Hydrophobic zeolite and method for producing same
A hydrophobic zeolite with low water adsorption and high toluene adsorption capabilities addresses the limitations of conventional zeolites, offering improved adsorption efficiency and energy savings.
Patent Information
- Application Number
- JP2020122648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-25
- Filing Date
- 2020-07-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-07-17
AI Technical Summary
Conventional zeolites exhibit high water adsorption, leading to reduced adsorption of volatile organic compounds and require significant energy for regeneration, limiting their effectiveness as organic compound adsorbents.
A hydrophobic zeolite with a water adsorption amount of 6 g/100 g or less at 25°C and 60% RH, and a toluene adsorption amount of 9 g/100 g or more at 25°C and 0.01 kPa, achieved through dealumination and steam treatment of a BEA structure zeolite without using fluorine compounds.
The hydrophobic zeolite demonstrates both high hydrophobicity and organic compound adsorption capacity, enhancing adsorption performance and reducing energy consumption for regeneration.
Smart Images

Figure 0007585639000003 
Figure 0007585639000004 
Figure 0007585639000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrophobic zeolite and a method for producing the same. TECHNICAL FIELD The present invention relates to a hydrophobic zeolite and a method for producing the same. [Background technology]
[0002] Organic compounds discharged from painting equipment, printing equipment, industrial product cleaning equipment, etc. are considered to be the cause of air pollution such as suspended particulate matter and photochemical oxidants, and there is a demand for a reduction in the amount of emissions. In order to reduce the amount of organic compounds, various organic compound adsorbents have been developed.
[0003] In recent years, zeolite-based organic compound adsorbents have been proposed, but since zeolites generally have a high water adsorption capacity, the adsorption capacity of volatile organic compounds is relatively low, and a large amount of energy is required to heat and remove the adsorbed organic compounds and water to regenerate the adsorbent. For this reason, there is a demand for zeolites that have a low water adsorption capacity, i.e., are highly hydrophobic.
[0004] As a zeolite with relatively high hydrophobicity, Patent Document 1 proposes BEA-type zeolite with an improved SiO2 / Al2O3 molar ratio by acid treatment. However, the zeolite described in Patent Document 1 has a water adsorption capacity of about 1.0 to 5.0% at P / P0=0.1, which corresponds to a relative humidity of 10%, and the acid treatment alone is not sufficient to obtain hydrophobicity sufficient for use as an organic compound adsorbent.
[0005] Moreover, Patent Document 2 proposes a hydrocarbon adsorbent made of BEA-type zeolite having a SiO2 / Al2O3 molar ratio of 300 or more. The hydrocarbon adsorbent described in Patent Document 2 has a high desorption temperature for the hydrocarbons adsorbed in the zeolite, and is insufficient as an adsorbent for organic compounds that are required to desorb the adsorbate at a low temperature. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 3429011 [Patent Document 2] Patent Publication No. 2008-080195 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a hydrophobic zeolite that combines high hydrophobicity and high organic compound adsorption capacity, which have not been achieved with conventional zeolites. [Means for solving the problem]
[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that a specific hydrophobic zeolite can solve the above problems, and have thus completed the present invention.
[0009] That is, the present invention relates to a hydrophobic zeolite having a water adsorption amount of (6 g / 100 g of zeolite) or less at 25° C. and a relative humidity (hereinafter also referred to as “RH”) of 60%, and a toluene adsorption amount of (9 g / 100 g of zeolite) or more at 25° C. and 0.01 kPa. Note that the hydrophobic zeolite is preferably a hydrophobic zeolite produced without using a fluorine compound, in that it has both high hydrophobicity and high organic compound adsorption capacity.
[0010] The present invention will be described in detail below.
[0011] The present invention relates to a hydrophobic zeolite having a water adsorption amount of not more than 6 g / 100 g of zeolite at 25° C. and RH 60%, and a toluene adsorption amount of not less than 9 g / 100 g of zeolite at 25° C. and 0.01 kPa.
[0012] In the present invention, the water adsorption amount is the equilibrium water adsorption amount at a temperature of 25° C., equilibrium pressure P / P0=0.6, P=1.90 kPa (RH 60%) converted into mass per 100 g of zeolite, and the toluene adsorption amount is the equilibrium water adsorption amount at a temperature of 25° C., equilibrium pressure P=0.01 kPa converted into mass per 100 g of zeolite. The lower the water adsorption amount, the higher the "hydrophobicity" is evaluated, and the higher the toluene adsorption amount, the higher the "organic compound adsorption ability". The present invention is characterized by having both high hydrophobicity and high organic compound adsorption ability, with the water adsorption amount at 25° C., RH 60% being (6 g / 100 g of zeolite) or less and the toluene adsorption amount at 25° C., 0.01 kPa being (9 g / 100 g of zeolite) or more. Furthermore, the water adsorption amount at 25°C and RH 60% is preferably 5g / 100g zeolite or less, more preferably 4g / 100g zeolite or less. There is no lower limit to the water adsorption amount, but the lower the limit, the better. The toluene adsorption amount at 25°C and 0.01 kPa is preferably 10g / 100g zeolite or more, more preferably 10.5g / 100g zeolite or more. There is no upper limit to the toluene adsorption amount, but the higher the limit, the better.
[0013] The hydrophobic zeolite of the present invention preferably has a water adsorption amount of 1 g / 100 g of zeolite or less, more preferably 0.5 g / 100 g of zeolite or less, at 25° C. and 10% RH. There is no lower limit to the water adsorption amount, and the lower the amount, the more preferable it is.
[0014] The hydrophobic zeolite of the present invention may have, for example, a BEA structure, an MEI structure, or an MSE structure. Since the zeolite has a high organic compound adsorption capacity, the BEA structure is preferable. Here, the BEA structure, the MEI structure, and the MSE structure are respectively defined as " * This refers to the zeolite framework structures classified as "BEA", "MEI" and "MSE".
[0015] The hydrophobic zeolite of the present invention is1 The amount of hydroxyl groups calculated from the sum of the integrals of the peaks around 1.8 ppm and 2.2 ppm in the H MAS NMR chemical shifts is 3×10 20 It is preferable that the number of particles is less than 1 / g and that there is no peak around 0.7 ppm.
[0016] 1 H MAS NMR was measured using a solid-state NMR: Varian Nuclear Magnetic Resonance Spectrometer VNMRS-400, rotating the sample tube at a rotation speed of 15 kHz. The chemical shift was based on tetramethylsilane as the chemical shift standard (0 ppm). Hydroxy groups were quantified using a calibration curve of the amount of hydrogen created using benzene in deuterated dimethyl sulfoxide. The samples were dehydrated by evacuating to a vacuum at 400°C for 5 hours before measurement.
[0017] The hydrophobic zeolite of the present invention 1 1 H MAS NMR is characterized by a main peak at about 1.8 ppm chemical shift and a shoulder peak at about 2.2 ppm in the spectrum shape due to high hydrophobicity. 1 The amount of hydroxyl groups calculated from the sum of the integrals of the peaks at chemical shifts of 1.8 ppm and 2.2 ppm in the quantitative value of H MAS NMR is 3 × 10 20 It is preferable that the number of particles is less than 2.5×10 20 It is more preferable that the number of particles / g or less is 1.0 or less. In addition, it is preferable that the number of particles / g or less is 1.0 or less. In addition, it is more preferable that the number of particles / g or less is 1.0 or less.
[0018] The hydrophobic zeolite of the present invention preferably has a SiO2 / Al2O3 molar ratio in the range of 100-500, more preferably 300-480, from the viewpoint of achieving both high hydrophobicity and high crystallinity.
[0019] The hydrophobic zeolite of the present invention preferably has a crystal size of 0.02 μm to 2.0 μm, more preferably 0.03 μm to 1.0 μm. If the crystal size is 0.02 μm or more, it is possible to obtain properties that make it easier to handle during molding or honeycomb coating, and if it is 2.0 μm or less, it is possible to suppress a decrease in adsorption performance due to a deterioration in intracrystalline diffusion of the adsorbate.
[0020] The hydrophobic zeolite of the present invention may contain one or more metals selected from the group consisting of sodium, potassium, cesium, iron, copper, silver, platinum, ruthenium, rhodium, palladium, and iridium, from the viewpoints of higher adsorption selectivity and heat resistance when used as an organic compound adsorbent, and from the viewpoint of imparting functions such as oxidative decomposition of the adsorbed organic compounds.
[0021] The method of incorporating the metal component is not particularly limited, and an ion exchange method, an impregnation method, an evaporation to dryness method, etc. can be used. An example of the ion exchange method is a method in which the zeolite is contacted with a solution containing desired ions until the amount of ions in the zeolite reaches a desired concentration. General ion exchange methods such as a batch method and a flow method can be applied. When manufacturing an organic compound adsorbent in the form of a molded body or a honeycomb structure, it is possible to either modify the zeolite powder with a metal and then form the molded body or honeycomb structure, or to modify the zeolite powder with a metal and then form the molded body or honeycomb structure.
[0022] Next, the method for producing the hydrophobic zeolite of the present invention will be described.
[0023] The production method is not particularly limited as long as the hydrophobic zeolite of the present invention can be produced, and an example of the production method includes contacting a zeolite with an acidic solution and then contacting it with water vapor at a temperature of 600°C to 900°C.
[0024] In the present invention, the term "acidic solution" refers to a solution having a pH of 3 or less, and more preferably a solution having a pH of 2 or less.
[0025] As the zeolite base material, a synthetic zeolite having a BEA structure, which can be obtained without using fluorine during production, can be suitably used.
[0026] A method for producing a synthetic zeolite having the BEA structure includes, for example, hydrothermal crystallization of a mixture of a silica source, an alumina source, an alkali source, and, if necessary, a structure-directing agent (hereinafter, also referred to as a "raw material mixture").
[0027] As the silica source, for example, colloidal silica, amorphous silica, sodium silicate, tetraethyl orthosilicate, aluminosilicate gel, etc. can be used.
[0028] The alumina source may be, for example, aluminum sulfate, sodium aluminate, aluminum hydroxide, aluminum chloride, aluminosilicate gel, metallic aluminum, etc. The silica source and alumina source are preferably in a form that can be mixed sufficiently uniformly with other raw materials.
[0029] As the alkali source, for example, various salts such as hydroxides, halides, sulfates, nitrates and carbonates of sodium, potassium and ammonium, alkali components in aluminates, silicates and aluminosilicate gels, etc. can be used.
[0030] A structure directing agent may also be used as necessary, such as tetraethylammonium hydroxide or tetraethylammonium bromide.
[0031] The crystallization of the zeolite can be performed using an autoclave, and the crystallization temperature can be 100° C. or higher and 250° C. or lower, preferably 110° C. or higher and 200° C. or lower, and more preferably 120° C. or higher and 190° C. or lower. The crystallization time can be 12 hours or higher and 96 hours or lower, preferably 14 hours or higher and 84 hours or lower, and more preferably 16 hours or higher and 72 hours or lower. The crystallization can be performed either by leaving the mixture to stand or by stirring.
[0032] After the crystallization is completed, solid-liquid separation is performed, and the excess alkaline solution can be washed with pure water, hot water, or the like. After washing, the product can be dried. The drying temperature is 80°C or higher and 200°C or lower, preferably 90°C or higher and 190°C or lower. If a structure-directing agent is included, it can be removed by a thermal decomposition treatment after drying.
[0033] After removing the structure directing agent used in the production of the zeolite, the zeolite can be suitably dealuminated into a BEA structure zeolite by contacting the zeolite with an acidic solution.
[0034] The acid used in the acidic solution may be any of inorganic acids, organic acids, and mixtures thereof, but inorganic acids such as hydrochloric acid, sulfuric acid, and nitric acid are preferred.
[0035] The amount of acid in the acidic solution is preferably 10 to 100 times the equivalent of aluminum in the zeolite, and more preferably 20 to 80 times the equivalent.
[0036] When contacting with the acidic solution, the solution is preferably heated to 40°C to 95°C, more preferably 50°C to 95°C, in order to promote dealumination.
[0037] The dealumination with an acidic solution may be carried out once or may be repeated two or more times until a desired SiO2 / Al2O3 molar ratio is achieved. By this dealumination, the SiO2 / Al2O3 molar ratio can be adjusted to, for example, 100 to 500, preferably 300 to 480.
[0038] The hydrophobic zeolite of the present invention can be produced by contacting the dealuminated zeolite obtained by dealumination with steam of preferably 20 to 100% by volume, more preferably 40 to 100% by volume at a temperature of 600° C. to 900° C., more preferably 700 to 850° C. When the steam concentration is 20% by volume to 100% by volume, better hydrophobicity can be exhibited. Also, when the contact temperature is 600° C. to 900° C., better hydrophobicity and higher crystallinity can be exhibited.
[0039] The organic compound adsorbent containing the hydrophobic zeolite of the present invention has an excellent effect, particularly as an adsorbent for volatile organic compounds. The organic compound adsorbent can adsorb and remove or adsorb and recover organic compounds in a humid atmosphere or in water while reducing the influence of moisture. Therefore, the organic compound adsorbent is useful as a method for removing organic compounds by contacting with a fluid containing at least one organic compound and removing the organic compound from the fluid. For example, it can be useful as an adsorbent used for adsorbing and removing / recovering exhaust gas or organic compounds in wastewater discharged from painting equipment, printing equipment, industrial product washing equipment, etc., or as an adsorbent for adsorbing and removing organic hydrocarbon components in automobile exhaust gas.
[0040] The hydrophobic zeolite of the present invention can be used as an organic compound adsorbent in the powder state as produced, but it can also be used as a molded body formed into a desired shape such as beads, pellets, or a trefoil shape, or it can be used as a honeycomb structure in which the hydrophobic zeolite powder of the present invention is made into a slurry and applied to a honeycomb-shaped substrate.
[0041] When the hydrophobic zeolite of the present invention is used as an adsorbent for organic compounds, it can be mixed with other zeolites, for example, zeolites having an FAU structure such as USY, or zeolites having an MFI structure such as ZSM-5. Effect of the Invention
[0042] It is possible to provide a hydrophobic zeolite that has both high hydrophobicity and high organic compound adsorption capacity, which was not possible with conventional zeolites. [Brief description of the drawings]
[0043] [Figure 1] Water adsorption isotherms at 25°C for Examples, Comparative Examples, and Reference Examples [Diagram 2] Adsorption isotherms of toluene at 25°C for Examples, Comparative Examples, and Reference Examples [Diagram 3] 1H MAS NMR Spectra of Examples and Comparative Examples [Figure 4] 1H MAS NMR spectra of the examples and comparative examples (Y axis of FIG. 3 is magnified 5 times) EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0045] <Measurement of water adsorption and toluene adsorption> The amount of adsorption was measured using a constant volume adsorption measuring device (BELSORP MAXII: manufactured by Microtrack Belt Co., Ltd.). The sample was pretreated at 350°C for 2 hours under a vacuum of 10 Pa or less. The adsorption temperature was 25°C.
[0046] < 1 H MAS NMR Measurement 1 H MAS NMR was measured using a solid-state NMR: Varian Nuclear Magnetic Resonance Spectrometer VNMRS-400, rotating the sample tube at a rotation speed of 15 kHz. The chemical shift was based on tetramethylsilane as the chemical shift standard (0 ppm). Hydroxy groups were quantified using a calibration curve of the amount of hydrogen created using benzene in deuterated dimethyl sulfoxide. The samples were dehydrated by evacuating to a vacuum at 400°C for 5 hours before measurement.
[0047] Example 1 10 g of commercially available proton type BEA type zeolite (HSZ-940HOA: manufactured by Tosoh Corporation, SiO2 / Al2O3 molar ratio 40) was added to 100 g of 2N hydrochloric acid and stirred at 70°C for 2 hours. After that, the solid-liquid separation was performed, washed with 2 L of warm pure water, and dried overnight at 110°C. The SiO2 / Al2O3 molar ratio of the obtained dealuminated zeolite was 480 by ICP emission spectrometry.
[0048] This dealuminated zeolite was heat-treated (contacted with water vapor) for 2 hours at 840°C in an 80% by volume water vapor atmosphere to obtain the hydrophobic zeolite of the present invention. The SiO2 / Al2O3 molar ratio was 480. The water adsorption amount and toluene adsorption amount at 25°C are shown in Figures 1 and 2, and Table 1, respectively.
[0049] Regarding the hydrophobic zeolite of the present invention obtained in Example 1, 1 The H MAS NMR spectrum was measured. The results are shown in Figure 3. The spectrum intensity (Y axis) of this figure is magnified 5 times and shown in Figure 4. The amount of hydroxyl groups calculated from the sum of the integral values of the peaks at chemical shifts around 0.7 ppm, 1.8 ppm, and 2.2 ppm is shown in Table 2.
[0050] As is clear from Fig. 3, the hydrophobic zeolite of the present invention obtained in Example 1 had a main peak at a chemical shift of about 1.8 ppm and a shoulder peak at a chemical shift of about 2.2 ppm, and as is clear from Fig. 4, the hydrophobic zeolite of the present invention obtained in Example 1 had no peaks at any of the chemical shifts of about 0.7 ppm, about 4 ppm, and about 5 ppm.
[0051] Example 2 The dealuminated zeolite obtained in Example 1 before steam treatment was heat-treated (contacted with steam) for 2 hours at 740°C in a 60% by volume steam atmosphere to obtain a hydrophobic zeolite of the present invention. The SiO2 / Al2O3 molar ratio was 480. The water adsorption amount and toluene adsorption amount at 25°C are shown in Figures 1 and 2, and Table 1, respectively.
[0052] Regarding the hydrophobic zeolite of the present invention obtained in Example 2, 1 The H MAS NMR spectrum was measured. The results are shown in Figure 3. The spectrum intensity (Y axis) of this figure is magnified 5 times and shown in Figure 4. The amount of hydroxyl groups calculated from the sum of the integral values of the peaks at chemical shifts around 0.7 ppm, 1.8 ppm, and 2.2 ppm is shown in Table 2.
[0053] As is clear from Fig. 3, the hydrophobic zeolite of the present invention obtained in Example 2 had a main peak at a chemical shift of about 1.8 ppm and a shoulder peak at a chemical shift of about 2.2 ppm, and as is clear from Fig. 4, the hydrophobic zeolite of the present invention obtained in Example 2 had no peaks at any of the chemical shifts of about 0.7 ppm, about 4 ppm, and about 5 ppm.
[0054] Comparative Example 1 The dealuminated zeolite with a SiO2 / Al2O3 molar ratio of 480 obtained in Example 1 before steam treatment was subjected to measurement of the water adsorption amount and toluene adsorption amount at 25°C without steam treatment. The results are shown in Figures 1 and 2 and Table 1, respectively.
[0055] Regarding the dealuminated zeolite with a SiO2 / Al2O3 molar ratio of 480 obtained in Example 1 above before steam treatment, 1 The H MAS NMR spectrum was measured. The results are shown in Figure 3. The spectrum intensity (Y axis) of this figure is magnified 5 times and shown in Figure 4. The amount of hydroxyl groups calculated from the sum of the integral values of the peaks at chemical shifts around 0.7 ppm, 1.8 ppm, and 2.2 ppm is shown in Table 2.
[0056] As is clear from Fig. 3, the dealuminated zeolite before steam treatment with a SiO2 / Al2O3 molar ratio of 480 obtained in Example 1 above had a main peak at a chemical shift of about 2.2 ppm and a shoulder peak at about 1.8 ppm. Also, as is clear from Fig. 4, the dealuminated zeolite before steam treatment above did not have a peak at a chemical shift of about 0.7 ppm, but had a peak at about 4 ppm to 5 ppm.
[0057] Comparative Example 2 The water adsorption and toluene adsorption amounts of a commercially available USY-type hydrophobic zeolite (manufactured by Tosoh Corporation, SiO2 / Al2O3 molar ratio 115) at 25°C were measured, and the results are shown in Figures 1 and 2 and Table 1, respectively.
[0058] Comparative Example 3 The water adsorption and toluene adsorption amounts of a commercially available MFI-type hydrophobic zeolite (manufactured by Tosoh Corporation, SiO2 / Al2O3 molar ratio 1880) at 25°C were measured, and the results are shown in Figures 1 and 2 and Table 1, respectively.
[0059] Comparative Example 4 Regarding the commercially available proton type BEA zeolite used as the raw material in Example 1, 1 The H MAS NMR spectrum was measured. The results are shown in Figure 3. The spectrum intensity of this figure is magnified 5 times and shown in Figure 4. The amount of hydroxyl groups calculated from the sum of the integral values of the peaks at chemical shifts of around 0.7 ppm, 1.8 ppm, and 2.2 ppm is shown in Table 2.
[0060] As is clear from Fig. 3, the commercially available proton type BEA zeolite has a main peak at a chemical shift of about 2.2 ppm and a shoulder peak at a chemical shift of about 1.8 ppm, and as is clear from Fig. 4, the commercially available proton type BEA zeolite has peaks at chemical shifts of about 0.7 ppm, about 4 ppm, and about 5 ppm.
[0061] Reference example 1 According to Example 2 described in JP 2008-080195 A, zeolite with an increased SiO2 / Al2O3 molar ratio was heat-treated (contacted with water vapor) at 850°C in a 10% by volume water vapor atmosphere for 1 hour to obtain BEA-type zeolite of this Reference Example 1. The SiO2 / Al2O3 molar ratio was 530. The water adsorption amount and toluene adsorption amount at 25°C are shown in Figures 1 and 2, and Table 1, respectively.
[0062] [Table 1]
[0063] As is clear from FIGS. 1 and 2 and Table 1, the hydrophobic zeolite of the present invention has both high hydrophobicity and high organic compound adsorption performance.
[0064] As described above, for the organic compound adsorbent, zeolite with low water adsorption, i.e., high hydrophobicity, is required in order to increase the amount of volatile organic compounds adsorbed and to increase the regeneration efficiency of the adsorbent. The zeolite of the present invention has high hydrophobicity not found in conventional products, and therefore can provide an extremely effective adsorbent.
[0065] [Table 2]
Claims
1. A hydrophobic zeolite having a BEA structure, a moisture adsorption amount of (6 g / 100 g of zeolite) or less at 25°C and RH 60%, and a toluene adsorption amount of (9 g / 100 g of zeolite) or more at 25°C and 0.01 kPa, and a SiO 2 / Al 2 O 3 molar ratio of 300 to 480.
2. The hydrophobic zeolite according to claim 1, having a water adsorption amount of (1 g / 100 g of zeolite) or less at 25°C and RH 10%.
3. 1 The amount of hydroxyl groups calculated from the sum of the integral values of the peaks at chemical shifts of about 1.8 ppm and 2.2 ppm in H MAS NMR is 3×10 20 3. The hydrophobic zeolite according to claim 1 or 2, characterized in that it has a molecular weight of 1,000 or less per gram and has no peak near 0.7 ppm.
4. The hydrophobic zeolite of claim 3, which does not have peaks at chemical shifts of around 4 ppm and around 5 ppm in 1H MAS NMR.
5. 5. The hydrophobic zeolite according to claim 1, wherein the crystal size is 0.02 to 2.0 μm.
6. The hydrophobic zeolite according to any one of claims 1 to 5, characterized in that it contains one or more metals selected from the group consisting of sodium, potassium, cesium, iron, copper, silver, platinum, ruthenium, rhodium, palladium and iridium.
7. The method for producing a hydrophobic zeolite according to any one of claims 1 to 6, characterized in that the zeolite is contacted with the acidic solution and then with steam at a temperature of 700 to 850°C.
8. An adsorbent for organic compounds, comprising the hydrophobic zeolite according to any one of claims 1 to 6.
9. A method for removing organic compounds, comprising contacting the organic compound adsorbent according to claim 8 with a fluid containing at least one organic compound to remove the organic compound from the fluid.
Citation Information
Patent Citations
Hydrocarbon adsorbent composed of silica-enriched beta-type zeolite
JP2008080195A
Adsorption sheet, manufacturing method for obtaining the adsorption sheet, recovery method of adsorption performance and adsorption method
JP2014193454A
Process for dealuminizing synthetic zeolite with large pore size, catalyst and selective organophilic adsorbent comprising dealuminated zeolite obtained by said process, and zeolite β mainly composed of silica
JP3429011B2