Graphene oxide dispersion and method for producing graphene oxide dispersion
The aqueous graphene oxide dispersion with controlled absorbance and O/C ratios, combined with high shear dispersion, addresses stacking and aggregation issues, resulting in stable and effective coating applications.
Patent Information
- Application Number
- JP2021062605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-08
- Filing Date
- 2021-04-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-04-01
AI Technical Summary
Graphene oxide dispersions in aqueous solutions tend to stack and aggregate due to hydrogen bonding, leading to poor coating properties and sedimentation over time.
An aqueous graphene oxide dispersion with a specific absorbance ratio of 230 nm to 270 nm (230 nm/270 nm) of 1.5 or more and an O/C ratio of 0.60 to 0.80, achieved by dispersing graphene oxide through a hole-shaped or slit-shaped gap with defined dimensions and using high shear forces to break hydrogen bonds.
The dispersion effectively prevents sedimentation and enhances coating properties by maintaining graphene oxide in a single or thin layer state, ensuring uniform application and improved adhesion.
Smart Images

Figure 0007582030000001 
Figure 0007582030000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a graphene oxide dispersion and a method for producing a graphene oxide dispersion. [Background technology]
[0002] Graphene oxide is a two-dimensional carbon sheet-like material synthesized from graphite. Graphene oxide is expected to exhibit excellent properties as a functional material such as a lubricant or catalyst. Graphene, which is being researched as a new energy material such as a battery material, is obtained by a reduction reaction of graphene oxide, and graphene oxide is also attracting attention as a raw material for reduced graphene oxide. In recent years, technology has also been attracting attention for forming graphene oxide and reduced graphene oxide into various shapes such as lines and sheets and applying them to wiring materials, separation membranes, etc.
[0003] In order to utilize graphene oxide industrially, methods for producing a dispersion of graphene oxide with excellent dispersibility have been investigated. For example, a method for obtaining a dispersion of graphene oxide by dispersing graphene oxide obtained by oxidizing graphite in a solvent (see, for example, Patent Document 1), and a method for exfoliating a layered mineral powder including an addition step of adding layered mineral powder and a salt to be dispersed in the organic solvent to an organic solvent and a mixing step of stirring the obtained mixture (see, for example, Patent Document 2) have been proposed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-79176 A [Patent Document 2] JP 2019-73401 A Summary of the Invention [Problem to be solved by the invention]
[0005] In order to expand the range of applications of graphene oxide, a technology for forming a graphene oxide dispersion into various shapes is required, and for this purpose, it is effective to prepare a dispersion in which graphene oxide is dispersed in a single layer or multiple thin layers. Since graphene oxide is hydrophilic, dispersing graphene oxide in water increases the interlayer distance between graphene oxide sheets, making it easy to make the graphene oxide in a thin layer state. However, in an aqueous dispersion, thin-layer graphene oxide is prone to stacking and aggregation, and further, since it has many functional groups, it is easy to form a strong hydrogen bond network between graphene oxides. Therefore, the graphene oxide dispersions and dispersion methods described in Patent Documents 1 and 2 have a problem of insufficient coatability.
[0006] Therefore, an object of the present invention is to provide a graphene oxide aqueous dispersion having excellent coatability. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides a graphene oxide aqueous dispersion in which graphene oxide is dispersed in water, wherein, when the graphene oxide concentration is adjusted to 0.0013% by weight, the graphene oxide aqueous dispersion has an absorbance at a wavelength of 230 nm of 0.6 or more and a ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) of 1.5 or more. Effect of the Invention
[0008] The graphene oxide aqueous dispersion of the present invention suppresses sedimentation of graphene oxide over time and has good coatability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Graphene oxide aqueous dispersion> The graphene oxide aqueous dispersion of the present invention is obtained by dispersing graphene oxide in water. By dispersing graphene oxide in water, the graphene oxide is made into a single or multiple thin layers, and the coatability can be improved. Here, the term "dispersed" in the present invention refers to a state in which no gelation is observed by visual observation of the graphene oxide aqueous dispersion, and when the graphene oxide aqueous dispersion is passed through a mesh filter having a line diameter of 160 μm and an opening diameter of 250 μm, no trapped matter is observed on the mesh filter by visual observation.
[0010] The graphene oxide aqueous dispersion of the present invention is characterized in that, when the graphene oxide concentration is adjusted to 0.0013% by weight, the absorbance at a wavelength of 230 nm is 0.6 or more, and the ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) is 1.5 or more.
[0011] In the present invention, as an index of dispersibility of graphene oxide, we focused on the absorbance when the graphene oxide concentration was adjusted to 0.0013 wt %. By adjusting the graphene oxide concentration to 0.0013 wt %, a suitable amount of graphene oxide is present in the liquid, and therefore noise can be suppressed and the absorbance can be measured with high accuracy.
[0012] The absorption spectrum of graphene oxide has a peak derived from aromatic rings at a wavelength of about 230 nm. The absorbance of graphene oxide changes depending on the exfoliation state of graphene oxide, with single-layer graphene oxide having the highest absorbance, and the absorbance decreases with an increase in the number of layers or the formation of aggregates. When the absorbance at a wavelength of 230 nm is less than 0.6, the degree of exfoliation of graphene oxide is low, and most of the graphene oxide is in a state of stacked and aggregated, and the graphene oxide settles in the dispersion liquid over time, resulting in a decrease in coatability. The absorbance of graphene oxide at a wavelength of 230 nm is preferably 0.65 or more, more preferably 0.70 or more, and even more preferably 0.75 or more. On the other hand, from the viewpoint of suppressing the viscosity of the graphene oxide dispersion liquid and improving the fluidity, the absorbance of graphene oxide at a wavelength of 230 nm is preferably 1.0 or less, and even more preferably 0.95 or less.
[0013] The absorption spectrum of graphene oxide has a peak at 230 nm, but since graphene oxide absorbs a wide range of light in the visible light region from 200 nm to 700 nm, there is a shoulder in the absorption spectrum at a wavelength of around 270 nm. When the hydrogen bond network between graphenes is strong, the aromatic rings tend to approach each other, and the peak of the graphene that is close to each other shifts to a longer wavelength side than 230 nm. The shoulder near the wavelength of 270 nm is thought to be due to this shift, and therefore, the stronger the hydrogen bond network between graphenes, the greater the absorbance at 270 nm. In other words, the ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) becomes smaller. As mentioned above, when the hydrogen bond network between graphenes is strong, graphene oxide tends to aggregate, and the coatability decreases. Therefore, in the present invention, it is preferable that the ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) is large, and the ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) when the graphene oxide concentration of the graphene oxide aqueous dispersion is adjusted to 0.0013 wt % needs to be 1.5 or more. The absorbance ratio (230 nm / 270 nm) is preferably 1.55 or more, more preferably 1.60 or more, and even more preferably 1.65 or more. On the other hand, from the viewpoint of increasing the contact points between graphene oxides and suppressing coating unevenness and smearing during coating, the absorbance ratio (230 nm / 270 nm) is preferably 1.90 or less, more preferably 1.85 or less, and even more preferably 1.80 or less.
[0014] The absorbance of the graphene oxide dispersion can be measured by the method described in Measurement Example 2 below. In addition, examples of means for adjusting the absorbance of the graphene oxide dispersion to fall within the above-mentioned range include a method for obtaining a graphene oxide dispersion by a production method described below.
[0015] The graphene oxide contained in the graphene oxide aqueous dispersion of the present invention preferably has an elemental ratio of oxygen to carbon (O / C ratio) of 0.60 or more and 0.80 or less, as measured by X-ray photoelectron spectroscopy. The oxygen atoms on the graphene oxide surface are oxygen atoms contained in the acidic groups of the graphene oxide. Since such oxygen atoms have the effect of further improving the dispersibility of the graphene oxide, when the O / C ratio of the graphene oxide is 0.60 or more, the dispersibility of the graphene oxide can be further improved and the coatability can be further improved. The O / C ratio of the graphene oxide is more preferably 0.65 or more. On the other hand, from the viewpoint of suppressing steric hindrance due to functional groups and further improving dispersibility, the O / C ratio of the graphene oxide is preferably 0.80 or less, more preferably 0.75 or less.
[0016] In X-ray photoelectron spectroscopy, the graphene oxide dispersion is pre-dried using a vacuum dryer or freeze dryer, and the dried sample is then introduced into a measurement room equipped with a high vacuum chamber. The surface of the sample placed in the ultra-high vacuum is irradiated with soft X-rays, and photoelectrons emitted from the surface are detected by an analyzer. These photoelectrons are measured using wide and narrow scans to determine the binding energy value of the bound electrons in the material, thereby obtaining elemental information on the material surface. Specifically, the O / C ratio of graphene oxide can be measured by the method described in Measurement Example 3 below.
[0017] When graphene oxide is measured by X-ray photoelectron spectroscopy, a C1s peak derived from carbon is detected at around 284 eV, but it is known that when carbon is bonded to oxygen, the peak shifts to the higher energy side. Specifically, peaks derived from C-C bonds, C=C double bonds, and CH bonds, in which carbon is not bonded to oxygen, are detected at around 284 eV without shifting, and in the case of C-O single bonds, the peaks shift to around 286.5 eV, in the case of C=O double bonds, the peaks shift to around 287.5 eV, and in the case of CO-O bonds, the peaks shift to around 288.5 eV. Therefore, the signal derived from carbon is detected in the form of overlapping peaks at around 284 eV, 286.5 eV, 287.5 eV, and 288.5 eV. At the same time, an O1s peak derived from oxygen is detected at around 533 eV. The O / C ratio can be calculated from the peak areas of the C1s peak and the O1s peak. The O / C ratio of graphene oxide can be adjusted to a desired range, for example, by the amount of oxidizing agent used during the production of graphene oxide.
[0018] <Method of manufacturing graphene oxide dispersion> The graphene oxide aqueous dispersion of the present invention can be prepared, for example, by a production method in which graphene oxide is dispersed in water. In the present invention, it is preferable to have a step of passing a slurry containing graphene oxide and water through a hole-like gap with an opening diameter of 0.1 mm to 3.0 mm or a slit-like gap with a width of 0.1 mm to 1.0 mm, which can eliminate stacks of graphene oxide particles and greatly improve dispersibility.
[0019] [Method of producing graphene oxide] Examples of the method for producing graphene oxide include the Hummers method. Alternatively, commercially available graphene oxide having a desired O / C ratio may be purchased. As an example of the method for producing graphene oxide, a method using the Hummers method is illustrated below.
[0020] In an ice bath, graphite (graphite powder) and sodium nitrate are added to concentrated sulfuric acid and stirred, and potassium permanganate is gradually added so as not to raise the temperature. The mixture is stirred for 0.2 to 5 hours while maintaining the temperature in the range of 25 to 50°C. Ion-exchanged water is then added to dilute the mixture into a suspension, which is stirred for 5 to 50 minutes at a temperature range of 80 to 100°C. Hydrogen peroxide and ion-exchanged water are then added and stirred for 1 to 30 minutes to obtain a graphene oxide aqueous dispersion. The obtained graphene oxide aqueous dispersion is filtered and washed to obtain a graphene oxide wet cake.
[0021] As the graphite, natural graphite is preferred, and the mesh number is preferably 5,000 or less. For 10 g of natural graphite, the amount of sodium nitrate added is preferably 2 to 8 g, the amount of concentrated sulfuric acid added is preferably 150 to 300 ml, the amount of potassium permanganate added is preferably 10 to 40 g, and the amount of hydrogen peroxide added is preferably 40 to 80 g, and the amount of ion-exchanged water added is preferably 10 to 20 times the amount of hydrogen peroxide added. The oxidation degree of graphene oxide can be adjusted to a desired range, for example, by the amount of sodium nitrate or potassium permanganate added as an oxidizing agent. Specifically, the ratio of the amount of sodium nitrate added to graphite (sodium nitrate / graphite) is preferably 0.200 or more and 0.800 or less, and the ratio of the amount of potassium permanganate added to graphite (potassium permanganate / graphite) is preferably 1.4 or more and 4.0 or less.
[0022] [Dispersion process] As described above, in the present invention, it is preferable to have a step of passing a slurry obtained by mixing graphene oxide wet cake with water through a hole-like gap having an opening diameter of 0.1 mm or more and 3.0 mm or less, or a slit-like gap having a width of 0.1 mm or more and 1.0 mm or less, which can eliminate stacks of graphene oxide particles and greatly improve dispersibility.
[0023] Examples of the shape of the hole-like gap include circular holes and polygonal holes such as square holes. The shape of the hole-like gap is preferably a square hole, and a square hole shape with a corner at the edge of the hole increases the shear force when the slurry passes through the gap, making it easier to peel off the stacked graphene oxide and cut the hydrogen bond network, thereby eliminating stacks of graphene oxide, and further improving dispersibility. A square hole is more preferable. Here, the opening diameter of the square hole in the present invention refers to the length of the short side. The shape of the square gap is preferably a long-short ratio (long side / short side) that is the ratio of the long side to the short side, which is the width, of 1.0 to 3.0. By setting the long-short ratio to 3.0 or less, the shear force applied to the graphene oxide dispersion during stirring of the slurry is increased, and dispersibility can be further improved. The long-short ratio of the square hole is more preferably 2.0 or less, and even more preferably 1.5 or less. On the other hand, the shape of the slit-like gap preferably has a long-short ratio (long side / short side), which is the ratio of the long side to the short side, which is the width, of 20 or more.
[0024] When the gap has an opening diameter of less than 0.1 mm or a width of less than 0.1 mm, the speed of passing through the gap during stirring of the slurry is slow, and the shear force applied to the graphene oxide dispersion is small, making it difficult to peel off the laminated graphene oxide or cut the hydrogen bond network. In addition, clogging of the gap of the graphene oxide wet cake occurs, making it difficult to pass the slurry through the gap. On the other hand, when the opening diameter exceeds 3.0 mm or the slit width exceeds 1.0 mm, the shear force applied to the graphene oxide dispersion is small, making it difficult to peel off the laminated graphene oxide or cut the hydrogen bond network. From the viewpoint of increasing the shear force applied to the graphene oxide dispersion passing through the gap during stirring of the slurry, the opening diameter is more preferably 2.0 mm or less, and even more preferably 1.0 mm or less. In particular, when the shape of the hole-like gap is circular, the shear force applied to the graphene oxide dispersion passing through the gap during stirring of the slurry tends to be smaller than that in the case of a corner hole shape having corners, so in the case of a round hole, the opening diameter is preferably 1.0 mm or less.
[0025] For example, when producing a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.1% by weight to 2.0% by weight, the dispersion step preferably includes a step of passing a slurry obtained by mixing a graphene oxide wet cake having a graphene oxide concentration of 40% by weight to 50% by weight with water through a hole-shaped gap having an opening diameter of 0.1 mm to 3.0 mm, more preferably an opening diameter of 0.1 mm to 1.0 mm, or a slit-shaped gap having a width of 0.1 mm to 1.0 mm. Regarding the size of the gap, by setting the opening diameter in the case of a hole-shaped gap and the width in the case of a slit-shaped gap to 0.1 mm or more, the speed of passing through the gap during stirring of the slurry is high and the shear force applied to the graphene oxide dispersion is large, making it easy to peel off the graphene oxide in a laminated state or to break the hydrogen bond network. In addition, clogging of the gap in the graphene oxide wet cake can be suppressed. The opening diameter or width is more preferably 0.5 mm or more. On the other hand, by setting the opening diameter in the case of a hole shape and the width in the case of a slit shape to 3.0 mm or less, more preferably 1.0 mm or less, stacks of graphene oxide particles can be more effectively eliminated and dispersibility can be further improved.
[0026] Dispersing machines having holes with an opening diameter of 0.1 mm to 3.0 mm or slit-like gaps with a width of 0.1 mm to 1.0 mm are preferably thin film rotating machines, rotor / stator machines, etc., with a short shape in which the distance between the rotating blade and the wall is 10 mm or less. Examples of such dispersing machines include "Filmix" (registered trademark) 30-30 type (Primix Corporation), "Clearmix" (registered trademark) CLM-0.8S (M Technique Co., Ltd.), and "Silverson Mixer" (registered trademark) L5M-A (Silverson Nippon Co., Ltd.).
[0027] In the step of passing a slurry obtained by mixing the graphene oxide wet cake with water through a hole-like gap having an opening diameter of 0.1 mm to 3.0 mm, more preferably 0.1 mm to 1.0 mm, or a slit-like gap having a width of 0.1 mm to 1.0 mm, the slurry is preferably stirred at a peripheral speed of 15 m / s or more. The higher the peripheral speed at which the slurry is passed through the gap, the more effectively the graphene oxide can be peeled off by shear force, and the more the dispersibility can be improved.
[0028] For example, when producing a graphene oxide aqueous dispersion with a lower concentration of 0.1 wt% or more and 0.6 wt% or less, the dispersion process preferably has two steps: (1) a step of passing a slurry obtained by mixing water with a graphene oxide wet cake having a graphene oxide concentration of 40 wt% or more and 50 wt% or less through hole-shaped gaps having an opening diameter of 0.1 mm or more and 3.0 mm or less, more preferably an opening diameter of 0.1 mm or more and 1.0 mm or less, or a slit-shaped gap having a width of 0.1 mm or more and 1.0 mm or less, to obtain a graphene oxide aqueous dispersion with a graphene oxide concentration of 0.8 wt% or more and 2.0 wt% or less; and (2) a step of passing the graphene oxide aqueous dispersion with a graphene oxide concentration of 0.8 wt% or more and 2.0 wt% or less through hole-shaped gaps having an opening diameter of 0.1 mm or more and 3.0 mm or less, more preferably an opening diameter of 0.1 mm or more and 1.0 mm or less, or a slit-shaped gap having a width of 0.1 mm or more and 1.0 mm or less. By going through two steps, the hydrogen bond network can be broken more efficiently, and the coatability of graphene oxide can be improved. In the step (1), the lower the viscosity of the slurry passed through the gap, the more effectively the graphene oxide can be peeled off. Therefore, it is more preferable to set the graphene oxide concentration in the graphene oxide aqueous dispersion obtained in the step (1) to 0.8 wt % or more and 1.5 wt % or less.
[0029] The size and shape of the gap in steps (1) and (2) and specific examples of the dispersing machine used in steps (1) and (2) are as described above.
[0030] In the step (1), as described above, in the step of passing a slurry obtained by mixing the graphene oxide wet cake with water through a hole-shaped gap having an opening diameter of 0.1 mm to 3.0 mm, more preferably a hole-shaped gap having an opening diameter of 0.1 mm to 1.0 mm, or a slit-shaped gap having a width of 0.1 mm to 1.0 mm, the slurry is preferably stirred at a peripheral speed of 15 m / s or more. In the step (2), the graphene oxide aqueous dispersion is preferably stirred at a peripheral speed of 15 m / s or more, since the graphene oxide aqueous dispersion is more effectively peeled off by shear force when the peripheral speed is higher when the graphene oxide aqueous dispersion is passed through the gap. In the step (2), the graphene oxide aqueous dispersion is preferably stirred at a peripheral speed of 15 m / s or more, since the graphene oxide aqueous dispersion is more effectively peeled off by shear force when the graphene oxide aqueous dispersion is passed through a hole-shaped gap having an opening diameter of 0.1 mm to 3.0 mm, more preferably a hole-shaped gap having an opening diameter of 0.1 mm to 1.0 mm, or a slit-shaped gap having a width of 0.1 mm to 1.0 mm. EXAMPLES
[0031] [Measurement Example 1: Graphene oxide wet cake or graphene oxide aqueous dispersion concentration] The graphene oxide wet cake or the graphene oxide aqueous dispersion was placed on an aluminum cup with a known weight, the weight was measured, and the solvent (water) was evaporated by heating for 1.5 hours on a hot plate adjusted to 100°C. The concentration of the graphene oxide wet cake or the graphene oxide aqueous dispersion was measured from the weight of the graphene oxide wet cake or the graphene oxide aqueous dispersion before heating and the amount of solvent evaporated calculated from the weight difference before and after heating. This was repeated three times to calculate the average value.
[0032] [Measurement Example 2: Absorbance and Absorbance Ratio] The absorbance of the graphene oxide aqueous dispersions prepared in each Example and Comparative Example was measured using a U-3010 spectrophotometer (Hitachi High-Tech Science Corporation). A quartz cell with an optical path length of 10 mm was used. Ion-exchanged water was added to the graphene oxide aqueous dispersions prepared in each Example and Comparative Example so that the graphene oxide concentration was 0.0013% by weight, and the diluted solution was treated for 10 minutes at high output setting using an ultrasonic cleaner (ASU-6M, AS ONE Corporation) with an output of 130 W and an oscillation frequency of 40 kHz. The measurement was performed after a baseline measurement was performed with ion-exchanged water in advance. From the obtained absorbances at 230 nm and 270 nm, the absorbance ratio defined by the following formula was calculated. Absorbance ratio = absorbance (230nm) / absorbance (270nm).
[0033] [Measurement example 3: O / C ratio] The O / C ratio of the graphene oxide used in each example and comparative example was measured using Quantera SXM (manufactured by PHI). The excitation X-ray was monochromatic Al Kα1,2 ray (1486.6 eV), the X-ray diameter was 200 μm, and the photoelectron escape angle was 45°. The C1s main peak due to carbon atoms was assigned to 284.3 eV, and the O1s peak due to oxygen atoms was assigned to a peak near 533 eV, and the O / C ratio was calculated from the area ratio of each peak.
[0034] [Evaluation Example 1: Dispersibility - Residual dissolution or gelation] The graphene oxide aqueous dispersions prepared in each of the Examples and Comparative Examples were visually observed to evaluate the presence or absence of gelation. In addition, the graphene oxide aqueous dispersions prepared in each of the Examples and Comparative Examples were passed through a mesh filter having a line diameter of 160 μm and an opening diameter of 250 μm, and the remaining graphene oxide wet cake captured on the mesh filter was visually observed.
[0035] [Evaluation Example 2: Dispersibility - Settling over time] 100 cc of each of the graphene oxide aqueous dispersions prepared in each Example and Comparative Example was placed in a 200 cc beaker and left to stand at room temperature for 48 hours, after which the upper and lower layers of the graphene oxide aqueous dispersion were sampled with a dropper and their concentrations were measured by Measurement Example 1, and the ratio of the concentration in the upper layer to the concentration in the lower layer (upper layer concentration / lower layer concentration) was calculated. If the concentration ratio was 0.9 or more, it was determined that there was no settling over time.
[0036] [Evaluation Example 3: Paste application] The graphene oxide aqueous dispersions prepared in each of the Examples and Comparative Examples were subjected to solid-liquid separation by suction filtration to obtain wet cakes of graphene oxide. The obtained wet cakes were mixed with a carboxymethyl cellulose aqueous solution having a concentration of 2% by weight so that the graphene oxide was 1.5% by weight as a solid content, and kneaded with a planetary mixer to obtain graphene oxide pastes. The obtained graphene oxide pastes were applied to aluminum foil (thickness 18 μm) using a doctor blade (300 μm), and the coatability was evaluated on a 5-point scale by visual observation of the coating film surface. The evaluation criteria were as follows, and coatability was determined to be good if the evaluation score was 3 points or more. 5 points: No unevenness or smudges on the coating surface are observed 4 points: Approximately 95% of the coating surface area is free of uneven coating or smudges 3 points: No unevenness or smudges are found on approximately 90% to less than 95% of the coating surface area 2 points: No unevenness or smudges are observed on approximately 80% to less than 90% of the coating surface area 1 point: There is a lot of unevenness or smudges on the coating surface.
[0037] [Synthesis Example 1: Method for producing graphene oxide wet cake] Using 1500 mesh natural graphite powder (Shanghai Yifan Graphite Co., Ltd.) as the raw material, 220 ml of 98% concentrated sulfuric acid, 5 g of sodium nitrate, and 30 g of potassium permanganate were added to 10 g of natural graphite powder in an ice bath, and the mixture was stirred for 1 hour to maintain the temperature of the mixture below 20 ° C. The mixture was removed from the ice bath and stirred in a water bath at 35 ° C. for 4 hours, after which 500 ml of ion-exchanged water was added, and the resulting suspension was stirred at 90 ° C. for another 15 minutes. Finally, 600 ml of ion-exchanged water and 50 ml of hydrogen peroxide were added and stirred for 5 minutes to obtain a graphene oxide aqueous dispersion. The obtained graphene oxide aqueous dispersion was filtered, metal ions were washed with dilute hydrochloric acid, acid was washed with ion-exchanged water, and washing was repeated until the pH reached 7 to produce graphene oxide wet cake-1. The element ratio of oxygen atoms to carbon atoms (O / C ratio) of the produced graphene oxide wet cake-1, measured by Measurement Example 3, was 0.70, and the concentration of the graphene oxide wet cake-1, measured by Measurement Example 1, was 44.5% by weight.
[0038] [Synthesis Example 2: Method for producing graphene oxide wet cake-2] Except for changing the oxidation degree, graphene oxide wet cake-2 was produced in the same manner as in Synthesis Example 1. The element ratio of oxygen atoms to carbon atoms (O / C ratio) of the produced graphene oxide wet cake-2 measured by Measurement Example 3 was 0.53, and the concentration of graphene oxide wet cake-1 measured by Measurement Example 1 was 46.3 wt%.
[0039] [Synthesis Example 3: Method for producing graphene oxide wet cake-3] Except for changing the type of natural graphite powder, graphene oxide wet cake-3 was produced in the same manner as in Synthesis Example 1. The element ratio of oxygen atoms to carbon atoms (O / C ratio) of the produced graphene oxide wet cake-3 measured by Measurement Example 3 was 0.63, and the concentration of graphene oxide wet cake-3 measured by Measurement Example 1 was 6.5% by weight.
[0040] [Example 1] 11.23 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 was mixed with 988.77 g of ion-exchanged water, and the mixture was stirred at 7,500 rpm for 30 minutes using a Silverson mixer L5M-A equipped with a round-hole stator having an opening diameter of 0.8 mm to obtain a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.5 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0041] [Example 2] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that 997.76 g of ion-exchanged water was mixed with 2.24 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 to change the graphene oxide concentration to 0.1 wt %. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0042] [Example 3] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that 977.53 g of ion-exchanged water was mixed with 22.47 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 to change the graphene oxide concentration to 1.0 wt %. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0043] [Example 4] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that 955.06 g of ion-exchanged water was mixed with 44.94 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 to change the graphene oxide concentration to 2.0 wt %. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0044] [Example 5] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that the stator was changed to a slit-shaped stator with a width of 0.6 mm and a length-to-short ratio of 22. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0045] [Example 6] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that the rotation speed of the Silverson mixer L5M-A was changed to 10,000 rpm. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0046] [Example 7] 10.80 g of the graphene oxide wet cake-2 obtained in Synthesis Example 2 was mixed with 989.20 g of ion-exchanged water and stirred at 10,000 rpm for 30 minutes using a Silverson mixer L5M-A equipped with a round-hole stator with an opening diameter of 0.8 mm to produce a graphene oxide aqueous dispersion with a graphene oxide concentration of 0.5 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0047] [Example 8] 22.47 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 was mixed with 977.53 g of ion-exchanged water, and the mixture was stirred at a rotation speed of 7,500 rpm for 30 minutes using a Silverson mixer L5M-A equipped with a round-hole stator having an opening diameter of 0.8 mm, to obtain a graphene oxide aqueous dispersion having a graphene oxide concentration of 1.0 wt%.
[0048] 500 g of the obtained graphene oxide aqueous dispersion was mixed with 500 g of ion-exchanged water and stirred for 30 minutes at 7,500 rpm using a Silverson mixer L5M-A equipped with a round-hole stator with an opening diameter of 0.8 mm to produce a graphene oxide aqueous dispersion with a graphene oxide concentration of 0.5 wt%. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0049] [Example 9] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that the stator was changed to a square-hole stator with an opening diameter of 1.6 mm and a length-to-short ratio of 1.2. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0050] [Example 10] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that the stator was changed to a square-hole stator with an opening diameter of 0.8 mm and a length-to-short ratio of 1.2. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0051] [Example 11] A graphene oxide aqueous dispersion was prepared in the same manner as in Example 10, except that the rotation speed of the Silverson mixer L5M-A was changed to 10,000 rpm. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0052] [Example 12] A graphene oxide aqueous dispersion with a graphene oxide concentration of 0.5 wt % was prepared in the same manner as in Example 9, except that the stator was changed to a square hole stator with an opening diameter of 1.6 mm and a length-to-short ratio of 1.2. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0053] [Comparative Example 1] 67.41 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 was mixed with 932.59 g of ion-exchanged water, and the mixture was stirred for 30 minutes at 7,500 rpm using a Silverson mixer L5M-A equipped with a round-hole stator having an opening diameter of 0.8 mm to produce a graphene oxide aqueous dispersion having a graphene oxide concentration of 3.0 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0054] [Comparative Example 2] 22.47 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 was mixed with 977.53 g of ion-exchanged water, and the mixture was stirred for 30 minutes at a rotation speed of 8,000 rpm using a dispersing mixer, Homo Disper 2.5 (Primix Corporation), instead of a Silverson mixer, to produce a graphene oxide aqueous dispersion having a graphene oxide concentration of 1.0 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0055] [Comparative Example 3] 22.47 g of the graphene oxide wet cake-1 obtained in Synthesis Example 1 was mixed with 977.53 g of ion-exchanged water, and the mixture was stirred for 30 minutes at a rotation speed of 300 rpm using a planetary kneader, Hivis Dispermix 3D-2 (Primix Corporation), instead of a Silverson mixer, to produce a graphene oxide aqueous dispersion having a graphene oxide concentration of 1.0 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0056] [Comparative Example 4] Except for changing the stator to a stator with a round hole having an opening diameter of 1.6 mm, a graphene oxide aqueous dispersion was produced in the same manner as in Example 1. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0057] [Comparative Example 5] A graphene oxide aqueous dispersion was produced in the same manner as in Example 1, except that the stator was changed to a slit-shaped stator having a width of 1.6 mm and a length-to-short ratio of 8.3. The results of evaluating the obtained graphene oxide aqueous dispersion by the above-mentioned method are summarized in Table 2.
[0058] [Comparative Example 6] 76.92 g of the graphene oxide wet cake-3 obtained in Synthesis Example 3 was mixed with 923.08 g of ion-exchanged water, and the mixture was stirred for 30 minutes at 7,500 rpm using a Silverson mixer L5M-A equipped with a round-hole stator having an opening diameter of 0.8 mm to produce a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.5 wt %. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0059] [Comparative Example 7] A graphene oxide aqueous dispersion was prepared in the same manner as in Example 1, except that the stator was changed to a round-hole stator with an opening diameter of 1.6 mm and the stirring time was changed to 3 hours. The obtained graphene oxide aqueous dispersion was evaluated by the above-mentioned method, and the results are summarized in Table 2.
[0060] The main production methods and evaluation results of each of the examples and comparative examples are shown in Tables 1 and 2.
[0061] [Table 1]
[0062] [Table 2]
Claims
1. A graphene oxide aqueous dispersion in which graphene oxide is dispersed in water, the graphene oxide aqueous dispersion having an absorbance at a wavelength of 230 nm of 0.6 or more and a ratio of the absorbance at a wavelength of 230 nm to the absorbance at a wavelength of 270 nm (230 nm / 270 nm) of 1.5 or more when a graphene oxide concentration is adjusted to 0.0013 wt%.
2. The graphene oxide aqueous dispersion according to claim 1 , wherein the graphene oxide has an oxygen / carbon atomic ratio (O / C ratio) of 0.60 or more and 0.80 or less, as determined by X-ray photoelectron spectroscopy.
3. 3. A method for producing a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.1 wt % or more and 2.0 wt % or less, comprising a step of passing a slurry obtained by mixing a graphene oxide wet cake having a graphene oxide concentration of 40 wt % or more and 50 wt % or less with water through a hole-like gap having an opening diameter of 0.1 mm or more and 1.0 mm or a slit-like gap having a width of 0.1 mm or more and 1.0 mm or less.
4. 3. A method for producing a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.1 wt % or more and 0.6 wt % or less according to claim 1 or 2, comprising: a step of passing a slurry obtained by mixing water with a graphene oxide wet cake having a graphene oxide concentration of 40 wt % or more and 50 wt % or less through hole-shaped gaps having an opening diameter of 0.1 mm or more and 1.0 mm or a slit-shaped gap having a width of 0.1 mm or more and 1.0 mm or less to obtain a graphene oxide aqueous dispersion having a graphene oxide concentration of 0.8 wt % or more and 2.0 wt % or less; and a step of passing the graphene oxide aqueous dispersion having a graphene oxide concentration of 0.8 wt % or more and 2.0 wt % or less through hole-shaped gaps having an opening diameter of 0.1 mm or more and 1.0 mm or a slit-shaped gap having a width of 0.1 mm or more and 1.0 mm or less.
5. The method for producing a graphene oxide aqueous dispersion according to claim 3 or 4, wherein the shape of the hole-like gaps having an opening diameter of 0.1 mm or more and 1.0 mm or less is rectangular.
6. The method for producing a graphene oxide aqueous dispersion according to any one of claims 3 to 5, wherein in the step of passing the slurry through a hole-like gap having an opening diameter of 0.1 mm to 1.0 mm or a slit-like gap having a width of 0.1 mm to 1.0 mm, the slurry is stirred at a peripheral speed of 15 m / s or more.
7. 7. The method for producing a graphene oxide aqueous dispersion according to claim 6, wherein in the step of passing the graphene oxide aqueous dispersion having a graphene oxide concentration of 0.8 wt % to 2.0 wt % through a hole-shaped gap having an opening diameter of 0.1 mm to 1.0 mm or a slit-shaped gap having a width of 0.1 mm to 1.0 mm, the graphene oxide aqueous dispersion having a graphene oxide concentration of 0.8 wt % to 2.0 wt % is stirred at a peripheral speed of 15 m / s or more.
Citation Information
Patent Citations
Modified graphene, film and molding
JP2013079176A
Method for delaminating layered mineral powder and method for producing layered nanoplate composite
JP2019073401A
Graphene powder, electrode paste for lithium ion battery and electrode for lithium ion battery
WO2016056557A1
Graphene dispersion, process for producing same, process for producing particles of graphene / active material composite, and process for producing electrode paste
WO2017047521A1
Graphene dispersion, process for producing same, process for producing particles of graphene / active material composite, and process for producing electrode paste
WO2017047523A1