Hydrophilic treatment agent

The hydrophilic treatment agent forms a film with enhanced hydrophilicity, antifogging properties, and superior scratch resistance by using a polymer with a betaine structure and ionic crosslinked networks, addressing the limitations of conventional agents in humid heat environments.

JP7586910B2Active Publication Date: 2024-11-19NIPPON PAINT SURF CHEM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022526900
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-29
Filing Date
2021-05-17
Publication Date
2024-11-19
Estimated Expiration
2041-05-17

AI Technical Summary

Technical Problem

Conventional hydrophilic coating agents suffer from deterioration of antifogging properties in humid heat environments and lack scratch resistance.

Method used

A hydrophilic treatment agent comprising a hydrophilic polymer with a betaine structure and alkoxysilyl or silanol group, and a hydrophilic polymer with ionic or polar functional groups, forming an ionic crosslinked network to enhance heat, humidity, and scratch resistance.

Benefits of technology

The hydrophilic film exhibits improved hydrophilicity, antifogging properties, and excellent scratch resistance, maintaining performance in moist heat environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586910000004
    Figure 0007586910000004
  • Figure 0007586910000001
    Figure 0007586910000001
  • Figure 0007586910000002
    Figure 0007586910000002
Patent Text Reader

Abstract

Provided is a hydrophilizing treatment agent capable of forming a hydrophilic coating film in which the preferred hydrophilicity and antifogging properties are obtained and which has exceptional moist heat resistance and scratch resistance. A hydrophilizing treatment agent that includes: a hydrophilic polymer (A) having at least one of an alkoxysilyl group and a hydrolysate thereof, and also having a betaine structure, in each molecule; and a hydrophilic polymer (B) that is a hydrophilic polymer having an ionic functional group and / or a non-ionic hydrophilic polymer. B / (A+B) is 1.0-51.0%. The preferred moist heat resistance and scratch resistance of the hydrophilic coating film formed by the hydrophilizing treatment agent are obtained due to the hydrophilic polymer (A) and the hydrophilic polymer (B) forming an ionically crosslinked network or a dipole-dipole interaction network.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydrophilic treatment agent. [Background technology]

[0002] Conventionally, hydrophilic treatment agents that impart anti-fogging properties to substrates such as glass include those containing silicate oligomers or silica gel. Hydrophilic treatment agents having a betaine structure are also known (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2014 / 084219

[0004] Patent Document 1 discloses a hydrophilic coating agent obtained by polymerizing a monomer component containing a betaine monomer and an alkoxysilyl group-containing compound. The coating film formed by the hydrophilic coating agent is said to have excellent anti-fogging and abrasion resistance. However, conventional hydrophilic coating agents, including the technology disclosed in Patent Document 1, have a problem that the anti-fogging properties of the formed hydrophilic coating film are easily deteriorated in a humid and hot environment. In addition, there is still room for improvement in the scratch resistance of the hydrophilic coating film. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above, and has an object to provide a hydrophilic treatment agent capable of obtaining preferable hydrophilicity and antifogging properties and forming a hydrophilic coating film having excellent moist heat resistance and abrasion resistance. [Means for solving the problem]

[0006] The present invention relates to a hydrophilization treatment agent comprising: a hydrophilic polymer (A) having, in the molecule, at least one of an alkoxysilyl group and a hydrolyzate thereof and a betaine structure; and a hydrophilic polymer (B) which is at least one of a hydrophilic polymer having an ionic functional group and a nonionic hydrophilic polymer having a polar functional group, wherein the solid content mass ratio B / (A+B) of the hydrophilic polymer (B) to the total mass of the solid contents of the hydrophilic polymer (A) and the hydrophilic polymer (B) is 1.0 to 51.0%. Effect of the Invention

[0007] According to the present invention, it is possible to provide a hydrophilic treatment agent which can obtain preferable hydrophilicity and antifogging properties and can form a hydrophilic coating film which is excellent in moist heat resistance and abrasion resistance. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing the results of a wet heat test using hydrophilic treatment agents according to examples and comparative examples of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An embodiment of the present invention will be described below, but the present invention is not limited to the following embodiment.

[0010] <Hydrophilic treatment agent> The hydrophilic treatment agent according to this embodiment includes a hydrophilic polymer (A) having an alkoxysilyl group and / or its hydrolyzate in the molecule and a betaine structure, and a hydrophilic polymer (B) having at least one of a hydrophilic polymer having an ionic functional group and a nonionic hydrophilic polymer having a polar functional group. The hydrophilic polymer (A) and the hydrophilic polymer (B) form an ion-crosslinked network or a network due to dipole-dipole interaction in the hydrophilic coating formed by the hydrophilic treatment agent, thereby obtaining preferable moist heat resistance and abrasion resistance of the hydrophilic coating.

[0011] (Hydrophilic polymer (A)) The hydrophilic polymer (A) has a betaine structure and preferably has an alkoxysilyl group or a silanol group at least at the terminal in the molecule. The hydrophilic polymer (A) can be obtained, for example, by polymerizing a betaine monomer and a compound containing an alkoxysilyl group or a silanol group.

[0012] The betaine monomer is a compound having a betaine structure in the molecule. When the hydrophilic polymer (A) has a betaine structure in the molecule, it can impart preferable anti-fogging properties to the hydrophilic coating formed by the hydrophilic treatment agent. The betaine structure is composed of a cation and an anion in the same molecule of the betaine monomer. The cation is not particularly limited, but examples thereof include quaternary ammonium, sulfonium, and phosphonium. The anion is not particularly limited, but examples thereof include -SO3 - , -CO2 - , -POH - , -OPO3 - For example, it is preferable that the betaine monomer has a quaternary ammonium cation. In addition, it is preferable that the quaternary ammonium cation has a sulfoxy group (-SO3 - It is more preferable that the betaine monomer is an anion. These betaine monomers may be used alone or in combination of two or more.

[0013] In addition to the betaine structure, the betaine monomer has one or more polymerizable functional groups such as an acryloyl group or a methacryloyl group (hereinafter, sometimes referred to as "(meth)acryloyl group"). The polymerizable functional group is not particularly limited, but examples thereof include a (meth)acryloylaminoalkyl group having an alkyl group with 1 to 4 carbon atoms, and a (meth)acryloyloxyalkyl group having an alkyl group with 1 to 4 carbon atoms.

[0014] Examples of the (meth)acryloylaminoalkyl group having 1 to 4 carbon atoms include a (meth)acryloylaminomethyl group, a (meth)acryloylaminoethyl group, a (meth)acryloylaminopropyl group, a (meth)acryloylaminobutyl group, etc. Examples of the (meth)acryloyloxyalkyl group having 1 to 4 carbon atoms in the alkyl group include a (meth)acryloyloxymethyl group, a (meth)acryloyloxyethyl group, a (meth)acryloyloxypropyl group, a (meth)acryloyloxybutyl group, etc.

[0015] The above quaternary ammonium is treated as a cation, and the sulfoxy group (-SO3 - ) as the anion, there is no particular limitation, and examples thereof include N-(meth)acryloyloxyalkyl-N,N-dimethylammonium alkyl-α-sulfobetaine, N-(meth)acryloyloxyalkoxyanelkoxy-N,N-dimethylammonium alkyl-α-sulfobetaine, N,N-di(meth)acryloyloxyalkyl-N-methylammonium alkyl-α-sulfobetaine, and N,N,N-tri(meth)acryloyloxyalkylammonium alkyl-α-sulfobetaine.

[0016] The above quaternary ammonium is treated as a cation, and the carboxylate group (-CO2 - The betaine monomer having N-(meth)acryloyloxyalkyl-N,N-dimethylammonium-α-carboxyl betaine as the anion is not particularly limited, and examples thereof include N-(meth)acryloyloxyalkyl-N,N-dimethylammonium-α-carboxyl betaine, N,N-di(meth)acryloyloxyalkyl-N-methylammonium-α-carboxyl betaine, and N,N,N-tri(meth)acryloyloxyalkylammonium-α-carboxyl betaine.

[0017] The compound containing an alkoxysilyl group is not particularly limited, but for example, it is preferable that the compound has at least one alkoxy group having 1 to 4 carbon atoms in the molecule. In addition to the above, it is preferable that the compound has a mercapto group represented by (-R1-SH) in the molecule. In the above case, R1 represents an alkylene group having 1 to 12 carbon atoms. Specific examples of such compounds include 2-mercaptomethyltrimethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptopropyltrimethoxysilane, 2-mercaptobutyltrimethoxysilane, 2-mercaptomethyltriethoxysilane, 2-mercaptoethyltriethoxysilane, 2-mercaptopropyltriethoxysilane, 2-mercaptobutyltriethoxysilane, 2-mercaptomethyltripropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptopropyltripropoxysilane, 2-mercaptobutyltripropoxysilane, 2-mercaptomethyltributoxysilane, 2-mercaptoethyltributoxysilane, 2-mercaptopropyltributoxysilane, and 2-mercaptobutyltributoxysilane.

[0018] The compound containing an alkoxysilyl group is preferably a compound in which the molecules of two compounds having at least one alkoxy group having 1 to 4 carbon atoms in the molecule are linked by an azo group. This improves the abrasion resistance of the formed hydrophilic coating. The above compound may also have a methylene group, -O- group, -C(O)O- group, -O(O)C- group, -NH- group, -CO- group, arylene group, urethane bond, 1,2-imidazoline group, etc. Specific examples of such compounds include 2,2'-azobis[2-(1-(trimethoxysilylpropylcarbamoyl)-2-imidazolin-2-yl)propane], 2,2'-azobis[2-(1-(triethoxysilylpropylcarbamoyl)-2-imidazolin-2-yl)propane], 2,2'-azobis[2-(1-(tripropoxysilylpropylcarbamoyl)-2-imidazolin-2-yl)propane], 2,2'-azobis[N-[2-(trimethoxysilylpropylcarbamoyl)ethyl]isobutyramide], 2,2'-azobis[N-[2-(triethoxysilylpropylcarbamoyl)ethyl]isobutyramide], and 2,2'-azobis[N-[2-(tripropoxylpropylcarbamoyl)ethyl]isobutyramide].

[0019] The compound containing a silanol group is not particularly limited, but for example, the alkoxysilyl group of the compound containing an alkoxysilyl group is hydrolyzed to form a silanol group. In addition to the above, the compound containing a silanol group can be obtained by reacting a silyl chloride such as trimethylsilyl chloride or dimethyl (t-butyl) chloride with an active hydrogen-containing compound.

[0020] The above-mentioned compounds having an alkoxysilyl group or a silanol group may be used alone or in combination of two or more kinds.

[0021] The content of the compound having an alkoxysilyl group or a silanol group in the hydrophilic polymer (A) is preferably from 0.01 to 30 parts by mass per 100 parts by mass of the hydrophilic polymer (A).

[0022] The hydrophilic polymer (A) may contain compounds other than the above-mentioned betaine monomer and the compound having an alkoxysilyl group or a silanol group, within the range that does not impair the effects of the present invention. Such compounds are not particularly limited, and conventionally known compounds can be used.

[0023] The method for obtaining the hydrophilic polymer (A) by polymerizing the above-mentioned betaine monomer and the compound having an alkoxysilyl group or a silanol group is not particularly limited, and includes a solution polymerization method in which each component is dissolved in a solvent and polymerized by adding a polymerization initiator as necessary. The amount of the solvent is not particularly limited, and can be adjusted so that the concentration of the monomer component in the solution is 10 to 80 mass %, for example.

[0024] (Hydrophilic polymer (B)) The hydrophilic polymer (B) may be at least one of an ionizable hydrophilic polymer having an ionic functional group and a nonionic hydrophilic polymer having a polar functional group. By including the hydrophilic polymer (B) in the hydrophilic treatment agent, the resulting hydrophilic coating can have favorable wet heat resistance and scratch resistance. The hydrophilic polymer (B) is preferably an ionizable hydrophilic polymer having an ionic functional group.

[0025] The reason why the hydrophilic polymer (B) is contained in the hydrophilic treatment agent and the above-mentioned effect is obtained is not clear, but when FT-IR measurement was performed on the hydrophilic coating formed by the hydrophilic treatment agent according to the present embodiment, which contains the hydrophilic polymer (A) and the ionizable hydrophilic polymer (B) having an ionic functional group, it was confirmed that an ionic crosslinked network was formed between the hydrophilic polymer (A) and the hydrophilic polymer (B). Therefore, it is considered that the formed hydrophilic coating has favorable scratch resistance compared to conventional hydrophilic treatment agents. Furthermore, since the coating mainly composed of this ionic crosslinked network does not contain functional groups that are thought to cause a decrease in hydrophilicity due to chemical reactions in a humid and hot environment, it is considered that the decrease in hydrophilicity in a humid and hot environment is unlikely to occur. In addition, it is considered that the hydrophilic treatment agent containing the hydrophilic polymer (A) and the nonionic hydrophilic polymer (B) having a polar functional group also has the same effect as the above-mentioned by forming a network due to dipole-dipole interaction.

[0026] The ionic functional group of the hydrophilic polymer (B) having an ionic functional group is preferably an anionic functional group or an amphoteric functional group, more preferably an anionic functional group. The anionic functional group is not particularly limited, but is preferably either a carboxy group or a sulfo group.

[0027] The hydrophilic polymer (B) having a carboxy group is not particularly limited, but examples thereof include polyacrylic acid, sodium polyacrylate, ammonium polyacrylate, maleic anhydride copolymer, itaconic acid copolymer, and derivatives thereof.

[0028] The hydrophilic polymer (B) having a sulfo group is not particularly limited, but examples thereof include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, poly (2-acrylamide-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, and copolymers of these with polyacrylic acid, poly (ethyl acrylate) sulfonic acid, and poly (butyl acrylate) sulfonic acid.

[0029] The hydrophilic polymer (B) having an amphoteric functional group is not particularly limited, and examples thereof include allylamine-maleic acid copolymer, styrene-acrylic acid-acrylic acid dialkylamino ester copolymer, aminoethyl methacrylate-methacrylic acid copolymer, methylaminoethyl methacrylate-acrylic acid copolymer, vinylpyridine-maleic acid copolymer, vinylpyridine-itaconic acid copolymer, methylallylamine-itaconic acid copolymer, and the like.

[0030] The hydrophilic polymer (B) having a nonionic polar functional group is a hydrophilic polymer having a nonionic hydrophilic group. Examples of the hydrophilic polymer (B) having a nonionic polar functional group include polyvinylpyrrolidone, a copolymer of vinylpyrrolidone and vinyl acetate, and a copolymer of vinylpyrrolidone and a compound having a vinyl group. In addition to the above, the hydrophilic polymer (B) may be a hydrophilic polymer (B) having a hydroxyl group. Examples of the hydrophilic polymer (B) having a hydroxyl group include polyvinyl alcohol. The hydrophilic polymer having a nonionic polar functional group is preferably polyvinylpyrrolidone or polyvinyl alcohol.

[0031] The hydrophilic polymer (B) may be one of the above-mentioned examples, or two or more of the hydrophilic polymers (B) may be used in combination.

[0032] The molecular weight of the hydrophilic polymer (B) is not particularly limited, but the weight average molecular weight is preferably 1000 to 1000000. The weight average molecular weight is more preferably 5000 to 800000, so that the obtained hydrophilic coating exhibits excellent moist heat resistance. Furthermore, the weight average molecular weight is further preferably 5000 to 50000. This allows the obtained hydrophilic coating to have preferable abrasion resistance and moist heat resistance.

[0033] The solid content mass ratio of the hydrophilic polymer (B) to the total mass of the solid contents of the hydrophilic polymer (A) and the hydrophilic polymer (B), B / (A+B), is preferably 1.0% to 51.0%. From the viewpoint of obtaining a preferable moist heat resistance of the resulting hydrophilic coating, the above B / (A+B) is more preferably 5.0% to 23.8%. From the viewpoint of obtaining a preferable scratch resistance of the resulting hydrophilic coating, the above B / (A+B) is more preferably 5.0% to 38.5%. In other words, taking the above into consideration, the above B / (A+B) is most preferably 5.0% to 23.8%.

[0034] (Surfactant) The hydrophilic treatment agent according to the present embodiment may contain a surfactant. By containing a surfactant in the hydrophilic treatment agent, the dispersibility of each component is improved, and when applying the hydrophilic treatment agent, more uniform application is possible. The surfactant is not particularly limited, and known anionic surfactants, cationic surfactants, nonionic surfactants, etc. can be used.

[0035] (Other Ingredients) The hydrophilic treatment agent according to the present embodiment may contain components other than those described above within the scope of not impairing the effects of the present invention. For example, it may contain other types of polymer components, solvents such as water, and inorganic salts such as NaCl, Na2SO4, KCl, KBr, KNO3, K2SO4, CaCl2, Si, Ti, and alumina.

[0036] <Method of preparing hydrophilic treatment agent> The method for preparing the hydrophilic treatment agent according to the present embodiment is not particularly limited. For example, the hydrophilic treatment agent can be obtained by blending the above-mentioned hydrophilic polymer (A) and hydrophilic polymer (B) and other components in predetermined amounts, adding a solvent such as water as necessary, and stirring the mixture.

[0037] <How to apply hydrophilic treatment agent> The method for applying the hydrophilic treatment agent is a method for applying the hydrophilic treatment agent obtained above to a substrate to form a hydrophilic coating on the substrate surface. The substrate to which the hydrophilic treatment agent is applied is not particularly limited, but examples thereof include inorganic substrates such as glass and aluminum used in vehicles, and organic substrates such as PET, PC, and PMMA.

[0038] The method of applying the hydrophilic treatment agent includes, for example, a pretreatment step, a coating step, and a baking step.

[0039] The pretreatment step may include, for example, a polishing step of polishing the substrate surface to which the hydrophilic treatment agent is applied, and a cleaning step of cleaning the polishing agent or the like. The polishing step can be performed using a known polishing material or polishing machine. The cleaning step removes the polishing material or organic matter remaining on the substrate surface by a method such as water cleaning or UV cleaning. When water cleaning is performed as the cleaning step, it is preferable to provide a drying step after the cleaning step. When an inorganic substrate such as glass is used as the substrate, the pretreatment step includes a polishing step and a cleaning step, and after polishing in the polishing step, water cleaning and UV cleaning are preferably performed in the cleaning step. When the organic substrate is used as the substrate, the pretreatment step includes a cleaning step, and UV cleaning is preferably performed in the cleaning step. In addition, when an organic substrate is used, a primer treatment may be performed instead of or after the cleaning step.

[0040] The coating process is a process of coating the surface of the substrate with a hydrophilic treatment agent. The coating method is not particularly limited, and examples thereof include a method of immersing the substrate in the hydrophilic treatment agent, and a method using a bar coater or a spin coater.

[0041] The baking process is a process of baking the substrate coated with the hydrophilic treatment agent. The coating method of the hydrophilic treatment agent according to the present embodiment does not need to include the baking process, but it is preferable to include the baking process because it promotes the crosslinking reaction between the substrate and the silanol group contained in the hydrophilic treatment agent. The baking temperature and time are not particularly limited, but can be performed under conditions such as 120°C and 15 minutes.

[0042] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and appropriate modifications that do not impair the effects of the present invention are also included in the scope of the present invention. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the description of the following examples.

[0044] [Preparation of hydrophilic treatment agent] Example 1 A PTFE rotor with a total length of 20 mm and a diameter of 7 mm was placed in a 500 ml death cup, and while slowly rotating the rotor, the raw materials shown in Table 1 were mixed with the solid content calculated. After that, the rotor was rotated at 400 rpm for 10 minutes to perform stirring, thereby preparing the hydrophilic treatment agent of Example 1.

[0045] (Examples 2 to 27, Comparative Examples 1 to 9) The hydrophilic treatment agents of Examples 2 to 27 and Comparative Examples 3 to 9 were prepared in the same manner as in Example 1, except that the raw materials to be blended were the raw materials listed in Tables 1 and 2. The raw materials listed below were used as shown in Tables 1 and 2. A predetermined amount of surfactant was added in each Example and Comparative Example. The values ​​in Tables 1 and 2 indicate the solid content (parts by mass) of each component, and the commercially available silicate-based hydrophilic treatment agent shown below was used in Comparative Examples 1 and 2. Comparative Example 1: Surfcoat AF1 (manufactured by Nippon Paint Surf Chemicals) Comparative Example 2: Excelpure BD-S01 (manufactured by Chuo Motors)

[0046] AMK: Amoogen K (lauroyl dimethylaminoacetate betaine, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 1000W: LAMBIC-1000W (hydrophilic polymer containing betaine structure and silanol group, manufactured by Osaka Organic Chemical Industry Co., Ltd.) 771W: LAMBIC-771W (hydrophilic polymer containing betaine structure and silanol group, manufactured by Osaka Organic Chemical Industry Co., Ltd.) 10L: Julimer AC-10L (polyacrylic acid, weight average molecular weight 50,000, manufactured by Toagosei Co., Ltd.) 10H: Julimer AC-10H (polyacrylic acid, weight average molecular weight 800,000, manufactured by Toagosei Co., Ltd.) 10SL: Aron A-10SL (polyacrylic acid, weight average molecular weight 5000, manufactured by Toa Gosei Co., Ltd.) AN: Sharol AN-103P (sodium polyacrylate, weight average molecular weight 10,000, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) AH: Sharol AH-103P (ammonium polyacrylate, weight average molecular weight 10,000, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) PA-PS: Aron A-12SL (a copolymer of acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid, weight-average molecular weight 10,000, manufactured by Toagosei Co., Ltd.) PAA: PAA-1151 (allylamine-maleic acid copolymer, manufactured by Nitbo Medical Co., Ltd.) PVA: PVA-105MC (polyvinyl alcohol resin, saponification degree: 98-99%, polymerization degree: 500, manufactured by Kuraray Co., Ltd.) PVP: Pitcol K-90L (polyvinylpyrrolidone, weight average molecular weight 1200000, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) NaCl: Sodium chloride (grade 1, manufactured by Kanto Chemical Co., Ltd.) KCl: Potassium chloride (Wako Grade 1, Fujifilm Wako Pure Chemical Industries, Ltd.) KBr: Potassium bromide (1st grade pure, manufactured by Junsei Chemical Co., Ltd.) Si: Snowtex O (colloidal silica, manufactured by Nissan Chemical) Ti: TiNoc M-6 (titanium oxide sol, manufactured by Taki Chemical) Alumina: Aluminasol 520-A (Aluminasol, manufactured by Nissan Chemical)

[0047] [Table 1]

[0048] [Table 2]

[0049] [Hydrophilic treatment coating] In Examples 1 to 18, Examples 22 to 27, and Comparative Examples 1 to 9, a glass substrate (S9213 (76 x 52 mm) manufactured by Matsunami Glass Industry Co., Ltd.) was used as the substrate to be coated with the hydrophilic treatment agent. A PET substrate was used in Example 19, a PC substrate in Example 20, and a PMMA substrate in Example 21. The glass substrates used in Examples 1 to 18, Examples 22 to 27, and Comparative Examples 1 to 9 were pretreated with Kiirobin Gold (manufactured by Prostaff Co., Ltd.) before coating. The pretreatment was performed by polishing pretreatment using a PROXXON micropolisher (equipped with a Japanese wool pad 50), then washing the Kiirobin Gold with pure water, and drying the substrate with a dryer. The substrates used in Examples 19 to 21 were pretreated by UV cleaning. After the above pretreatment, the contact angle of the substrate was measured by the method shown below. After confirming that the contact angle was 10° or less, the hydrophilic treatment agent was coated on each substrate. If the contact angle exceeded 10°, the above pretreatment was performed again.

[0050] Each of the pretreated substrates was coated by immersing in the hydrophilic treatment agent of the Examples and Comparative Examples prepared above. The setting time was 1 minute. Thereafter, the samples coated on the glass substrates of Examples 1 to 18, Examples 22 to 27, and Comparative Examples 1 to 9 were baked at 120°C for 15 minutes. The samples coated on the PET, PC, and PMMA substrates of Examples 19 to 21 were baked at 80°C for 30 minutes. In this manner, samples coated with the hydrophilic treatment agents of the Examples and Comparative Examples were prepared.

[0051] The samples of the examples and comparative examples prepared above were evaluated by the methods described below. The results are shown in Table 3.

[0052] (hydrophilic) 5 μl of pure water was dropped onto the surface of each sample substrate in an environment of 25°C and 50% RH, and the contact angle was measured. The measurement device used was an automatic contact angle meter DM501 manufactured by Kyowa Interface Science. Hydrophilicity was evaluated according to the following criteria, with 3 being a pass. 3 Contact angle is 10° or less 2. Contact angle is between 10° and 20° 1 Contact angle is more than 20°

[0053] (Anti-fogging) The degree of fogging when breath was applied to the surface of each sample substrate in an environment of 25° C. and 50% RH was evaluated according to the following criteria, with a score of 3 or higher being considered a pass. 4. Does not fog up 3 It doesn't cloud up, but the water film that spreads out is slightly uneven. 2 It doesn't cloud up, but the water film that spreads out is quite uneven. 1. Cloudy

[0054] (Scratch resistance test) A nonwoven fabric (product name: Elleair Pro Wipe Strong Towel E50, manufactured by Daio Paper Co., Ltd.) was brought into contact with the surface of each sample substrate in the Examples and Comparative Examples, and a load of 500 g was applied and the nonwoven fabric was moved back and forth 100 times. After the test, each sample was evaluated by the above-mentioned methods for evaluating hydrophilicity and anti-fogging properties.

[0055] (Heat and humidity resistance test) Each sample of the Examples and Comparative Examples was exposed to a humid heat environment of 60°C and 90% RH for 24 hours. After the test, each sample was evaluated by the above-mentioned methods for evaluating hydrophilicity and anti-fogging property. In addition, the samples of Example 2, Comparative Example 1, and Comparative Example 4 were exposed under the above-mentioned conditions for 5 days, 10 days, 15 days, and 20 days, respectively, and a moist heat resistance test was performed. After the test, each sample was measured for contact angle (°) by the above-mentioned method for evaluating hydrophilicity. The results are shown in Figure 1.

[0056] [Table 3]

[0057] As is clear from the evaluation results of the Examples and Comparative Examples, the hydrophilic coating film formed by the hydrophilic treatment agent of the Examples has preferable hydrophilicity and antifogging properties compared to the hydrophilic coating film formed by the hydrophilic treatment agent of the Comparative Examples, and it was confirmed that the preferable hydrophilicity and antifogging properties are maintained even after the moist heat resistance test and the abrasion resistance test.

Claims

1. A hydrophilic polymer (A) having, in the molecule, an alkoxysilyl group, at least one of a hydrolyzate thereof, and a betaine structure; and (B) a hydrophilic polymer which is at least one of a hydrophilic polymer having an ionic functional group and a nonionic hydrophilic polymer having a polar functional group and does not have a betaine structure in the molecule, The hydrophilic polymer (A) is obtained by polymerizing at least a betaine monomer and a compound containing an alkoxysilyl group or a silanol group, The betaine monomer has one or more polymerizable functional groups in addition to the betaine structure, the polymerizable functional group is an acryloyl group or a methacryloyl group, The compound containing an alkoxysilyl group or a silanol group is a compound having at least one alkoxy group or silanol group having 1 to 4 carbon atoms in the molecule, or a compound having at least one alkoxy group or silanol group having 1 to 4 carbon atoms in the molecule linked via an azo group, The hydrophilic polymer (A) has at least one of an alkoxysilyl group and a silanol group, the content of the compound having an alkoxysilyl group or a silanol group in the hydrophilic polymer (A) is 0.01 to 30 parts by mass per 100 parts by mass of the hydrophilic polymer (A), the ionic functional group is an anionic functional group or an amphoteric functional group, the hydrophilic polymer (B) having an amphoteric functional group is at least any one of an allylamine-maleic acid copolymer, a styrene-acrylic acid-acrylic acid dialkylamino ester copolymer, an aminoethyl methacrylate-methacrylic acid copolymer, a methylaminoethyl methacrylate-acrylic acid copolymer, a vinylpyridine-maleic acid copolymer, a vinylpyridine-itaconic acid copolymer, and a methylallylamine-itaconic acid copolymer; The nonionic hydrophilic polymer having a polar functional group is polyvinylpyrrolidone or polyvinyl alcohol, The weight average molecular weight of the hydrophilic polymer (B) is 1,000 to 1,000,000, The hydrophilic treatment agent has a solid content mass ratio of the hydrophilic polymer (B) to the total mass of the solid contents of the hydrophilic polymer (A) and the hydrophilic polymer (B), B / (A+B), of 1.0 to 51.0%.

2. The hydrophilic treatment agent according to claim 1 , wherein the hydrophilic polymer (A) has at least one of an alkoxysilyl group and a silanol group at least at an end of the molecule.

3. 3. The hydrophilic treatment agent according to claim 1, wherein at least a part of the ionic functional groups is anionic functional groups.

4. The hydrophilic treatment agent according to claim 1 , wherein the ionic functional group is either a carboxy group or a sulfo group.

Citation Information

Patent Citations

  • Two-pack type Anti-fogging agent

    JP2013079306A

  • Hydrophilic film-forming liquid chemical and hydrophilic film forming method

    JP2016074868A

  • Hydrophilic coating agent

    WO2014084219A1