Abrasive composition
The polishing liquid composition with optimized silica particles and controlled conditions addresses silica residue and scratches, enhancing substrate quality and productivity in magnetic disk drives.
Patent Information
- Application Number
- JP2023188703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-17
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2043-11-02
AI Technical Summary
The increasing recording density in magnetic disk drives leads to silica particles remaining on the substrate surface after polishing, causing drive failures and surface scratches, which conventional polishing liquid compositions fail to address effectively.
A polishing liquid composition containing silica particles with specific ignition loss and particle size distribution, optimized to reduce silica residue and scratches, using a multi-stage polishing method with a polishing liquid kit and controlled polishing conditions.
The composition effectively reduces silica residue and scratches on the substrate surface, improving substrate quality and productivity by minimizing drive failures and enhancing polishing efficiency.
Smart Images

Figure 0007587661000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polishing composition, a method for producing a magnetic disk substrate, and a method for polishing a substrate. [Background technology]
[0002] In recent years, magnetic disk drives have become smaller and have larger capacities, and there is a demand for higher recording density. To achieve higher recording density, it is necessary to reduce the unit recording area and improve the detection sensitivity of the weakened magnetic signal. For this reason, technological development is being carried out to lower the flying height of the magnetic head. In order to lower the flying height of the magnetic head and ensure the recording area, magnetic disk substrates are strictly required to improve smoothness and flatness (reduce surface roughness, waviness, and edge sagging) and reduce surface defects (reduce residual abrasive grains, scratches, protrusions, pits, etc.).
[0003] In response to such demands, in order to improve the surface quality (smoothness and less scratches) and productivity, a multi-stage polishing method having two or more polishing steps is often adopted in the manufacturing method of magnetic disk substrates. In general, to meet the demand for smoothness, an abrasive containing colloidal silica particles is used, and in order to improve productivity, a polishing composition containing alumina particles as abrasive particles is used. However, when alumina particles are used as abrasive particles, the penetration of the alumina particles into the substrate may cause defects in the magnetic disk substrate or the magnetic disk having a magnetic layer applied to the magnetic disk substrate.
[0004] Therefore, for example, Patent Documents 1 and 2 propose polishing compositions that do not contain alumina particles but contain silica particles as abrasive grains. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-19978 A [Patent Document 2] JP 2021-175774 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, with the increasing recording density of magnetic disk drives, the read head is positioned within a few nanometers of the substrate that rotates at high speed. Drive failures have occurred due to the low position of the read head. As a result of the inventors' investigation, it was found that silica particles remaining on the substrate surface after polishing (hereinafter also referred to as "silica residue") are one of the causes of drive failure. In particular, it was found that even silica residues that cannot be detected by a scanning electron microscope (SEM) after finish polishing are one of the causes of drive failure. Furthermore, as the capacity of magnetic disk drives increases, the requirements for the surface quality of substrates become more stringent, and there is a demand for the development of a polishing composition that can further reduce scratches on the substrate surface. In the present disclosure, "silica residue" is a general term for silica particles remaining on the substrate to be polished, and can be expressed as the number of particles per unit area. In one or more embodiments, "silica residue" includes silica particles that are simply in contact with the substrate, silica particles that are electrostatically bonded to the substrate, and silica particles that are partially embedded in the substrate.
[0007] Therefore, in one aspect, the present disclosure provides a polishing composition that can reduce silica residue and scratches on a substrate surface after polishing. [Means for solving the problem]
[0008] In one aspect, the present disclosure relates to a polishing liquid composition comprising silica particles and an aqueous medium, wherein the silica particles have an ignition loss of 2% or less on a dry weight basis, and the silica particles have a particle size D90 of 65 nm or less, where D90 is the particle size at which a cumulative frequency from the small particle size side is 90% in a particle size distribution calculated by weight conversion obtained by a centrifugal sedimentation method.
[0009] In one aspect, the present disclosure relates to a method for producing a magnetic disk substrate, the method including a polishing step of polishing a substrate to be polished with the polishing liquid composition of the present disclosure.
[0010] In one aspect, the present disclosure relates to a method for polishing a substrate, comprising polishing a substrate to be polished with the polishing liquid composition of the present disclosure, wherein the substrate to be polished is a substrate used in the manufacture of magnetic disk substrates.
[0011] In one aspect, the present disclosure relates to a method for reducing residual silica on a substrate after polishing, the method comprising polishing a substrate to be polished with the polishing liquid composition of the present disclosure.
[0012] In one aspect, the present disclosure relates to a method for manufacturing a magnetic disk substrate, comprising the steps of: selecting silica particles as abrasive grains having an ignition loss of 2% or less on a dry weight basis and a D90 of 65 nm or less, where D90 is the particle diameter at which a cumulative frequency from the small particle size side in a particle size distribution converted by weight obtained by centrifugal sedimentation is 90%, and polishing a substrate to be polished using a polishing liquid composition containing the silica particles and an aqueous medium. Effect of the Invention
[0013] According to one aspect of the present disclosure, it is possible to provide a polishing composition that can reduce silica residue and scratches on a substrate surface after polishing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The silica particles (silica residues) remaining on the substrate surface after polishing are time-consuming to measure, and are rarely recognized as an item for evaluating the quality of the substrate surface after polishing, nor have they been recognized as a cause of drive failure. Note that the "silica residues" that were considered a problem in the prior art are physical defects such as particles stuck in scratches or piercing the surface, and are relatively easily detectable by model testing using simple cleaning or by using an electron microscope, and therefore have different problems and effects from the "silica residues" in this disclosure. In Patent Document 1, since heat-treated silica, which generally has a high surface hardness, is used, there is a problem that the substrate surface tends to have many dent defects and protrusions. In addition, in Patent Document 2, a high polishing rate and excellent substrate surface quality are compatible, but a further improvement in the polishing rate is desired in terms of improving substrate productivity. However, Patent Documents 1 and 2 do not address the issue of reducing residual silica. In the present disclosure, by using residual silica at a level that cannot be detected by a scanning electron microscope (SEM) but is detected by inductively coupled plasma mass spectrometry (ICP-MS) as an indicator, in one or a plurality of embodiments, it is possible to reduce the residual silica to a level that is difficult to detect by fluorescent X-ray analysis. The present disclosure is based, in one aspect, on the discovery that the amount of residual silica, which is undetectable by scanning electron microscopy (SEM) and detected by inductively coupled plasma mass spectrometry (ICP-MS), correlates with the loss on ignition of silica particles having a given particle size distribution.
[0015] That is, in one aspect, the present disclosure relates to a polishing liquid composition (hereinafter also referred to as "the polishing liquid composition of the present disclosure") that contains silica particles and an aqueous medium, wherein the silica particles have an ignition loss of 2% or less on a dry weight basis, and the silica particles have a particle diameter D90 of 65 nm or less, where D90 is the particle diameter at which a cumulative frequency from the small particle diameter side is 90% in a particle size distribution converted into weight obtained by centrifugal sedimentation.
[0016] The mechanism by which the effects of the present disclosure are manifested is not clear, but is speculated as follows. As a result of the study by the inventors, it is believed that the residual silica that leads to drive failure is related to D90, which means the ratio of large diameter particles. Large diameter particles have a large force to transmit the polishing load to the substrate to be polished, so they are more likely to remain on the substrate. However, simply reducing D90 reduces the polishing speed, resulting in a trade-off. Another factor that causes the residual silica is thought to be the hydrogen bond between the silanol group of the silica particle and the substrate surface. However, the amount of residual silica shows only a weak correlation with the "silanol group density" of the silica particle compared to the ignition loss of the silica particle. It is believed that a further mechanism is involved in the correlation between the amount of residual silica and the ignition loss. The silanol group density is generally determined by titration, and only the silanol groups on the outermost surface are detected. On the other hand, the ignition loss detects all silanol groups, including those inside the particles. In addition, a high load is applied to the particles during polishing, and it is believed that some particles collapse and the internal silanol groups are exposed. Since these internal silanol groups are also thought to be involved in the residual silica on the substrate, it is believed that processing to a state where the ignition loss is small (for example, forming a dense particle structure by slowing the growth rate of silica particles) contributes to reducing the residual silica. Furthermore, by reducing D90, not only can the residual silica be reduced, but also the coarse particles that cause localized damage can be reduced, which is thought to reduce scratches as well. However, the present disclosure need not be construed as being limited to these mechanisms.
[0017] In the present disclosure, unless otherwise specified, the silica residue refers to the amount of silica residue detected by inductively coupled plasma mass spectrometry (ICP-MS). Specifically, it can be evaluated by the method described in the Examples. In one or more embodiments, the silica residue refers to the amount of silica residue detected by inductively coupled plasma mass spectrometry (ICP-MS) that is not detectable by scanning electron microscope (SEM). In the present disclosure, scratches on the substrate surface can be detected, for example, by an optical defect inspection device and can be quantitatively evaluated as the number of scratches. The number of scratches can be specifically evaluated by the method described in the Examples.
[0018] [Silica particles A (component A)] The polishing liquid composition of the present disclosure contains silica particles A (hereinafter also referred to as "component A") as abrasive grains. In one or more embodiments, the silica particles A (component A) are silica particles having an ignition loss of 2% or less on a dry weight basis, and a D90 of 65 nm or less, where D90 is the particle diameter at which the cumulative frequency from the small particle diameter side is 90% in a particle size distribution in weight conversion obtained by centrifugal sedimentation. The use form of component A is preferably a slurry-like polishing liquid component. Component A may be used alone or in combination of two or more types.
[0019] From the viewpoint of improving the polishing rate, the particle diameter D10 of component A in terms of weight measured by centrifugal sedimentation is preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 11 nm or more, and from the viewpoint of improving the substrate surface quality, it is preferably 35 nm or less, more preferably 25 nm or less, and even more preferably 14 nm or less. More specifically, the particle diameter D10 of component A measured by centrifugal sedimentation is preferably 5 nm or more and 35 nm or less, more preferably 10 nm or more and 25 nm or less, and even more preferably 11 nm or more and 14 nm or less.
[0020] From the viewpoint of improving the polishing rate, the particle diameter D50 of component A in terms of weight as measured by centrifugal sedimentation is preferably 10 nm or more, more preferably 15 nm or more, and even more preferably 17 nm or more, and from the viewpoint of improving the substrate surface quality, it is preferably 40 nm or less, more preferably 30 nm or less, and even more preferably 20 nm or less. More specifically, the particle diameter D50 of component A as measured by centrifugal sedimentation is preferably 10 nm or more and 40 nm or less, more preferably 15 nm or more and 30 nm or less, and even more preferably 17 nm or more and 20 nm or less.
[0021] The particle diameter D90 of component A in terms of weight conversion by centrifugal sedimentation method is 65 nm or less, preferably 60 nm or less, more preferably 55 nm or less, and even more preferably 52 nm or less, from the viewpoint of reducing scratches, and from the viewpoint of improving the polishing rate, it is preferably 30 nm or more, more preferably 35 nm or more, and even more preferably 39 nm or more or 40 nm or more. More specifically, the particle diameter D90 of component A by centrifugal sedimentation method is preferably 30 nm or more and 60 nm or less, more preferably 35 nm or more and 55 nm or less, more preferably 39 nm or more and 52 nm or less, or even more preferably 40 nm or more and 52 nm or less.
[0022] In the present disclosure, D10, D50 and D90 refer to particle sizes at which the cumulative frequency from the small diameter side is 10%, 50% and 90%, respectively, in the particle size distribution in weight conversion obtained by centrifugal sedimentation. In the present disclosure, the centrifugal sedimentation is, in one or more embodiments, a method of classifying and detecting particles by size based on the difference in sedimentation velocity (disk centrifugal sedimentation light transmission method). The particle size distribution by centrifugal sedimentation can be measured, for example, using a disk centrifugal particle size distribution measuring device (CPS Disc Centrifuge). In the following description, the particle size distribution by centrifugal sedimentation is sometimes referred to as "particle size distribution by CPS measurement". Specifically, it can be calculated by the measurement method described in the examples.
[0023] Examples of the method for adjusting the particle size distribution of component A by centrifugal sedimentation include a method for adjusting the particle growth time, particle temperature, particle concentration, etc. during the growth process of silica particles. Other embodiments of the method for adjusting the particle size distribution of component A by centrifugal sedimentation include a method for providing a desired particle size distribution by adding new core particles during the particle growth process in the production stage, and a method for providing a desired particle size distribution by mixing two or more types of silica particles having different particle size distributions.
[0024] From the viewpoint of improving the polishing rate and reducing scratches, the average secondary particle diameter of component A is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more, and from the same viewpoint, it is preferably 500 nm or less, more preferably 300 nm or less, more preferably 100 nm or less, more preferably 70 nm or less, more preferably 40 nm or less, and even more preferably less than 40 nm. More specifically, the average secondary particle diameter of component A is preferably 1 nm or more and 500 nm or less, more preferably 1 nm or more and 300 nm or less, more preferably 1 nm or more and 100 nm or less, more preferably 5 nm or more and 70 nm or less, more preferably 10 nm or more and 40 nm or less, and even more preferably 10 nm or more and less than 40 nm. In the present disclosure, the average secondary particle diameter of component A refers to the average particle diameter based on the scattering intensity distribution measured by dynamic light scattering. In the present disclosure, the "scattering intensity distribution" refers to the particle size distribution of submicron or smaller particles calculated by dynamic light scattering (DLS) or quasielastic light scattering (QLS) in terms of volume. The average secondary particle size of component A in the present disclosure can be specifically obtained by the method described in the Examples.
[0025] The ignition loss of component A on a dry weight basis is 2% or less, preferably 1.9% or less, more preferably 1.6% or less, and even more preferably 1.5% or less, from the viewpoint of reducing residual silica, and is preferably 0% or more, more preferably 0.5% or more, and even more preferably 1.0% or more, from the viewpoint of storage stability. More specifically, the ignition loss of component A on a dry weight basis is preferably 0% or more and 1.9% or less, more preferably 0.5% or more and 1.6% or less, and even more preferably 1.0% or more and 1.5% or less. In the present disclosure, the loss on ignition based on the dry weight of component A (hereinafter, simply referred to as "loss on ignition") is, in one or more embodiments, a sample is prepared by mixing component A with water to form a silica slurry, drying the mixture at a constant temperature between 105°C and 180°C, leaving the mixture to stand and return to room temperature, and then drying the mixture at a constant temperature between 105°C and 180°C. The loss on drying LOD (wt%) and the loss on ignition LOI (wt%) after the sample is heat-treated at 800°C or higher are measured, and the value is calculated from the following formula. Specifically, it can be calculated by the method described in the Examples. It can be evaluated that the smaller the loss on ignition, the smaller the total number of silanol groups contained in 1g of component A. Loss on ignition of component A on a dry weight basis = 100 x {1-(100-LOI) / (100-LOD)}
[0026] Examples of the method for adjusting the ignition loss of component A include a method for adjusting the dropping speed, reaction temperature, and concentration of the silicic acid liquid during the growth process of the silica particles. Other embodiments of the method for adjusting the ignition loss of component A include a method for adjusting the desired ignition loss by subjecting existing silica particles to heat treatment, metal modification of surface silanol groups, organic acid modification, and silane coupling treatment, and a method for mixing two or more types of silica particles having different ignition losses to give the desired ignition loss.
[0027] An index showing a stronger correlation with silica residue than "loss on ignition" is "the value represented by the following formula (I) when WL is the loss on ignition based on the dry weight of component A". From the viewpoint of reducing silica residue, the value represented by the following formula (I) when WL is the loss on ignition based on the dry weight of component A is preferably 5 or less, more preferably 2.5 or less, and even more preferably 2 or less, and from the viewpoint of maintaining the polishing rate and storage stability, it is preferably 0 or more, more preferably 0.1 or more, and even more preferably 0.5 or more. More specifically, the value represented by the following formula (I) is preferably 0 or more and 5 or less, more preferably 0.1 or more and 2.5 or less, and even more preferably 0.5 or more and 2 or less. {(WL) 3 ×D90} / 100 (I) By adjusting the value represented by the above formula (I) to a predetermined value or less, it is possible to achieve both a high effect of reducing residual silica and a good removal rate.
[0028] Examples of component A include colloidal silica, precipitated silica, fumed silica, pulverized silica, and surface-modified silica thereof. From the viewpoints of improving the polishing rate and easy availability, component A is preferably at least one selected from colloidal silica and precipitated silica, and from the viewpoints of improving the polishing rate and improving the quality of the substrate, such as reducing scratches, colloidal silica, which is less likely to give a sharp surface shape or localized high surface hardness sites, is more preferable. The colloidal silica may be obtained, for example, by a method of particle growth using an aqueous solution of alkali silicate as a raw material (hereinafter also referred to as the "water glass method"), or by a method of condensation of a hydrolyzate of an alkoxysilane (hereinafter also referred to as the "sol-gel method"). From the viewpoint of ease of production and economic efficiency, the silica obtained by the water glass method is preferred. Silica particles obtained by the water glass method and the sol-gel method can be produced by a conventionally known method. The precipitated silica is silica particles obtained by a precipitation method. Examples of methods for producing precipitated silica particles include known methods such as those described in Tosoh Research and Technology Report, Vol. 45 (2001), pp. 65-69. Specific examples of methods for producing precipitated silica particles include a precipitation method in which silica particles are precipitated by a neutralization reaction between a silicate such as sodium silicate and a mineral acid such as sulfuric acid. The neutralization reaction is preferably carried out under alkaline conditions at a relatively high temperature, whereby the growth of primary silica particles proceeds quickly, and the primary particles are aggregated and precipitated in the form of flocks, which are preferably further pulverized to obtain precipitated silica particles.
[0029] The shape of component A may be a so-called spherical shape and / or a so-called cocoon shape, from the viewpoints of improving the removal rate and reducing scratches. As component A, from the viewpoints of improving the polishing rate and reducing scratches, spherical silica is preferably used.
[0030] From the viewpoint of improving the polishing rate, the average aspect ratio of component A is preferably 1.00 or more, more preferably 1.02 or more, and from the viewpoint of reducing scratches, it is preferably 1.20 or less, more preferably 1.1 or less, and even more preferably 1.06 or less. More specifically, the average aspect ratio of component A is preferably 1.00 or more and 1.20 or less, more preferably 1.02 or more and 1.1 or less, and even more preferably 1.02 or more and 1.06 or less.
[0031] The content of component A in the polishing liquid composition of the present disclosure is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and even more preferably 1.5% by mass or more from the viewpoint of improving the polishing rate and reducing scratches, and is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and even more preferably 10% by mass or less from the viewpoint of economic efficiency. More specifically, the content of component A in the polishing liquid composition of the present disclosure is preferably 0.1% by mass or more and 30% by mass or less, more preferably 0.5% by mass or more and 20% by mass or less, even more preferably 1% by mass or more and 15% by mass or less, and even more preferably 1.5% by mass or more and 10% by mass or less. When component A is composed of two or more kinds of silica particles, the content of component A refers to the total content thereof.
[0032] [Aqueous medium] The aqueous medium contained in the polishing liquid composition of the present disclosure may be water such as distilled water, ion-exchanged water, pure water, and ultrapure water, or a mixed solvent of water and a solvent. The above-mentioned solvent may be a solvent miscible with water (e.g., alcohol such as ethanol). When the aqueous medium is a mixed solvent of water and a solvent, the proportion of water to the entire mixed medium is not particularly limited as long as the effects of the present disclosure are not hindered. From the viewpoint of economy, for example, 95% by mass or more is preferable, 98% by mass or more is more preferable, and substantially 100% by mass is even more preferable. The content of the aqueous medium in the polishing liquid composition of the present disclosure can be the remainder excluding component A and any optional components (component B, component C, and other components) described below that are blended as necessary.
[0033] [Acid (component B)] The polishing composition of the present disclosure may contain an acid (hereinafter also referred to as "Component B") from the viewpoint of further improving the polishing rate and further reducing scratches. In the present disclosure, the use of an acid includes the use of an acid and / or a salt thereof. Component B may be one type or a combination of two or more types. Examples of component B include inorganic acids such as nitric acid, sulfuric acid, sulfurous acid, persulfuric acid, hydrochloric acid, perchloric acid, phosphoric acid, phosphonic acid, phosphinic acid, pyrophosphoric acid, polyphosphoric acid, and amidosulfuric acid; organic acids such as organic phosphoric acid and organic phosphonic acid; and the like. Among them, from the viewpoint of further improving the polishing rate and further reducing scratches, component B is preferably at least one selected from phosphoric acid, sulfuric acid, and 1-hydroxyethylidene-1,1-diphosphonic acid, more preferably at least one selected from sulfuric acid and phosphoric acid, and even more preferably phosphoric acid. Examples of salts of these acids include salts of the above acids and at least one selected from metals, ammonia, and alkylamines. Specific examples of the above metals include metals belonging to Groups 1 to 11 of the periodic table. Among them, from the viewpoint of further improving the polishing rate and further reducing scratches, salts of the above acids and metals belonging to Group 1 or ammonia are preferred.
[0034] When the polishing liquid composition of the present disclosure contains component B, the content of component B in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, from the viewpoint of further improving the polishing rate and further reducing scratches, and from the same viewpoint, it is preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 3 mass% or less, and even more preferably 2.5 mass% or less. More specifically, the content of component B in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more and 5 mass% or less, more preferably 0.01 mass% or more and 4 mass% or less, even more preferably 0.05 mass% or more and 3 mass% or less, and even more preferably 0.1 mass% or more and 2.5 mass% or less. When component B is a combination of two or more kinds, the content of component B refers to the total content thereof.
[0035] [Oxidizing agent (component C)] The polishing composition of the present disclosure may contain an oxidizing agent (hereinafter also referred to as "Component C") from the viewpoint of further improving the polishing rate and further reducing scratches. Component C may be one type or a combination of two or more types. From the same viewpoint, examples of component C include peroxides, permanganic acid or its salts, chromic acid or its salts, peroxoacids or its salts, oxyacids or its salts, nitric acids, sulfuric acids, etc. Among these, component C is preferably at least one selected from hydrogen peroxide, iron(III) nitrate, peracetic acid, ammonium peroxodisulfate, iron(III) sulfate, and ammonium iron(III) sulfate, and hydrogen peroxide is more preferable from the viewpoints of increasing the polishing rate, preventing metal ions from adhering to the surface of the substrate to be polished, and ease of availability.
[0036] When the polishing liquid composition of the present disclosure contains component C, the content of component C in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.1 mass% or more from the viewpoint of further improving the polishing rate, and is preferably 4 mass% or less, more preferably 2 mass% or less, and even more preferably 1.5 mass% or less from the viewpoint of further improving the polishing rate and further reducing scratches. More specifically, the content of component C in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more and 4 mass% or less, more preferably 0.05 mass% or more and 2 mass% or less, and even more preferably 0.1 mass% or more and 1.5 mass% or less. When component C is a combination of two or more kinds, the content of component C refers to the total content thereof.
[0037] [Nitrogen-containing compounds (component D)] The polishing liquid composition of the present disclosure may further contain a nitrogen-containing compound (hereinafter also referred to as "component D") from the viewpoint of improving the polishing rate without significantly increasing the amount of silica residue. In one or more embodiments, component D is an organic amine compound having 10 or less nitrogen atoms in the molecule. From the viewpoint of improving the polishing rate without significantly increasing the amount of silica residue, component D is preferably one or more compounds having any of primary to tertiary amino groups. In one or more embodiments, component D may have a hydroxyl group from the viewpoint of workability taking into account odor and / or boiling point. Component D may be one type or a combination of two or more types.
[0038] From the viewpoint of improving the polishing rate without significantly increasing the amount of residual silica, the number of nitrogen atoms in the molecule of component D is preferably 10 or less, more preferably 5 or less, even more preferably 4 or less, and even more preferably 2 or less.
[0039] From the viewpoint of improving the polishing rate without significantly increasing the amount of residual silica, in one or a plurality of embodiments, Component D may be at least one compound selected from an aliphatic amine compound having 10 or less nitrogen atoms in the molecule and an alicyclic amine compound having 10 or less nitrogen atoms in the molecule. From the same viewpoint, examples of the aliphatic amine compound include at least one selected from monoethanolamine, ethylenediamine, N,N,N',N'-tetramethylethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, 3-(diethylamino)propylamine, 3-(dibutylamino)propylamine, 3-(methylamino)propylamine, 3-(dimethylamino)propylamine, N-aminoethylethanolamine, N-(2-aminoethyl)diethanolamine, N-aminoethylisopropanolamine, N-aminoethyl-N-methylethanolamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine. Among these, at least one selected from monoethanolamine (MEA), N-aminoethylethanolamine (AEA), and tetraethylenepentamine (TEPA) is preferred, and monoethanolamine (MEA) and / or N-aminoethylethanolamine (AEA) are more preferred. From the same viewpoint, examples of the alicyclic amine compound include at least one selected from piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, 1-amino-4-methylpiperazine, N-methylpiperazine, 1-(2-aminoethyl)piperazine, hydroxyethylpiperazine, and piperazine-1,4-bisethanol, and among these, hydroxyethylpiperazine (HEP) is preferred.
[0040] In one or a plurality of embodiments, from the viewpoint of improving the polishing rate without significantly increasing the amount of residual silica, Component D has a molecular weight of preferably 60 or more and 500 or less, more preferably 60 or more and 300 or less, even more preferably 60 or more and 150 or less, and still more preferably 60 or more and 135 or less.
[0041] When the polishing liquid composition of the present disclosure contains component D, the content of component D in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, and even more preferably 0.05 mass% or more from the viewpoint of improving the polishing rate without significantly increasing the silica residue, and from the same viewpoint, it is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 1 mass% or less. More specifically, the content of component D in the polishing liquid composition of the present disclosure is preferably 0.001 mass% or more and 10 mass% or less, more preferably 0.01 mass% or more and 5 mass% or less, and even more preferably 0.05 mass% or more and 1 mass% or less. When component D is a combination of two or more types, the content of component D refers to the total content thereof.
[0042] In one or more embodiments, the mass ratio D / A of the content of component D to the content of component A in the polishing liquid composition of the present disclosure is preferably 0.00018 or more, more preferably 0.0018 or more, and even more preferably 0.0054 or more, from the viewpoint of improving the polishing rate without significantly increasing the silica residue, and from the same viewpoint, is preferably 0.18 or less, more preferably 0.09 or less, and even more preferably 0.054 or less. More specifically, the mass ratio D / A in the polishing liquid composition of the present disclosure is preferably 0.00018 or more and 0.18 or less, more preferably 0.0018 or more and 0.09 or less, and even more preferably 0.0054 or more and 0.054 or less.
[0043] [Other ingredients] The polishing liquid composition of the present disclosure may contain other components as necessary. Examples of other components include corrosion inhibitors, thickeners, dispersants, rust inhibitors, basic substances, surfactants, water-soluble polymers, etc. The other components are preferably contained in the polishing liquid composition within a range that does not impair the effects of the present disclosure. When the polishing liquid composition of the present disclosure contains other components, the content of the other components in the polishing liquid composition of the present disclosure is preferably more than 0 mass%, more preferably 0.1 mass% or more, and preferably 10 mass% or less, and more preferably 5 mass% or less. More specifically, the content of the other components in the polishing liquid composition of the present disclosure is preferably more than 0 mass% and 10 mass% or less, more preferably 0.1 mass% or more and 10 mass% or less, and even more preferably 0.1 mass% or more and 5 mass% or less.
[0044] [Alumina abrasive grains] From the viewpoint of reducing protrusion defects, the polishing liquid composition of the present disclosure preferably does not substantially contain alumina abrasive grains. In the present disclosure, "substantially does not contain alumina abrasive grains" may include, in one or more embodiments, not containing alumina particles, not containing an amount of alumina particles that functions as abrasive grains, or not containing an amount of alumina particles that affects the polishing result. Specifically, in one or more embodiments, the content of alumina abrasive grains in the polishing liquid composition of the present disclosure is preferably 5% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, even more preferably 0.1% by mass or less, even more preferably 0.05% by mass or less, even more preferably 0.02% by mass or less, and even more preferably substantially 0% by mass (i.e., not contained). In addition, in one or more embodiments, the content of alumina particles in the polishing liquid composition of the present disclosure is preferably 2% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and even more preferably substantially 0% by mass (i.e., not contained), based on the total amount of abrasive grains in the polishing liquid composition.
[0045] [pH] The pH of the polishing composition of the present disclosure is preferably 0.5 or more, more preferably 0.7 or more, even more preferably 0.9 or more, and even more preferably 1 or more, from the viewpoint of improving the polishing rate and reducing scratches, and from the same viewpoint, it is preferably 9 or less, more preferably 6 or less, even more preferably 4 or less, even more preferably 3 or less, even more preferably 2.5 or less, and even more preferably 2 or less. More specifically, the pH of the polishing composition of the present disclosure is preferably 0.5 to 9 or less, more preferably 0.5 to 6 or less, even more preferably 0.7 to 4 or less, even more preferably 1 to 3 or less, even more preferably 1 to 2.5 or less, and even more preferably 1 to 2 or less. The pH can be adjusted using the above-mentioned acid (component B) or a known pH adjuster. The above pH is the pH of the polishing composition at 25°C, and can be measured using a pH meter, and is preferably the value 2 minutes after immersing the electrode of the pH meter in the polishing composition.
[0046] [Method of manufacturing the polishing composition] The polishing liquid composition of the present disclosure can be produced, for example, by blending component A, an aqueous medium, and optional components (component B, component C, component D, and other components) as necessary by a known method. Therefore, in one aspect, the present disclosure relates to a method for producing a polishing liquid composition, which includes a step of blending at least component A and an aqueous medium. In the present disclosure, "blending" includes mixing component A, an aqueous medium, and optional components (component B, component C, component D, and other components) as necessary simultaneously or in any order. The blending can be performed using a mixer such as a homomixer, a homogenizer, an ultrasonic disperser, and a wet ball mill. The preferred blending amount of each component in the method for producing a silica slurry and a polishing liquid composition can be the same as the preferred content of each component in the polishing liquid composition according to the present disclosure described above.
[0047] In the present disclosure, the "content of each component in the polishing liquid composition" refers to the content of each component at the time of use, i.e., at the time when the use of the polishing liquid composition for polishing is started. In one or more embodiments, the content of each component in the polishing liquid composition in the present disclosure can be regarded as the blending amount of each component.
[0048] The polishing composition of the present disclosure may be stored and supplied in a concentrated state to the extent that its storage stability is not impaired. In this case, it is preferable in that the manufacturing and transportation costs can be further reduced. The concentrated polishing composition of the present disclosure may be used by diluting it appropriately with the above-mentioned water as necessary when used. The dilution ratio is not particularly limited as long as the content (at the time of use) of each of the above-mentioned components can be secured after dilution, and may be, for example, 10 to 100 times.
[0049] [Polishing liquid kit] In one aspect, the present disclosure relates to a polishing liquid kit for producing the polishing liquid composition of the present disclosure, the polishing liquid kit including a container-containing silica dispersion in which a silica dispersion containing component A and an aqueous medium is contained in a container (hereinafter, also referred to as the "polishing liquid kit of the present disclosure"). The polishing liquid kit according to the present disclosure may further include an aqueous additive solution containing component B, and at least one selected from component C and component D, contained in a container separate from the container-containing silica dispersion. According to the present disclosure, in one or more embodiments, a polishing liquid composition capable of reducing silica residue and scratches on a substrate surface after polishing can be obtained. In one or more embodiments, the polishing liquid kit of the present disclosure may be, for example, a polishing liquid kit (two-liquid type polishing liquid composition) that contains a silica dispersion (slurry) containing component A and an aqueous medium, and an additive aqueous solution containing components B, C, and D as necessary, in a mutually unmixed state, which are mixed at the time of use and diluted with an aqueous medium as necessary. The aqueous medium contained in the silica dispersion may be the entire amount of the aqueous medium used to prepare the polishing liquid composition, or may be a part of it. The silica dispersion and the additive aqueous solution may each contain the above-mentioned other components as necessary.
[0050] [Substrate to be polished] In one or more embodiments, the substrate to be polished is a substrate used for manufacturing a magnetic disk substrate. In one or more embodiments, the surface of the substrate to be polished is polished with the polishing composition of the present disclosure, and then a magnetic layer is formed on the substrate surface by sputtering or the like, thereby manufacturing a magnetic disk substrate.
[0051] The material of the substrate to be polished preferably used in the present disclosure includes, for example, metals or semimetals such as silicon, aluminum, nickel, tungsten, copper, tantalum, titanium, or alloys thereof, glassy materials such as glass, glassy carbon, amorphous carbon, ceramic materials such as alumina, silicon dioxide, silicon nitride, tantalum nitride, titanium carbide, and resins such as polyimide resin. Among them, the substrate to be polished is preferably a substrate to be polished that contains metals such as aluminum, nickel, tungsten, copper, or alloys mainly composed of these metals. As the substrate to be polished, for example, Ni-P plated aluminum alloy substrates, and glass substrates such as crystallized glass, reinforced glass, aluminosilicate glass, and aluminoborosilicate glass are more suitable, and Ni-P plated aluminum alloy substrates are even more suitable. In the present disclosure, the term "Ni-P plated aluminum alloy substrate" refers to an aluminum alloy substrate that has been subjected to electroless Ni-P plating after the surface of the aluminum alloy substrate is ground.
[0052] The shape of the substrate to be polished may be, for example, a shape having a flat surface such as a disk, plate, slab, or prism, or a shape having a curved surface such as a lens, and is preferably a disk-shaped substrate to be polished. In the case of a disk-shaped substrate to be polished, the outer diameter is, for example, 2 to 100 mm, and the thickness is, for example, 0.4 to 2 mm.
[0053] In general, a magnetic disk is manufactured by polishing a substrate that has been subjected to a grinding step through a rough polishing step and a finish polishing step, and then through a magnetic layer forming step. In one or more embodiments, the polishing composition of the present disclosure is preferably used for polishing in the finish polishing step. In one or more embodiments, the polishing composition of the present disclosure is a polishing composition for magnetic disk substrates.
[0054] [Method for reducing residual silica] In one aspect, the present disclosure relates to a method for reducing residual silica on a substrate after polishing, which comprises polishing a substrate to be polished with the polishing liquid composition of the present disclosure (hereinafter, also referred to as the "method for reducing residual silica of the present disclosure"). The substrate to be polished in the method for reducing residual silica of the present disclosure may be the above-mentioned substrate to be polished. In one or more embodiments, the method for reducing silica residue according to the present disclosure may further include selecting silica particles A (component A) contained in the polishing liquid composition according to the present disclosure. In the present disclosure, "selecting silica particles A" includes purchasing a product that describes in a catalog, product manual, label, or the like the physical properties of silica particles A (component A) and / or the ability to reduce silica residue. Therefore, in one or a plurality of embodiments, the method for reducing silica residue of the present disclosure relates to a method for reducing silica residue, comprising selecting silica particles A (component A) and polishing a substrate to be polished using the polishing liquid composition of the present disclosure containing the selected silica particles A (component A). In another aspect, the present disclosure relates to a method for reducing residual silica, comprising: selecting silica particles as abrasive grains, the ignition loss on a dry weight basis being 2% or less, and the particle size D90 being 65 nm or less, where D90 is the particle size at which the cumulative frequency from the small particle size side is 90% in the particle size distribution in weight conversion obtained by centrifugal sedimentation; and polishing a substrate to be polished using a polishing liquid composition containing the silica particles and an aqueous medium. The silica particles in the method for reducing residual silica of this aspect include the above-mentioned silica particles A (component A). The polishing liquid composition in the method for reducing residual silica of this aspect includes the above-mentioned polishing liquid composition of the present disclosure. According to the method for reducing silica residue of the present disclosure, the use of the polishing composition of the present disclosure can reduce silica residue and scratches on the substrate surface after polishing. The specific polishing method and conditions can be the same as those of the substrate manufacturing method of the present disclosure described below.
[0055] [Polishing method] In one aspect, the present disclosure relates to a method for polishing a substrate (hereinafter also referred to as the "polishing method of the present disclosure"), which comprises using the polishing liquid composition of the present disclosure to polish a substrate, and the substrate is a substrate used in the manufacture of a magnetic disk substrate. The substrate to be polished in the polishing method of the present disclosure may be the substrate to be polished described above. The polishing method of the present disclosure may be used, for example, in a final polishing step. According to the polishing method of the present disclosure, by using the polishing composition of the present disclosure, the silica residue and scratches on the substrate surface after polishing can be reduced. Therefore, the productivity of the substrate (e.g., magnetic disk substrate) with improved substrate quality can be improved. The specific polishing method and conditions can be the same as the substrate manufacturing method of the present disclosure described later.
[0056] [Method of manufacturing magnetic disk substrate] In one aspect, the present disclosure relates to a method for producing a magnetic disk substrate (hereinafter also referred to as the "substrate production method of the present disclosure"), which includes a polishing step (hereinafter also referred to as the "polishing step") of polishing a substrate to be polished using the polishing liquid composition of the present disclosure. The polishing step in the substrate production method of the present disclosure is, for example, a finish polishing step. In one or more embodiments, the substrate manufacturing method of the present disclosure may further include a step of selecting silica particles A (component A) contained in the polishing liquid composition of the present disclosure. In the present disclosure, "selecting silica particles A" includes, as described above, purchasing a product that describes in a catalog, product manual, label, etc. the physical properties of silica particles A (component A) and / or the ability to reduce silica residue. Therefore, in one or more embodiments, the substrate manufacturing method of the present disclosure relates to a method for manufacturing a magnetic disk substrate, comprising the steps of selecting silica particles A (component A) and polishing a substrate to be polished using the polishing liquid composition of the present disclosure containing the selected silica particles A (component A). In another aspect, the present disclosure relates to a method for producing a magnetic disk substrate, comprising the steps of selecting silica particles as abrasive grains, the ignition loss on a dry weight basis being 2% or less, and the D90 being 65 nm or less, where D90 is the particle diameter at which the cumulative frequency from the small particle diameter side is 90% in the particle size distribution in weight conversion obtained by centrifugal sedimentation, and polishing a substrate to be polished using a polishing liquid composition containing the silica particles and an aqueous medium. The silica particles in the method for producing a magnetic disk substrate of this aspect include the above-mentioned silica particles (component A). The polishing liquid composition in the method for producing a magnetic disk substrate of this aspect includes the above-mentioned polishing liquid composition of the present disclosure.
[0057] In one or more embodiments, the polishing process is a process in which the polishing liquid composition of the present disclosure is supplied to the surface to be polished of a substrate to be polished, a polishing pad is brought into contact with the surface to be polished, and at least one of the polishing pad and the substrate to be polished is moved to polish the substrate. In one or more embodiments, the polishing step is a step in which a substrate to be polished is sandwiched between a platen having a polishing pad such as a nonwoven organic polymer-based abrasive cloth attached thereto, and the platen and the substrate to be polished are moved while the polishing liquid composition of the present disclosure is supplied to a polishing machine to polish the substrate.
[0058] When the polishing process of the substrate to be polished is carried out in multiple stages, the polishing process using the polishing liquid composition of the present disclosure is preferably carried out in the second stage or later, and more preferably in the final polishing process or the finish polishing process. In this case, in order to avoid the mixing of the abrasive or the polishing liquid composition of the previous process, a separate polishing machine may be used for each step, and when a separate polishing machine is used, it is preferable to wash the substrate to be polished after each polishing process. Furthermore, the polishing liquid composition of the present disclosure can be used in the circulating polishing in which the used polishing liquid is reused. The polishing machine is not particularly limited, and a known polishing machine for substrate polishing can be used.
[0059] The polishing pad used in the present disclosure is not particularly limited, and for example, a suede type, a nonwoven fabric type, a polyurethane independent foam type, or a two-layer type in which these are laminated can be used, and from the viewpoint of polishing speed, a suede type polishing pad is preferred.
[0060] The polishing load in the polishing process using the polishing composition of the present disclosure is preferably 5.9 kPa or more, more preferably 6.9 kPa or more, and even more preferably 7.5 kPa or more from the viewpoint of ensuring the polishing rate, and is preferably 20 kPa or less, more preferably 18 kPa or less, and even more preferably 16 kPa or less from the viewpoint of reducing scratches. In the present disclosure, the "polishing load" refers to the pressure of the platen applied to the polishing surface of the substrate to be polished during polishing. The polishing load can be adjusted by applying air pressure or a weight to at least one of the platen and the substrate to be polished.
[0061] In the polishing process, 2 From the viewpoints of improving the polishing rate and reducing scratches, the polishing amount per cm2 of the substrate to be polished is preferably 0.05 mg or more, more preferably 0.1 mg or more, and even more preferably 0.2 mg or more, and from the same viewpoints, it is preferably 2.5 mg or less, more preferably 2 mg or less, and even more preferably 1.6 mg or less. 2 The amount of polishing per unit is preferably 0.05 mg or more and 2.5 mg or less, more preferably 0.1 mg or more and 2 mg or less, and even more preferably 0.2 mg or more and 1.6 mg or less.
[0062] In the polishing step using the polishing composition of the present disclosure, the supply rate of the polishing composition of the present disclosure is set to 1 cm per 1 cm of the substrate to be polished from the viewpoint of reducing scratches. 2 The flow rate is preferably 0.05 mL / min or more and 15 mL / min or less, more preferably 0.06 mL / min or more and 10 mL / min or less, even more preferably 0.07 mL / min or more and 1 mL / min or less, and even more preferably 0.07 mL / min or more and 0.5 mL / min or less.
[0063] The method of supplying the polishing liquid composition of the present disclosure to the polishing machine can be, for example, a method of continuously supplying the composition using a pump or the like. When supplying the polishing liquid composition to the polishing machine, in addition to a method of supplying the composition as a single liquid containing all components, the composition can be divided into a plurality of blending component liquids and supplied as two or more liquids, taking into consideration the storage stability of the polishing liquid composition. In the latter case, the plurality of blending component liquids are mixed, for example, in the supply pipe or on the substrate to be polished, to form the polishing liquid composition of the present disclosure.
[0064] According to the substrate manufacturing method of the present disclosure, the use of the polishing composition of the present disclosure can reduce residual silica and scratches on the substrate surface after polishing, thereby enabling efficient manufacture of substrates (e.g., magnetic disk substrates) with improved substrate quality.
[0065] [Silica particles] In one aspect, the present disclosure relates to silica particles having an ignition loss of 2% or less on a dry weight basis, and a D90 of 65 nm or less when the particle size D90 is the particle size at which the cumulative frequency from the small particle size side is 90% in the particle size distribution in weight conversion obtained by centrifugal sedimentation (hereinafter, the silica particles having the ignition loss and D90 are also referred to as "silica particles of the present disclosure"). The silica particles of the present disclosure can be suitably used as abrasive grains for polishing magnetic disk substrates. In one or more embodiments, the silica particles of the present disclosure are the above-mentioned component A. The ignition loss of the silica particles of the present disclosure based on dry weight is preferably 1.9% or less, more preferably 1.6% or less, and even more preferably 1.5% or less from the viewpoint of reducing silica residue when the silica particles of the present disclosure are used as abrasive grains for polishing magnetic disk substrates, and from the viewpoint of storage stability, it is preferably 0% or more, more preferably 0.5% or more, and even more preferably 1.0% or more.More specifically, the ignition loss of component A based on dry weight is preferably 0% or more and 1.9% or less, more preferably 0.5% or more and 1.6% or less, and even more preferably 1.0% or more and 1.5% or less. The D90 of the silica particles of the present disclosure is preferably 60nm or less, more preferably 55nm or less, and even more preferably 52nm or less from the viewpoint of reducing scratches when the silica particles of the present disclosure are used as abrasive grains for polishing magnetic disk substrates, and is preferably 30nm or more, more preferably 35nm or more, and even more preferably 40nm or more from the viewpoint of improving polishing speed.More specifically, the D90 of the silica particles of the present disclosure is preferably 30nm or more and 60nm or less, more preferably 35nm or more and 55nm or less, and even more preferably 40nm or more and 52nm or less. When the ignition loss on dry weight basis of the silica particles of the present disclosure is WL, the value represented by the following formula (II) is preferably 5 or less, more preferably 2.5 or less, and even more preferably 2 or less from the viewpoint of reducing silica residue when the silica particles of the present disclosure are used as abrasive grains for polishing magnetic disk substrates, and is preferably 0 or more, more preferably 0.1 or more, and even more preferably 0.5 or more from the viewpoint of maintaining polishing rate and storage stability. More specifically, the value represented by the following formula (II) is preferably 0 or more and 5 or less, more preferably 0.1 or more and 2.5 or less, and even more preferably 0.5 or more and 2 or less. {(WL) 3 ×D90} / 100 (II) The ignition loss on a dry weight basis of the silica particles of the present disclosure, the value represented by formula (II), and D90 are preferably the same as the value represented by formula (I) described for the silica particles (component A) contained in the polishing liquid composition of the present disclosure. EXAMPLES
[0066] The present disclosure will be described in more detail below with reference to examples, but these are merely illustrative and the present disclosure is not limited to these examples.
[0067] 1. Preparation of polishing composition (Examples 1 to 4 and Comparative Examples 1 to 4) Silica particles (component A or non-component A), acid (component B), oxidizing agent (component C) and water were mixed to prepare the polishing liquid compositions of Examples 1 to 4 and Comparative Examples 1 to 4 shown in Table 1. The content (active content) of each component in the polishing liquid composition was 5.5 mass% for silica particles (component A or non-component A), 1.0 mass% for acid (component B), and 0.3 mass% for oxidizing agent (component C). The content of water is the remainder excluding component A or non-component A, component B, and component C. The polishing liquid compositions of Examples 1 to 4 and Comparative Examples 1 to 4 do not contain alumina abrasive grains. The silica particles used as the abrasive grains are colloidal silica produced by a water glass method. The pH of the polishing liquid compositions of Examples 1 to 4 and Comparative Examples 1 to 4 was 1.8. (Examples 5 to 15 and Reference Examples 1 to 3) Silica particles (component A), acid (component B), oxidizing agent (component C), nitrogen-containing compound (component D or non-component D) and water were mixed to prepare the polishing liquid compositions of Examples 5 to 15 and Reference Examples 1 to 3 shown in Table 1. The content (effective content) of each component in the polishing liquid composition was 5.5 mass% for silica particles (component A), 1.0 mass% for acid (component B), 0.3 mass% for oxidizing agent (component C), and 0.10 mass% for nitrogen-containing compound (component D or non-component D). The content of water is the remainder excluding components A, B, C, and D or non-component D. The polishing liquid compositions of Examples 5 to 15 and Reference Examples 1 to 3 do not contain alumina abrasive grains. The silica particles used as the abrasive grains were manufactured by the water glass method. The pH of the polishing liquid compositions of Examples 5 to 15 and Reference Examples 1 to 3 was 1.8.
[0068] The following were used as component A or non-component A, component B, component C, component D or non-component D for preparing the polishing composition. (Component A) (Preparation of Silica Particles A1 to A4) To 500 g of a metal silicate aqueous solution adjusted to pH 10-12 and silica concentration 2%, 7 kg of an acidic silicic acid solution adjusted to a silica concentration of 5% is intermittently added dropwise over 1-24 hours to increase the particle size (build-up). At this time, by adjusting the dropping speed of the dropping liquid, silicic acid concentration, reaction temperature, pressure, pH, etc., silica particles having a desired range of silanol groups can be obtained. In particular, by slowing down the dropping speed to slowly grow the particles, a dense surface and internal structure are formed, and the number of siloxane bonds increases, making it possible to adjust the silanol groups and ignition loss. By the above-mentioned production method, the following silica particles A1 to A4 were prepared. Silica particles A1: spherical silica particles [colloidal silica (water glass method), aspect ratio 1.04, average secondary particle diameter 21 nm, ignition loss 1.10%] Silica particles A2: spherical silica particles [colloidal silica (water glass method), aspect ratio 1.06, average secondary particle size 17 nm, ignition loss 1.11%] Silica particles A3: Spherical silica particles [colloidal silica (water glass method), aspect ratio 1.05, average secondary particle size 18 nm, ignition loss 1.17%] Silica particles A4: Spherical silica particles [colloidal silica (water glass method), aspect ratio 1.04, average secondary particle diameter 25 nm, ignition loss 1.58%] (Non-ingredient A) Silica particles A5: non-spherical silica particles [colloidal silica (water glass method), aspect ratio 1.12, average secondary particle size 142 nm, ignition loss 4.13%, manufactured by JGC Catalysts and Chemicals] Silica particles A6: Mixed silica [Spherical colloidal silica A1 and spherical colloidal silica A8 were mixed in a weight ratio of A1 / A8 = 50 / 50 to form mixed silica (aspect ratio 1.03, average secondary particle diameter 27 nm, ignition loss 1.75%).] Silica particles A7: spherical silica particles [colloidal silica (water glass method), aspect ratio 1.03, average secondary particle size 110 nm, ignition loss 2.38%, JGC Catalysts and Chemicals, SI-80] Silica particles A8: spherical silica particles [colloidal silica (water glass method), aspect ratio 1.03, average secondary particle size 48 nm, ignition loss 1.96%, JGC Catalysts and Chemicals, SI-45] (Component B) Phosphoric acid [75% concentration, manufactured by Nippon Chemical Industry Co., Ltd.] (Component C) Hydrogen peroxide [concentration 35% by mass, manufactured by ADEKA] (Component D) MEA: Monoethanolamine (molecular weight 61, nitrogen atom number 1) AEA: N-(β-aminoethyl)ethanolamine (molecular weight 104.5, number of nitrogen atoms 2) TEPA: Tetraethylenepentamine (molecular weight 189.3, number of nitrogen atoms 5) (Non-ingredient D) PEI: Polyethyleneimine (number average molecular weight 600, number of nitrogen atoms approximately 20, "Epomin SP-006" manufactured by Nippon Shokubai Co., Ltd.)
[0069] 2.Measuring methods for each parameter [Method for measuring silica particle sizes D10, D50 and D90 by centrifugal sedimentation method (CPS measurement)] The silica particles were diluted with ion-exchanged water to prepare a dispersion containing 0.4% by mass of silica particles, which was used as a sample. In Comparative Example 2, the spherical silica particles (A1) and the spherical silica particles (A8) were mixed in a mass ratio of 50 / 50. The particle size distribution of the prepared samples was measured by centrifugal sedimentation using the following measuring device. The particle sizes at which the cumulative frequency from the small diameter side in the particle size distribution in weight conversion obtained by centrifugal sedimentation was 10%, 50%, and 90%, respectively, were defined as D10, D50, and D90. <Measurement conditions> Measurement device: "CPS DC24000 UHR" manufactured by CPS Instruments Measurement range: 0.0004~1μm Particle extinction coefficient: 0.1 Particle shape factor: 1.0 Revolution speed: 20,000 rpm Calibration standard particle size: 0.476μm Standard particle density: 1.0465 (13%, 34℃) Density gradient solution: Sucrose aqueous solution (8%, 24%) Solvent viscosity: 1.16cp (13%, 34℃) Refractive index of solvent: 1.3592 (18%, 34°C) Measurement temperature: 15~45℃ Measurement time: 100 to 420 minutes
[0070] [Method of measuring silica particle diameter D50 (average secondary particle diameter) by DLS measurement] Silica particles were mixed with phosphoric acid and ion-exchanged water to prepare a 1% by mass silica particle dispersion. In Comparative Example 2, the spherical silica particles (A1) and the spherical silica particles (A8) were mixed so that the mass ratio was 50 / 50. The prepared 1% by mass silica particle dispersion was placed in the following measuring device and measured under the following conditions. In the obtained particle size distribution, the particle diameter at which the cumulative volume frequency from the small diameter side was 50% was taken as D50. The D50 measured by DLS was taken as the average secondary particle diameter (volume average particle diameter) of the silica particles. The measurement results are shown in Table 1. <Measurement conditions> Measurement equipment: Malvern Zetasizer Nano "Nano S" Sample volume: 1.5mL Laser: He-Ne, 3.0mW, 633nm Scattered light detection angle: 173°
[0071] [Average aspect ratio of silica particles] Photographs of silica particles observed with a TEM (JEOL "JEM-2000FX", 80 kV, 10,000 to 50,000 magnification) were scanned into a personal computer as image data, and the projection images of 500 silica particles were analyzed using analysis software (Mitani Corporation "WinROOF (Ver. 3.6)") as described below. The minor axis and major axis of each silica particle were determined, and the average aspect ratio (average aspect ratio) was calculated by dividing the major axis by the minor axis. In the case of the mixed silica of Comparative Example 2, the spherical silica particles (A1) and the spherical silica particles (A8) were mixed in a mass ratio of 50 / 50, dried, and observed by TEM, and the average aspect ratio was calculated from the minor axis / major axis ratio in image analysis.
[0072] [Ignition loss] The silica particles were mixed with ion-exchanged water to prepare a 40% by mass silica slurry. In Comparative Example 2, the spherical silica particles (A1) and the spherical silica particles (A8) were mixed in a mass ratio of 50 / 50. The prepared silica slurry was adjusted to pH 3.5 with sulfuric acid and heated at 180°C using a Shimadzu Corporation MOC63u infrared moisture meter to remove moisture. It was then left to stand for 10 minutes to return to room temperature, yielding 2g of sample. Of this, 1g of sample was used again to determine loss on drying LOD (how much moisture it absorbs at room temperature). The remaining 1g of sample was placed in a ceramic crucible and fired in a firing furnace at 1000°C for 2 hours, then cooled in a desiccator for 30 minutes, after which the loss on ignition LOI (weight lost due to dehydration of silanol groups) was determined. Finally, the loss on ignition WL based on dry weight was calculated using the following formula: Loss on ignition on a dry weight basis WL = 100 × {1-(100-LOI) / (100-LOD)}
[0073] [pH measurement] The pH of the polishing composition was measured at 25° C. using a pH meter (manufactured by DKK-Toa Corporation), and the value measured 2 minutes after immersing the electrode in the polishing composition was recorded.
[0074] 3. Polishing the substrate Using the prepared polishing compositions of Examples 1 to 15, Comparative Examples 1 to 4, and Reference Examples 1 to 3, the following substrates to be polished were finish-polished under the polishing conditions shown below. [Substrate to be polished] The substrate to be polished was an aluminum alloy substrate plated with Ni-P and roughly polished with a polishing composition containing silica abrasive grains. The substrate to be polished had a thickness of 0.6 mm, an outer diameter of 97 mm, an inner diameter of 25 mm, and a center line average roughness Ra of 1 nm measured by an AFM (Digital Instrument NanoScope IIIa Multi Mode AFM). The ratio of Ni to P in the Ni-P plating was 88:12 by mass. [Finishing polishing conditions] Polishing machine: Double-sided polishing machine (9B type double-sided polishing machine, manufactured by SpeedFam) Number of substrates to be polished: 10 Polishing liquid: polishing liquid composition Polishing pad: Suede type (foam layer: polyurethane elastomer, thickness 0.9 mm, average pore size 10 μm, Fujibo Co., Ltd.) Plate rotation speed: 32.5 rpm Polishing load: 10.5kPa (set value) Polishing liquid supply amount: 100mL / min Substrate to be polished 1cm 2 Feed rate per: 0.076mL / min Substrate to be polished 1cm 2 Polishing amount per piece: 0.23mg Polishing time: 6 minutes
[0075] 4. Evaluation Methodology [Evaluation of polishing speed] The polishing rates of the polishing compositions of Examples 1 to 15, Comparative Examples 1 to 4, and Reference Examples 1 to 3 were evaluated as follows. First, the mass of each substrate was measured before and after polishing (using an electronic balance manufactured by Sartorius, "BP-210S"), and the mass loss was calculated from the change in mass of each substrate. The polishing rate was calculated by dividing the average mass loss of all 10 substrates by the polishing time (unit: minutes), and was calculated by introducing the value into the following formula. Then, a relative value was calculated with the polishing rate of Comparative Example 1 taken as 100, and this was used as the evaluation item. Mass loss (mg) = {mass before polishing (mg) - mass after polishing (mg)} Polishing speed (mg / min) = mass loss (mg) / polishing time (min)
[0076] [Evaluation of remaining silica] After cleaning the polished substrate using a cleaning machine manufactured by Hikari Co., Ltd., one substrate was immersed in 20 mL of ultrapure water, and ultrasonic cleaning was performed for 15 minutes. By this operation, the silica particles remaining on the substrate surface are extracted into the ultrapure water. The substrate was removed, and a solution obtained by adding 0.2 g of nitric acid and 0.5 g of hydrofluoric acid to 20 mL of ultrapure water was allowed to stand for 15 minutes to completely dissolve the silica particles. Then, the solution was measured for the Si intensity under the following measurement conditions using an inductively coupled plasma mass spectrometry (ICP-MS) apparatus "Agilent 8900" manufactured by Agilent Technologies. The lower the Si intensity in the solution, the less the remaining silica. Then, a relative value with the remaining silica in Comparative Example 1 taken as 100 was calculated and used as an evaluation item. [ICP-MS measurement conditions] Measured element: Si (mass number 28.1) Gas: Argon (purity 99.99%) Plasma flow rate: 15 L / min, auxiliary 1.0 L / min, carrier - 1.35 mL Integration time: 0.34 seconds per mass number Number of integrations: 3 times Calibration curve: Calculated from 5 points of Si standard samples of 0, 0.1, 0.25, 0.5 ppm The values of the remaining silica shown in Table 1 are the average values obtained by performing the same operations and analyses using 5 substrates for each condition.
[0077] [Evaluation of scratches] Measuring instrument: "Candela OSA7100" manufactured by KLA-Tencor Corporation Evaluation: Among the substrates loaded into the polishing tester, 4 substrates were randomly selected, and each substrate was irradiated with a laser at 10,000 rpm to measure the number of scratches. The total number of scratches (pieces) on both sides of each of the 4 substrates was divided by 8 to calculate the number of scratches per substrate surface. The evaluation results of the number of scratches are shown in Table 1 as relative values with Comparative Example 4 taken as 100.
[0078] 5. Results The results of each evaluation are shown in Table 1.
[0079] [Table 1]
[0080] As shown in Table 1, it was found that the polishing liquid compositions of Examples 1 to 15 using the specified silica particles were able to reduce silica residue and scratches on the substrate surface after polishing, compared to Comparative Examples 1 to 4. It was also found that Examples 5 to 15 containing the specified nitrogen-containing compound were able to improve the polishing rate without significantly increasing silica residue, compared to Reference Examples 1 to 3 not containing the specified nitrogen-containing compound. [Industrial Applicability]
[0081] According to one aspect of the present disclosure, since it is possible to reduce silica residue and scratches on the substrate surface after polishing, it is possible to improve the productivity of substrates with improved substrate quality. The present disclosure can be suitably used in the manufacture of magnetic disk substrates.
Claims
1. Contains silica particles and an aqueous medium, The silica particles have an ignition loss of 1.6% or less on a dry weight basis; The polishing liquid composition for Ni-P plated aluminum alloy substrates has a particle diameter D90 of 65 nm or less, where D90 is the particle diameter at which a cumulative frequency from the small particle diameter side is 90% in a particle size distribution calculated by weight obtained by a centrifugal sedimentation method.
2. Further comprising a nitrogen-containing compound, The polishing composition according to claim 1 , wherein the nitrogen-containing compound is an organic amine compound having 10 or less nitrogen atoms in the molecule.
3. 2. The polishing composition according to claim 1, wherein the silica particles have a value represented by the following formula (I) of 5 or less, where WL is an ignition loss on a dry weight basis of the silica particles: {(WL) 3 ×D90} / 100 (I)
4. 2. The polishing composition according to claim 1, wherein the silica particles have a particle diameter D10 of 5 nm or more and 35 nm or less, where D10 is a particle diameter at which a cumulative frequency from the small particle diameter side in the particle size distribution is 10%.
5. 2. The polishing composition according to claim 1, wherein the silica particles have a particle diameter D50 of 10 nm or more and 40 nm or less, where D50 is a particle diameter at which a cumulative frequency from the small particle diameter side in the particle size distribution is 50%.
6. 6. A method for producing a magnetic disk substrate, comprising a polishing step of polishing a substrate to be polished with the polishing composition according to claim 1, wherein the substrate to be polished is an Ni-P plated aluminum alloy substrate.
7. The method for manufacturing a magnetic disk substrate according to claim 6, wherein the polishing step is a finish polishing step.
8. 6. A method for polishing a substrate, comprising polishing a substrate to be polished with the polishing composition according to claim 1, wherein the substrate to be polished is a substrate used in the manufacture of magnetic disk substrates, and is a Ni-P plated aluminum alloy substrate.
9. 1. A method for reducing residual silica on a polished substrate, comprising:
6. A method for reducing residual silica, comprising polishing a substrate to be polished with the polishing composition according to claim 1, wherein the substrate to be polished is an Ni-P plated aluminum alloy substrate.
10. a step of selecting silica particles as the abrasive grains, the silica particles having an ignition loss of 1.6% or less on a dry weight basis, and a particle size D90 of 65 nm or less, where D90 is the particle size at which the cumulative frequency from the small particle size side is 90% in a particle size distribution calculated by weight conversion obtained by a centrifugal sedimentation method; polishing a substrate to be polished using a polishing composition containing the silica particles and an aqueous medium; A method for manufacturing a magnetic disk substrate, wherein the substrate to be polished is an aluminum alloy substrate plated with Ni-P.
Citation Information
Patent Citations
Method for manufacturing magnetic disk substrate
JP2012178209A
Manufacturing method of magnetic disk substrate
JP2015130219A
Polishing composition, magnetic disk substrate manufacturing method and magnetic disk substrate
JP2017019978A
Polishing composition, and magnetic disk substrate manufacturing method
JP2020128479A
Silica particles, silica sol, polishing composition, polishing method, method for producing semiconductor wafer, and method for producing semiconductor device