refractive indices. The Abbe number vD is calculated as follows. That is, the refractive indices nD, nF, and nC of the test piece were measured at 25°C using a multi-wavelength Abbe refractometer DR-M4 manufactured by Atago Co., Ltd. for the NaD line with a wavelength of 589 nm, the NaF line with a wavelength of 486 nm, and the NaC line with a wavelength of 656 nm, and the Abbe number vD was calculated from these three refractive indices according to the following formula. Abbe number vD=(nD-1) / (nF-nC)

[0043] (End point detection evaluation) The endpoint detection evaluation of the film thickness of the wafer as the object to be polished was performed by the following method. An 8-inch silicon wafer with an oxide film of 1 μm was used as the wafer, and polished under the following conditions using a chemical mechanical polishing device (MIRRA (manufactured by Applied Materials)). The endpoint was the time when the oxide film of the wafer was polished away. This was performed for 10 wafers. Slurry supply rate: 200mL / min Retainer Ring Pressure: 5psi Membrane pressure: 4.5psi Inner tube pressure: 4.5psi Plate rotation speed: 70 rpm Head rotation speed: 65 rpm After polishing, each wafer was subjected to film thickness measurement in the wavelength region of 400 to 800 nm using an interference film thickness measurement device (manufactured by Otsuka Electronics Co., Ltd.). As shown in Table 1, the calculated film thickness results were marked with an ◯ when they were highly reproducible and the film thickness values ​​were measured with high precision without any variation, while those with poor reproducibility and insufficient detection precision were marked with an ×. [Table 1]

[0044] As described above, according to this embodiment, by increasing the Abbe number of the material used for the end point detection window, it is possible to suppress color aberration (color shift) of the inspection light and reflected light passing through the end point detection window, and therefore the detection mechanism 7 can perform highly accurate end point detection. In addition, the difference between the refractive index of the NaF line at a wavelength of 486 nm, nF, and the refractive index of the NaC line at a wavelength of 656 nm, nC, is 0.0124 ~ 0.0147 This means that there is no variation in the refractive index for various types of light from long wavelengths to short wavelengths, making it possible to detect the end point with stable accuracy.

[0045] As described above, the polishing pad 3 of this embodiment uses a material having the above-mentioned refractive index and Abbe number values ​​for the end point detection window 3B, so that the color aberration (color shift) of the reflected light passing through the end point detection window 3B can be suppressed. Therefore, the detection mechanism 7 can perform high-precision end point detection. [Explanation of symbols]

[0046] 2... Object to be polished 3... Polishing pad 3A: Polished surface 3B: Window for detecting end point 3C... Polishing layer 7... Detection mechanism L1: Inspection light L2: Reflected light

Claims

1. A polishing pad comprising: a polishing layer for polishing an object to be polished; and an end point detection window provided in the polishing layer for transmitting an inspection light to be irradiated onto the object to be polished and a light reflected from the object to be polished, the end point of a polishing process being detectable based on the light reflected from the object to be polished, The polishing pad is characterized in that a material having an Abbe number vD of 38.1 to 42.2 calculated from Formula 1 based on the refractive indices nD, nF, and nC of the reflected light at the NaD line having a wavelength of 589 nm, the NaF line having a wavelength of 486 nm, and the NaC line having a wavelength of 656 nm is used as the end point detection window. Abbe number vD=(nD−1) / (nF−nC) Formula 1

2. The polishing pad described in claim 1, characterized in that a material is used for the end point detection window, the difference between the refractive index nF at the NaF line with a wavelength of 486 nm and the refractive index nC at the NaC line with a wavelength of 656 nm being 0.0124 to 0.0147.

Citation Information

Patent Citations

  • Polishing pad

    JP2003048151A

  • Polishing pad

    JP2007044814A

  • Polishing pad with excellent airtightness

    JP2020516474A