Stainless steel material for solid oxide fuel cells, method for forming oxide film, solid oxide fuel cell member, and solid oxide fuel cell
A stainless steel material with controlled oxide film composition and formation process addresses conductivity and adhesion issues in low-temperature solid oxide fuel cells, ensuring excellent performance and durability.
Patent Information
- Application Number
- JP2021036741
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-03-08
AI Technical Summary
Conventional stainless steel materials used in high-temperature solid oxide fuel cells experience decreased electrical conductivity and poor adhesion of conductive coating layers at lower operating temperatures due to rapid oxide film growth and mismatched thermal expansion coefficients, particularly in low-Cr content stainless steels.
A stainless steel material with controlled oxide film composition and formation process, including specific elemental ranges and oxidation heat treatment, forms a spinel-type oxide film with optimized thermal expansion and conductivity properties, enhancing adhesion to conductive coating layers.
The solution provides stainless steel materials with excellent conductivity and adhesion to conductive coating layers at temperatures below 600°C, suitable for low-temperature solid oxide fuel cells, improving performance and durability.
Smart Images

Figure 0007579721000003 
Figure 0007579721000004 
Figure 0007579721000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a stainless steel material for solid oxide fuel cells, a method for forming an oxide film, a solid oxide fuel cell member, and a solid oxide fuel cell. [Background technology]
[0002] Conventional solid oxide fuel cells (SOFCs) are of the high-temperature operation type, with operating temperatures exceeding 600°C. However, in recent years, low-temperature operation type solid oxide fuel cells that operate in a temperature range of 600°C or less have been proposed (for example, Patent Documents 1 and 2). Stainless steel materials are generally used as components of such solid oxide fuel cells from the viewpoints of cost, corrosion resistance, and the like.
[0003] Solid oxide fuel cells have been developed primarily as stationary power sources, but in recent years, their use is expected to expand to a variety of mobile devices, including commercial and industrial vehicles, automobiles, and airplanes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-53388 A [Patent Document 2] Patent No. 6696992 Summary of the Invention [Problem to be solved by the invention]
[0005] The components that make up a solid oxide fuel cell (e.g., separators, interconnectors, current collectors, etc.) are required to be electrically conductive. However, the electrical conductivity of these components decreases as the operating temperature decreases, so the electrical conductivity of the components used in conventional high-temperature operating solid oxide fuel cells may not be sufficient. In addition, in order to ensure electrical conductivity, the member has a conductive coating layer formed on the surface of the base made of stainless steel. However, in stainless steel with a low Cr content (e.g., Cr content less than 22 mass%), the oxide film grows faster than in stainless steel with a high Cr content (e.g., Cr content 22 mass% or more), and the adhesion of the conductive coating layer is likely to decrease. In addition, the oxide film (layer containing Cr2O3) formed on the surface of the stainless steel has a large difference in thermal expansion coefficient from the conductive coating layer, so the conductive coating layer is likely to peel off.
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a stainless steel material for solid oxide fuel cells that has excellent electrical conductivity at temperatures of 600° C. or less and excellent adhesion to a conductive coating layer, and a method for forming an oxide film. Another aim of the present invention is to provide a solid oxide fuel cell member and a solid oxide fuel cell that include a stainless steel material for solid oxide fuel cells having such characteristics. [Means for solving the problem]
[0007] As a result of extensive research into stainless steel materials, the inventors have discovered that the above problems can be solved by controlling the composition of the base material and the oxide film on its surface to specific compositions, and have thus completed the present invention. That is, the present invention relates to a composition comprising, on a mass basis, C: More than 0% 0.050% or less, Si: More than 0% 1.50% or less, Mn: More than 0% 1.00% or less, P: More than 0% 0.050% or less, S: More than 0% 0.0300% or less, Cr: 10.5% or more but less than 22.0%, Mo: More than 0% 3.00% or less, N: More than 0% 0.030% or less, Al: More than 0% 0.30% or less, Nb: More than 0% 1.00% or less, Ti: More than 0% 1.00% or less, Ni: More than 0% 1.00% or less, Cu: More than 0%A stainless steel material for a solid oxide fuel cell, comprising a base material containing 1.00% or less of Cu, with the balance being Fe and impurities, and an oxide film formed on a surface of the base material, The oxide film is It has an outermost layer containing a spinel-type oxide, In the element concentration profile in the depth direction by glow discharge optical emission spectrometry, The oxide film is defined as a film extending from the surface to a depth where the O concentration is 10%. This stainless steel material for solid oxide fuel cells has a maximum peak concentration of Cr of 30.0 mass% or more, and a total maximum peak concentration of Al and Si of more than 1.5 mass% and less than 10.0 mass%, when the total amount of cationic elements excluding O, C, and N is 100 mass%.
[0008] The present invention also provides a method for producing a semiconductor device comprising the steps of: In the production of the stainless steel material for solid oxide fuel cells, a method for forming an oxide film on a surface of a base material, comprising the steps of: By mass, C: More than 0% 0.050% or less, Si: More than 0% 1.50% or less, Mn: More than 0% 1.00% or less, P: More than 0% 0.050% or less, S: More than 0% 0.0300% or less, Cr: 10.5% or more but less than 22.0%, Mo: More than 0% 3.00% or less, N: More than 0% 0.030% or less, Al: More than 0% 0.30% or less, Nb: More than 0% 1.00% or less, Ti: More than 0% 1.00% or less, Ni: More than 0% 1.00% or less, Cu: More than 0% Cold-rolled material containing 1.00% or less, with the balance being Fe and impurities. is used as the base material, and the cold-rolled material The material is subjected to an oxidation heat treatment at 300 to 1000°C for 1000 hours or less in a gas having a dew point of -30°C or less and containing O2 and at least one selected from CO, CO2, Ar, N2 and H2. Who It is law.
[0009] The present invention also relates to a solid oxide fuel cell member comprising the above-mentioned stainless steel material for solid oxide fuel cells. Furthermore, the present invention relates to a solid oxide fuel cell comprising the solid oxide fuel cell member. Effect of the Invention
[0010] According to the present invention, it is possible to provide a stainless steel material for solid oxide fuel cells, which has excellent electrical conductivity at temperatures of 600° C. or less and excellent adhesion to a conductive coating layer, and a method for forming an oxide film. Furthermore, according to the present invention, it is possible to provide a solid oxide fuel cell member and a solid oxide fuel cell comprising the stainless steel material for solid oxide fuel cells having such characteristics. [Brief description of the drawings]
[0011] [Figure 1] 1 shows the results of glow discharge optical emission spectroscopy (element concentration profile in the depth direction) in Test No. 10 of the embodiment. [Diagram 2] FIG. 2 is a schematic top view of a test piece for measuring electrical conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention. In this specification, the "%" designation for components means "% by mass" unless otherwise specified.
[0013] A stainless steel material for a solid oxide fuel cell according to an embodiment of the present invention (hereinafter, abbreviated as "stainless steel material") has a base material and an oxide film formed on the surface of the base material. The base material has a composition containing C: 0.050% or less, Si: 1.50% or less, Mn: 1.00% or less, P: 0.050% or less, S: 0.0300% or less, Cr: 10.5% or more and less than 22.0%, Mo: 3.00% or less, N: 0.030% or less, Al: 0.30% or less, Nb: 1.00% or less, Ti: 1.00% or less, Ni: 1.00% or less, Cu: 1.00% or less, with the balance being Fe and impurities. Here, the "impurities" refer to components (such as inevitable impurities) that are mixed in due to raw materials such as ore and scrap, and various factors in the manufacturing process when industrially manufacturing stainless steel materials, and are those that are allowed within a range that does not adversely affect the present invention. Also, the "stainless steel material" is a concept that includes various shapes such as stainless steel strips, stainless steel plates, and stainless steel foils.
[0014] Further, the base material can further contain one or more selected from B: 0.0100% or less, V: 1.00% or less, Sn: 0.50% or less, W: 2.0% or less, Ca: 0.010% or less, Mg: 0.010% or less, Zr: 1.00% or less, Co: 2.0% or less, Ga: 0.01% or less, Hf: 0.10% or less, REM: 0.10% or less as required.
[0015] <C: 0.050% or less> C is an element that affects the conductivity of the stainless steel material at a temperature of 600°C or lower. If the C content is too high, the conductivity decreases. Therefore, the C content is 0.050% or less, preferably 0.030% or less, more preferably 0.020% or less. On the other hand, the lower limit of the C content is not particularly limited, but the lower the C content, the more time is required for the refining process, and the manufacturing cost may increase. Therefore, the C content is preferably 0.0002% or more, more preferably 0.0005% or more.
[0016] <Si: 1.50% or less> Si is an element effective for suppressing Fe enrichment in the oxide film (especially spinel-type oxide film) and improving conductivity. However, if the Si content is too high, a continuous oxide of SiO2 may be formed at the interface of the stainless steel material, resulting in a decrease in conductivity and a possible decrease in toughness due to hardening. Therefore, the Si content is 1.50% or less, preferably 1.30% or less, more preferably 1.00% or less, still more preferably 0.80% or less. On the other hand, the lower limit of the Si content is not particularly limited. From the viewpoint of obtaining the above effects of Si, the Si content is preferably 0.05% or more, more preferably 0.08% or more.
[0017] <Mn: Below 1.00%> Mn is an element effective in improving the electrical conductivity of the oxide film at temperatures of 600°C or lower and the adhesion to the conductive coating layer by forming a first layer containing a spinel-type oxide (e.g., (Fe,Cr,Mn)3O4-type oxide) on the outermost surface of the oxide film. Also, Mn is an element that improves the toughness of the stainless steel material. However, if the Mn content is too high, the heat resistance may decrease. Therefore, the Mn content is 1.00% or less, preferably 0.80% or less. On the other hand, the lower limit of the Mn content is not particularly limited. From the viewpoint of obtaining the above effects by Mn, the Mn content is preferably 0.05% or more, more preferably 0.08% or more.
[0018] <P: Below 0.050%> P is an element that may reduce the toughness of the stainless steel material. Therefore, the P content is 0.050% or less, preferably 0.040% or less. On the other hand, the lower limit of the P content is not particularly limited, but the more the P content is reduced, the more time is required for the refining process, and the manufacturing cost may increase. Therefore, the P content is preferably 0.001% or more, more preferably 0.010% or more.
[0019] <S: Below 0.0300%> S is an element that may generate sulfide-based inclusions and reduce the power generation efficiency of the SOFC due to evaporation and poisoning of the electrodes. Therefore, the S content is 0.0300% or less, preferably 0.0100% or less, more preferably 0.0050% or less. On the other hand, the lower limit of the S content is not particularly limited, but the more the S content is reduced, the more time is required for the refining process, and the manufacturing cost may increase. Therefore, the S content is preferably 0.0001% or more, more preferably 0.0002% or more.
[0020] <Cr: 10.5% or more and less than 22.0%> Cr is a major element for forming a passive film (oxide film) on the surface of stainless steel materials, and properties such as corrosion resistance and heat resistance can be improved by the oxide film. From the viewpoint of forming an oxide film with excellent conductivity at temperatures below 600 °C, the Cr content is 10.5% or more, preferably 13.0% or more. On the other hand, if the Cr content is too high, Cr2O3 with a coefficient of thermal expansion smaller than that of the conductive coating layer is generated on the outermost layer, resulting in a decrease in the adhesion to the conductive coating layer. Therefore, the Cr content is less than 22.0%, preferably 21.0% or less.
[0021] <Mo: 3.00% or less> Mo is a major element for strengthening the oxide film of stainless steel materials, and properties such as corrosion resistance and heat resistance can be improved by the oxide film. Also, Mo is an element that promotes the formation of the oxide film of stainless steel materials and improves conductivity. Usually, since the Cr oxide constituting the oxide film contains Fe, although the conductivity is low, the conductivity can be improved by the presence of Mo in the Cr oxide. However, if the Mo content is too high, properties such as toughness may be impaired due to hardening. Therefore, the Mo content is 3.00% or less, preferably 2.50% or less, more preferably 1.50% or less. On the other hand, the lower limit of the Mo content is not particularly limited. From the viewpoint of obtaining the above effects of Mo, the Mo content is preferably 0.05% or more, more preferably 0.30% or more.
[0022] <N: 0.030% or less> N is an element that may combine with Al to form AlN, which is a starting point for abnormal oxidation, and may reduce the toughness of stainless steel materials. Therefore, the N content is 0.030% or less, preferably 0.025% or less. On the other hand, the lower limit of the N content is not particularly limited, but the lower the N content, the more time is required for the refining process, and the manufacturing cost may increase. Therefore, the N content is preferably 0.001% or more, more preferably 0.010% or more.
[0023] <Al: 0.30% or less> Al is an element effective in suppressing Fe enrichment in the oxide film (especially the first layer containing a spinel-type oxide film) and improving conductivity. However, if the Al content is too high, a continuous oxide layer of Al2O3 is formed, resulting in a decrease in conductivity. In addition, AlN, which is a starting point for abnormal oxidation, is likely to be generated, and the toughness of the stainless steel material may be impaired. Therefore, the Al content is 0.30% or less, preferably 0.25% or less. On the other hand, the lower limit of the Al content is not particularly limited. From the viewpoint of obtaining the above effects of Al, the Al content is preferably 0.01% or more, more preferably 0.03% or more.
[0024] <Nb: 1.00% or less> Similar to Ti, Nb preferentially binds to C and N to form Nb carbonitride, so it is an element effective for purifying the stainless steel material. Therefore, Nb promotes the formation of the oxide film and contributes to the improvement of conductivity. In addition, Nb is also an element that suppresses the decrease in corrosion resistance due to the formation of Cr carbonitride. However, if the Nb content is too high, the amount of solid-solution Nb that has not been consumed in the formation of Nb carbonitride increases. As a result, the toughness may be impaired due to hardening. Therefore, the Nb content is 1.00% or less, preferably 0.50% or less. On the other hand, the lower limit of the Nb content is not particularly limited. From the viewpoint of obtaining the above effects of Nb, the Nb content is preferably 0.01% or more, more preferably 0.05% or more.
[0025] <Ti: 1.00% or less> Like Nb, Ti preferentially combines with C and N to form Ti carbonitrides, making it an element effective for purifying stainless steel materials. Therefore, Ti promotes the formation of the oxide film and contributes to the improvement of conductivity. Also, Ti is an element that suppresses the decrease in corrosion resistance due to the formation of Cr carbonitrides. However, if the Ti content is too high, the Ti carbonitrides will coarsen, which will serve as a starting point for a decrease in toughness. Therefore, the Ti content should be 1.00% or less, preferably 0.50% or less. On the other hand, the lower limit of the Ti content is not particularly limited. From the perspective of obtaining the above effects of Ti, the Ti content is preferably 0.01% or more, more preferably 0.05% or more.
[0026] <Ni: 1.00% or less> Ni is an element that improves the corrosion resistance of stainless steel materials and suppresses the decrease in toughness. However, since Ni is an austenite phase stabilizing element, if the Ni content is too high, the coefficient of thermal expansion will increase and the adhesion between the oxide film and the conductive coating layer will decrease. Therefore, the Ni content should be 1.00% or less, preferably 0.80% or less. On the other hand, the lower limit of the Ni content is not particularly limited. From the perspective of obtaining the above effects of Ni, the Ni content is preferably 0.01% or more, more preferably 0.05% or more.
[0027] <Cu: 1.00% or less> Cu is an element that improves the corrosion resistance and conductivity of stainless steel materials. However, since Cu is an austenite phase stabilizing element, if the Cu content is too high, the coefficient of thermal expansion will increase and the adhesion between the oxide film and the conductive coating layer will decrease. Therefore, the Cu content is 1.00% or less, preferably 0.80% or less. On the other hand, the lower limit of the Cu content is not particularly limited. From the perspective of obtaining the above effects of Cu, the Cu content is preferably 0.01% or more, more preferably 0.03% or more.
[0028] <B: 0.0100% or less> B is an element effective for improving the secondary workability by enhancing the grain boundary strength through preferential enrichment at grain boundaries and is contained in the stainless steel material as required. However, when the B content becomes excessive, the boride (Cr2B) at the grain boundary coarsens, thereby reducing the adhesion between the oxide film and the conductive coating layer. Therefore, the B content is 0.0100% or less, preferably 0.0030% or less. On the other hand, the lower limit of the B content is not particularly limited. From the viewpoint of obtaining the effect of B, the B content is preferably 0.0002% or more, more preferably 0.0005% or more.
[0029] <V: 1.00% or less> V is an element that improves the strength without impairing the toughness of the stainless steel material and is contained in the stainless steel material as required. However, if the V content is too high, it forms a low-melting-point complex oxide, significantly reducing the oxidation resistance and increasing the cost. Therefore, the V content is 1.00% or less, preferably 0.50% or less. On the other hand, the lower limit of the V content is not particularly limited. From the viewpoint of obtaining the effect of V, the V content is preferably 0.01% or more, more preferably 0.05% or more.
[0030] <Sn: 0.50% or less> Sn is an element effective for improving the corrosion resistance and conductivity and is contained in the stainless steel material as required. However, if the Sn content is too high, the hot workability and toughness decrease. Therefore, the Sn content is 0.50% or less, preferably 0.30% or less. On the other hand, the lower limit of the Sn content is not particularly limited. From the viewpoint of obtaining the effect of Sn, the Sn content is preferably 0.01% or more, more preferably 0.05% or more.
[0031] <W: 2.0% or less> W is an element that improves the strength of stainless steel without impairing its toughness and is contained in the stainless steel as required. However, if the W content is too high, the workability and toughness may decrease, and the cost may increase. Therefore, the W content should be 2.0% or less, preferably 0.5% or less. On the other hand, the lower limit of the W content is not particularly limited. From the viewpoint of obtaining the effect of W, the W content is preferably 0.01% or more, more preferably 0.05% or more.
[0032] <Ca: 0.010% or less> Ca is an element that fixes S to enhance oxidation resistance and promotes the formation of an oxide film and is contained in the stainless steel as required. However, if the Ca content is too high, the amount of inclusions generated will increase and the conductivity will decrease. Therefore, the Ca content should be 0.010% or less, preferably 0.005% or less. On the other hand, the lower limit of the Ca content is not particularly limited. From the viewpoint of obtaining the effect of Ca, the Ca content is preferably 0.0005% or more, more preferably 0.001% or more.
[0033] <Mg: 0.010% or less> Mg is an element effective for refining stainless steel and is contained in the stainless steel as required. However, if the Mg content is too high, the amount of inclusions generated will increase and the conductivity will decrease. Therefore, the Mg content should be 0.010% or less, preferably 0.005% or less. On the other hand, the lower limit of the Mg content is not particularly limited. From the viewpoint of obtaining the effect of Mg, the Mg content is preferably 0.0001% or more, more preferably 0.0005% or more.
[0034] <Zr: 1.00% or less> Zr is an element effective for purifying stainless steel by fixing C and is included in the stainless steel as needed. However, if the Zr content is too high, the workability of the stainless steel will deteriorate. Therefore, the Zr content is 1.00% or less, preferably 0.50% or less. On the other hand, the lower limit of the Zr content is not particularly limited. From the viewpoint of obtaining the effect of Zr, the Zr content is preferably 0.001% or more, more preferably 0.005% or more.
[0035] <Co: 2.0% or less> Co is an element that improves the strength of stainless steel without impairing its toughness and is included in the stainless steel as needed. However, if the Co content is too high, there is a risk of deterioration in workability and toughness, and the cost will increase. Therefore, the Co content is 2.0% or less, preferably 0.5% or less. On the other hand, the lower limit of the Co content is not particularly limited. From the viewpoint of obtaining the effect of Co, the Co content is preferably 0.01% or more, more preferably 0.05% or more.
[0036] <Ga: 0.01% or less> Ga is an element that improves the hot workability of stainless steel and is included in the stainless steel as needed. However, if the Ga content is too high, the manufacturability will deteriorate. Therefore, the Ga content is 0.01% or less, preferably 0.005% or less. On the other hand, the lower limit of the Ga content is not particularly limited. From the viewpoint of obtaining the effect of Ga, the Ga content is preferably 0.0001% or more, more preferably 0.0005% or more.
[0037] <Hf: 0.10% or less> Hf is an element effective for purifying stainless steel by fixing C and is included in the stainless steel as needed. However, if the Hf content is too high, the workability of the stainless steel will deteriorate. Therefore, the Hf content is 0.10% or less, preferably 0.08% or less. On the other hand, the lower limit of the Hf content is not particularly limited. From the viewpoint of obtaining the effect of Hf, the Hf content is preferably 0.001% or more, more preferably 0.005% or more.
[0038] <REM:Less than 0.10%> Since REM (rare earth elements) preferentially binds to S and P to form compounds, it is possible to suppress the decrease in conductivity due to S and P. REM is contained in the stainless steel material as required. However, if the REM content is too high, the stainless steel material may be hardened, and the toughness and workability may be reduced. Therefore, the REM content is 0.10% or less, preferably 0.08% or less. On the other hand, the lower limit of the REM content is not particularly limited. From the viewpoint of obtaining the effect of REM, the REM content is preferably 0.001% or more, more preferably 0.005% or more. Note that REM refers to the general term for two elements, scandium (Sc) and yttrium (Y), and 15 elements (lanthanoids) from lanthanum (La) to lutetium (Lu). These may be used alone or as a mixture. Among REM, La and Y are preferred.
[0039] The base material preferably satisfies the following formula (1). 15% ≦ 55 + 32Mn - Cr - 84Al < 50% ··· (1) In the formula, each element symbol represents the content of each element. By using a base material that satisfies formula (1), a first layer containing a spinel-type oxide (for example, (Fe, Cr, Mn)3O4-type oxide) is formed on the outermost layer of the oxide film, and the Fe concentration in the spinel-type oxide is small, and at a temperature of 600°C or lower, a good oxidation resistance with a parabolic rate constant (log Kp) of the total thickness of the oxide film less than -16.0 can be exhibited. If the lower limit of formula (1) is less than 15%, the formation of the spinel-type oxide is suppressed, and the adhesion between the oxide film and the conductive coating layer is likely to decrease. On the other hand, if the upper limit of formula (1) is 50% or more, the growth of the oxide film is fast, so the oxide film becomes thick and the conductivity is likely to decrease. The upper limit value of formula (1) is preferably 45%, more preferably 40%. Also, the lower limit value of formula (1) is preferably 18%, more preferably 20%.
[0040] In the element concentration profile in the depth direction by glow discharge optical emission spectroscopy (hereinafter referred to as "GDS"), when the total amount of cationic elements excluding O, C, and N is taken as 100%, the oxide film has a maximum peak concentration of Cr of 30.0% or more and a total maximum peak concentration of Al and Si of more than 1.5% and less than 10.0%. By setting the maximum peak concentration of Cr to 30.0% or more, there are locations where Cr exists at a high concentration, and therefore the electrical conductivity can be increased at temperatures of 600° C. or less. From the viewpoint of stably ensuring such an effect, the maximum peak concentration of Cr is preferably 40.0% to 90.0%. Furthermore, by setting the total of the maximum peak concentrations of Al and Si to more than 1.5 mass% and less than 10.0 mass%, it is possible to suppress Fe concentration in the first layer of the oxide film and increase the electrical conductivity at temperatures equal to or lower than 600° C. From the viewpoint of stably ensuring such effects, the total of the maximum peak concentrations of Al and Si is preferably 2.0% to 9.0%.
[0041] The oxide film can have a first layer containing a spinel-type oxide (e.g., an (Fe, Cr, Mn) 3 O 4 type oxide) as the outermost layer. By forming the first layer containing a spinel-type oxide as the outermost layer, the difference in thermal expansion coefficient with respect to the conductive coating layer is reduced, thereby improving adhesion to the conductive coating layer. In addition, since spinel-type oxides and Cr 2 O 3 have similar electrical conductivity, electrical conductivity at temperatures of 600°C or less can be improved. Note that when the first layer contains Cr 2 O 3, the difference in thermal expansion coefficient with respect to the conductive coating layer is large, making the conductive coating layer more likely to peel off. The thickness of the outermost layer (first layer) of the oxide film is not particularly limited, but from the viewpoint of ensuring stable adhesion with the conductive coating layer, it is preferably 5 nm or more, more preferably 20 to 200 nm.
[0042] The oxide film may further have a second layer below the first layer. The second layer is not particularly limited, but preferably contains (Fe,Cr)2O3 or Cr2O3, and more preferably contains Cr2O3. The thickness of the second layer of the oxide film is not particularly limited, but is preferably 15 to 100 nm.
[0043] The structure of the oxide film can be identified by analyzing the composition of the oxide film by GDS. Here, the oxide film can be defined as the depth from the surface where the O concentration is 10% in the element concentration profile in the depth direction by GDS, and this depth can be regarded as the thickness of the oxide film. In addition, the first layer of the oxide film can be defined as the depth from the surface to the midpoint between the maximum value and the minimum value when the concentration profile of Fe or Mn has a maximum value in the oxide film in the element concentration profile in the depth direction by GDS, and this depth can be regarded as the thickness of the first layer. In addition, when both Fe and Mn have a maximum value, the one with a greater depth from the surface is regarded as the first layer of the oxide film, and this depth is regarded as the thickness of the first layer. In addition, the second layer of the oxide film can be defined as the part of the oxide film excluding the first layer, and the value obtained by subtracting the thickness of the first layer of the oxide film from the thickness of the oxide film can be regarded as the thickness of the second layer.
[0044] The shape of the stainless steel material according to the embodiment of the present invention is not particularly limited, but is preferably a plate or foil. When the stainless steel material is a plate or foil, its thickness is, for example, 0.1 to 5.0 mm, preferably 0.1 to 3.0 mm, more preferably 0.1 to 1.0 mm, and even more preferably 0.1 to 0.5 mm.
[0045] The stainless steel material according to the embodiment of the present invention can be produced in accordance with a known method, except that a slab having the above-mentioned composition is used. Here, an example of a typical method for producing a stainless steel material according to an embodiment of the present invention will be described. Note that the stainless steel material according to the embodiment of the present invention is not limited to the following production method.
[0046] The stainless steel material according to the embodiment of the present invention can be manufactured by hot rolling a slab having the above composition, followed by cold rolling to obtain a cold-rolled material, and then subjecting the cold-rolled material to an oxidation heat treatment. The conditions for hot rolling and cold rolling are not particularly limited and may be appropriately adjusted depending on the composition. The cold-rolled material may be subjected to annealing, pickling, or the like.
[0047] The oxidizing heat treatment is carried out on the cold-rolled material under conditions where the dew point is -30°C or lower and the gas contains O2 and at least one selected from CO, CO2, Ar, N2 and H2 (e.g., air) at 300 to 1000°C for 1000 hours or less. By carrying out the oxidizing heat treatment under such conditions, it is possible to stably form an oxide film having the above-mentioned properties, in particular the first layer containing a spinel-type oxide.
[0048] The stainless steel material according to the embodiment of the present invention has an oxide film with a specific composition, and therefore has excellent electrical conductivity and adhesion to a conductive coating layer at temperatures of 600° C. or less. Therefore, the stainless steel material according to the embodiment of the present invention is suitable for use in solid oxide fuel cells, particularly low-temperature solid oxide fuel cells that operate in a temperature range of 600° C. or less (e.g., 500 to 600° C.).
[0049] When the stainless steel material according to the embodiment of the present invention is used in a solid oxide fuel cell, the stainless steel material can be used for members such as separators, current collectors (e.g., air electrode current collectors and anode current collectors), interconnectors, bus bars, end plates, anode frames, etc. Among these, the stainless steel material according to the embodiment of the present invention is preferably used for one or more members selected from separators, interconnectors, and current collectors.
[0050] The solid oxide fuel cell member according to the embodiment of the present invention comprises the stainless steel material according to the embodiment of the present invention. Also, the solid oxide fuel cell according to the embodiment of the present invention comprises the solid oxide fuel cell member according to the embodiment of the present invention. The solid oxide fuel cell member is not particularly limited, and examples thereof include the various members described above. The stainless steel material can be appropriately shaped to match the shape of various components. A conductive coating layer may be formed on the surface of the stainless steel material. The conductive coating layer is not particularly limited and can be formed from a material known in the art. For example, the conductive coating layer can be formed using a metal with excellent conductivity, such as Ag or Co. The conductive coating layer may be a layer of a single metal or a layer of an alloy, and may have a single-layer structure or a multilayer structure. Examples of alloys include MnCo2O4 and TiN. In order to improve adhesion to the conductive coating layer, the stainless steel material may be modified (roughened) by modifying the oxide film. For example, the oxide film may be modified (roughened) by a known method such as immersing the stainless steel material in a hydrofluoric / nitric acid solution. EXAMPLES
[0051] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these.
[0052] A slab having the composition shown in Table 1 was melted and hot rolled to form a hot-rolled stainless steel sheet having a thickness of 3.5 mm, which was then annealed and pickled. The hot-rolled sheet was then cold rolled to form a cold-rolled stainless steel sheet having a thickness of 0.3 mm, which was then annealed and pickled. The cold-rolled stainless steel sheet was then subjected to an oxidation heat treatment in dry air with a dew point of -40°C to obtain a stainless steel material having an oxide film on the surface. Details of the oxidation heat treatment are shown in Table 2. [Table 1]
[0053] Next, the obtained stainless steel material was subjected to glow discharge optical emission spectroscopy (GDS). In the element concentration profile in the depth direction obtained by this analysis, the maximum peak concentration of Cr (represented as "Cr" in Table 2) and the sum of the maximum peak concentrations of Al and Si (represented as "Al+Si" in Table 2) were determined when the total amount of cationic elements excluding O, C, and N was taken as 100 mass%. The GDS analysis was carried out under the conditions of Ar gas pressure 600 Pa, power 35 W, frequency 100 Hz, and duty cycle 0.25. As an example, the element concentration profile in the depth direction in Test No. 10 is shown in Figure 1. In the element concentration profile in the depth direction shown in Figure 1, the signal intensity is expressed in terms of cation fraction. In addition, only Fe, Si, Mn, Cr, and Al were selected as elements, and the cation fractions of Si and Al were both multiplied by 10.
[0054] In addition, the first and second layers of the oxide film were identified using X-ray diffraction measurements, and it was confirmed that the first layer was a layer containing a spinel-type oxide (Fe, Cr, Mn)3O4 type oxide, and the second layer was a layer containing Cr2O3.
[0055] Furthermore, the obtained stainless steel material was evaluated for electrical conductivity and adhesion to a conductive coating layer. The evaluation methods were as follows. (1) Conductivity A conductive coating layer was formed on the stainless steel material by coating treatment. The coating treatment was adjusted so that a Co plating was formed with a thickness of 2 to 5 μm. Two stainless steel sheets on which a conductive coating layer was formed (hereinafter referred to as "stainless steel sheets with a conductive coating layer") were thermally exposed to 600°C for 1000 hours in an atmosphere adjusted to humidified air (H2O concentration: approximately 2.3%) with a dew point of 20°C, and then these two stainless steel sheets with a conductive coating layer were used to prepare a test piece for measurement as shown in Figure 2, and measurements were performed by the four-terminal method using a potentiostat. Specifically, the measurements were performed as follows. First, a conductive paste (Ag paste) was applied in a square shape (10 mm on one side, 10 μm thick) to the center of two stainless steel materials 10 with a conductive coating layer, and dried to form a conductive part 20. Next, the conductive parts 20 of the two stainless steel materials 10 with a conductive coating layer were stacked and arranged in a cross shape, then sandwiched between alumina plates, a weight (200 g) was placed on top, and the conductive part 20 was baked in an electric furnace (600 ° C × 30 minutes). Next, the surface was scraped using a minitor until the metal base material was exposed, and the wiring attachment part 30 shown in FIG. 2 was formed. Next, a silver wire 40 (φ 0.3 mm) was wound around the wiring attachment part 30, a conductive paste was applied, and the test piece for measurement was obtained by drying at 150 ° C for 30 minutes. Next, this test piece for measurement was placed in a high-temperature electrochemical measurement device, and a voltage-current curve was obtained by a four-terminal method using a potentiostat. In this measurement, the measurement temperature was set to 600°C, and the voltage was swept up to 10 mV. The resistance value was calculated from the slope of the voltage-current curve. In this evaluation, the resistance value was 20 mΩ cm 2 If it is less than 20mΩ cm, it is classified as A (excellent high temperature conductivity). 2 Exceeding 50mΩ·cm 2 If the resistance is less than 50mΩ cm, it is classified as B (excellent high temperature conductivity). 2 If it exceeded the limit, it was judged as C (insufficient high temperature conductivity).
[0056] (2) Adhesion to the conductive coating layer (abbreviated as "adhesion" in Table 2) A conductive coating layer was formed by coating the stainless steel plate. The coating process was adjusted so that a Co plating was formed to a thickness of 2 to 5 μm on the surface of the surface-modified stainless steel material. The adhesion to the conductive coating layer was evaluated by repeatedly heating and cooling the stainless steel material with the conductive coating layer. Specifically, the stainless steel material with the conductive coating layer was cut to prepare a 10 mm x 25 mm test piece. Next, the test piece was placed in a moving muffle furnace heated to 800°C, held in the atmosphere for 25 minutes (in the muffle furnace), and an intermittent heating test was performed for 100 cycles, with one cycle being released to the atmosphere and cooled for 5 minutes (moving the muffle furnace). In the intermittent heating test, the case where the conductive coating layer did not peel off was judged as A (high coating adhesion), the case where the conductive coating layer did not peel off but cracks occurred was judged as B (insufficient coating adhesion), and the case where the conductive coating layer completely peeled off was judged as C (low coating adhesion). The results of the above evaluations are shown in Table 2.
[0057] [Table 2]
[0058] As shown in Table 2, the stainless steel materials of test Nos. 1 to 11 (examples of the present invention) were composed of a base material and an oxide film having a predetermined composition, and therefore had excellent electrical conductivity and adhesion to the conductive coating layer. However, Nos. 1 and 7 used a steel type with a composition outside the preferred range of formula (1), and therefore had reduced electrical conductivity or adhesion to the conductive coating layer. In contrast, the stainless steel materials of Test Nos. 12 to 15 (Comparative Examples) had compositions outside the range of the base material and oxide film, and therefore either or both of the electrical conductivity and the adhesion to the conductive coating layer were insufficient.
[0059] As can be seen from the above results, the present invention can provide a stainless steel material for solid oxide fuel cells and a method for forming an oxide film that has excellent electrical conductivity and adhesion to a conductive coating layer at temperatures of 600° C. or less. The present invention also can provide a solid oxide fuel cell member and a solid oxide fuel cell that include a stainless steel material for solid oxide fuel cells having such characteristics. [Explanation of symbols]
[0060] 10 Stainless steel material with conductive coating layer 20 Conductive part 30 Wiring attachment part 40 silver wire
Claims
1. A stainless steel material for a solid oxide fuel cell comprising: a base material containing, on a mass basis, C: more than 0.050% and less than 0.050%, Si: more than 0% and less than 1.50%, Mn: more than 0% and less than 1.00%, P: more than 0.050%, S: more than 0.0300%, Cr: 10.5% or more and less than 22.0%, Mo: more than 0% and less than 3.00%, N: more than 0% and less than 0.030%, Al: more than 0.30%, Nb: more than 0% and less than 1.00%, Ti: more than 0% and less than 1.00%, Ni: more than 0% and less than 1.00%, Cu: more than 0% and less than 1.00%, with the balance being Fe and impurities; and an oxide film formed on a surface of the base material, The oxide film has an outermost surface layer containing a spinel-type oxide, and in a depth direction element concentration profile by glow discharge optical emission spectroscopy, the oxide film extends from the surface to a depth where the O concentration is 10%, and when the total amount of cationic elements excluding O, C, and N is taken as 100 mass%, the stainless steel material for solid oxide fuel cells has a maximum peak concentration of Cr of 30.0 mass% or more and a sum of the maximum peak concentrations of Al and Si of more than 1.5 mass% and less than 10.0 mass%.
2. The stainless steel material for solid oxide fuel cells according to claim 1 , wherein the base material satisfies the following formula (1): 15% by mass≦55+32Mn-Cr-84Al<50% by mass... (1) In the formula, each element symbol represents the content of each element.
3. The stainless steel material for solid oxide fuel cells according to claim 1 or 2, wherein the base material further contains, by mass, one or more selected from B: more than 0% and not more than 0.0100%, V: more than 0% and not more than 1.00%, Sn: more than 0% and not more than 0.50%, W: more than 0% and not more than 2.0%, Ca: more than 0% and not more than 0.010%, Mg: more than 0% and not more than 0.010%, Zr: more than 0% and not more than 1.00%, Co: more than 0% and not more than 2.0%, Ga: more than 0% and not more than 0.01%, Hf: more than 0% and not more than 0.10%, and REM: more than 0% and not more than 0.10%.
4. The spinel oxide is (Fe, Cr, Mn) 3 O 4 The stainless steel material for solid oxide fuel cells according to any one of claims 1 to 3, which is a type oxide.
5. A method for forming an oxide film on a surface of a base material in the manufacture of a stainless steel material for a solid oxide fuel cell according to any one of claims 1 to 4, comprising the steps of: The base material is a cold-rolled material containing, on a mass basis, C: more than 0.050% and less than 0.050%, Si: more than 0% and less than 1.50%, Mn: more than 0% and less than 1.00%, P: more than 0.050%, S: more than 0.0300%, Cr: 10.5% or more and less than 22.0%, Mo: more than 0% and less than 3.00%, N: more than 0% and less than 0.030%, Al: more than 0.30%, Nb: more than 0% and less than 1.00%, Ti: more than 0% and less than 1.00%, Ni: more than 0% and less than 1.00%, Cu: more than 0% and less than 1.00%, with the balance being Fe and impurities. The base material has a dew point of -30°C or less and O 2 And CO, CO 2 , Ar, N 2 and H 2 and performing an oxidation heat treatment at 300 to 1000° C. for 1000 hours or less in a gas containing at least one selected from the group consisting of:
6. The method according to claim 5 , wherein the cold-rolled material satisfies the following formula (1): 15% by mass≦55+32Mn-Cr-84Al<50% by mass... (1) In the formula, each element symbol represents the content of each element.
7. The method according to claim 5 or 6, wherein the cold-rolled material further contains, by mass, one or more selected from B: more than 0% and not more than 0.0100%, V: more than 0% and not more than 1.00%, Sn: more than 0% and not more than 0.50%, W: more than 0% and not more than 2.0%, Ca: more than 0% and not more than 0.010%, Mg: more than 0% and not more than 0.010%, Zr: more than 0% and not more than 1.00%, Co: more than 0% and not more than 2.0%, Ga: more than 0% and not more than 0.01%, Hf: more than 0% and not more than 0.10%, and REM: more than 0% and not more than 0.10%.
8. A solid oxide fuel cell member comprising the stainless steel material for solid oxide fuel cells according to any one of claims 1 to 4.
9. 9. The solid oxide fuel cell member according to claim 8, further comprising a conductive coating layer provided on a surface of the stainless steel material for a solid oxide fuel cell.
10. A solid oxide fuel cell comprising the solid oxide fuel cell member according to claim 8 or 9.
Citation Information
Patent Citations
Surface treatment for stainless steel member
JP1993033117A
Surface treatment of stainless steel
JP1995268669A
Ferritic stainless steel sheet excellent in carburization and oxidation resistance, and method of manufacturing the same
JP2016183375A
Fuel cell system and operation method therefor and electrochemical system
JP2020053388A
Interconnects for low-temperature solid oxide fuel cells.
JP6696992B2