Sealant composition
The sealant composition for self-sealing tires, with a balanced formulation of butyl rubber, organic peroxide, sulfur, and crosslinking aid, addresses viscosity and adhesion issues, ensuring effective sealing and tire durability by suppressing plasticizer migration and maintaining performance over time.
Patent Information
- Application Number
- JP2020132458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-04
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-08-04
AI Technical Summary
Existing sealant compositions for self-sealing pneumatic tires face challenges in maintaining balanced sealing performance, adhesion to the tire, and durability over time, with issues arising from viscosity, migration of plasticizer components, and changes in physical properties due to temperature variations.
A sealant composition comprising 10% or more butyl rubber, 1 to 40 parts by mass of organic peroxide, 0.1 to 40 parts by mass of sulfur, and a crosslinking aid, with specific shear modulus and tanδ values, ensuring appropriate elasticity and adhesion, and suppressing plasticizer migration.
The composition maintains good sealing properties, suppresses sealant flow during driving, ensures sufficient adhesion to tires, and prevents plasticizer migration, thereby enhancing tire durability and long-term performance.
Smart Images

Figure 0007587108000002 
Figure 0007587108000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a sealant material composition that constitutes a sealant layer of a self-sealing type pneumatic tire having a sealant layer on the inner surface of the tire. [Background technology]
[0002] It has been proposed to provide a sealant layer on the radially inner side of the inner liner layer in the tread portion of a pneumatic tire (see, for example, Patent Document 1). In such a pneumatic tire (a so-called self-sealing type pneumatic tire), when a foreign object such as a nail penetrates the tread portion, the sealant material constituting the sealant layer flows into the through hole, thereby suppressing the decrease in air pressure and enabling the tire to continue traveling.
[0003] In the above-mentioned self-sealing type pneumatic tire, if the viscosity of the sealant is low, the sealant can be expected to improve the sealing performance in that the sealant can easily flow into the through-holes, but if the sealant flows toward the tire center due to the influence of heat and centrifugal force applied during driving, and as a result, if the through-holes are out of the tire center region, there is a risk that the sealant will be insufficient and sufficient sealing performance will not be obtained. On the other hand, if the viscosity of the sealant is high, the flow of the sealant can be prevented, but the sealant will not easily flow into the through-holes, and there is a risk that the sealing performance will be reduced. Therefore, it is required for the sealant composition constituting the sealant to have a good balance between suppressing the flow of the sealant during driving and ensuring good sealing performance.
[0004] Furthermore, since the sealant only functions when a puncture occurs, it remains in the tire until a puncture occurs. In other words, it is required to maintain the above-mentioned sealing properties and fluidity for a long period of time. In addition, if the sealant remains in the tire for a long period of time, there is a risk that the components contained in the sealant (such as plasticizer components) will migrate to the rubber that constitutes the tire. If the components in the sealant migrate to the tire in this way, the adhesion of the sealant to the tire will be impaired, causing the sealant to peel off during driving and affecting tire performance (for example, tire durability). Therefore, it is also required to maintain the adhesion of the sealant to the tire for a long period of time and to maintain good tire durability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-152110 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a sealant composition which exhibits good sealing properties, inhibits flow of the sealant during driving, ensures sufficient adhesion to tires, and further enables good tire durability to be maintained while maintaining these performance properties well over a long period of time. [Means for solving the problem]
[0007] The sealant material composition of the present invention for achieving the above object is a sealant material composition constituting a sealant layer disposed on the inner surface of a pneumatic tire, comprising: Contains 10% or more by mass of butyl rubber For 100 parts by mass of the rubber component, 1 part by mass to 40 parts by mass of organic peroxide, 0.1 to 40 parts by mass of sulfur, more than 0 parts by mass but less than 1 part by mass of a cross-linking aid, and 50 to 400 parts by mass of a plasticizer component are blended, The vulcanizate of the sealant material compositionIt is characterized in that the shear modulus at 20°C is 5 kPa to 30 kPa, the shear modulus at 80°C is 1 kPa to 10 kPa, and the maximum value of tan δ measured in the temperature range of 20°C to 100°C is 1.0 or less. Effect of the Invention
[0008] Since the sealant composition of the present invention is composed of the above-mentioned blend, it exhibits good sealing properties, suppresses the flow of the sealant during driving, and ensures sufficient adhesion to the tire. Specifically, since it contains sulfur (is crosslinked by sulfur), it can enhance adhesion to the inner surface of the tire, and since the above-mentioned blend ensures sufficient viscosity to obtain good sealing properties, it has an appropriate elasticity that does not flow during driving or storage, which is advantageous for achieving a good balance between these performances. In addition, since the sealant composition of the present invention has the above-mentioned characteristics, it ensures appropriate elasticity in the sealant and can suppress the migration of the plasticizer component to other components (tires), so that it can suppress changes over time in the physical properties (sealing properties, fluidity, adhesiveness) of the sealant, and can suppress the effects on tire performance (durability). In particular, since the shear modulus at 20°C is within the above-mentioned range, it is possible to suppress the migration of the plasticizer component over time in an environment at about room temperature. Furthermore, since the shear modulus at 80°C is within the above-mentioned range, it is possible to suppress the migration of the plasticizer component during driving.
[0009] In the sealant composition of the present invention, the shear modulus at 40°C is preferably 5 kPa to 30 kPa, and the shear modulus at 100°C is preferably 1 kPa to 10 kPa. This ensures appropriate elasticity in the sealant and can suppress the migration of plasticizer components to other components (tires), which is advantageous in suppressing changes in the physical properties (sealing properties, fluidity, adhesiveness) of the sealant over time and suppressing the effects on tire performance (durability). In particular, by having the shear modulus at 40°C in the above range, the migration of plasticizer components over time in high-temperature regions can be suppressed. In addition, by having the shear modulus at 100°C in the above range, the migration of plasticizer components during high-speed driving can be suppressed.
[0010] The sealant composition of the present invention preferably contains 1 to 40 parts by mass of an organic peroxide per 100 parts by mass of the rubber component. By containing an organic peroxide in this manner and using the above-mentioned sulfur and organic peroxide in combination to effect crosslinking, it is advantageous to obtain a suitable elasticity that does not flow during driving or storage while ensuring sufficient viscosity to obtain good sealing properties, thereby achieving a good balance between these performances.
[0011] The sealant material composition of the present invention preferably contains 10% by mass or more of butyl rubber relative to 100% by mass of the rubber component. Furthermore, it is preferable that the butyl rubber contains chlorinated butyl rubber, and the content of the chlorinated butyl rubber relative to 100% by mass of the rubber component is 5% by mass or more. By using such a blending method, the adhesion to the inner surface of a tire can be improved.
[0012] In the sealant composition of the present invention, the plasticizer component is preferably a liquid polymer. In particular, it is preferable that the liquid polymer is paraffin oil. Furthermore, it is preferable that the molecular weight of the paraffin oil is 800 or more. This makes it possible to reduce the temperature dependency of the physical properties of the adhesive sealant, which is advantageous for ensuring good sealing properties in low-temperature environments. It is also advantageous for suppressing migration to tires and suppressing effects on tire performance.
[0013] In a pneumatic tire having a sealant layer made of an adhesive sealant obtained by vulcanizing the above-mentioned sealant composition of the present invention, the excellent physical properties of the above-mentioned sealant composition enable the sealant to exhibit good sealing properties while suppressing the flow of the sealant during driving, and ensure sufficient adhesion to the tire. In addition, the above-mentioned blending and physical properties prevent the plasticizer component contained in the sealant from migrating over time to the rubber constituting the tire, so that the performance of the sealant can be maintained well over a long period of time and the impact on tire performance (durability) can be suppressed.
[0014] In this case, the adhesive sealant is preferably vulcanized at a vulcanization temperature of 150° C. or higher for a vulcanization time of 5 to 60 minutes. By performing vulcanization under these conditions, it is possible to suppress the remaining unreacted sulfur in the adhesive sealant, which is advantageous for maintaining the performance of the adhesive sealant well over a long period of time.
[0015] In the present invention, the "shear modulus" is a value measured using a test piece prepared by press-vulcanizing the sealant composition in a specified mold at 160°C for 10 minutes, using a viscoelasticity measuring device under various temperature conditions (20°C, 40°C, 80°C, 100°C) and a shear strain of 10%. Also, "tan δ" is a value measured using a viscoelasticity spectrometer in accordance with JIS K6394, in a temperature range of 20°C to 100°C, under conditions of an elongation deformation strain rate of 10%±2%, and a vibration frequency of 20 Hz. [Brief description of the drawings]
[0016] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.
[0018] As shown in FIG. 1, the pneumatic tire of the present invention (self-sealing type pneumatic tire) includes a tread portion 1 extending in the tire circumferential direction to form an annular shape, a pair of sidewall portions 2 disposed on both sides of the tread portion 1, and a pair of bead portions 3 disposed on the tire radially inner side of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction to form an annular shape, thereby forming a toroidal basic structure of a pneumatic tire. In addition, other tire components in the meridian cross section also extend in the tire circumferential direction to form an annular shape unless otherwise specified.
[0019] In the example of Fig. 1, a carcass layer 4 is installed between a pair of left and right bead portions 3. The carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the inside to the outside of the vehicle around the bead cores 5 and bead fillers 6 arranged in each bead portion 3. The bead fillers 6 are arranged on the outer peripheral side of the bead cores 5, and are enclosed by the main body and folded back portions of the carcass layer.
[0020] A plurality of belt layers 7 (two layers in FIG. 1) are embedded on the outer circumferential side of the carcass layer 4 in the tread portion 1. Of these belt layers 7, the layer with the smallest belt width is called the minimum belt layer 7a, and the layer with the largest belt width is called the maximum belt layer 7b. Each belt layer 7 includes a plurality of reinforcing cords inclined with respect to the tire circumferential direction, and is arranged so that the reinforcing cords cross each other between layers. In these belt layers 7, the inclination angle of the reinforcing cords with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. A belt reinforcing layer 8 is provided on the outer circumferential side of the belt layer 7 in the tread portion 1. In the illustrated example, two belt reinforcing layers 8 are provided, which are a full cover layer that covers the entire width of the belt layer 7, and an edge cover layer that is further arranged on the outer circumferential side of the full cover layer and covers only the end portion of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction, and the angle of the organic fiber cords with respect to the tire circumferential direction is set to, for example, 0° to 5°.
[0021] An inner liner layer 9 is provided on the inner surface of the tire along the carcass layer 4. This inner liner layer 9 is a layer for preventing air filled in the tire from permeating to the outside of the tire. The inner liner layer 9 is composed of, for example, a rubber composition mainly composed of butyl rubber having air permeation prevention properties. Alternatively, it can be composed of a resin layer having a thermoplastic resin as a matrix. In the case of a resin layer, an elastomer component may be dispersed in a thermoplastic resin matrix.
[0022] As shown in FIG. 1, a sealant layer 10 is provided on the inner side of the inner liner layer 9 in the tread portion 1 in the tire radial direction. In particular, the sealant layer 10 is provided on the inner surface of the tire corresponding to the ground contact area of the tread portion 1, that is, an area where a foreign object such as a nail may be stuck during running. In particular, it is preferable to provide the sealant layer 10 in an area wider than the width of the minimum belt layer 7a. The sealant material composition of the present invention is used for this sealant layer 10. The sealant layer 10 is attached to the inner surface of a pneumatic tire having the above-mentioned basic structure. For example, when a foreign object such as a nail is stuck in the tread portion 1, the adhesive sealant material constituting the sealant layer 10 flows into the through hole and seals the through hole, thereby suppressing the decrease in air pressure and enabling the tire to continue running.
[0023] The sealant layer 10 has a thickness of, for example, 0.5 mm to 5.0 mm. With a thickness of this order, it is possible to suppress the flow of the sealant during running while ensuring good sealing properties. In addition, the processability when attaching the sealant layer 10 to the inner surface of the tire is also good. If the thickness of the sealant layer 10 is less than 0.5 mm, it is difficult to ensure sufficient sealing properties. If the thickness of the sealant layer 10 exceeds 5.0 mm, the tire weight increases and the rolling resistance deteriorates. The thickness of the sealant layer 10 is an average thickness.
[0024] The sealant layer 10 can be formed by subsequently attaching it to the inner surface of a vulcanized pneumatic tire. For example, an adhesive sealant obtained by vulcanizing a sealant composition described below may be attached to the inner surface of the tire to form the sealant layer 10. When attaching the adhesive sealant, an adhesive sealant molded in a sheet shape may be attached over the entire circumference of the inner surface of the tire, or an adhesive sealant molded in a string or band shape may be attached in a spiral shape to the inner surface of the tire.
[0025] The vulcanization conditions for vulcanizing the sealant composition described below to obtain the above-mentioned adhesive sealant are not particularly limited, but considering the composition and physical properties of the sealant composition described below, the vulcanization temperature is preferably 150° C. or higher, more preferably 150° C. to 180° C., and the vulcanization time is preferably 5 minutes to 60 minutes, more preferably 10 minutes to 30 minutes. By carrying out the vulcanization under these conditions, it is possible to suppress the unreacted sulfur from remaining in the adhesive sealant, which is advantageous for maintaining the performance of the adhesive sealant well over a long period of time.
[0026] Since the present invention mainly relates to a sealant material composition that constitutes the sealant layer 10 (adhesive sealant material) of the above-mentioned self-sealing type pneumatic tire, the basic structure of the pneumatic tire and the structure of the sealant layer 10 are not limited to the above-mentioned examples.
[0027] The shear modulus of the sealant material composition of the present invention at 20°C was 20 , shear modulus at 80°C is G 80 Then, the sealant composition of the present invention has a shear modulus G 20 is 5 kPa to 30 kPa, preferably 10 kPa to 20 kPa, and the shear modulus G 80The sealant composition of the present invention has a physical property that the shear modulus G is 1 kPa to 10 kPa, preferably 3 kPa to 7 kPa. Furthermore, the sealant composition of the present invention is characterized in that the maximum value of tan δ in the temperature range of 20°C to 100°C is 1.0 or less. Due to the cooperation of these physical properties, when used as a sealant, the sealant composition of the present invention ensures appropriate elasticity and can inhibit the migration of plasticizer components to other components (tires), thereby inhibiting changes over time in the physical properties (sealing ability, fluidity, adhesiveness) of the sealant and suppressing the effects on tire performance (durability). In particular, the shear modulus G 20 By setting the shear modulus G in the above range, the migration of the plasticizer component over time in an environment at room temperature can be suppressed. 80 When the maximum value of tan δ measured in the temperature range of 20°C to 100°C is within the above range, the fluidity can be improved.
[0028] At this time, the shear modulus G 20 If the shear modulus is less than 5 kPa, the migration of the plasticizer component over time in an environment of about room temperature cannot be sufficiently suppressed, making it difficult to ensure long-term sealing performance and to obtain the effect of suppressing the deterioration of tire durability. It also becomes difficult to suppress the flow of the sealant material. 20 If the shear modulus G exceeds 30 kPa, the sealing performance decreases. 80 If the shear modulus G is less than 1 kPa, the migration of the plasticizer component during driving cannot be sufficiently suppressed, and it becomes difficult to obtain the effect of ensuring long-term sealing performance and suppressing the deterioration of the tire durability. 80If the viscosity exceeds 10 kPa, tire durability decreases. If the maximum value of tan δ in the above-mentioned temperature range exceeds 1.0, fluidity decreases. In addition, as long as the above-mentioned relationship is satisfied, tan δ at each temperature in the above-mentioned temperature range is not particularly limited. However, tan δ at 20°C, which is the lower limit of the temperature range, is preferably 0.2 to 0.8, more preferably 0.4 to 0.6. In addition, tan δ at 100°C, which is the upper limit of the temperature range, is preferably 0.2 to 0.8, more preferably 0.4 to 0.6.
[0029] The sealant material composition of the present invention was further measured for shear modulus at 40°C. 40 , shear modulus at 100°C is G 100 Then, the sealant composition of the present invention has a shear modulus G 40 is preferably 5 kPa to 30 kPa, more preferably 10 kPa to 20 kPa, and the shear modulus G 100 is preferably 1 kPa to 10 kPa, and more preferably 3 kPa to 7 kPa. This further improves the physical properties of the sealant composition, and when used as a sealant, the sealant has an appropriate elasticity and can effectively suppress the migration of the plasticizer component to other components (tires). As a result, it is possible to suppress the change over time in the physical properties (sealing properties, fluidity, adhesiveness) of the sealant, and to enhance the effect of suppressing the influence on tire performance (durability). In particular, the shear modulus G 40 By keeping the shear modulus G in the above range, the migration of plasticizer components over time in high temperature regions can be suppressed. 100 By ensuring that the content is within the above range, migration of the plasticizer component during high-speed running can be suppressed.
[0030] At this time, the shear modulus G 40 If the shear modulus is less than 5 kPa, the migration of the plasticizer component over time in high temperature regions cannot be sufficiently suppressed. 40 If the shear modulus G exceeds 30 kPa, the sealing performance decreases. 100 If the shear modulus is less than 1 kPa, the migration of the plasticizer component during high-speed driving cannot be sufficiently suppressed.100 If the pressure exceeds 10 kPa, the tire durability decreases.
[0031] The sealant material composition of the present invention has the above-mentioned physical properties and is composed of the following composition.
[0032] In the sealant composition of the present invention, the rubber component may contain a butyl-based rubber. The proportion of the butyl-based rubber in the rubber component is preferably 10% by mass or more, more preferably 20% by mass to 90% by mass. By containing the butyl-based rubber in this way, good adhesion to the inner surface of a tire can be ensured. If the proportion of the butyl-based rubber is less than 10% by mass, sufficient adhesion to the inner surface of a tire cannot be ensured.
[0033] In the sealant composition of the present invention, it is preferable to include halogenated butyl rubber as the butyl-based rubber. Examples of halogenated butyl rubber include chlorinated butyl rubber and brominated butyl rubber, and chlorinated butyl rubber can be particularly preferably used. When using chlorinated butyl rubber, the ratio of chlorinated butyl rubber to 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass to 85% by mass. By including halogenated butyl rubber (chlorinated butyl rubber), the reactivity of the rubber component with the crosslinking agent and organic peroxide described below is increased, which is advantageous for ensuring the sealing property and suppressing the flow of the sealant. In addition, the processability of the sealant composition can be improved. If the ratio of chlorinated butyl rubber is less than 5% by mass, the reactivity of the rubber component with the crosslinking agent and organic peroxide described below is not sufficiently improved, and the desired effect cannot be sufficiently obtained.
[0034] In the sealant composition of the present invention, the entire amount of the butyl-based rubber does not need to be halogenated butyl rubber (chlorinated butyl rubber), and non-halogenated butyl rubber can also be used in combination. Examples of non-halogenated butyl rubber include unmodified butyl rubbers that are usually used in sealant compositions, such as BUTYL-065 manufactured by JSR and BUTYL-301 manufactured by LANXESS. When halogenated butyl rubber and non-halogenated butyl rubber are used in combination, the amount of non-halogenated butyl rubber is preferably less than 20% by mass, more preferably less than 10% by mass, based on 100% by mass of the rubber component.
[0035] In the sealant composition of the present invention, it is preferable to use two or more kinds of rubbers in combination as the butyl-based rubber. That is, it is preferable to use chlorinated butyl rubber in combination with other halogenated butyl rubber (e.g., brominated butyl rubber) or non-halogenated butyl rubber. Since the three types of chlorinated butyl rubber, other halogenated butyl rubber (brominated butyl rubber), and non-halogenated butyl rubber have different vulcanization rates, when at least two types are used in combination, the physical properties (viscosity, elasticity, etc.) of the sealant composition after vulcanization are not uniform due to the difference in vulcanization rate. That is, due to the distribution (variation in concentration) of rubbers with different vulcanization rates in the sealant composition, relatively hard parts and relatively soft parts are mixed in the sealant layer after vulcanization. As a result, the flowability is suppressed in the relatively hard parts, and the sealing property is exhibited in the relatively soft parts, which is advantageous for achieving a good balance between these performances.
[0036] In the sealant composition of the present invention, other diene rubbers than butyl rubber can be blended as the rubber component. As the other diene rubbers, rubbers generally used in sealant compositions, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR), can be used. These other diene rubbers can be used alone or as any blend.
[0037] In the sealant composition of the present invention, sulfur is always blended as a crosslinking agent. The blending amount of sulfur is 0.1 to 40 parts by mass, preferably 0.5 to 20 parts by mass, based on 100 parts by mass of the rubber component. This allows the adhesive sealant to be crosslinked by sulfur, improving its adhesion to tires. If the blending amount of sulfur is less than 0.1 parts by mass, it is essentially the same as not containing a crosslinking agent, and appropriate crosslinking cannot be performed. If the blending amount of sulfur exceeds 40 parts by mass, crosslinking of the sealant composition proceeds too much, resulting in a decrease in sealing properties. Note that even if a crosslinking agent other than sulfur (e.g., quinone dioxime, zinc oxide, etc.) is used, it is not possible to ensure sufficient adhesion to tires.
[0038] In the sealant composition of the present invention, it is preferable to compound an organic peroxide together with the above-mentioned crosslinking agent (sulfur). By compounding sulfur and an organic peroxide in combination in this way, suitable crosslinking can be realized to ensure sealing properties and prevent the sealant from flowing at the same time. The amount of the organic peroxide is preferably 1 to 40 parts by mass, more preferably 1.0 to 20 parts by mass, relative to 100 parts by mass of the above-mentioned rubber component. If the amount of the organic peroxide is less than 1 part by mass, the amount of the organic peroxide is too small to sufficiently crosslink, and desired physical properties cannot be obtained. If the amount of the organic peroxide is more than 40 parts by mass, crosslinking of the sealant proceeds too much, resulting in a decrease in sealing properties.
[0039] In using sulfur and an organic peroxide in combination in this way, the mass ratio A / B of the amount of sulfur blended A to the amount of organic peroxide blended B is preferably 5 / 1 to 1 / 200, more preferably 1 / 10 to 1 / 20. By using such a blending ratio, it is possible to achieve a better balance between ensuring sealing properties and preventing the flow of the sealant material.
[0040] Examples of organic peroxides include dicumyl peroxide, t-butylcumyl peroxide, benzoyl peroxide, dibenzoyl peroxide, butyl hydroperoxide, p-chlorobenzoyl peroxide, and 1,1,3,3-tetramethylbutyl hydroperoxide. In particular, organic peroxides having a one-minute half-life temperature of 100°C to 200°C are preferred, and among the above-mentioned specific examples, dicumyl peroxide and t-butylcumyl peroxide are particularly preferred. In the present invention, the "one-minute half-life temperature" generally refers to the value described in NOF Corporation's "Organic Peroxide Catalog, 10th Edition." If not described, the value obtained from thermal decomposition in an organic solvent in the same manner as described in the catalog is used.
[0041] The sealant composition of the present invention is necessarily blended with a crosslinking aid together with the crosslinking agent (sulfur). The crosslinking aid is a compound that acts as a crosslinking reaction catalyst when blended with a crosslinking agent containing a sulfur component. By blending the crosslinking agent (sulfur) and the crosslinking aid, the vulcanization speed can be increased, and the productivity of the sealant can be improved. The blending amount of the crosslinking aid is preferably more than 0 part by mass and less than 1 part by mass, more preferably 0.1 part by mass to 0.9 parts by mass, relative to 100 parts by mass of the rubber component. By suppressing the blending amount of the crosslinking aid in this way, it is possible to suppress deterioration (thermal deterioration) of the sealant while promoting the crosslinking reaction as a catalyst. If the blending amount of the crosslinking aid is 1 part by mass or more, the effect of suppressing thermal deterioration cannot be sufficiently obtained. Incidentally, since the crosslinking aid acts as a crosslinking reaction catalyst when blended with a crosslinking agent containing a sulfur component as described above, even if it is coexisted with an organic peroxide instead of the sulfur component, it does not act as a crosslinking reaction catalyst, and a large amount of the crosslinking aid must be used, which promotes thermal deterioration.
[0042] When the crosslinking agent (sulfur) and the crosslinking assistant are used in combination, the amount of the crosslinking agent (sulfur) is preferably 50% by mass to 400% by mass, more preferably 100% by mass to 200% by mass of the amount of the crosslinking assistant. By mixing the crosslinking agent (sulfur) and the crosslinking assistant in a well-balanced manner, the crosslinking assistant can exhibit its catalytic function well, which is advantageous for ensuring both sealing properties and preventing the sealant from flowing. If the amount of the crosslinking agent (sulfur) is less than 50% by mass of the amount of the crosslinking assistant, the flowability decreases. If the amount of the crosslinking agent (sulfur) is more than 400% by mass of the amount of the crosslinking assistant, the deterioration resistance decreases.
[0043] Examples of the crosslinking aid include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamate-based, aldehyde-amine-based, aldehyde-ammonia-based, imidazoline-based, and xanthogenic acid-based compounds (vulcanization accelerators). Among these, thiazole-based, thiuram-based, guanidine-based, and dithiocarbamate-based vulcanization accelerators can be preferably used. Examples of the thiazole-based vulcanization accelerators include 2-mercaptobenzothiazole and dibenzothiazyl disulfide. Examples of the thiuram-based vulcanization accelerators include tetramethylthiuram monosulfide and tetramethylthiuram disulfide. Examples of the guanidine-based vulcanization accelerators include diphenylguanidine and diorthotolylguanidine. Examples of the dithiocarbamate vulcanization accelerator include sodium dimethyldithiocarbamate, sodium diethyldithiocarbamate, etc. In particular, in the present invention, it is preferable to use a thiazole- or thiuram-based vulcanization accelerator, which can suppress variation in the performance of the resulting sealant composition.
[0044] In addition, a compound that actually functions as a crosslinking agent, such as quinone dioxime, may be conveniently called a crosslinking auxiliary, but since the crosslinking auxiliary in the present invention is a compound that functions as a catalyst for the crosslinking reaction by the crosslinking agent (sulfur) as described above, quinone dioxime does not correspond to the crosslinking auxiliary in the present invention.
[0045] A plasticizer component (e.g., liquid polymer) is always blended into the sealant composition of the present invention. By blending the plasticizer component in this way, the viscosity of the adhesive sealant can be increased, improving the sealing property. The blending amount of the plasticizer component is 50 parts by mass to 400 parts by mass, preferably 70 parts by mass to 200 parts by mass, relative to 100 parts by mass of the rubber component. If the blending amount of the plasticizer component is less than 50 parts by mass, the effect of increasing the viscosity of the adhesive sealant may not be sufficiently obtained. If the blending amount of the plasticizer component exceeds 400 parts by mass, the flow of the sealant cannot be sufficiently prevented.
[0046] As the plasticizer component, liquid polymers can be exemplified as described above, and liquid polymers that can be co-crosslinked with the rubber component (butyl rubber) in the sealant material composition are particularly preferred. Examples of such liquid polymers include paraffin oil, polybutene oil, polyisoprene oil, polybutadiene oil, polyisobutene oil, aromatic oil, and polypropylene glycol. From the viewpoint of keeping the temperature dependency of the physical properties of the sealant material composition low and ensuring good sealing properties in a low-temperature environment, paraffin oil, polybutene oil, polyisoprene oil, polybutadiene oil, aromatic oil, and polypropylene glycol are preferred, and paraffin oil is particularly preferred. By using paraffin oil, it is advantageous to set the viscosity in a low-temperature environment to an appropriate range. The molecular weight of the liquid polymer is preferably 800 or more, more preferably 1000 or more, and even more preferably 1200 to 3000. By using a polymer with such a large molecular weight, it is possible to prevent the plasticizer component (oil content) from migrating from the sealant layer provided on the inner surface of the tire to the tire body and affecting the tire.
[0047] The sealant composition of the present invention exerts good sealing properties by combining the above-mentioned physical properties and compounding, suppresses the flow of the sealant during driving, and ensures sufficient adhesion to the tire, and further maintains these properties well for a long period of time. In addition, when used in a tire, the plasticizer component is unlikely to migrate to the tire over time, and the durability of the tire can be well maintained. Therefore, the sealant composition of the present invention can be suitably used for the sealant layer 10 (adhesive sealant) of a self-sealing type pneumatic tire. And, a tire having a sealant layer 10 composed of an adhesive sealant obtained by vulcanizing the sealant composition of the present invention can reliably seal a through hole caused by a puncture for a long period of time without impairing the durability of the tire due to the excellent performance based on the cooperation of the above-mentioned physical properties and compounding.
[0048] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0049] Sealant compositions (Comparative Examples 1 to 7, Examples 1 to 2) were prepared with the compositions shown in Table 1. Specifically, the rubber component and carbon black were mixed in a 1.7 L Banbury mixer for 10 minutes, then the plasticizer component (liquid polymer) was added, and finally the crosslinking agent (sulfur) and organic peroxide were added and mixed for another 10 minutes to prepare each sealant composition. The sealant compositions were vulcanized under the conditions shown in Table 1 to obtain adhesive sealants.
[0050] Table 1 also lists the shear modulus and tan δ of the sealant composition. 20 ,G 40 ,G 80 ,G 100 In each case, the sealant composition was press-vulcanized in a specified mold at 160°C for 10 minutes to prepare a test piece, and the measurements were performed using a viscoelasticity measuring device (RPA2000 manufactured by Alpha Technology Co., Ltd.) under a shear strain of 10%. The shear modulus G0 was measured at a temperature of 0°C, and the shear modulus G 20 is the value measured at a temperature of 20°C, and the shear modulus G 40 is the value measured at a temperature of 40°C, and the shear modulus G 80 is the value measured at a temperature of 80°C, and the shear modulus G 100 is a value measured at a temperature of 100°C. In addition, tan δ was measured in accordance with JIS K6394 using a viscoelasticity spectrometer under conditions of an elongation deformation strain rate of 10%±2% and a vibration frequency of 20 Hz, with "tan δ (maximum value)" being the maximum value measured in the temperature range of 20°C to 100°C, "tan δ (20°C)" being the value measured at a temperature of 20°C, and "tan δ (100°C)" being the value measured at a temperature of 100°C.
[0051] These sealant compositions were evaluated for sealing ability, fluidity during running, load durability, high-speed durability, and adhesion by the following test methods. The results are shown in Table 1.
[0052] Sealing ability (condition 1) Each adhesive sealant immediately after vulcanization was attached to the radially inner side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire. Each test tire was then mounted on a wheel with a rim size of 20 x 9J and mounted on a test vehicle, and a nail with a diameter of 4.0 mm was driven into the tread under conditions of an initial air pressure of 250 kPa and a load of 8.5 kN. The air pressure was measured after the nail was removed and the tire was left to stand for 1 hour. The evaluation results were shown on a 5-point scale as follows. A score of "3" or higher indicates sufficient sealing performance, and a higher score indicates better sealing performance. 5: Air pressure after standing is 240kPa or more and 250kPa or less 4: Air pressure after standing is 230kPa or more and less than 240kPa 3: Air pressure after standing is 215kPa or more and less than 230kPa 2: Air pressure after standing is 200kPa or more and less than 215kPa 1: Air pressure after standing is less than 200kPa
[0053] Sealing ability (condition 2) Each adhesive sealant material was applied to the radially inner side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire, which was then stored in an environment at 30°C for two weeks. Each test tire was then mounted on a wheel with a rim size of 20x9J and mounted on a test vehicle, and a nail with a diameter of 4.0 mm was driven into the tread under conditions of an initial air pressure of 250 kPa and a load of 8.5 kN. The air pressure was then measured after the nail was removed and the tire was left to stand for one hour. The evaluation results were shown on a five-point scale. A score of "3" or higher in the evaluation results indicates sufficient sealing performance, and a higher score indicates a better sealing performance. 5: Air pressure after standing is 240kPa or more and 250kPa or less 4: Air pressure after standing is 230kPa or more and less than 240kPa 3: Air pressure after standing is 215kPa or more and less than 230kPa 2: Air pressure after standing is 200kPa or more and less than 215kPa 1: Air pressure after standing is less than 200kPa
[0054] Fluidity during driving Each adhesive sealant immediately after vulcanization was attached to the inner radial side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire. The test tire was then mounted on a wheel with a rim size of 20 x 9J and mounted on a drum testing machine, and the tire was driven for 1 hour under the conditions of an air pressure of 220 kPa, a load of 8.5 kN, and a running speed of 100 km / h, and the flow state of the adhesive sealant after the run was examined. The evaluation results were obtained by drawing 20 x 40 squares of 5 mm grid lines on the surface of the sealant layer before the run, and counting the number of squares whose shape was distorted after the run. If no flow of the adhesive sealant was observed at all (the number of distorted squares was 0), it was indicated as "good", if the number of distorted squares was less than 1 / 4 of the total, it was indicated as "passable", and if the number of distorted squares was 1 / 4 or more of the total, it was indicated as "not good".
[0055] Load durability Each adhesive sealant immediately after vulcanization was attached to the radially inner side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire. The test tire was then mounted on a wheel with a rim size of 20 x 9J and attached to a drum testing machine, and the load was increased by 10% every hour (up to a maximum of 250%) under the conditions of an air pressure of 250 kPa, an initial load of 8.5 kN, and a running speed of 80 km / h, and the running distance until the tire failed was measured. The evaluation results were shown on a five-point scale as follows. A score of "3" or higher indicates sufficient load durability, and a higher score indicates better load durability. 5: Mileage is over 1200km 4: Mileage is between 1040km and 1200km 3: Mileage is between 880km and 1040km 2: Mileage is between 640km and 880km 1: Mileage less than 640km
[0056] fast durability Each adhesive sealant immediately after vulcanization was attached to the inner radial side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire. The test tire was then mounted on a wheel with a rim size of 20x9J and mounted on a drum testing machine, and the tire was driven for 1 hour at an initial speed of 200km / h under conditions of an air pressure of 250kPa and an initial load of 8.5kN, and then driven for another hour at a speed of 220km / h. After that, the speed was increased by 20km / h every hour, and the running distance until the tire broke down was measured. The evaluation results were shown on a 5-point scale as follows. If the evaluation result score was "3" or more, it meant that the tire exhibited sufficient load durability, and the higher the score, the better the load durability. 5: Mileage is over 2160km 4: Mileage is between 1,500km and 2,160km 3: Mileage is between 920km and 1500km 2: Mileage is between 660km and 920km 1: Mileage less than 660km
[0057] Adhesiveness Each adhesive sealant immediately after vulcanization was attached to the inner side of the inner liner layer in the tread of a pneumatic tire (tire size: 255 / 40R20) having the basic structure shown in Figure 1 to produce a test tire. Each test tire was then mounted on a wheel with a rim size of 20 x 9J and mounted on a test vehicle. After running 100,000 km under the conditions of an air pressure of 250 kPa, a load of 5.0 kN, and a speed of 80 km / h, the peeling state of the adhesive sealant at the splice of the adhesive sealant was visually confirmed. The evaluation results were as follows: "Good" if no peeling occurred, "Fair" if the area where peeling occurred was less than 1 / 3 of the width of the sealant layer from the end of the splice in the tire width direction, and "Not Good" if the area where peeling occurred was 1 / 3 or more of the width of the sealant layer from the end of the splice in the tire width direction.
[0058] [Table 1]
[0059] The types of raw materials used in Table 1 are shown below. Chlorinated butyl rubber: JSR CHLOROBUTYL1066 Natural rubber: SRI TRANG natural rubber Carbon black: Seast KH manufactured by Tokai Carbon Co., Ltd. Sulfur: small lump sulfur manufactured by Hosoi Chemical Industries Quinone dioxime: Valnoc GM manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Crosslinking aid: Thiuram-based vulcanization accelerator, Noccela TT-P manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Organic peroxide: Di-(2-t-butylperoxyl)isopropylbenzene, NOF Corp. Perbutyl P-40 (1-minute half-life temperature: 175°C) Liquid polymer 1: Aromatic oil, Diana Process Oil AH-58 (molecular weight: 1000) manufactured by Idemitsu Kosan Co., Ltd. Liquid polymer 2: Paraffin oil, Kaneda Hicoll K-350 (molecular weight: 850)
[0060] As is clear from Table 1, the sealant material compositions of Examples 1 and 2, when used as a sealant layer of a self-sealing type pneumatic tire, exhibited good sealing properties both immediately after production and after storage under the above-mentioned conditions. That is, the sealant material compositions were able to maintain good sealing properties over a long period of time. In addition, the sealant material compositions were able to ensure adhesion to the tire and suppress flow of the sealant during running. In addition, the tire durability (load durability and high-speed durability) was also able to be exhibited well. On the other hand, Comparative Example 1 did not contain sulfur and did not satisfy the conditions of shear modulus and tan δ, so the sealant property deteriorated after storage under the above-mentioned conditions. In addition, the flowability could not be suppressed, and the tire durability (load durability and high-speed durability) also deteriorated. Comparative Example 2 contained a small amount of sulfur, did not contain a plasticizer component (liquid polymer), and did not satisfy the conditions of tan δ, so the sealant property deteriorated after storage under the above-mentioned conditions. In addition, the flowability could not be suppressed, and the tire durability (load durability and high-speed durability) also deteriorated. Comparative Example 3 did not satisfy the conditions of shear modulus and tan δ, and therefore the sealing property deteriorated after storage under the above-mentioned conditions. In addition, the fluidity could not be suppressed, and the durability of the tire (load durability and high-speed durability) also deteriorated. Comparative Examples 5 to 7 contained quinone dioxime instead of sulfur, and therefore the adhesion to the tire could not be ensured. [Explanation of symbols]
[0061] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt reinforcement layer 9 Inner liner layer 10 Sealant Layer CL Tire Equator
Claims
1. A sealant material composition constituting a sealant layer disposed on an inner surface of a pneumatic tire, comprising: 100 parts by mass of a rubber component containing 10% by mass or more of butyl rubber is blended with 1 part by mass to 40 parts by mass of an organic peroxide, 0.1 parts by mass to 40 parts by mass of sulfur, more than 0 part by mass and less than 1 part by mass of a cross-linking aid, and 50 parts by mass to 400 parts by mass of a plasticizer component, A vulcanizate of the sealant material composition has a shear modulus of 5 kPa to 30 kPa at 20°C, a shear modulus of 1 kPa to 10 kPa at 80°C, and a maximum value of tan δ measured in a temperature range of 20°C to 100°C of 1.0 or less.
2. A sealant material composition as described in claim 1, characterized in that the shear modulus of the vulcanizate of the sealant material composition at 40°C is 5 kPa to 30 kPa, and the shear modulus at 100°C is 1 kPa to 10 kPa.
3. 3. The sealant material composition according to claim 1, wherein the butyl rubber comprises a chlorinated butyl rubber, and the amount of the chlorinated butyl rubber is 5% by mass or more relative to 100% by mass of the rubber component.
4. 4. The sealant material composition according to claim 1, wherein the plasticizer component is a liquid polymer.
5. A sealant material composition according to any one of claims 1 to 3, characterized in that the plasticizer component is selected from paraffin oil, polybutene oil, polyisoprene oil, polybutadiene oil, and aromatic oil.
6. 6. The sealant material composition according to claim 5, wherein the plasticizer component is paraffin oil.
7. 7. The sealant material composition according to claim 6, wherein the molecular weight of the paraffin oil is 800 or more.
8. A pneumatic tire comprising a sealant layer made of an adhesive sealant obtained by vulcanizing the sealant composition according to any one of claims 1 to 7.
9. 9. The pneumatic tire according to claim 8, wherein the adhesive sealant is vulcanized at a vulcanization temperature of 150° C. or higher for a vulcanization time of 5 to 60 minutes.
Citation Information
Patent Citations
Selffsealed air tire
JP1980022591A
JP2006‐152110A
Tires with self-sealing plies
JP2010513120A
Rubber composition for sealant material