Dielectric composition, electronic component, and laminated electronic component

A dielectric composition with controlled segregated phases and specific element ratios enhances grain boundary components, addressing grain growth issues to achieve high density, relative permittivity, and specific resistance, thereby improving the reliability and performance of laminated electronic components.

JP7594928B2Active Publication Date: 2024-12-05TDK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021019233
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-09
Publication Date
2024-12-05
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

Existing dielectric compositions face challenges in achieving high density, relative permittivity, specific resistance, and high temperature load life due to variations in grain growth and reduced grain boundaries, which affect the reliability and performance of laminated electronic components.

Method used

A dielectric composition comprising a main phase with a perovskite crystal structure and segregated phases with controlled atomic ratios and equivalent circle diameters, along with specific content of rare earth elements and silicon, is used to enhance grain boundary components and suppress grain growth, ensuring high density and improved electrical properties.

Benefits of technology

The solution results in a dielectric composition with enhanced dielectric constant, specific resistance, and high temperature load life, improving the reliability and performance of laminated electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594928000008
    Figure 0007594928000008
  • Figure 0007594928000009
    Figure 0007594928000009
  • Figure 0007594928000010
    Figure 0007594928000010
Patent Text Reader

Abstract

To provide a dielectric composition and the like having a high density and favorable relative permittivity, specific resistance, and high-temperature load life.SOLUTION: A dielectric composition includes a main phase and segregation phases each including RE (rare earth element). The main phase includes a main component having a perovskite crystal structure of ABO3 (A is one or more selected from Ba, Sr, and Ca, and B is one or more selected from Ti, Zr, and Hf). The segregation phases are classified into first segregation phases whose atomic ratio of Si to RE is 0 or more and 0.20 or less and second segregation phases whose atomic ratio of Si to RE is more than 0.20. 0≤S1 / S2≤0.10 is satisfied on a cross section of the dielectric composition, where S1 is an area ratio of the first segregation phases, and S2 is an area ratio of the second segregation phases. An atomic ratio of Si to RE in the second segregation phases is 0.80 or less on average.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dielectric composition, an electronic component, and a laminated electronic component. [Background technology]

[0002] 2. Description of the Related Art In recent years, as electronic devices become smaller and more dense, there is a demand for smaller electronic components and laminated electronic components used in the electronic devices, with increased capacity and improved reliability.

[0003] Patent Document 1 describes a dielectric composition having a γ-RE2Si2O7 (RE is any of Y, Dy, and Ho) crystal phase in the grain boundary phase present between dielectric particles. The crystal phase exists in the grain boundary phase as a composite oxide of a rare earth element and Si, and acts as a sintering aid. Furthermore, since the insulation resistance is relatively high, the sinterability of the dielectric composition is improved, and the dielectric properties can be improved. Therefore, by having the γ-RE2Si2O7 crystal phase in the grain boundary phase, it is possible to increase the number of layers in a laminated electronic component, reduce the thickness of the dielectric layer itself, and improve reliability at the same time.

[0004] However, the γ-RE2Si2O7 crystal phase has a strong role as a sintering aid and is weak in suppressing the grain growth of dielectric particles. Therefore, when the γ-RE2Si2O7 crystal phase is included, grain growth tends to vary. When the grain growth varies greatly, the number of grain boundaries decreases, which can lead to reduced reliability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4663141 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a dielectric composition etc. having high density and excellent specific dielectric constant, specific resistivity and high temperature accelerated life. [Means for solving the problem]

[0007] In order to achieve the above object, the dielectric composition of the present invention comprises: A dielectric composition comprising a main phase and a segregation phase containing a rare earth element RE, the main phase contains a main component having a perovskite crystal structure represented by ABO3 (A is one or more selected from Ba, Sr, and Ca, and B is one or more selected from Ti, Zr, and Hf), Among the segregation phases, a segregation phase in which the atomic ratio of Si to RE is 0 or more and 0.20 or less is defined as a first segregation phase, and a segregation phase in which the atomic ratio of Si to RE is more than 0.20 is defined as a second segregation phase, In a cross section of the dielectric composition, when an area ratio of the first segregation phase is S1 and an area ratio of the second segregation phase is S2, 0≦S1 / S2≦0.10, The atomic ratio of Si to RE in the second segregation phase is 0.80 or less on average.

[0008] The dielectric composition may further include M in addition to Si and RE, M is one or more selected from Mg, Mn, V and Cr; With respect to the main component, the RE content may be 0.90 mol % or more and 3.60 mol % or less in terms of RE2O3, the M content may be 0.20 mol % or more and 1.00 mol % or less in terms of MO, and the Si content may be 0.60 mol % or more and 1.80 mol % or less in terms of SiO2.

[0009] The atomic ratio of Ba to Ti in the first segregation phase may be less than 1.00, and the atomic ratio of Ba to Ti in the second segregation phase may be greater than 1.00.

[0010] In a cross section of the dielectric composition, the average of the first segregation phase Equivalent circle diameter A1, the average of the second segregation phase Equivalent circle diameter where A1 / A2 is A2, 0≦A1 / A2<1.00 may be satisfied.

[0011] The electronic device of the present invention comprises the above-mentioned dielectric composition.

[0012] The laminated electronic component of the present invention is formed by alternately laminating dielectric layers made of the above-mentioned dielectric composition and electrode layers. [Brief description of the drawings]

[0013] [Figure 1A] FIG. 1A is a cross-sectional view of a multilayer ceramic capacitor. [Figure 1B] FIG. 1B is a cross-sectional view of the multilayer ceramic capacitor taken along line IB-IB in FIG. 1A. [Diagram 2] FIG. 2 is a mapping image of sample number 3. [Diagram 3] FIG. 3 is a schematic diagram of a cross section of the dielectric composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] < 1. Multilayer ceramic capacitors > 1.1 Overall structure of multilayer ceramic capacitor A multilayer ceramic capacitor 1 as an example of the multilayer electronic component according to this embodiment is shown in Figures 1A and 1B. The multilayer ceramic capacitor 1 has an element body 10 in which dielectric layers 2 and internal electrode layers 3 are alternately laminated. A pair of external electrodes 4 are formed on both ends of the element body 10, and are electrically connected to the internal electrode layers 3 arranged alternately inside the element body 10. There is no particular restriction on the shape of the element body 10, but it is usually a rectangular parallelepiped. There is also no particular restriction on the dimensions of the element body 10, and the dimensions may be appropriate depending on the application.

[0015] In this embodiment, the vertical dimension L0 (see FIG. 1A) of the element body 10 may be 5.7 to 0.4 mm. The width dimension W0 (see FIG. 1B) of the element body 10 may be 5.0 to 0.2 mm. The height dimension H0 (see FIG. 1B) of the element body 10 may be 5.0 to 0.2 mm.

[0016] Specific sizes of the element body 10 include L0×W0 of (5.7±0.4)mm×(5.0±0.4)mm, (4.5±0.4)mm×(3.2±0.4)mm, (3.2±0.3)mm×(2.5±0.2)mm, (3.2±0.3)mm×(1.6±0.2)mm, (2.0±0.2)mm×(1.2±0.1)mm, (1.6±0.2)mm×(0.8±0.1)mm, (1.0±0.1)mm×(0.5±0.05)mm, (0.6±0.06)mm×(0.3±0.03)mm, (0.4±0.04)mm×(0.2±0.02)mm, etc. H0 is not particularly limited, and is, for example, approximately equal to or less than W0.

[0017] 1.2 Dielectric layer The dielectric layer 2 is made of a dielectric composition according to the present embodiment, which will be described later.

[0018] The thickness of each dielectric layer 2 (interlayer thickness) is not particularly limited and can be set arbitrarily depending on the desired characteristics, applications, etc. Typically, the interlayer thickness may be 20 μm or less, 10 μm or less, or 5 μm or less. The number of layers of the dielectric layers 2 is not particularly limited, but in this embodiment of the multilayer ceramic, it may be, for example, 10 or more, 100 or more, or 200 or more.

[0019] 1.3 Internal electrode layer In this embodiment, the internal electrode layers 3 are laminated so that their ends are alternately exposed on the surfaces of two opposing end faces of the element body 10.

[0020] The conductive material contained in the internal electrode layer 3 is not particularly limited. Examples of precious metals used as conductive materials include Pd, Pt, and Ag-Pd alloys. Examples of base metals used as conductive materials include Ni, Ni-based alloys, Cu, and Cu-based alloys. Note that Ni, Ni-based alloys, Cu, or Cu-based alloys may contain various trace components such as P and / or S at about 0.1 mass% or less. The internal electrode layer 3 may be formed using a commercially available electrode paste. The thickness of the internal electrode layer 3 may be appropriately determined depending on the application, etc.

[0021] 1.4 External electrode There is no particular limitation on the conductive material contained in the external electrodes 4. For example, known conductive materials such as Ni, Cu, Sn, Ag, Pd, Pt, Au, alloys of these, conductive resins, etc. may be used. The thickness of the external electrodes 4 may be appropriately determined depending on the application, etc.

[0022] < 2. Dielectric composition > Fig. 2 is a mapping image created by using STEM-EDS for the dielectric composition constituting the dielectric layer 2 according to this embodiment, and Fig. 3 is a schematic diagram of the dielectric composition constituting the dielectric layer 2 according to this embodiment. As shown in Figs. 2 and 3, the dielectric composition constituting the dielectric layer 2 according to this embodiment contains a first segregation phase 16 and a second segregation phase 18 between main phases 14. The dielectric composition may also be a dielectric ceramic composition.

[0023] 2.1 Main phase The main phase 14 of the present embodiment contains a compound having a perovskite crystal structure represented by ABO3 as a main component. The main component of the main phase 14 is a component that occupies 80 to 100 parts by mass, and preferably 90 to 100 parts by mass, with respect to 100 parts by mass of the main phase.

[0024] A is one or more selected from barium (Ba), strontium (Sr) and calcium (Ca). It may be one or more selected from Ba and Sr. A may contain 80 mol% or more of Ba, or 90 mol% or more of Ba. A may be only Ba.

[0025] B is at least one selected from titanium (Ti), zirconium (Zr) and hafnium (Hf). It may be at least one selected from Ti and Zr. B may contain 70 mol % or more of Ti, or 80 mol % or more of Ti. B may be only Ti.

[0026] A is one or more selected from Ba, Sr and Ca, and B is one or more selected from Ti and Zr. The composition of the main components is as follows: { {Ba 1-x-y Ca x Sr y}O} u (Ti 1-z Zr z ) v It's O2.

[0027] x is preferably 0≦x≦0.10, more preferably 0≦x≦0.05. y is preferably 0≦y≦0.10, more preferably 0≦y≦0.05. z is preferably 0≦z≦0.30, more preferably 0≦z≦0.15. u / v is preferably 0.997≦u / v≦1.010, more preferably 0.998≦u / v≦1.005.

[0028] In this embodiment, the dielectric composition may contain one or more elements selected from magnesium (Mg), manganese (Mn), vanadium (V) and chromium (Cr) as M. Furthermore, the dielectric composition contains RE (one or more elements selected from rare earth elements) and silicon (Si). Furthermore, M is likely to be contained in the main phase 14 of the dielectric composition. M is contained in the dielectric composition mainly as an oxide of M.

[0029] The content of RE may be 0.90 mol % or more and 3.60 mol % or less in terms of RE2O3 relative to the main component. The content of M may be 0.10 mol % or more and 2.00 mol % or less, or 0.20 mol % or more and 1.00 mol % or less in terms of MO. The content of Si may be 0.50 mol % or more and 1.90 mol % or less, or 0.60 mol % or more and 1.80 mol % or less in terms of SiO2. When the contents of each element are within the above ranges, the reliability of the multilayer ceramic capacitor containing the dielectric composition is improved, and the high temperature load life is likely to be improved.

[0030] There is no particular limit to the type of RE. For example, it may be one or more selected from dysprosium (Dy), gadolinium (Gd), yttrium (Y) and ytterbium (Yb). The smaller the ionic radius of the RE, the more difficult it is for the RE to dissolve in the main component. As a result, the relative dielectric constant tends to decrease and the resistivity tends to decrease.

[0031] 2.2 Segregation phase (first segregation phase, second segregation phase) The first segregation phase 16 is a segregation phase in which the atomic ratio of Si to RE is 0 or more and 0.20 or less. That is, the first segregation phase 16 does not need to contain Si. The second segregation phase 18 is a segregation phase in which the atomic ratio of Si to RE is more than 0.20. Each segregation phase may contain, for example, A, Ti, and oxygen (O) in addition to RE and Si.

[0032] The total content of RE, A, Si and Ti relative to the total content of elements other than O in the first segregation phase 16 may be 90 atomic % or more. The total content of RE, A, Si and Ti relative to the total content of elements other than O in the second segregation phase 18 may be 90 atomic % or more.

[0033] A cross section perpendicular to the lamination direction of the multilayer ceramic capacitor 1 includes a cross section of the dielectric composition constituting the dielectric layer 2. In the cross section of the dielectric composition, the area ratio of the first segregation phase 16 is S1, the area ratio of the second segregation phase 18 is S2, and 0≦S1 / S2≦0.10 is satisfied. In other words, the dielectric composition does not need to include the first segregation phase 16.

[0034] By segregating each segregation phase so as to satisfy 0≦S1 / S2≦0.10, the amount of Si required to obtain a dielectric composition having good characteristics is present at the grain boundaries. Therefore, by segregating each segregation phase so as to satisfy 0≦S1 / S2≦0.10, the density of the dielectric composition is increased, and the relative dielectric constant and resistivity are also increased. Furthermore, the high temperature load life of the dielectric composition is extended. This is because the first segregation phase, i.e., the region containing a large amount of Ti, becomes sufficiently small, thereby suppressing the generation of oxygen defects caused by the change in the valence of Ti.

[0035] A method for calculating S1 / S2 in a dielectric composition will be described below.

[0036] First, a mapping analysis is performed on the measurement points of the cross section of the dielectric composition using a scanning transmission electron microscope (STEM) equipped with an energy dispersive X-ray analyzer (EDS). Hereinafter, a STEM equipped with an EDS is referred to as a STEM-EDS. There is no particular limit to the size of the measurement range, but for example, when the area of ​​the dielectric composition is 50 μm 2 The measurement range is set so that the measured value is equal to or greater than 0.02 μm / pixel. The obtained mapping image is divided into dots of 0.02 μm / pixel to 0.05 μm / pixel, and the contrast intensity of each element at each dot is quantified. Specifically, the contrast intensity is classified into 91 levels from 0 to 90, with the lowest contrast intensity (no detection) being 0 and the highest being 90. Dots with a contrast intensity of 75 or more for rare earth elements are considered to be dots in which rare earth elements are segregated. The area where dots in which rare earth elements are segregated are considered to be segregated phases. The area of ​​each segregated phase must be a minimum of 0.005 μm 2 0.005μm 2Phases smaller than are not considered to be segregated phases.

[0037] There is no particular limitation on the content ratios of RE, A, Ti, and O in the first segregation phase 16 and the second segregation phase 18, as long as it is possible to confirm that RE, A, Ti, and O are contained using STEM-EDS. Then, a mapping image is prepared in which the first segregation phase and the second segregation phase are distinguished by changing the color as shown in Fig. 2. Then, the area ratio S1 of the first segregation phase and the area ratio S2 of the second segregation phase are calculated from the mapping image, and S1 / S2 is calculated.

[0038] Moreover, the atomic ratio of Si to RE in the second segregation phase 18 (hereinafter, may be referred to as Si2 / RE2) is 0.80 or less on average. If Si2 / RE2 is too large, the relative dielectric constant and reliability are likely to decrease, and the high temperature accelerated life is shortened.

[0039] A method for calculating the average value of Si2 / RE2 will be described. In principle, the Si2 / RE2 is measured for all dots of the second segregation phase included in the mapping image and averaged to calculate the average value. However, each second segregation phase included in the mapping image may have a uniform composition. That is, the value obtained by calculating Si2 / RE2 for any one dot included in each second segregation phase may be used as the Si2 / RE2 for all dots included in the second segregation phase. Also, the value obtained by calculating Si2 / RE2 for any two or more dots included in each second segregation phase and averaging them may be used as the Si2 / RE2 for all dots included in the second segregation phase.

[0040] The average equivalent circle diameter of the first segregation phase 16 is A1, and the average equivalent circle diameter of the second segregation phase 18 is A2, and 0≦A1 / A2<1.00 may be satisfied. 0≦A1 / A2≦0.86 may be satisfied. When A1 / A2 is less than 1.00, the reliability of the multilayer ceramic capacitor including the dielectric composition is improved, and the high temperature load life is likely to be improved. This is because the first segregation phase, i.e., the region containing a large amount of Ti, becomes sufficiently small, thereby suppressing the generation of oxygen oxides due to the change in the valence of Ti.

[0041] The circle-equivalent diameters of all the segregation phases included in the mapping image are measured, and the average circle-equivalent diameter A1 of the first segregation phase and the average circle-equivalent diameter A2 of the second segregation phase are calculated, and A1 / A2 is then calculated.

[0042] In addition, the atomic ratio of Ba to Ti in the first segregation phase may be less than 1.00, and may be 0.52 or less. The atomic ratio of Ba to Ti in the second segregation phase may be more than 1.00, and may be 1.46 or more. Hereinafter, the atomic ratio of Ba to Ti may be referred to as Ba / Ti. When Ba / Ti in the first segregation phase and Ba / Ti in the second segregation phase are within the above ranges, the generation of oxygen defects due to the change in valence of Ti in the segregation phase can be suppressed. Therefore, the reliability of the multilayer ceramic capacitor containing the dielectric composition is improved, and the high temperature load life is likely to be improved.

[0043] A method of calculating Ba / Ti in the first segregation phase will be described. In principle, Ba / Ti is calculated for all dots included in the first segregation phase included in the mapping image, and the Ba / Ti of the first segregation phase is calculated by averaging. However, each of the first segregation phases included in the mapping image may have a uniform composition. That is, the value obtained by calculating Ba / Ti for any one dot included in each first segregation phase may be used as the Ba / Ti of all dots included in the first segregation phase. Also, the value obtained by calculating Ba / Ti for any two or more dots included in each first segregation phase and averaging them may be used as the Ba / Ti of all dots included in the first segregation phase. Ba / Ti of the second segregation phase is calculated in the same manner.

[0044] There is no particular limit to the total area ratio of the segregation phases relative to the entire dielectric composition. For example, it may be 0.5% or more and 3.0% or less. If the total area ratio of the segregation phases is too small, uneven abnormal grain growth occurs due to a lack of grain boundary components. Therefore, the reliability of the dielectric composition is likely to decrease. If the total area ratio of the segregation phases is too large, the area ratio of the main phase decreases relatively, and the content ratio of the main phase components decreases relatively. The dielectric properties of the dielectric composition are expressed particularly by the main phase components. Therefore, if the total area ratio of the segregation phases is too high, it becomes difficult to ensure sufficient dielectric properties of the dielectric composition, and the relative dielectric constant of the dielectric composition is likely to decrease.

[0045] < 3. Manufacturing method of multilayer ceramic capacitors > Next, an example of a method for manufacturing the multilayer ceramic capacitor 1 shown in FIG. 1 will be described below.

[0046] The multilayer ceramic capacitor 1 of this embodiment is manufactured in the same manner as a conventional multilayer ceramic capacitor, by preparing a green chip by a normal printing method or sheet method using a paste, firing the green chip, and then printing or transferring external electrodes onto the green chip and firing the chip. The manufacturing method will be specifically described below.

[0047] First, a dielectric material for forming the dielectric layer is prepared, and then this is made into a paint to prepare a paste for the dielectric layer.

[0048] As the dielectric raw material, a raw material of ABO3, which is the main component, and raw materials of various other oxides are prepared. As these raw materials, oxides of the above-mentioned components, mixtures thereof, and composite oxides can be used, but other raw materials can also be appropriately selected from various compounds that become the above-mentioned oxides or composite oxides by firing, such as carbonates, oxalates, nitrates, hydroxides, and organometallic compounds, and mixed for use. In this embodiment, it is preferable to use a mixture in which the oxides of the above-mentioned components are uniformly dispersed in the main component, but a dielectric raw material in which the main component is covered with the above-mentioned components may also be used.

[0049] In addition, the raw material for the main component ABO3 can be produced by various methods, including the so-called solid phase method as well as various liquid phase methods (e.g., the oxalate method, hydrothermal synthesis method, alkoxide method, sol-gel method, etc.).

[0050] Furthermore, when the dielectric layer contains components other than those described above, the raw materials for the components can be oxides, mixtures, or composite oxides of those components. In addition, various compounds that become the above-mentioned oxides or composite oxides upon firing can be used.

[0051] The content of each compound in the dielectric material may be determined so as to give the above-mentioned dielectric composition after firing.

[0052] The dielectric layer paste may be an organic paint in which a dielectric material and an organic vehicle are kneaded together, or may be a water-based paint.

[0053] The organic vehicle is a binder dissolved in an organic solvent. The binder and the solvent may be any known ones.

[0054] In addition, when the dielectric layer paste is a water-based paint, the dielectric raw material may be kneaded with a water-based vehicle in which a water-soluble binder, a dispersant, etc. are dissolved in water. The water-soluble binder is not particularly limited, and examples thereof include polyvinyl alcohol, cellulose, and water-soluble acrylic resin.

[0055] The internal electrode layer paste may be prepared by kneading the conductive material made of Ni or Ni alloy, or various oxides, organometallic compounds, resinates, etc. that become the Ni or Ni alloy after firing, with the organic vehicle. The internal electrode layer paste may also contain a co-material. The co-material is not particularly limited, and may have the same composition as the main component.

[0056] The external electrode paste may be prepared in the same manner as the internal electrode layer paste described above.

[0057] The content of the organic vehicle in each of the above pastes is not particularly limited, and may be a normal content, for example, about 1 to 15 mass% of the binder and about 10 to 60 mass% of the solvent. Each paste may contain additives selected from various dispersants, plasticizers, dielectrics, insulators, etc., as necessary. The total content of these may be 10 mass% or less.

[0058] When the printing method is used, the dielectric layer paste and the internal electrode layer paste are printed and laminated on a substrate such as PET, cut into a predetermined shape, and then peeled off from the substrate to form a green chip.

[0059] When the sheet method is used, a green sheet is formed using the dielectric layer paste, and the internal electrode layer paste is printed thereon, after which these are laminated and cut into a predetermined shape to obtain a green chip.

[0060] Before firing, the green chip is subjected to a binder removal treatment. The binder removal conditions are a temperature rise rate of preferably 5 to 300°C / hour, a binder removal temperature of preferably 180 to 900°C, and a holding time of preferably 0.5 to 48 hours. The binder removal treatment is performed in air or a reducing atmosphere (for example, a humidified N2+H2 mixed gas atmosphere).

[0061] After the binder is removed, the green chip is fired. For example, the temperature rise rate may be 200 to 20,000° C. / h, the firing temperature may be 1,150 to 1,350° C., and the holding time may be 0.1 to 10 hours.

[0062] The slower the heating rate, the higher the firing temperature, and the longer the holding time, the more the firing will proceed. As the firing proceeds, the proportion of the first segregation phase tends to decrease and the proportion of the second segregation phase tends to increase. That is, S1 / S2 tends to decrease. Also, as the firing proceeds, the average circle equivalent diameter of the second segregation phase tends to increase compared to the average circle equivalent diameter of the first segregation phase. That is, A1 / A2 tends to decrease. Also, as the Si content in the dielectric layer paste increases, the content of the first segregation phase decreases, making it easier for the firing to proceed. As the Si content in the dielectric layer paste decreases, the content of the second segregation phase decreases, making it more difficult for the firing to proceed.

[0063] When the firing temperature is low, the second segregation phase is less likely to form. As a result, the dielectric density is less likely to increase. Furthermore, the main phase is less likely to undergo grain growth. As a result, the relative dielectric constant is more likely to decrease. Furthermore, the solid solution of various components in the main phase is less likely to progress, and the resistivity and high-temperature load life are more likely to decrease. When the firing temperature is high, the second segregation phase is more likely to form. Furthermore, the main phase is more likely to undergo abnormal grain growth, and the relative dielectric constant is more likely to increase. Furthermore, the solid solution of each main component in the main phase is more likely to progress, and the resistivity is more likely to increase. However, the size of the main phase is more likely to vary, and the high-temperature load life is more likely to decrease.

[0064] The atmosphere during firing is not particularly limited. Air or a reducing atmosphere may be used. In addition, the oxygen partial pressure is 1.0×10 -14 ~1.0×10 -9 It may also be expressed as MPa.

[0065] Furthermore, the microstructure of the dielectric composition after firing also changes depending on the composition of the dielectric composition, particularly the content ratio of the various oxides mentioned above.

[0066] The higher the Si content, the higher the proportion of the secondary segregation phase and the lower the S1 / S2 ratio. The dielectric density also tends to increase. The firing temperature required to optimize the S1 / S2 ratio is lower. Furthermore, the average Si2 / RE2 tends to increase.

[0067] The lower the Si content, the lower the proportion of the secondary segregation phase and the higher the S1 / S2 ratio. The dielectric density also tends to decrease. The firing temperature for optimizing the S1 / S2 ratio becomes higher. Furthermore, the average Si2 / RE2 also tends to decrease.

[0068] When the RE content is high, RE and Si react sufficiently. Therefore, the proportion of the first segregation phase, which has a low Si content, decreases, and S1 / S2 tends to decrease. In addition, when the RE content is high, the proportion of the segregation phase increases, which makes it easier for the relative dielectric constant to decrease. Furthermore, the amount of RE that is not contained in the main phase and segregation phase increases, which makes it easier for the high-temperature load life to decrease.

[0069] When the RE content is reduced, the amount of RE reacting with Si is reduced, and the reaction product between RE and Si is reduced. Therefore, the proportion of the first segregation phase increases, and S1 / S2 tends to increase. The reaction product between RE and Si promotes densification of the dielectric composition. Therefore, when the RE content is reduced, the dielectric density tends to decrease. In addition, when the RE content is low, the solid solution of RE in the main phase is reduced, and the resistivity and high temperature load life tend to decrease.

[0070] When the ionic radius of RE becomes small, RE is less likely to be fully dissolved in the main phase. RE that is not dissolved in the main phase is more likely to remain as a grain boundary component. Therefore, when the ionic radius of RE is small, the grain growth of the main phase is suppressed, and the particle size of the main phase is reduced. The relative dielectric constant of the dielectric composition is more likely to decrease. Furthermore, since RE is less likely to be fully dissolved in the main phase, the resistivity and high-temperature load life of the dielectric composition are more likely to decrease. When the ionic radius of RE becomes large, RE is more likely to be fully dissolved in the main phase. The grain growth of the main phase through the reaction between the grain boundary component and the main phase, such as the solid solution of RE in the main phase, is promoted, and the grain size of the main phase increases. Therefore, the relative dielectric constant of the dielectric composition is more likely to increase. Therefore, the increase in the ionic radius of RE promotes the solid solution of RE in the main phase, and the resistivity and high-temperature load life of the dielectric composition are more likely to increase.

[0071] Changing the content of M does not have much effect on the formation of each segregation phase. However, M dissolves in the main phase and acts as an acceptor component. Therefore, if there is a large amount of M, the high temperature load life of the dielectric composition tends to be easily shortened. If there is a small amount of M, the resistivity tends to be easily shortened.

[0072] In addition to the main component, the alloy may contain an oxide of A. The higher the content of the oxide of A, the easier it is to increase the average Si2 / RE2.

[0073] The firing atmosphere is preferably a reducing atmosphere, and the atmospheric gas may be, for example, a humidified mixed gas of N2 and H2.

[0074] In addition, the oxygen partial pressure during firing may be appropriately determined depending on the type of conductive material in the internal electrode layer paste. When a base metal such as Ni or a Ni alloy is used as the conductive material, the oxygen partial pressure in the atmosphere is 1.0×10 -14 ~1.0×10 -9 It may also be expressed as MPa.

[0075] In this embodiment, it is preferable to perform an annealing treatment (oxidation treatment of the dielectric layer) on the element body after firing. Specifically, the annealing temperature may be 950 to 1100°C. The holding time may be 0.1 to 20 hours. The atmosphere during the oxidation treatment is humidified N2 gas (oxygen partial pressure: 1.0×10 -9 ~1.0×10 -6 MPa).

[0076] In the above-mentioned binder removal treatment, firing and annealing treatment, when N2 gas or mixed gas is to be humidified, for example, a wetter may be used. In this case, the water temperature is preferably about 5 to 75°C.

[0077] The binder removal treatment, firing and annealing treatment may be carried out consecutively or independently.

[0078] The capacitor element body obtained as described above is subjected to end surface polishing, for example, by barrel polishing or sandblasting, and then an external electrode paste is applied and fired to form the external electrodes 4. Then, if necessary, a coating layer is formed on the surface of the external electrodes 4 by plating or the like.

[0079] The multilayer ceramic capacitor of this embodiment thus manufactured is mounted on a printed circuit board by soldering or the like and used in various electronic devices.

[0080] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention.

[0081] In the above-described embodiment, the microstructure is controlled by controlling the composition and the firing conditions, in particular. However, the present invention is not limited to this method, and the microstructure may be controlled, for example, by a method of preparing and mixing calcined powders that constitute the first segregation phase and the second segregation phase.

[0082] [ Variations ] In the above-described embodiment, the case where the electronic component according to the present invention is a multilayer ceramic capacitor has been described. However, the electronic component according to the present invention is not limited to a multilayer ceramic capacitor and may be any electronic component having the above-described dielectric composition.

[0083] For example, it may be a single-plate ceramic capacitor in which a pair of electrodes are formed on the above-mentioned dielectric composition.

[0084] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention.

[0085] The electronic components and laminated electronic components containing the dielectric composition according to the present invention have a relative dielectric constant within a range suitable for in-vehicle use, and have high dielectric density, resistivity and high-temperature loaded life, and are therefore particularly suitable for in-vehicle use.

[0086] The higher the dielectric constant, the better the dielectric properties. However, a dielectric composition with a high dielectric constant experiences a large decrease in dielectric constant due to the application of voltage. Therefore, a capacitor using a dielectric composition with too high a dielectric constant has a low effective capacitance. Therefore, a dielectric composition contained in an in-vehicle capacitor cannot be used suitably if its dielectric constant is too high or too low. EXAMPLES

[0087] The present invention will be described in more detail below using examples and comparative examples, although the present invention is not limited to the following examples.

[0088] (Preparation of dielectric paste) First, BaTiO3 powder (Ba / Ti=1.004), RE2O3 powder, SiO2 powder, BaCO3 powder, MgO powder, and MnCO3 powder were prepared as raw material powders. They were then weighed out to obtain the dielectric compositions of the examples and comparative examples shown in Tables 1 to 7. The atomic ratio of Mg and Mn contained as M was Mg:Mn=4:3.

[0089] Next, 10 parts by weight of polyvinyl butyral resin, 5 parts by weight of dioctyl phthalate (DOP) as a plasticizer, and 100 parts by weight of alcohol as a solvent were mixed in a bead mill to form a paste, with the total of all of the above raw material powders being 100 parts by mass, to obtain a paste for the dielectric layer.

[0090] (Preparation of Internal Electrode Layer Paste) Ni powder, terpineol, ethyl cellulose, and benzotriazole were prepared so that the mass ratio was 44.6:52.0:3.0:0.4. These were then kneaded with a triple roll to form a slurry, thereby producing a paste for the internal electrode layers.

[0091] (Green chip fabrication) A green sheet was formed on a PET film using the dielectric layer paste. The thickness of the green sheet was set to 4.0 to 5.0 μm after drying. Next, an electrode layer was printed in a predetermined pattern on the green sheet using the internal electrode layer paste. After that, the green sheet was peeled off from the PET film to produce a green sheet having an electrode layer. Next, a plurality of green sheets having an electrode layer were stacked and pressure-bonded to obtain a green laminate. This green laminate was cut to a predetermined size to produce a green chip.

[0092] (Fabrication of the element body) The resulting green chip was then subjected to a binder removal treatment, sintering and oxidation treatment to obtain a device body as a sintered body.

[0093] The conditions for the binder removal treatment were a temperature rise rate of 25° C. / h, a binder removal temperature of 235° C., a holding time of 8 hours, and an atmosphere of air.

[0094] The firing conditions are as shown in Tables 1 to 7. The atmosphere was a humidified N2+H2 mixed gas atmosphere, and the oxygen partial pressure was 1.0×10 -12 MPa or 1.0×10 -13 In Tables 1 to 4 and 6, the oxygen partial pressure was 1.0 × 10 -12 In Tables 5 and 7, the oxygen partial pressure was 1.0×10 -12 MPa is "high", and the oxygen partial pressure is 1.0×10 -13 MPa was rated as "low".

[0095] The oxidation treatment conditions were a heating rate and a cooling rate of 200°C / h, an oxidation treatment temperature of 1050°C, a holding time of 3 hours, and a humidified N2 gas atmosphere. The oxygen partial pressure was 1.0×10 -7 The pressure was measured in MPa.

[0096] A wetter was used to humidify the atmosphere during the firing and oxidation treatment.

[0097] (Preparation of multilayer ceramic capacitor samples) Next, the end faces of the obtained element body were polished by sandblasting, and then Cu was applied as an external electrode to obtain a multilayer ceramic capacitor sample shown in Figure 1. The size of the obtained capacitor sample was 3.2 mm x 1.6 mm x 0.7 mm, the thickness of the dielectric layer was 3.2 to 4.2 μm, and the thickness of the internal electrode layer was 0.8 to 1.2 μm. The number of dielectric layers was 10.

[0098] (Confirmation of segregation phase) The obtained multilayer ceramic capacitor sample was cut in a cross section perpendicular to the dielectric layers (cross section in the lamination direction). STEM-EDS mapping analysis was performed on the sections obtained to determine the presence or absence of segregation phases. In a field of view large enough to observe five or more internal electrode layers, the obtained mapping image was divided into dots of 0.027 μm / pixel, and the contrast intensity of each element in each dot was quantified. Specifically, the contrast intensity was classified into 91 levels from 0 to 90, with the smallest contrast intensity (not detected) being 0 and the largest being 90. Dots with a contrast intensity of 75 or more for rare earth elements were determined to be dots in which rare earth elements were segregated. A portion where dots in which rare earth elements were segregated were determined to be a segregation phase. Among the segregation phases, a segregation phase in which the atomic ratio of Si to RE was 0 to 0.20 was determined to be a first segregation phase, and a segregation phase in which the atomic ratio of Si to RE was greater than 0.20 was determined to be a second segregation phase. In addition, it was confirmed by STEM-EDS that each segregation phase contained RE, A, Ti, and O. As shown in Figure 2, a mapping image was prepared in which the first and second segregation phases were shown in different colors to make them distinguishable.

[0099] S1 / S2 was calculated from the area ratio of the first segregation phase and the area ratio of the second segregation phase contained in the obtained mapping image.

[0100] The circle-equivalent diameters of the segregation phases included in the obtained mapping image were measured, and the average circle-equivalent diameter A1 of the first segregation phase and the average circle-equivalent diameter A2 of the second segregation phase were calculated, and A1 / A2 was calculated.

[0101] Moreover, the average Ba / Ti in each of the first segregation phases and the average Ba / Ti in each of the second segregation phases were calculated by the above-mentioned method.

[0102] Furthermore, the average of Si2 / RE2 was calculated by the above method. The results are shown in Tables 1 to 7.

[0103] (Measurement of porcelain properties) The dielectric constant of the multilayer ceramic capacitor sample was measured using a digital LCR meter (YHP 4274A). Specifically, the capacitance was measured at a reference temperature of 25°C, a frequency of 1 kHz, and an input signal level (measurement voltage) of 1.0 Vrms, and the dielectric constant was calculated from the capacitance. A dielectric constant of 2000 or more and 3000 or less was considered good, and a dielectric constant of 2200 or more and 2800 or less was considered particularly good.

[0104] The resistivity of the multilayer ceramic capacitor samples was measured using an insulation resistance meter (R8340A manufactured by Advantest Corporation). Specifically, the temperature was set to 125°C, a direct current voltage of 20 V / μm was applied to the multilayer ceramic capacitor for 10 seconds, and the capacitor was then left for 50 seconds, after which the insulation resistance was measured. The resistivity was calculated from the measured insulation resistance, electrode area, and interlayer thickness. The resistivity was 1.0×10 9 Ω·m or more is considered good, and 1.0×10 10 Ω·m or more was considered particularly good.

[0105] The high temperature accelerated life was evaluated by measuring the life time while applying a direct current voltage of 40V / μm at 190°C to the multilayer ceramic capacitor sample. In this example, the life time was determined as the time from the start of application until the insulation resistance dropped by one digit. In this example, the above evaluation was performed on 20 capacitor samples, and the mean time to failure (MTTF) was calculated from the life time of each capacitor sample. The high temperature accelerated life was determined as good when the MTTF was 2.0 hours or more, and as particularly good when the MTTF was 5.0 hours or more.

[0106] The dielectric density was measured by measuring the density of a disk-shaped dielectric produced using the above dielectric layer paste. The conditions for binder removal, firing, and oxidation were the same as those for producing the multilayer ceramic capacitor. The diameter and thickness of the dielectric were measured at three locations and averaged. The volume was calculated from the obtained diameter and thickness, and the dielectric density was calculated from the mass and volume of the dielectric.

[0107] The theoretical density of BaTiO3, the main component of this experiment, is 6.02 g / cm 3 In this experimental example, the dielectric density was 90% or more (5.4 g / cm) of the theoretical density of the main component. 3 A dielectric density of 95% or more (5.7 g / cm3 or more) of the theoretical density of the main component is considered good. 3 The case where the condition was as follows:

[0108] [Table 1]

[0109] [Table 2]

[0110] [Table 3]

[0111] [Table 4]

[0112] [Table 5]

[0113] [Table 6]

[0114] [Table 7]

[0115] Table 1 shows the results when only the RE2O3 content was changed while keeping all other conditions the same. When S1 / S2 is between 0 and 0.10, and the average of Si2 / RE2 is 0.80 or less, good characteristics are shown.

[0116] The lower the RE2O3 content, the larger the S1 / S2. This is because the lower the RE2O3 content, the more difficult it is for the segregation phase to form, and in particular the second segregation phase to form more difficultly than the first segregation phase. If S1 / S2 exceeds 0.10, the dielectric composition is less likely to be densified. As a result, the dielectric density decreases. Furthermore, the solid solution of RE in the main component becomes insufficient. As a result, the relative dielectric constant becomes too high, and the MTTF decreases.

[0117] The higher the RE2O3 content, the smaller the S1 / S2. This is because the higher the RE2O3 content, the easier it is for segregation phases to form, and in particular the second segregation phase to form more easily than the first segregation phase. And the higher the Re2O3 content, the lower the relative dielectric constant. Furthermore, the number of locations where RE exists alone increases, so the MTTF also decreases.

[0118] Table 2 shows the results when only the SiO2 content is changed under the same conditions except for the SiO2 content. The higher the SiO2 content, the smaller the S1 / S2 tends to be. When S1 / S2 is 0 or more and 0.10 or less, good characteristics are shown. When the SiO2 content is low and S1 / S2 is too large, the Ti-Dy ratio becomes too high, and the dielectric composition is difficult to densify. As a result, the dielectric density decreases, the relative dielectric constant decreases, the resistivity decreases, and the MTTF decreases. When the SiO2 content is high, the average Si2 / RE2 tends to increase. When the average Si2 / RE2 is too large, the relative dielectric constant tends to increase and the MTTF decreases.

[0119] Table 3 shows the results when only the MO content was changed while keeping all other conditions the same. In all experimental examples, S1 / S2 = 0, and good characteristics were obtained. Furthermore, the higher the MO content, the lower the relative dielectric constant and the higher the resistivity tended to be. Furthermore, whether the MO content was high or low, the MTTF tended to decrease.

[0120] Table 4 shows the results when only the BaO content is changed under the same conditions except for the BaO content. The higher the BaO content, the smaller the S1 / S2 tends to be. When S1 / S2 is 0 or more and 0.10 or less, good characteristics are shown. When the BaO content is small and S1 / S2 is too large, the Ti-Dy ratio becomes too high, and the dielectric composition is difficult to densify. As a result, the dielectric density decreases, the relative dielectric constant decreases, the resistivity decreases, and the MTTF decreases. When the BaO content is high, the average Si2 / RE2 tends to increase. And the relative dielectric constant tends to increase and the MTTF tends to decrease.

[0121] Table 5 shows the results when the conditions were the same except for the changes in the heat treatment conditions. The lower the sintering temperature and the shorter the sintering time, the more difficult it is for the second segregation phase to form, and S1 / S2 tends to increase. If the sintering temperature is so low that S1 / S2 exceeds 0.10, the dielectric composition is less likely to be densified, and the dielectric density decreases. Furthermore, the grain growth of the main component is insufficient, and the relative dielectric constant decreases. Furthermore, the solid solution of RE in the main component is also insufficient, so that the resistivity and MTTF tend to decrease.

[0122] When the firing temperature is high and the firing time is long, the second segregation phase is sufficiently formed, but the first grain boundary phase is difficult to form, and S1 / S2 tends to become small. However, the average Si2 / RE2 also tends to become high. And when the firing temperature is too high and Si2 / RE2 is too high, the main component may undergo abnormal grain growth, and the relative dielectric constant becomes too large. Furthermore, the resistivity increases as the RE dissolves in the main component. And the particle size of the main component tends to vary widely, and the MTTF tends to decrease.

[0123] Table 6 shows the results of samples 51 to 54, which were carried out under the same conditions except for the type of RE. Sample 3, which has a different RE2O3 content and SiO2 content, is also shown. The smaller the ionic radius of an RE used, the more difficult it is for the RE to dissolve in the main component. As a result, grain growth is suppressed, the relative dielectric constant increases, and the resistivity and MTTF tend to decrease. The size of the ionic radius of the RE listed in Table 6 is Gd>Dy>Y>Yb.

[0124] Table 7 shows the results when the SiO2 content, BaO content, and firing conditions were mainly changed. Basically, the higher the SiO2 content and BaO content, the easier it is to densify the dielectric at a lower firing temperature. Therefore, the higher the SiO2 content and BaO content, the lower the suitable firing temperature tends to be.

[0125] Each of the examples in which S1 / S2 is within a specified range and the average of Si2 / RE2 is within a specified range shows good characteristics. In contrast, in sample numbers 61 and 62 in which S1 / S2 is too large, the dielectric composition is difficult to densify. As a result, the dielectric density is reduced, the relative dielectric constant is reduced, the resistivity is reduced, and the MTTF is reduced. In sample numbers 67 and 70 in which the average of Si2 / RE2 is too high, the relative dielectric constant is high and the rinsing MTTF is reduced. [Explanation of symbols]

[0126] 1. Multilayer ceramic capacitor 10... Element body 2... Dielectric layer 14… Main phase 16... 1st segregated phase 18…Second segregation phase 3… Internal electrode layer 4… External electrode

Claims

1. A dielectric composition comprising a main phase and a segregation phase containing a rare earth element RE (RE is one or more selected from Dy, Gd, Y and Yb), The main phase contains a main component having a perovskite crystal structure represented by BaTiO3, Among the segregation phases, a segregation phase in which the atomic ratio of Si to RE is 0 or more and 0.20 or less is defined as a first segregation phase, and a segregation phase in which the atomic ratio of Si to RE is more than 0.20 is defined as a second segregation phase, In a cross section of the dielectric composition, when an area ratio of the first segregation phase is S1 and an area ratio of the second segregation phase is S2, 0≦S1 / S2≦0.10 is satisfied, The atomic ratio of Si to RE in the second segregation phase is 0.80 or less on average, The dielectric composition further comprises, in addition to Si and RE, M, M is one or more selected from Mg and Mn; With respect to the main component, the RE content is 0.90 mol % or more and 5.00 mol % or less in terms of RE2O3, the M content is 0.10 mol % or more and 2.00 mol % or less in terms of MO, and the Si content is 0.50 mol % or more and 1.90 mol % or less in terms of SiO2, The dielectric composition contains an oxide of Ba in addition to the main component, and the content of the oxide of Ba is 0.70 mol % or more and 2.10 mol % or less.

2. The content of RE in the main component is RE 2 O 3 The M content is 0.20 mol % or more and 1.00 mol % or less in terms of MO, and the Si content is SiO 2 2. The dielectric composition according to claim 1, wherein the content is 0.60 mol % or more and 1.80 mol % or less in terms of the total molecular weight.

3. 3. The dielectric composition according to claim 1, wherein the atomic ratio of Ba to Ti in the first segregation phase is less than 1.00, and the atomic ratio of Ba to Ti in the second segregation phase is greater than 1.

00.

4. The dielectric composition according to any one of claims 1 to 3, wherein, in a cross section of the dielectric composition, the first segregation phase has an average equivalent circular diameter A1, the second segregation phase has an average equivalent circular diameter A2, and 0≦A1 / A2<1.

00.

5. An electronic component comprising the dielectric composition according to any one of claims 1 to 4.

6. A laminated electronic component comprising dielectric layers made of the dielectric composition according to any one of claims 1 to 4 and electrode layers laminated alternately.

Citation Information

Patent Citations

  • Dielectric ceramic composition and electronic component

    JP2006008460A

  • Ceramic electronic part and method for manufacturing the same

    JP2011057511A

  • Laminated ceramic electronic part

    JP2015046589A

  • Ceramic electronic part

    JP2017120853A

  • Dielectric composition and laminate electronic component

    JP2018035026A