Nitrogen oxide storage material and its manufacturing method
The composite oxides with Rudolsden-Popper and perovskite structures, incorporating specific metals, address the inefficiencies of traditional nitrogen oxide storage materials by enhancing NO and NO2 storage performance at low temperatures, reducing precious metal reliance and maintaining catalyst activity.
Patent Information
- Application Number
- JP2021002486
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-28
- Filing Date
- 2021-01-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-11
AI Technical Summary
Existing nitrogen oxide storage materials, particularly those composed of alkaline earth metal oxides like barium oxide, struggle to effectively store NO, necessitating the use of precious metals like platinum to oxidize NO to NO2 for purification, which increases costs and risks catalyst degradation.
A nitrogen oxide storage material containing composite oxides with Rudolsden-Popper and perovskite structures, incorporating alkali metals, alkaline earth metals, lanthanoids, and 3d transition metals, such as Co and Mn, substituted into Ti sites, enhancing NO and NO2 storage performance without relying on precious metals.
The composite oxides exhibit superior NO and NO2 storage capabilities at low temperatures, reducing the need for precious metals, lowering costs, and maintaining catalyst activity, while being resistant to moisture, carbon dioxide, and sulfur oxides.
Smart Images

Figure 0007586424000005 
Figure 0007586424000006 
Figure 0007586424000007
Abstract
Description
[Technical Field]
[0001] The present invention relates to a nitrogen oxide storage material containing a composite oxide and a method for producing the same. [Background technology]
[0002] For example, harmful nitrogen oxides (NO) are contained in exhaust gases emitted from chemical processes in factories and internal combustion engines. x ) are included in the exhaust gas. Therefore, there is a demand for technology to purify nitrogen oxides in exhaust gas. For example, in internal combustion engines, improvements in combustion efficiency and fuel economy are desired, and from the perspective of fuel economy improvement, a lean burn method in which combustion is carried out under conditions of excess oxygen is sometimes used.
[0003] The lean burn system tends to produce a lot of nitrogen oxides in the exhaust gas, which has led to the need for development of nitrogen oxide storage materials with better purification performance.
[0004] For example, Patent Document 1 proposes a method for purifying exhaust gas by bringing exhaust gas into contact with an exhaust gas purification catalyst comprising an alkaline earth metal oxide such as barium oxide and platinum supported on a carrier. In this exhaust gas purification method, NO is oxidized to NO by the platinum, and the NO is further adsorbed onto the alkaline earth metal oxide, thereby purifying nitrogen oxides. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-317652 Summary of the Invention [Problem to be solved by the invention]
[0006] Nitrogen oxide storage materials made from alkaline earth metal oxides such as barium oxide can store NO2, but are unable to store much NO. To store NO, as mentioned above, it is necessary to oxidize NO to NO2 using a precious metal catalyst such as platinum.
[0007] The present invention has been made in view of the above problems, and aims to provide a nitrogen oxide storage material containing an oxide that exhibits excellent storage performance for NO2 and NO, and a method for producing the same. [Means for solving the problem]
[0008] One aspect of the present invention is a method for manufacturing a semiconductor device comprising: a semiconductor device including at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids; 、 Ti and 3d transition metals consisting of Co and / or Mn; The present invention comprises a complex oxide having a Rudolfsden-Popper structure, The above 3d transition metals are substituted into a part of the Ti site of the above Rudolfsden-Popper structure composite oxide. , in nitrogen oxide storage materials.
[0009] Another aspect of the present invention is a method for producing the nitrogen oxide storage material, comprising the steps of: a mixing step of mixing a metal source containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids with a Ti source to prepare a mixture; and a calcination step of calcining the mixture. [Effects of the Invention]
[0010] The nitrogen oxide storage material contains the predetermined composite oxide, and the composite oxide exhibits storage capacity for NO2 and NO. Specifically, the composite oxide has storage capacity for NO2 and the capacity to oxidize NO and store it as NO2. Therefore, the nitrogen oxide storage material can sufficiently store NO and NO2 even if the amount of precious metal is, for example, zero or a smaller amount than conventional. [Brief explanation of the drawings]
[0011] [Figure 1] FIG. 1(a) is an X-ray diffraction pattern diagram of the nitrogen oxide storage materials of Examples 1 to 4, and FIG. 1(b) is a partially enlarged view of FIG. 1(a). [Figure 2] FIG. 2 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 1 to 4 and Comparative Example 1) at a temperature of 300° C. in the absence of CO 2 or H 2 O. [Figure 3] FIG. 3 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 1 to 4) at a temperature of 50° C. in the absence of CO 2 or H 2 O. [Figure 4] FIG. 4 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 2 to 4) at a temperature of 300° C. in the presence of a mixture of CO 2 and H 2 O. [Figure 5] FIG. 5 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 2 to 4) at a temperature of 50° C. in the presence of a mixture of CO2 and H2O. [Figure 6] FIG. 6(a) shows X-ray diffraction patterns of the nitrogen oxide storage materials of Examples 5 to 7, FIG. 6(b) is a partially enlarged view of FIG. 6(a), and FIG. 6(c) shows specific peaks in the X-ray diffraction patterns of various composite oxides with perovskite structure and Ruddersden-Popper structure. [Figure 7] FIG. 7 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 5 to 7) at a temperature of 300° C. in the absence of CO2 or H2O. [Figure 8] FIG. 8 is a graph showing the NOx storage performance of nitrogen oxide storage materials (specifically, Examples 2 to 4) at a temperature of 300° C. in the presence of SO2. DETAILED DESCRIPTION OF THE INVENTION
[0012] (Embodiment) An embodiment of a nitrogen oxide storage material will be described. In this specification, when a numerical value or a physical property value is enclosed by "~", the values before and after the "~" are included. When a numerical value or a physical property value is expressed as a lower limit, it means that the value is equal to or greater than that numerical value or physical property value, and when a numerical value or a physical property value is expressed as an upper limit, it means that the value is equal to or less than that numerical value or physical property value.
[0013] In the following description, a composite oxide having a perovskite structure containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids and Ti will be referred to as a "first composite oxide," and a composite oxide having a Ruddersden-Popper structure containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids and Ti will be referred to as a "second composite oxide."
[0014] The nitrogen oxide storage material contains at least one oxide of the first composite oxide and the second composite oxide. That is, the nitrogen oxide storage material may contain both the first composite oxide and the second composite oxide, or may contain either the first composite oxide or the second composite oxide. Such a nitrogen oxide storage material exhibits storage performance for NO2 and NO. This is because the first composite oxide and the second composite oxide have storage performance for NO2 and oxidation performance for NO. It is also considered that the first composite oxide and the second composite oxide also have the ability to store NO directly. In any case, the first composite oxide and the second composite oxide are capable of absorbing NO, NO2, and other NOx-containing compounds. x Therefore, even if the amount of precious metal is 0 or small, the nitrogen oxide storage material can sufficiently store NO and NO2. This reduces the amount of expensive precious metal, lowering the manufacturing cost of the nitrogen oxide storage material and also lowering the risk of catalytic activity decreasing due to oxidation or aggregation of the precious metal. In addition, the nitrogen oxide storage material can store NO at low temperatures, for example, below 300°C. xOn the other hand, at high temperatures above 300°C, the oxidation rate of NO increases, and NO3 - Therefore, nitrogen oxide storage materials have even better NO production in high temperature environments. x It is possible to demonstrate storage performance.
[0015] The nitrogen oxide storage material may contain other substances to the extent that the object of the present invention is not impaired. Such substances include metal oxides that may be generated during the production of the first composite oxide and the second composite oxide. Specific examples include oxides of alkali metals, oxides of alkaline earth metals, oxides of lanthanoids, titanium oxide, etc. Furthermore, as described below, when Fe, Co, Mn, etc. are substituted and solid-solved at, for example, the Ti site of the first composite oxide or the second composite oxide, the nitrogen oxide storage material may also contain iron oxide, cobalt oxide, manganese oxide, etc. The NO of the nitrogen oxide storage material may be x From the viewpoint of further improving storage performance, the main component of the nitrogen oxide storage material is preferably the first composite oxide or the second composite oxide.
[0016] The first composite oxide has a perovskite structure and contains at least one metal selected from the group consisting of alkali metal elements, alkaline earth metal elements, and lanthanoids, and Ti. x From the viewpoint of further improving the storage performance, the first composite oxide preferably contains an alkaline earth metal, more preferably contains at least one element selected from the group consisting of Ca, Sr, and Ba, and even more preferably contains Sr.
[0017] The first composite oxide has an ionic radius of Ti 4+ It is preferable that the compound further contains a 3d transition metal which is close to NO at low temperatures and is prone to valence fluctuation. x The storage performance is further improved. NO at low temperatures xFrom the viewpoint of further improving the absorption performance, the 3d transition metal is preferably at least one metal selected from the group consisting of Cr, Ni, Cu, Fe, Co, and Mn, more preferably at least one metal selected from the group consisting of Fe, Co, and Mn, even more preferably Co and / or Mn, and even more preferably Co. The 3d transition metal is substituted into a solid solution at some of the Ti sites in the first composite oxide having a perovskite structure.
[0018] The first composite oxide may be, for example, a compound represented by the general formula I: MTi 1-a X a In general formula I, M is at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, and lanthanides. X is the above-mentioned 3d transition metal element. a is 0 or more and less than 1. NO at low temperatures x From the viewpoint of further improving the absorption performance, a is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more. On the other hand, from the viewpoint of maintaining the perovskite structure while the 3d transition metal is dissolved in the Ti site, a is preferably 0.6 or less, more preferably 0.5 or less, and even more preferably 0.4 or less. Furthermore, for example, the first composite oxide represented by general formula I may have oxygen lattice defects (specifically, oxygen non-stoichiometry) in the crystal structure within a range that does not impair the object of the present invention.
[0019] The first composite oxide may have cation defects in its crystal structure. Specifically, the first composite oxide may be, for example, a compound represented by the general formula I':M 1-δ1 {Ti a X (1-a)} 1-δ2The nitrogen oxide storage material may be an oxide represented by the general formula I' and a metal oxide. In the general formula I', the lower limits of δ1 and δ2 are 0. The upper limits of δ1 and δ2 are values that allow the first composite oxide to maintain a perovskite structure, and specifically, each is, for example, 0.1. M, X, and a in the general formula I' are the same as those in the general formula I. In the general formula I', when δ1 > 0 and δ2 > 0, for example, missing cations are precipitated as metal oxides during the production of the first composite oxide, and therefore the nitrogen oxide storage material may contain an oxide represented by the general formula I' and a metal oxide. Examples of metal oxides include oxides of metal element M such as SrO, oxides of metal element X such as iron oxide, manganese oxide, and cobalt oxide, and titanium oxide.
[0020] The first composite oxide having oxygen vacancies, cation vacancies, etc. has the same or better NOx performance than the first composite oxide without vacancies. x The reason for this is believed to be as follows: Generally, the introduction of oxygen vacancies improves the mobility of oxygen in metal oxides, which is advantageous for the oxidation of NO. In other words, when the first composite oxide has oxygen vacancies, the oxidation performance of the nitrogen oxide storage material for NO is improved, and NO x The introduction of cation defects also makes it possible to control the number of oxygen vacancies in the first composite oxide and the electronic state of the transition metal, resulting in improved NO storage performance in the nitrogen oxide storage material. x This leads to an improvement in the storage performance. The same can be said for the second composite oxides represented by general formula II, general formula II', etc., which will be described later.
[0021] The second composite oxide has a Ruddersden-Popper structure and contains at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids, and Ti. That is, the nitrogen oxide contains a second composite oxide having a Ruddersden-Popper structure that contains at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids, and Ti. NO at low temperatures xFrom the viewpoint of further improving the storage performance, the second composite oxide preferably contains an alkaline earth metal, more preferably contains at least one element selected from the group consisting of Ca, Sr, and Ba, and even more preferably contains Sr.
[0022] The second composite oxide preferably further contains a 3d transition metal. In this case, NO x The storage performance is further improved. NO at low temperatures x From the viewpoint of further improving the storage performance, the 3d transition metal is preferably at least one metal selected from the group consisting of Cr, Ni, Cu, Fe, Co, and Mn, more preferably at least one metal selected from the group consisting of Fe, Co, and Mn, even more preferably Co and / or Mn, and even more preferably Co. The 3d transition metal is substituted into a solid solution at some of the Ti sites in the second composite oxide having the Ruddersden-Popper structure.
[0023] The second composite oxide may be, for example, a compound represented by the general formula II: M3Ti 2-b X b In general formula II, M is at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, and lanthanides. X is the above-mentioned 3d transition metal element. b is 0 or more and less than 2. NO at low temperatures x From the viewpoint of further improving the storage performance, b is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more. On the other hand, from the viewpoint of maintaining the Rudlesden-Popper structure while the 3d transition metal is dissolved in the Ti site, b is preferably 1.2 or less, more preferably 1 or less, and even more preferably 0.8 or less. Furthermore, for example, the second composite oxide represented by general formula II may have oxygen lattice defects (specifically, oxygen non-stoichiometry) in its crystal structure, as long as the object of the present invention is not impaired.
[0024] The second composite oxide may have cation defects in its crystal structure, similar to the first composite oxide. Specifically, the second composite oxide may be, for example, a compound represented by the general formula II':M 3-δ3 {Ti b X (2-b)} 2-δ4 The nitrogen oxide storage material may be an oxide represented by the general formula II' and a metal oxide. In the general formula II', the lower limits of δ3 and δ4 are 0. The upper limits of δ3 and δ4 are values that allow the second composite oxide to maintain the Rudlesden-Popper structure. Specifically, the upper limit of δ3 is, for example, 0.3, and the upper limit of δ4 is, for example, 0.2. M, X, and b in the general formula II' are the same as those in the general formula II. In the general formula II', when δ1 > 0 and δ2 > 0, for example, the missing cations are precipitated as metal oxides during the production of the first composite oxide. Therefore, the nitrogen oxide storage material may contain an oxide represented by the general formula II' and a metal oxide. Examples of metal oxides include oxides of metal element M such as SrO, oxides of metal element X such as iron oxide, manganese oxide, and cobalt oxide, and titanium oxide.
[0025] Nitrogen oxide storage materials are used to store NO at low temperatures. x It has excellent absorption performance and can absorb NO even without containing precious metals. x On the other hand, the nitrogen oxide storage material may further contain a noble metal. In this case, for example, NO x The storage performance is improved. Examples of noble metals include Pt, Pd, and Rh.
[0026] Nitrogen oxide storage materials are used to absorb NOx in exhaust gases emitted from, for example, chemical processes in factories and internal combustion engines. x Nitrogen oxide storage materials are used to remove NO at low temperatures. x Since it can absorb NO sufficiently, it is particularly effective against NO in exhaust gases emitted from engines of vehicles such as automobiles. x It is suitable for removing
[0027] The nitrogen oxide storage material is used by being supported on, for example, a carrier. For example, a monolith substrate having a honeycomb structure is used as the carrier. In this case, the nitrogen oxide storage material is supported on, for example, the porous partition walls of the monolith substrate. The carrier is preferably made of a material with excellent heat resistance, such as cordierite or SiC.
[0028] The nitrogen oxide storage material is produced, for example, by performing a mixing step and a calcination step. In the mixing step, a metal source containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids is mixed with a Ti source. In the following description, the metal source will be referred to as the "M source." As the M source and Ti source, for example, various salts, oxides, hydroxides, etc. can be used.
[0029] In the mixing step, it is preferable to further mix a 3d transition metal source. In this case, it is possible to produce a first composite oxide and / or a second composite oxide in which the 3d transition metal is substituted and solid-solved at some of the Ti sites. In the following explanation, the 3d transition metal source will be referred to as an X source. For example, various salts, oxides, hydroxides, etc. can be used as the X source.
[0030] In the mixing step, the blending ratio of the M source, the Ti source, and the X source can be adjusted to a stoichiometric ratio that will yield a desired composite oxide.
[0031] The mixing of the raw materials in the mixing step may be carried out dry, with the addition of an organic solvent such as alcohol or acetone, or in a liquid such as water. Preferably, water-soluble salts are used as the M source, Ti source, and X source, and mixing is carried out in water. In this case, aqueous solutions of the M source, Ti source, and X source are obtained. This increases the reactivity between the raw materials during firing. When mixing is carried out in a liquid, the first composite oxide and the second composite oxide can be produced by, for example, a complex polymerization method or a coprecipitation method. Furthermore, when mixing is carried out in a liquid, it is preferable to obtain a solid mixture by drying after the mixing step and before the firing step in order to increase the reactivity during firing.
[0032] When mixing is performed in a liquid, such as in the coprecipitation method or complex polymerization method, it is preferable to use an M salt as the M raw material, a Ti salt as the Ti raw material, and an X salt as the X source. This allows metal ions to be formed in a liquid such as water, resulting in a mixture in which the metals are thoroughly mixed. It is also preferable to use an M salt, a Ti salt, and an X salt added as needed to form a metal complex of M and Ti, or M, Ti, and X, in water, and then gel the aqueous solution with a gelling agent. In other words, it is preferable to produce a nitrogen oxide storage material by the complex polymerization method. In this case, , for example, compared to solid-state reaction methods x It is possible to obtain a nitrogen oxide storage material with excellent storage performance for nitrogen oxides. This is thought to be because the M ions, Ti ions, and X ions, which are well dispersed through complex formation, are fixed by gelation, resulting in a sufficiently homogeneous gel, which increases the reactivity of the raw materials with each other during firing.
[0033] The M salt, Ti salt, and X salt are not particularly limited as long as they can supply M ions, Ti ions, and X ions, respectively, in water. Specifically, inorganic salts such as nitrates, carbonates, phosphates, and chlorides can be used. Organic acid salts such as acetates and oxalates, and alkoxide salts (i.e., metal alkoxides), can also be used. From the viewpoints of high chemical stability and ease of weighing, carbonates such as strontium carbonate and nitrates such as strontium nitrate are preferred as M salts. Furthermore, from the viewpoints of easy removal of impurity components during firing, nitrates such as iron nitrate, cobalt nitrate, and manganese nitrate are preferred as X salts. From the viewpoints of high reactivity with M ions and X ions and easy preparation of a uniform precursor, alkoxide salts and chlorides are preferred as Ti salts.
[0034] To form a metal complex, a ligand capable of forming a complex with metal ions such as M ions, Ti ions, and optionally X ions may be added to an aqueous solution containing these metal ions. The metal ions may be added to the aqueous solution containing the ligand, or an aqueous solution containing the ligand and an aqueous solution containing the metal ions may be mixed. Hydroxycarboxylic acids such as citric acid and malic acid can be used as sources of the ligand. These are widely used industrially and inexpensive. Therefore, citric acid is preferred. As the gelling agent, polyhydric alcohols such as ethylene glycol and propylene glycol can be used. In this case, gelation is possible by ester polymerization.
[0035] The nitrogen oxide storage material can also be produced by a solid-state reaction method. In this case, the mixing step is carried out in a dry manner as described above. Specifically, in the mixing step, a mixed powder of an M source, a Ti source, and an X source, which is added as needed, is produced. In this case, a homogeneous mixed powder can be obtained by adding an organic solvent when mixing the raw materials. Acetone, ethanol, etc. can be used as the organic solvent.
[0036] In the calcination step, the mixture is calcined. This produces a nitrogen oxide storage material containing the first composite oxide and / or the second composite oxide. The calcination temperature is, for example, 500 to 1200°C. From the viewpoint of producing a nitrogen oxide storage material with a large specific surface area, the calcination temperature is preferably 800 to 1000°C. Note that pre-calcination may be performed before the calcination.
[0037] The firing is carried out, for example, in an air atmosphere. Alternatively, firing can be carried out in an air atmosphere containing water (specifically, water vapor). The water vapor concentration can be adjusted, for example, in the range of 0 to 80% by volume. Firing in an air atmosphere containing water is called hydrothermal synthesis.
[0038] (Experimental Example 1) In this example, nitrogen oxide storage materials having a perovskite structure (specifically, Examples 1 to 4) were prepared, and the NO x The nitrogen oxide storage performance was evaluated. The nitrogen oxide storage materials of Examples 1 to 4 contained a first composite oxide having a perovskite structure containing Sr and Ti. In these examples, the nitrogen oxide storage materials containing the first composite oxide were prepared by a so-called complex polymerization method. 5 is a reference example.
[0039] The nitrogen oxide storage material of Example 1 contains SrTiO3. The nitrogen oxide storage material of Example 1 was prepared as follows.
[0040] First, strontium carbonate (SrCO3) and titanium tetraisopropoxide (Ti[(CH3)2CHO]4) were added to an aqueous solution of 400 mmol of citric acid dissolved in 180 ml of water, and the solution was stirred at 80°C for 2 hours. The molar ratio of the metal elements was Sr:Ti=1:1, and specifically, the amounts of SrCO3 and Ti[(CH3)2CHO]4 added were both 20 mmol. The process of stirring at a specified temperature is called aging. Aging allows the complex to be sufficiently formed, resulting in the production of a metal citrate complex.
[0041] Next, 400 mmol of ethylene glycol was added to the aqueous solution, and the aqueous solution was stirred for 4 hours at a temperature of 130° C. In other words, the aqueous solution was aged for 4 hours at a temperature of 130° C. This aging after the addition of ethylene glycol caused ester polymerization to proceed, and the aqueous solution gelled.
[0042] The gel was then calcined in air at 350°C for 3 hours, and then fired at 1000°C for 2 hours. This yielded an oxide. This oxide was the first composite oxide made of SrTiO3. In this way, the nitrogen oxide storage material of Example 1 was produced.
[0043] The nitrogen oxide storage material in Example 2 is SrTi 0.8 Fe 0.2The composition contains strontium carbonate (SrCO3), titanium tetraisopropoxide (Ti[(CH3)2CHO]4), and iron nitrate nonahydrate (Fe(NO3)3·9H2O) were first added to an aqueous solution of citric acid prepared in the same manner as in Example 1. The compounding ratio, in terms of the molar ratio of the metal elements, was Sr:Ti:Fe=1:0.8:0.2, specifically, the amount of SrCO3 added was 20 mmol, the amount of Ti[(CH3)2CHO]4 added was 16 mmol, and the amount of Fe(NO3)3·9H2O added was 4 mmol. Next, complex formation, gelation, calcination, and firing were carried out in the same manner as in Example 1 to obtain SrTi 0.8 Fe 0.2 A first composite oxide consisting of O3 was obtained. In this way, the nitrogen oxide storage material of Example 2 was produced.
[0044] The nitrogen oxide storage material in Example 3 is SrTi 0.8 Co 0.2 The compound contains strontium carbonate (SrCO3), titanium tetraisopropoxide (Ti[(CH3)2CHO]4), and cobalt nitrate hexahydrate (Co(NO3)3·6H2O) were first added to an aqueous solution containing dissolved citric acid. The compounding ratio, in terms of the molar ratio of the metal elements, was Sr:Ti:Co=1:0.8:0.2, specifically, the amount of SrCO3 added was 20 mmol, the amount of Ti[(CH3)2CHO]4 added was 16 mmol, and the amount of Co(NO3)3·6H2O added was 4 mmol. Next, complex formation, gelation, calcination, and firing were carried out in the same manner as in Example 1 to obtain SrTi 0.8 Co 0.2 A first composite oxide consisting of O3 was obtained. In this way, the nitrogen oxide storage material of Example 3 was produced.
[0045] The nitrogen oxide storage material in Example 4 is SrTi 0.8 Mn 0.2The compound contains strontium carbonate (SrCO3), titanium tetraisopropoxide (Ti[(CH3)2CHO]4), and manganese nitrate hexahydrate (Mn(NO3)3·6H2O) were first added to an aqueous solution containing dissolved citric acid. The compounding ratio, in terms of the molar ratio of the metal elements, was Sr:Ti:Mn=1:0.8:0.2, specifically, the amount of SrCO3 added was 20 mmol, the amount of Ti[(CH3)2CHO]4 added was 16 mmol, and the amount of Mn(NO3)3·6H2O added was 4 mmol. Next, complex formation, gelation, calcination, and firing were carried out in the same manner as in Example 1 to obtain SrTi 0.8 Mn 0.2 A first composite oxide consisting of O3 was obtained. In this way, the nitrogen oxide storage material of Example 4 was produced.
[0046] Next, X-ray diffraction analysis was performed on the nitrogen oxide storage materials of Examples 1 to 4 to obtain X-ray diffraction patterns. X-ray diffraction is referred to as XRD. XRD patterns are obtained by powder XRD analysis. The measurement conditions were: characteristic X-ray: Cu-Kα, measurement range: 3≦2θ≦70, and measurement mode: sweep scan 10° / min. Figures 1(a) and 1(b) show the XRD patterns of each Example. Figure 1(b) is an enlarged view of the peak position derived from the (110) plane in Figure 1(a). As can be seen from Figures 1(a) and 1(b), composite oxides having the above chemical composition and a perovskite structure were obtained in each Example. Note that in Examples 2 to 4, the peak position derived from the Ti site is shifted to a higher angle side compared to Example 1. This is due to the presence of Fe, Co, and Mn in solid solution at some of the Ti sites.
[0047] In addition, a nitrogen oxide storage material (specifically, Comparative Example 1) was prepared for comparison with the Examples. The nitrogen oxide storage material of Comparative Example 1 contains Pt / Ba / Al2O3. Ba in the nitrogen oxide storage material exists in the form of a divalent salt, and specifically, can take the form of barium carbonate, barium hydroxide, barium oxide, or the like depending on the gas atmosphere and temperature conditions. Comparative Example 1 was prepared as follows. First, Al2O3 was immersed in an aqueous solution of dinitrodiammine platinum and an aqueous solution of barium acetate, and evaporated to dryness, thereby adsorbing and supporting Pt and Ba on Al2O3 in a weight ratio of Pt:Ba:Al2O3 = 1:7:92. The material was then calcined in air at 1000°C for 2 hours.
[0048] NO of the nitrogen oxide storage materials of the Examples and Comparative Examples x The nitrogen oxide storage performance was evaluated as follows. First, each nitrogen oxide storage material was packed into the center of a quartz reactor. The reactor was a square cylinder with a height of 12 mm, a width of 10 mm, and a thickness of 1 mm. The packed amount in the example was 100 milligrams, and the packed amount in the comparative example was 70 milligrams.
[0049] A mixed gas containing nitrogen oxides was flowed into this reactor under conditions of a temperature of 300°C or 50°C. The mixed gas flowed in the height direction of the reactor. The mixed gas composition was NO: 500 or 200 ppm by volume, O2: 10 or 3% by volume, and He: the balance, and the flow rate was 100 mL / min. In the comparative example, a mixed gas with an NO content of 200 ppm by volume and an O2 concentration of 3% by volume was used, while in the example, a mixed gas with an NO content of 500 ppm by volume and an O2 concentration of 10% by volume was used. The mixed gas was flowed from the upstream side of the reactor, passed through the nitrogen oxide storage material, and then discharged from the downstream side. At this time, the NO contained in the gas discharged from the downstream side x The concentration of NO was monitored. x NOx of nitrogen oxide storage materials when the storage rate is below 10% x The storage capacity was calculated. The results are shown in Table 1, Figure 2, and Figure 3. Figure 2 shows the NO per unit area of the nitrogen oxide storage material at a measurement temperature of 300°C. xFigure 3 shows the NO per unit area of the nitrogen oxide storage material at a measurement temperature of 50°C. x This shows the amount of NO stored. x The absorption rate is the NOx discharged from the downstream side. x Calculated from the concentration of NO emitted x A concentration of 0 means that the NOx storage rate is 100%, and the amount of NO emitted x If the concentration increases by 10% (specifically, the monitored NO x concentration reaches 50 ppm by volume) x This means that the storage rate is 90%.
[0050] [Table 1]
[0051] As can be seen from Table 1 and FIG. 2, Examples 1 to 4 did not contain a precious metal such as Pt, but NO x High storage capacity, NO x On the other hand, Comparative Example 1 contains precious metals, has a large specific surface area, and has excellent NO absorption performance. x The use of a mixed gas with a lower NO content than in the example x Even though measurements were taken under conditions where the absorption rate was high, x The NO absorption capacity is low. x When the storage amount was measured under the same conditions, the NO x The storage amount is considered to be lower than that of any of the Examples. The specific surface area of the nitrogen oxide storage material is measured by the so-called BET method.
[0052] Examples 2 to 4, in which a part of the Ti sites of the first composite oxide was substituted with 3d transition metal elements such as Fe, Co, and Mn, were solid-solved, and the NOx content was further reduced compared to Example 1, in which no substitution solid solution was used. x As can be seen from Table 1 and Figure 2, at a temperature of 300°C, the substitutional solid solution element preferably contains Fe, Co or Mn, more preferably contains Co and / or Mn, and further preferably contains Co.
[0053] As can be seen from Table 1 and FIG. 3, Examples 1 to 4 were able to produce NO even at a low temperature of 50°C. x Examples 2 to 4, in which a part of the Ti sites of the first composite oxide is substituted with a 3d transition metal element such as Fe, Co, or Mn, have a higher NO 2 absorption capacity at a temperature of 50° C. than Example 1, in which no substitution or solid solution is present. x The results of Comparative Example 1 at a temperature of 50°C are omitted, but because Pt cannot oxidize NO at a temperature of 50°C, the NO absorption capacity of Comparative Example 1 is further improved. x The storage amount is even lower than in Example 1. As can be seen from Table 1 and Fig. 3, at a temperature of 50°C, the substitutional solid solution element preferably contains Fe, Co, or Mn, more preferably contains Fe and / or Co, and further preferably contains Co.
[0054] In this example, NO under a gas atmosphere in which H2O (specifically, moisture) and CO2 coexist x The storage performance was evaluated in the same manner as described above, except that the mixed gas composition was NO: 500 ppm by volume, O: 10% by volume, CO: 3% by volume, H2O: 3% by volume, and He: the balance. x NOx of nitrogen oxide storage materials when the storage rate is below 10% x The storage capacity was calculated, and the results are shown in Table 2, Figure 4, and Figure 5. Figure 4 shows the NO per unit area of the nitrogen oxide storage material at a measurement temperature of 300°C. x Figure 5 shows the NO per unit area of the nitrogen oxide storage material at a measurement temperature of 50°C. x Indicates the amount of storage.
[0055] [Table 2]
[0056] As can be seen from Table 2, Figures 4 and 5, the first composite oxides in which a part of the Ti sites in the composite oxides having a perovskite structure are replaced with 3d transition metal elements such as Fe, Co, and Mn to form a solid solution, as in the nitrogen oxide storage materials of Examples 2 to 4, are resistant to moisture and carbon dioxide. In other words, such first composite oxides are resistant to NO in an environment in which moisture and carbon dioxide are not present. x Absorption performance of NO in the presence of water and carbon dioxide x The nitrogen oxide storage material containing the first composite oxide substituted and solid-solved with a 3d transition metal element can adequately store nitrogen oxides in a gas atmosphere containing moisture and carbon dioxide. As can be seen from Table 2, Figures 4 and 5, the NO x In a gas atmosphere (such as exhaust gas from a vehicle) in which moisture and carbon dioxide are mixed together with Fe, Co, or Mn, the substitutional solid solution element preferably contains Fe, Co, or Mn, more preferably contains Co and / or Mn, and even more preferably contains Co.
[0057] (Experimental Example 2) In this example, nitrogen oxide storage materials having the Rudolfsden-Popper structure (specifically, Examples 5 to 7) were prepared, and the NO x The nitrogen oxide storage performance was evaluated. The nitrogen oxide storage materials of Examples 5 to 7 contained a second composite oxide with a Rudolfsden-Popper structure containing Sr and Ti. In these examples, the nitrogen oxide storage materials containing the second composite oxide were prepared by the so-called coprecipitation method.
[0058] The nitrogen oxide storage material of Example 5 contains Sr3Ti2O7. The nitrogen oxide storage material of Example 5 was prepared as follows.
[0059] First, a first aqueous solution was prepared by dissolving 100 mmol of sodium hydroxide (NaOH) and 100 mmol of sodium carbonate (Na2CO3) in 100 mL of water (H2O). A second aqueous solution was prepared by dissolving strontium nitrate (Sr(NO3)2) and titanium chloride (TiCl4) in 100 mL of water. The molar ratio of strontium nitrate to titanium chloride in the second aqueous solution was Sr:Ti = 3:2, specifically, 30 mmol of Sr(NO3)2 and 20 mmol of TiCl4. The metal concentration in the second aqueous solution was 0.5 mol / L.
[0060] Next, the second aqueous solution was added to the first aqueous solution, and the aqueous solutions were mixed for 1 hour. A precipitate was formed by mixing. The precipitate was collected by filtration, washed with water, and then dried at room temperature for 3 days. This precipitate was a precursor of the second composite oxide. The mixture was then calcined in air at 1000°C for 2 hours. This yielded a second composite oxide composed of SrTiO. In this way, the nitrogen oxide storage material of Example 5 was produced.
[0061] The nitrogen oxide storage material in Example 6 is Sr3Ti 1.6 Mn 0.4 The nitrogen oxide storage material of Example 6 was prepared in the same manner as in Example 5, except that a second aqueous solution was used in which strontium nitrate (Sr(NO3)2), titanium chloride (TiCl4), and manganese nitrate hexahydrate (Mn(NO3)3·6H2O) were dissolved in 100 mL of water. The compounding ratio of the metal elements in the second aqueous solution was Sr:Ti:Mn=3:1.6:0.4, in terms of molar ratio. Specifically, the amount of Sr(NO3)2 added was 30 mmol, the amount of TiCl4 added was 16 mmol, and the amount of Mn(NO3)3·6H2O added was 4 mmol. The metal concentration in the second aqueous solution was 0.5 mol / L, the same as in Example 5.
[0062] The nitrogen oxide storage material in Example 7 is Sr3Ti 1.6 Co 0.4The nitrogen oxide storage material of Example 7 was prepared in the same manner as in Example 5, except that a second aqueous solution was used in which strontium nitrate (Sr(NO3)2), titanium chloride (TiCl4), and cobalt nitrate hexahydrate (Co(NO3)3·6H2O) were dissolved in 100 mL of water. The compounding ratio of the second aqueous solution, in terms of the molar ratio of the metal elements, was Sr:Ti:Co=3:1.6:0.4. Specifically, the amount of Sr(NO3)2 added was 30 mmol, the amount of TiCl4 added was 16 mmol, and the amount of Co(NO3)3·6H2O added was 4 mmol. The metal concentration in the second aqueous solution was 0.5 mol / L, the same as in Example 5.
[0063] XRD analysis of the nitrogen oxide storage materials of Examples 5 to 7 was carried out in the same manner as in Experimental Example 1, and XRD patterns were obtained. The results are shown in Figures 6(a) and 6(b). Figure 6(c) shows the XRD pattern of SrTiO3 in the range of 2θ = 30.5° to 33.5°, and the XRD pattern of Sr4Ti3O3 in the range of 2θ = 30.5° to 33.5°. 10 The XRD patterns of SrTiO7 in the range of 2θ = 30.5° to 33.5° and SrTiO4 in the range of 2θ = 30.5° to 33.5° are shown. SrTiO3 has a perovskite structure, and SrTiO 10 , Sr3Ti2O7, and Sr2TiO4 have the Ruddersden-Popper structure. The Ruddersden-Popper structure has a structure in which perovskite layers and rock salt layers are alternately stacked. In Figure 6(c), n means the number of perovskite layers relative to the rock salt layers, and in the perovskite structure, n is infinite. In the general formula, Sr n+1 Ti n O 3n+1 It is expressed as:
[0064] As can be seen from Figures 6(a) to 6(c), second composite oxides with the above chemical composition and a Ruddersden-Popper structure were obtained in Examples 5 to 7. The nitrogen oxide storage material of Example 5 contains a second composite oxide of a single phase consisting of SrTiO (i.e., a single phase of the Ruddersden-Popper structure with n = 2). The nitrogen oxide storage material of Example 6 contains a second composite oxide having a Ruddersden-Popper structure with n = 1 as the main phase and a Ruddersden-Popper structure with n = 3 as the subphase. The nitrogen oxide storage material of Example 7 contains a second composite oxide having a Ruddersden-Popper structure with n = 2 as the main phase and a Ruddersden-Popper structure with n = 3 as the subphase.
[0065] NO of the nitrogen oxide storage materials of the Examples and Comparative Examples x The storage performance was evaluated in the same manner as in Experimental Example 1. The temperature condition was 300°C, and a mixed gas containing neither H2O nor CO2 was used. The evaluation results are shown in Table 3 and FIG.
[0066] [Table 3]
[0067] As can be seen from Tables 1 and 3, and FIGS. 2 and 7, Examples 5 to 7 had a higher NO than Comparative Example 1. x In addition, Examples 6 and 7, in which a part of the Ti sites of the second composite oxide was substituted with 3d transition metal elements such as Co and Mn, exhibited an even greater NO absorption capacity than Example 5, in which no substitution was performed. x As can be seen from Table 3 and Figure 7, the substitutional solid solution element more preferably contains Co and / or Mn, and even more preferably contains Co.
[0068] (Experimental Example 3) In this example, NO in an environment where sulfur oxides such as SO2 coexist with nitrogen oxides xThis is an example of evaluating storage performance. In this example, Examples 2 and 3 in Experimental Example 1 were used as the nitrogen oxide storage material. The evaluation method was the same as in Experimental Example 1, except that the mixed gas composition was NO: 500 volume ppm, O2: 10 volume %, SO2: 100 volume ppm, and He: the balance. NO x NOx of nitrogen oxide storage materials when the storage rate is below 10% x The amount of occlusion was calculated, and the results are shown in Table 4 and Figure 8. The measurement temperature was 300°C.
[0069] [Table 4]
[0070] As can be seen from Table 4 and Fig. 8, the first composite oxide, in which a part of the Ti sites in the composite oxide having a perovskite structure is replaced and solid-solved with a 3d transition metal element such as Fe, Co, or Mn, as in the nitrogen oxide storage materials of Examples 2 to 4, is resistant to SO2. In other words, taking into account the results of Experimental Example 1, the first composite oxide is resistant not only to moisture and carbon dioxide but also to sulfur oxides such as SO2. The first composite oxide is resistant to NO2 in an environment free of moisture, carbon dioxide, and sulfur oxides. x NO storage performance in the presence of water, carbon dioxide, and sulfur oxides x The decrease in storage performance is small. The nitrogen oxide storage material containing the first composite oxide substituted and solid-solved with 3d transition metal elements can sufficiently store nitrogen oxides in a gas atmosphere where moisture, carbon dioxide, and sulfur oxides coexist (see Tables 1, 2, 4, Figures 4 and 8). x In a gas atmosphere (e.g., exhaust gas from a vehicle) in which moisture, carbon dioxide, and sulfur oxides are mixed together with Fe, Co, or Mn, the substitutional solid solution element preferably contains Fe, Co, or Mn, more preferably contains Co and / or Mn, and further preferably contains Co.
[0071] The reason why the above nitrogen oxide storage materials exhibit resistance to moisture, carbon dioxide, and SO2 is not entirely clear, but it is speculated as follows. The adsorption sites for moisture, carbon dioxide, and inhibitory gases such as SO2, as well as NO, are usually on alkali metals or alkaline earth metals. However, in Ti-containing composite oxides with a perovskite structure, NO is thought to be selectively adsorbed on the Ti or transition metal sites, while inhibitory gases are adsorbed on the alkali metals or alkaline earth metals. This is also true for composite oxides with a Ruddersden-Popper structure. For these reasons, it is speculated that not only the first composite oxide with a perovskite structure, but also the second composite oxide with a Ruddersden-Popper structure, are resistant to moisture, carbon dioxide, and SO2.
[0072] The present invention is not limited to the above-described embodiments and examples, and can be applied to various embodiments without departing from the spirit and scope of the present invention. For example, in Experimental Example 1, the first composite oxide was produced by a complex polymerization method, but the first composite oxide can also be produced by a coprecipitation method as in Experimental Example 2, a solid-phase reaction method, or a hydrothermal synthesis method. Furthermore, in Experimental Example 2, the second composite oxide was produced by a coprecipitation method, but the second composite oxide can also be produced by a solid-phase reaction method or a hydrothermal synthesis method as in Experimental Example 1, a complex polymerization method as in Experimental Example 1, or a hydrothermal synthesis method. The same applies to Experimental Example 3.
[0073] In Examples 2 to 4, the compound of the general formula I:MTi 1-a X a The figure shows the case of a = 0.2 in O3, but from the viewpoint of maintaining the perovskite structure, the range of 0 ≦ a ≦ 0.4 is used to determine the NO equivalent as in the case of a = 0.2. x In Examples 6 and 7, the above general formula II: M3Ti 2-b X b The figure shows the case of b = 0.4 in O3. However, in order to maintain the Ruddersden-Popper structure, the range of 0 ≦ b ≦ 0.8 is used to show the same NO as in the case of b = 0.4. x It is thought to indicate storage performance.
[0074] In the examples, the NO 2 content of the nitrogen oxide storage material containing a composite oxide containing Sr, which is a type of alkaline earth metal, is x Although the absorption performance was evaluated, it is believed that similar results to those in the Examples will be obtained for composite oxides containing other alkaline earth metal elements. In addition, considering that perovskite structures and Ruddersden-Popper structures similar to those in the Examples can be formed by appropriately selecting the types and substitution amounts of M ions and X ions, it is believed that similar results to those in the Examples will be obtained for composite oxides with perovskite structures containing alkali metals and lanthanides.
Claims
1. The present invention comprises a composite oxide having a Rudolfden-Popper structure, the composite oxide including at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids, and a 3d transition metal consisting of Ti, Co, and / or Mn, The nitrogen oxide storage material comprises a composite oxide having a Rudolf Denne-Popper structure, the 3d transition metal being substituted and solid-solved in part of the Ti site of the composite oxide.
2. 2. The nitrogen oxide storage material according to claim 1, further comprising a composite oxide having a perovskite structure containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids, Ti, and a 3d transition metal consisting of Co and / or Mn.
3. 3. The nitrogen oxide storage material according to claim 1, further comprising a precious metal.
4. A method for producing the nitrogen oxide storage material according to any one of claims 1 to 3, comprising the steps of: A mixing step of mixing a metal source containing at least one metal selected from the group consisting of alkali metals, alkaline earth metals, and lanthanoids, a Ti source, and a 3d transition metal source containing Co and / or Mn to prepare a mixture; and a calcining step of calcining the mixture.
5. The method for producing a nitrogen oxide storage material according to claim 4, wherein a source of a 3d transition metal is further mixed in the mixing step.
Citation Information
Patent Citations
Removal of NOX
JP1992161220A
Method for purifying exhaust gas
JP1993317652A
Exhaust gas cleaning catalyst
JP2013226538A
Carbon dioxide absorbing material, and method and apparatus for separating carbon dioxide using the same
WO2006013695A1
Highly heat-resistant composite oxide catalyst for exhaust gas cleaning, and method for producing same
WO2018051890A1