Gas sensor element, gas sensor, and method of manufacturing gas sensor element

By using a porous ceramic buffer layer with a lower shrinkage temperature and a reinforcing layer, the gas sensor element manufacturing process minimizes cracks and maintains gas flow consistency, addressing the issue of structural defects caused by differential shrinkage.

JP7594987B2Active Publication Date: 2024-12-05NITERRA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021141677
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-31
Publication Date
2024-12-05
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

During the manufacturing of gas sensor elements, cracks occur in the gas introduction portion due to misalignment and differential shrinkage between the carbon paste layer and the unfired gas introduction part during firing, leading to defects.

Method used

Incorporating a buffer layer made of porous ceramic with a lower shrinkage start temperature than the gas introduction part, positioned to overlap the boundary between the gas introduction part and the second ceramic structure, and ensuring the buffer layer does not cover the end surface facing the space, along with a reinforcing layer to stabilize the structure.

Benefits of technology

This design effectively suppresses cracks in the gas introduction portion, maintaining structural integrity and ensuring consistent gas flow rates during the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594987000001
    Figure 0007594987000001
  • Figure 0007594987000002
    Figure 0007594987000002
  • Figure 0007594987000003
    Figure 0007594987000003
Patent Text Reader

Abstract

To provide a gas sensor element including a gas introduction part inhibiting generation of defects such as cracks.SOLUTION: A frame-like body includes: a gas introduction part 151 composed of porous ceramic, with an end 151a arranged outside and an end 151b arranged at a space 150a side; and a ceramic structure 100C composed of fine ceramic, a peripheral wall part surrounding the space 150a with the gas introduction part 151. A gap 150b connecting to the space 150a is formed between an opposing face 151b1 opposing a ceramic structure 100B, of the end 151b of the gas introduction part 151, and the ceramic structure 100B. A gas sensor element 10 includes ceramics formed of a material having contraction start temperature lower than that of the material for forming the gas introduction part 151, and comprises a buffer layer 300 formed on the opposing face 151b1 so as to, when viewed from a lamination direction, overlap with a boundary X between an edge 150b1 on the outer side of the gap 150b and the ceramic structure 100B.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas sensor element, a gas sensor, and a method for manufacturing a gas sensor element. [Background technology]

[0002] There is known a gas sensor for measuring the concentration of a specific component (oxygen concentration, etc.) in exhaust gas from an internal combustion engine. This type of gas sensor includes a gas sensor element mainly made of ceramic. The gas sensor element is made of a laminate of a plurality of plate-shaped ceramics (ceramic structures), and includes a space therein used as a measurement chamber. This space is surrounded by two plate-shaped ceramics arranged at a distance from each other in the lamination direction, and a frame-shaped ceramic arranged between the two ceramics. The frame-shaped ceramic mainly includes a gas inlet portion made of porous ceramics and a peripheral wall portion made of dense ceramics.

[0003] When manufacturing such a gas sensor element, for example, as shown in Patent Document 1, a printing technique is used. In this case, for example, a layer for forming an insulating layer is formed by printing using an alumina slurry on the surface of an unfired sheet on which an electrode pattern or the like is provided. In addition, an opening where no slurry is placed is formed in the layer at a position corresponding to the space, and a cutout where no slurry is placed is formed at a position corresponding to the gas inlet. This cutout is connected to the opening, and an unfired gas inlet prepared separately is placed so as to fill the cutout. In addition, a part of the layer surrounding the opening corresponds to the peripheral wall. Then, a layer of carbon paste (a burnt material that is burnt during firing) is formed by printing in the opening so that the shape (space) is maintained during firing.

[0004] After various printed layers etc. are formed on a given sheet in this manner, other unfired sheets etc. are laminated so as to cover the printed layers etc. Then, the obtained unfired laminate is fired at a given temperature to obtain a gas sensor element. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-3286 A Summary of the Invention [Problem to be solved by the invention]

[0006] When a layer of carbon paste (hereinafter, paste layer) is formed by printing so as to overlap the opening during the manufacture of the gas sensor element, the paste layer is usually formed large in advance so that its edge extends beyond the opening, taking into consideration the occurrence of printing misalignment, etc. Therefore, the edge of the paste layer overlaps with the unfired gas inlet portion surrounding the opening and the unfired peripheral wall portion in the thickness direction (stacking direction).

[0007] However, when an unfired laminate including such a paste layer is fired, defects such as cracks may occur in the gas inlet part in the portion that was in contact with the periphery of the paste layer. This is presumably because, when the laminate is fired, the paste layer starts to shrink before the unfired gas inlet part, and the unfired gas inlet part is pulled by the periphery of the shrinking paste layer, causing it to tear.

[0008] An object of the present invention is to provide a gas sensor element or the like including a gas introduction portion in which defects such as cracks are suppressed. [Means for solving the problem]

[0009] The means for solving the above problems are as follows. <1> A gas sensor element is formed by stacking a plurality of plate-shaped ceramic structures, the gas sensor element comprising: a first ceramic structure having a detection cell including a first solid electrolyte body and a pair of detection electrodes provided on both sides of the first solid electrolyte body; a second ceramic structure having a pump cell including a second solid electrolyte body and a pair of pump electrodes provided on both sides of the second solid electrolyte body, the second ceramic structure being disposed in a stacking direction while maintaining a gap with respect to the first ceramic structure; and a frame-shaped body disposed between the first ceramic structure and the second ceramic structure and surrounding a space formed between the first ceramic structure and the second ceramic structure, the frame-shaped body having one end disposed on an outer side and the other end disposed inside the space. a third ceramic structure including a gas inlet portion made of porous ceramic and arranged on the one end side of the second ceramic structure and for introducing an external detection target gas into the space while passing the external detection target gas from the one end side to the other end side, and a peripheral wall portion made of dense ceramic and surrounding the space together with the gas inlet portion, wherein a gap communicating with the space is formed between an opposing surface of the other end of the gas inlet portion that faces the second ceramic structure and the second ceramic structure, and a buffer layer made of a ceramic material having a lower shrinkage start temperature than a material for forming the gas inlet portion, the buffer layer being formed on the opposing surface so as to overlap an outer edge of the gap and a boundary portion between the second ceramic structure and the second ceramic structure when viewed from the stacking direction.

[0010] <2> The buffer layer is made of a porous ceramic having pores larger than the pores contained in the gas inlet portion. <1> The gas sensor element according to claim 1 .

[0011] <3> The buffer layer is formed on the opposing surface so as not to cover an end surface of the other end of the gas inlet portion that faces the space. <1> or <2> The gas sensor element according to claim 1 .

[0012] <4> The second ceramic structure includes a plate-shaped main body including the pump cell, an adhesive layer disposed between the plate-shaped main body and the third ceramic structure and made of a dense ceramic layer, and a reinforcing layer disposed between the plate-shaped main body and the adhesive layer and having a shape surrounding the space when viewed from the stacking direction. <1> from <3> 13. The gas sensor element according to claim 12,

[0013] <5> The material for forming the buffer layer contains zirconia as a main component, and the material for forming the gas inlet portion contains alumina as a main component. <1> from <4> 13. The gas sensor element according to claim 12,

[0014] <6> The above <1> from <5> A gas sensor comprising the gas sensor element according to any one of the above.

[0015] <7> a first ceramic structure having a detection cell including a first solid electrolyte body and a pair of detection electrodes provided on both sides of the first solid electrolyte body; a second ceramic structure having a pump cell including a second solid electrolyte body and a pair of pump electrodes provided on both sides of the second solid electrolyte body, the second ceramic structure being arranged in a stacking direction while maintaining a gap with respect to the first ceramic structure; and a third ceramic structure having a layered structure including a frame-shaped body arranged between the first ceramic structure and the second ceramic structure and surrounding a space formed between the first ceramic structure and the second ceramic structure, the frame-shaped body having one end arranged on an exterior side and the other end arranged on the space side, the frame-shaped body including a gas inlet part made of porous ceramic that introduces an external detection target gas into the space while passing the external detection target gas from the one end side to the other end side, and a peripheral wall part made of dense ceramic and surrounding the space together with the gas inlet part, a first forming step of forming an unsintered buffer layer made of a material having a lower shrinkage start temperature than the unsintered gas inlet portion so as to overlap an inner end portion of the unsintered gas inlet portion that corresponds to the other end portion arranged on the opening side of the unsintered gas inlet portion; a second forming step of forming a burnt-out portion made of a paste material containing a burnt-out material by printing, the burnt-out portion being filled in the opening on the first green sheet and overlapping with the unsintered buffer layer while its end portion protrudes towards the unsintered gas inlet portion located outside the opening; a lamination step of laminating the first green sheet on which the burnt-out portion is formed and a second green sheet for forming the second ceramic structure on one another; and a firing step of firing a laminate obtained after the lamination step.

[0016] <8> The unfired gas inlet contains a first burnable powder that is burned in the firing step, The unsintered buffer layer is burned in the firing step and contains a second burnable powder having a particle size larger than that of the first burnable powder. <7> A method for manufacturing the gas sensor element according to claim 1.

[0017] <9> The content of the second burnable powder in the unsintered buffer layer is lower than the content of the first burnable powder in the unsintered gas inlet portion. <8> A method for manufacturing the gas sensor element according to claim 1.

[0018] <10> The second burnable powder is spherical, and the first burnable powder is irregular. <8> or <9> A method for manufacturing the gas sensor element according to claim 1.

[0019] <11> The unsintered buffer layer contains zirconia as a main component, and the unsintered gas inlet portion contains alumina as a main component. <7> from <10> 13. A method for manufacturing the gas sensor element according to any one of the above.

[0020] <12> In the first forming step, the unsintered buffer layer is formed on the inner end portion so as not to cover an end surface of the inner end portion facing the opening. <7> from <11> 13. A method for manufacturing the gas sensor element according to any one of the above. Effect of the Invention

[0021] According to the present invention, it is possible to provide a gas sensor element and the like including a gas inlet portion in which defects such as cracks are suppressed. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a vertical cross-sectional view of a gas sensor according to a first embodiment. [Diagram 2] FIG. 1 is a perspective view of a gas sensor element according to a first embodiment; [Diagram 3] Cross section of line AA in Figure 2 [Figure 4] An exploded perspective view of a gas sensor element. [Diagram 5]FIG. 11 is an enlarged plan view of the frame-shaped body and its surroundings of the third ceramic structure; [Figure 6] Cross section of line BB in Figure 2 [Figure 7] A flow chart showing each step in a method for manufacturing a gas sensor element. [Figure 8] FIG. 1 is a plan view showing a portion of a first laminate obtained in an installation step. [Figure 9] FIG. 11 is a plan view showing a part of the first laminate in a state where a green buffer layer is formed on an inner end of a green gas inlet in a first forming step. [Figure 10] FIG. 11 is a plan view showing a part of the first laminate in a state where a burnt portion is formed so that an end portion overlaps with an unsintered buffer layer in a second forming step. [Figure 11] FIG. 1 is a cross-sectional view showing a schematic configuration of an unfired laminate for forming a gas sensor element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] <Embodiment 1> A first embodiment of the present invention will be described below with reference to Fig. 1 to Fig. 11. Fig. 1 is a vertical cross-sectional view of a gas sensor 1 according to the first embodiment, Fig. 2 is a perspective view of a gas sensor element 10 according to the first embodiment, Fig. 3 is a cross-sectional view taken along line AA in Fig. 2, and Fig. 4 is an exploded perspective view of the gas sensor element 10.

[0024] In Fig. 1, the axis AX of the gas sensor 1 is shown as a straight line (dotted line) along the up-down direction. In this specification, the direction along the axis AX of the gas sensor 1 may be referred to as the "longitudinal direction", and the direction perpendicular to the axis AX may be referred to as the "width direction". In this specification, the lower side of the gas sensor 1 shown in Fig. 1 may be referred to as the "front end side", and the opposite side (the upper side in Fig. 1) may be referred to as the "rear end side". For convenience of explanation, the upper sides in Figs. 2 to 4 are referred to as the "front side (front surface side)" of the gas sensor element 10, and the lower sides thereof are referred to as the "rear side (back surface side)" of the gas sensor element 10.

[0025] The gas sensor 1 detects NO in exhaust gas, which is the gas to be measured (gas to be detected). xThe gas sensor 1 is equipped with a gas sensor element 10 capable of detecting the concentration of, for example, an oxygen gas, an oxygen ion, etc. This gas sensor 1 is attached to an exhaust pipe (not shown) of an internal combustion engine when used, and is equipped with a cylindrical metal shell 20 having a threaded portion 21 formed at a predetermined position on its outer surface for fixing to the exhaust pipe. The gas sensor element 10 is generally in the form of a long and narrow plate extending along the axis AX, and such gas sensor element 10 is held inside the metal shell 20.

[0026] The gas sensor 1 includes a cylindrical holding member 60 having an insertion hole 62 into which the rear end portion 10k of the gas sensor element 10 is inserted, and six terminal members held inside the holding member 60. For ease of explanation, only two of the six terminal members, terminal members 75 and 76, are shown in FIG.

[0027] As shown in Fig. 2, a total of six electrode terminals 13 to 18 each having a rectangular shape in a plan view are formed on the rear end portion 10k of the gas sensor element 10. Note that Fig. 1 shows only the electrode terminals 14 and 17. The above-mentioned terminal members are elastically abutted against and electrically connected to the electrode terminals 13 to 18, respectively. For example, the element abutment portion 75b of the terminal member 75 elastically abuts against and electrically connected to the electrode terminal 14, and the element abutment portion 76b of the terminal member 76 elastically abuts against and electrically connected to the electrode terminal 17.

[0028] In addition, the six terminal members (terminal members 75, 76, etc.) are each provided with a different lead wire 71. 1, the core wire of lead wire 71 is crimped and held by lead wire gripping portion 77 of terminal member 75. Also, the core wire of another lead wire 71 is crimped and held by lead wire gripping portion 78 of terminal member 76.

[0029] 2, of the two main surfaces 10a, 10b at the rear end 10k of the gas sensor element 10, an open-shaped air inlet 10h is provided on one (front) main surface 10a at a location closer to the tip side than the electrode terminal portions 13 to 15 and closer to the rear end side than a ceramic sleeve 45 (see FIG. 1) described later. The air inlet 10h is disposed within an insertion hole 62 of a holding member 60.

[0030] The metallic shell 20 is a tubular member having a through hole 23 penetrating in the direction of the axis AX. The metallic shell 20 has a shelf portion 25 that protrudes radially inward and constitutes a part of the through hole 23. The metallic shell 20 holds the gas sensor element 10 in the through hole 23 with a front end portion 10s of the gas sensor element 10 protruding outward from its own front end side (downward in FIG. 1) and a rear end portion 10k of the gas sensor element 10 protruding outward from its own rear end side (upward in FIG. 1).

[0031] Further, an annular ceramic holder 42, two talc rings 43, 44 formed by filling talc powder in an annular shape, and a ceramic sleeve 45 are disposed inside the through hole 23 of the metallic shell 20. More specifically, the ceramic holder 42, the talc rings 43, 44, and the ceramic sleeve 45 are stacked in this order from the front end side to the rear end side of the metallic shell 20 so as to surround the gas sensor element 10 extending in the direction of the axis AX.

[0032] A metal cup 41 is disposed between the ceramic holder 42 and the shelf portion 25 of the metallic shell 20. A crimping ring 46 is disposed between the ceramic sleeve 45 and the crimped portion 22 of the metallic shell 20. The crimped portion 22 of the metallic shell 20 is crimped so as to press the ceramic sleeve 45 towards the tip side via the crimping ring 46.

[0033] An outer protector 31 and an inner protector 32 made of metal (e.g., stainless steel) having a plurality of holes are attached by welding to the front end 20b of the metallic shell 20 so as to cover the front end 10s of the gas sensor element 10. In addition, an outer cylinder 51 is attached by welding to the rear end of the metallic shell 20. The outer cylinder 51 has a generally cylindrical shape extending in the direction of the axis AX and surrounds the gas sensor element 10.

[0034] The holding member 60 is made of an insulating material (e.g., alumina) and is a cylindrical member having an insertion hole 62 penetrating in the direction of the axis AX. The six terminal members (terminal members 75, 76, etc.) described above are arranged in the insertion hole 62 (see FIG. 1). A flange portion 65 that protrudes radially outward is formed at the rear end of the holding member 60. The holding member 60 is held by the internal support member 53 with the flange portion 65 abutting against the internal support member 53. The internal support member 53 is held by a crimped portion 51g of the outer tube 51 that is crimped radially inward.

[0035] An insulating member 90 is disposed on the rear end surface 61 of the holding member 60. The insulating member 90 is made of an insulating material (e.g., alumina) and has an overall annular shape. A total of six through holes 91 are formed in the insulating member 90, penetrating in the direction of the axis AX. The lead wire gripping portions 77, 78 of the terminal members described above are disposed in the through holes 91.

[0036] In addition, an elastic seal member 73 made of fluororubber is disposed on the radially inner side of the rear end opening 51c disposed on the rear end side of the outer cylinder 51. A total of six cylindrical insertion holes 73c extending in the direction of the axis AX are formed in the elastic seal member 73. Each insertion hole 73c is formed by an insertion hole surface 73b (cylindrical inner wall surface) of the elastic seal member 73. A lead wire 71 is inserted into each insertion hole 73c. ​​Each lead wire 71 extends to the outside of the gas sensor 1 through the insertion hole 73c of the elastic seal member 73. The elastic seal member 73 is elastically compressed and deformed in the radial direction by crimping the rear end opening 51c of the outer cylinder 51 radially inward, thereby tightly contacting the insertion hole surface 73b and the outer peripheral surface 71b of the lead wire 71 to provide a watertight seal between the insertion hole surface 73b and the outer peripheral surface 71b of the lead wire 71.

[0037] 3, the gas sensor element 10 has a structure in which a plurality of plate-shaped ceramic structures are laminated. Such a gas sensor element 10 includes plate-shaped insulating layers 111s, 121s, and 131s, solid electrolyte bodies 111e, 121e, and 131e formed therein, and insulators 140 and 145 disposed between the insulating layers. Furthermore, the gas sensor element 10 includes a heater 161 disposed on the back surface side of the solid electrolyte body 131e. The heater 161 includes two plate-shaped insulators 162 and 163 mainly made of alumina, and a heater pattern 164 embedded between the insulators. The heater pattern 164 is a film-shaped pattern mainly made of platinum (Pt).

[0038] The solid electrolyte bodies 111e, 121e, and 131e each have a substantially rectangular shape in plan view. The solid electrolyte body 111e is formed so as to overlap with an opening 111a provided at the tip side (left side in FIG. 4) of the plate-shaped insulating layer 111s extending in the axis AX direction. The solid electrolyte body 121e is formed so as to overlap with an opening 121a provided at the tip side (left side in FIG. 4) of the plate-shaped insulating layer 121s extending in the axis AX direction. The solid electrolyte body 131e is formed so as to overlap with an opening 131a provided at the tip side (left side in FIG. 4) of the plate-shaped insulating layer 131s extending in the axis AX direction. The solid electrolyte bodies 111e, 121e, and 131e may be formed so as to be embedded in the corresponding openings 111a, 121a, and 131a, respectively, or may be formed so as to transfer a separately prepared sheet-shaped member to a predetermined location.

[0039] The solid electrolyte bodies 111e, 121e, and 131e are made of zirconia, which is a solid electrolyte, and have oxygen ion conductivity. A porous Ip1+ electrode 112 is provided on the front side of the solid electrolyte body 111e. A porous Ip1- electrode 113 is provided on the back side of the solid electrolyte body 111e. Furthermore, the front side of the Ip1+ electrode 112 is covered with a porous layer 114. An Ip1+ lead 116 is connected to the Ip1+ electrode 112. An Ip1- lead 117 is connected to the Ip1- electrode 113. The Ip1+ electrode 112 and the Ip1- electrode 113 correspond to a pair of pump electrodes 112, 113 of the present invention.

[0040] As shown in Fig. 4, a plate-shaped dense layer 118B extending in the direction of the axis AX is laminated on each surface of the Ip1+ electrode 112 and the Ip1+ lead 116. The dense layer 118B is made of a gas-impermeable material such as alumina. An opening 118Ba having a rectangular shape in a plan view is provided on the tip side of the dense layer 118B. The porous layer 114 described above is formed so as to fill the opening 118Ba.

[0041] As shown in FIG. 4, a gas-impermeable dense layer 118 made of alumina or the like and including voids 10G is disposed on the surface side of the dense layer 118B. The voids 10G are formed inside a groove extending in the longitudinal direction (axis AX direction). A part of the porous layer 114 is exposed from the voids 10G. The voids 10G extend straight in the plate-like dense layer 118 extending in the axis AX direction from the vicinity of the porous layer 114 to a portion communicating with the air inlet 10h. A through hole is provided on the rear end side of the plate-like dense layer 118 extending in the axis AX direction to electrically connect with the electrode terminals 13, 14, and 15.

[0042] Further, a gas-impermeable dense layer 115 made of alumina or the like is laminated on the surface of the dense layer 118. By laminating the dense layer 115 in this manner, the dense layer 115 closes the gap 10G.

[0043] An air inlet 10h is formed in the dense layer 115 at a position overlapping with the rear end of the gap 10G extending in the longitudinal direction (axis AX direction). The air inlet 10h is an opening provided in a manner penetrating the dense layer 115 in the thickness direction. Such an air inlet 10h is connected to the gap 10G. The air inlet 10h opens on the rear end side of the ceramic sleeve 45, and can introduce air instead of exhaust gas. As a result, the Ip1+ electrode 112 is exposed to the air introduced from the air inlet 10h through the porous layer 114.

[0044] The solid electrolyte body 111e, the Ip1+ electrode 112, and the Ip1- electrode 113 constitute an Ip1 cell (pump cell) 110 (see FIG. 3). The Ip1 cell 110 pumps oxygen between an atmosphere in contact with the Ip1+ electrode 112 (the atmosphere in the gap 10G) and an atmosphere in contact with the Ip1- electrode 113 (the atmosphere in the first measurement chamber 150 described later; that is, the measurement target gas outside the gas sensor element 10) in response to a pump current Ip1 (first pump current) flowing between the Ip1+ electrode 112 and the Ip1- electrode 113 (so-called oxygen pumping). In this specification, the plate-shaped portion including the Ip1 cell 110, the insulating layer 111s, etc. is referred to as the "second ceramic structure 100B."

[0045] A porous Vs-electrode 122 is provided on the front side of the solid electrolyte body 121e. A porous Vs+electrode 123 is provided on the back side of the solid electrolyte body 121e. The Vs-electrode 122 and the Vs+electrode 123 correspond to the pair of detection electrodes 122, 123 of the present invention.

[0046] In the stacking direction, a first measurement chamber 150 is formed between the solid electrolyte bodies 111e and 121e. The first measurement chamber 150 is an internal space into which the measurement target gas (exhaust gas) flowing through the exhaust passage in the exhaust pipe is first introduced into the gas sensor element 10, and communicates with the outside of the gas sensor element 10 through a first porous body (diffusion resistance portion) 151 (see FIGS. 2 and 4) having gas permeability and water permeability. The first porous body 151 is provided on the side of the first measurement chamber 150 as a partition between the gas sensor element 10 and the outside. Such a first porous body 151 limits the flow rate (diffusion speed) of exhaust gas into the first measurement chamber 150 per unit time.

[0047] A second porous body 152 is provided at the rear end side (right side in Figure 3) of the first measurement chamber 150 as a partition between the first measurement chamber 150 and the second measurement chamber 160 described later, which limits the amount of exhaust gas flowing per unit time.

[0048] The solid electrolyte body 121e, the Vs- electrode 122, and the Vs+ electrode 123 constitute a Vs cell (detection cell) 120. This Vs cell 120 generates an electromotive force mainly in response to the oxygen partial pressure difference between atmospheres separated by the solid electrolyte body 121e (the atmosphere in the first measurement chamber 150 to which the Vs- electrode 122 contacts and the atmosphere in the reference oxygen chamber 170 to which the Vs+ electrode 123 contacts). In this specification, the plate-like portion including the Vs cell 120, the insulating layer 121s, etc. is referred to as the "first ceramic structure 100A."

[0049] A porous Ip2+ electrode 132 and a porous Ip2- electrode 133 are provided on the front surface side of the solid electrolyte body 131e.

[0050] A reference oxygen chamber 170 is formed as an isolated small space between the Ip2+ electrode 132 and the Vs+ electrode 123. This reference oxygen chamber 170 is constituted by an opening 145b formed in the insulator 145. In addition, a ceramic porous body 171 is disposed on the Ip2+ electrode 132 side of the reference oxygen chamber 170 (see FIG. 3).

[0051] Further, a second measurement chamber 160 is formed at a position facing the Ip2-electrode 133 in the stacking direction. This second measurement chamber 160 is mainly composed of an opening 145c penetrating the insulator 145 in the stacking direction (thickness direction), an opening 125 penetrating the insulating layer 121s in the stacking direction (thickness direction), and an opening 152a penetrating the second porous body 152 in the stacking direction (thickness direction).

[0052] The first measurement chamber 150 and the second measurement chamber 160 communicate with each other via the second porous body 152, which has gas permeability and water permeability. Therefore, the second measurement chamber 160 communicates with the outside of the gas sensor element 10 through the first porous body 151, the first measurement chamber 150, and the second porous body 152.

[0053] The solid electrolyte body 131e, the Ip2+ electrode 132, and the Ip2- electrode 133 are connected to the NO xThe Ip2 cell 130 (second pump cell) is configured to detect the concentration of NO decomposed in the second measurement chamber 160. x The oxygen (oxygen ions) derived from the exhaust gas (measurement target gas) introduced into the second measurement chamber 160 is transferred to the reference oxygen chamber 170 through the solid electrolyte body 131e. At that time, NO ions contained in the exhaust gas (measurement target gas) introduced into the second measurement chamber 160 are transferred between the Ip2+ electrode 132 and the Ip2- electrode 133. x A current (second pump current) flows according to the concentration of Ip2 cell 130, insulating layer 131s, etc. In this specification, the plate-like portion including Ip2 cell 130, insulating layer 131s, etc. is referred to as "fourth ceramic structure 100D."

[0054] In this specification, the plate-like portion disposed between the first ceramic structure 100A and the second ceramic structure 100B is referred to as a "third ceramic structure 100C." Details of the third ceramic structure 100C will be described later.

[0055] In this embodiment, an alumina insulating layer 119 is formed on the rear surface of the insulating layer 111s, excluding the Ip1-electrode 113 and the like. The Ip1-electrode 113 is in contact with the solid electrolyte body 111e through a through-hole 119b (see FIG. 4) that penetrates the alumina insulating layer 119 in the stacking direction. This alumina insulating layer 119 constitutes a part of the second ceramic structure 100B.

[0056] An alumina insulating layer 128 (see FIG. 3) is formed on the surface of the insulating layer 121s, except for the Vs-electrode 122 and the like. For ease of explanation, the alumina insulating layer 128 is omitted in FIG. 4. The Vs-electrode 122 contacts the solid electrolyte body 121e through a through-hole (not shown) that passes through the alumina insulating layer 128 in the stacking direction. This alumina insulating layer 128 constitutes a part of the first ceramic structure 100A.

[0057] An alumina insulating layer 129 (see FIG. 3) is formed on the rear surface of the insulating layer 121s, except for the Vs+ electrode 123 and the like. For ease of explanation, the alumina insulating layer 129 is omitted in FIG. 4. The Vs+ electrode 123 contacts the solid electrolyte body 121e through a through hole (not shown) that penetrates the alumina insulating layer 129 in the stacking direction. This alumina insulating layer 129 constitutes a part of the first ceramic structure 100A.

[0058] An alumina insulating layer 138 (see FIG. 3) is formed on the surface of the insulating layer 131s, except for the Ip2+ electrode 132, the Ip2- electrode 133, etc. For convenience of explanation, the alumina insulating layer 138 is omitted in FIG. 4. The Ip2+ electrode 132 and the Ip2- electrode 133 are in contact with the solid electrolyte body 131e through through holes (not shown) that penetrate the alumina insulating layer 138 in the stacking direction. This alumina insulating layer 138 constitutes a part of the fourth ceramic structure 100D.

[0059] Here, the third ceramic structure 100C will be described with reference to FIG. 5 and the like. FIG. 5 is an enlarged plan view of the frame-shaped body 200 and its vicinity of the third ceramic structure 100C. The upper side of FIG. 5 corresponds to the front end side of the gas sensor element 10, and the lower side of FIG. 5 corresponds to the rear end side of the gas sensor element 10. The third ceramic structure 100C is a layered ceramic structure having a frame-shaped body 200 surrounding a space 150a formed between the first ceramic structure 100A and the second ceramic structure 100B. Such a third ceramic structure 100C mainly includes a layered (plate-shaped) insulator 140, two first porous bodies (gas introduction parts) 151, and a second porous body 152 (see FIG. 4). The insulator 140 is made of dense ceramic (for example, alumina). The space 150a is formed between the first ceramic structure 100A and the second ceramic structure 100B, and constitutes a space (main space) that occupies most of the first measurement chamber 150.

[0060] The frame-shaped body 200 is composed of two first porous bodies (gas introduction parts) 151, a second porous body 152, and a peripheral wall part 141 that surrounds the space 150a together with the first porous body 151 and the second porous body 152. The peripheral wall part 141 is composed of a part of the insulator 140 that faces the space 150a.

[0061] As shown in FIG. 5, a pair (two) of first porous bodies (gas inlet portions) 151 are arranged facing each other with a space 150a therebetween in the width direction (left-right direction) of the third ceramic structure 100C.

[0062] The first porous body (gas inlet) 151 has one end 151a disposed on the outside side and the other end 151b disposed on the space 150a side. The first porous body (gas inlet) 151 is made of porous ceramic that introduces an external measurement target gas (detection target gas) into the space 150a while allowing the gas to pass from the one end 151a side to the other end 151b side.

[0063] As shown in FIG. 5, a peripheral wall portion 141 is disposed so as to surround the space 150a together with the first porous body (gas inlet portion) 151 and the like.

[0064] Fig. 6 is a cross-sectional view taken along line BB in Fig. 2. For ease of explanation, Fig. 6 shows a cross-sectional configuration in the vicinity of a first porous body (gas inlet portion) 151 of a third ceramic structure 100C disposed between the first ceramic structure 100A and the second ceramic structure 100B in the gas sensor element 10.

[0065] 6, gaps 150b connected to the space 150a are formed between the second ceramic structure 100B and an opposing surface 151b1 of the other end 151b of the first porous body (gas inlet portion) 151, the opposing surface 151b1 facing the second ceramic structure 100B. The gaps 150b are part of the first measurement chamber 150. Furthermore, the gaps 150b are formed between each of the two first porous bodies (gas inlet portions) 151 and the second ceramic structure 100B (i.e., two gaps 150b are formed).

[0066] When the gas sensor element 10 is viewed from the stacking direction, the buffer layer 300 is formed so as to overlap an outer edge 150b1 of the gap 150b and a boundary portion X with the second ceramic structure 100B. The buffer layer 300 is made of a ceramic material having a lower shrinkage start temperature than the material for forming the first porous body (gas inlet portion) 151.

[0067] In this specification, the "shrinkage start temperature" refers to the temperature at which the projection ratio becomes 1.05 when green sheets having the same composition as each ceramic layer (e.g., buffer layer 300, first porous body 151) are prepared and heated in an air atmosphere to proceed with firing to form each ceramic layer. The projection ratio is also called the firing shrinkage ratio, and is calculated by taking the vertical or horizontal dimension of the green sheet before firing as 1 when the vertical or horizontal dimension of the ceramic layer after firing is taken as 1. In other words, the allocation ratio = (the vertical or horizontal dimension of the green sheet before firing) / (the dimension in the same direction of the ceramic layer after firing).

[0068] The buffer layer 300 is formed by printing as described below. The gas sensor element 10 of the present embodiment includes such a buffer layer 300, and thus the occurrence of defects such as cracks in the first porous body (gas inlet portion) 151 during the manufacture of the gas sensor element 10 is suppressed.

[0069] The buffer layer 300 is made of a porous ceramic containing pores larger than those contained in the first porous body (gas inlet portion) 151. Therefore, the amount of flow (diffusion rate) per unit time of the measurement target gas (detection target gas) moving inside the first porous body (gas inlet portion) 151 is prevented from being affected by the buffer layer 300 and from decreasing.

[0070] The material for forming the buffer layer 300 contains zirconia as a main component, and the material for forming the first porous body (gas inlet portion) 151 contains alumina as a main component. In this specification, the term "main component" refers to a component whose content (content ratio) in each component is 50 mass% or more. That is, in this embodiment, the buffer layer 300 contains 50 mass% or more of zirconia, and the first porous body (gas inlet portion) 151 contains 50 mass% or more of alumina.

[0071] 6, the buffer layer 300 is formed on the opposing surface 151b1 so as not to cover the end surface 151b2 facing the space 150a of the other end 151b of the first porous body (gas inlet portion) 151. Therefore, the flow rate (diffusion rate) per unit time of the measurement target gas (detection target gas) moving inside the first porous body (gas inlet portion) 151 is prevented from being affected by the buffer layer 300 and reduced.

[0072] In this embodiment, as shown in FIG. 6, the second ceramic structure 100B includes a plate-shaped main body 400 including an Ip1 cell (pump cell) 110, an alumina insulating layer 119, and the like, and an adhesive layer 193 made of a dense ceramic layer, which is disposed between the plate-shaped main body 400 and the third ceramic structure 100C. The second ceramic structure 100B further includes a reinforcing layer 192 disposed between the plate-shaped main body 400 and the adhesive layer 193 and shaped to surround the space 150a when viewed from the stacking direction (see FIG. 4). The adhesive layer 193 is generally layered (plate-shaped). An opening 193a is formed in the adhesive layer 193, penetrating the thickness direction, at a location overlapping the first measurement chamber 150 (main space 150a) in a plan view.

[0073] 6, an inner peripheral edge 192a of the reinforcing layer 192 is located outside an end face 151b2 of the first porous body (gas inlet portion) 151 and contacts an outer edge 150b1 of the gap 150b. The inner peripheral edge 192a of the reinforcing layer 192 is not in direct contact with the buffer layer 300. The reinforcing layer 192 is laminated on the third ceramic structure 100C via an adhesive layer 193. The adhesive layer 193 is made of, for example, dense ceramic (for example, alumina). The reinforcing layer 192 is made of, for example, ceramic containing zirconia as a main component.

[0074] 4, the third ceramic structure 100C of this embodiment is provided with a reinforcing layer 182 disposed between the frame-shaped body 200 and the insulating layer 121s of the first ceramic structure 100A and shaped to surround the space 150a when viewed from the stacking direction. The reinforcing layer 182 is provided with a notch 182a so as not to directly contact the first porous body (gas inlet portion) 151 of the frame-shaped body 200. The reinforcing layer 182 is made of a ceramic containing zirconia as a main component, for example, like the reinforcing layer 192.

[0075] As long as the object of the present invention is not impaired, the reinforcing layer 192 and the reinforcing layer 182 may be made of the same material as the buffer layer 300 described above.

[0076] Here, the NO x A method for detecting the concentration will be briefly described below. The solid electrolyte bodies 111e, 121e, and 131e of the gas sensor element 10 are heated and activated as the temperature of the heater pattern 164 increases. This causes the Ip1 cell 110, the Vs cell 120, and the Ip2 cell 130 to operate.

[0077] The exhaust gas flowing through an exhaust passage (not shown) in the exhaust pipe is introduced into the first measurement chamber 150 while the flow rate is restricted by the first porous body 151. At this time, a weak current (microcurrent) Icp is flowing from the Vs+ electrode 123 side to the Vs- electrode 122 side in the Vs cell 120. Therefore, oxygen in the exhaust gas can receive electrons from the Vs- electrode 122 in the first measurement chamber 150, which is the negative electrode side, and becomes oxygen ions, flows through the solid electrolyte body 121e, and moves into the reference oxygen chamber 170. In other words, the current Icp is flowed between the Vs- electrode 122 and the Vs+ electrode 123, so that oxygen in the first measurement chamber 150 is sent into the reference oxygen chamber 170.

[0078] When the oxygen concentration of the exhaust gas introduced into the first measuring chamber 150 is lower than a predetermined value, a current Ip1 is passed through the Ip1 cell 110 so that the Ip1+ electrode 112 becomes the negative electrode, and oxygen is pumped into the first measuring chamber 150 from outside the gas sensor element 10.

[0079] In contrast, when the oxygen concentration of the exhaust gas introduced into the first measuring chamber 150 is higher than the predetermined value, a current Ip1 is passed through the Ip1 cell 110 so that the Ip1-electrode 113 side becomes the negative electrode, and oxygen is pumped from inside the first measuring chamber 150 to the outside of the gas sensor element 10.

[0080] In this manner, the exhaust gas whose oxygen concentration has been adjusted in the first measurement chamber 150 is introduced into the second measurement chamber 160 through the second porous body 152. NO in the exhaust gas that has come into contact with the Ip2-electrode 133 in the second measurement chamber 160 x When a voltage Vp2 is applied between the Ip2+ electrode 132 and the Ip2- electrode 133, the NO is decomposed (reduced) on the Ip2- electrode 133, and the decomposed oxygen becomes oxygen ions, flows through the solid electrolyte body 131e, and moves into the reference oxygen chamber 170. At this time, the residual oxygen left behind in the first measurement chamber 150 is also moved by the Ip2 cell 130 into the reference oxygen chamber 170. As a result, the Ip2 cell 130 detects NO xA current derived from the oxygen and a current derived from the residual oxygen flow through the reference oxygen chamber 170. The oxygen that has moved into the reference oxygen chamber 170 is released to the outside (atmosphere) through the Vs+ electrode 123 and the Vs+ lead, and the Ip2+ electrode 132 and the Ip2+ lead, which are in contact with the inside of the reference oxygen chamber 170. For this reason, the Vs+ lead and the Ip2+ lead are porous.

[0081] Since the concentration of the residual oxygen remaining in the first measuring chamber 150 is adjusted to a predetermined value as described above, the current derived from the residual oxygen can be considered to be substantially constant. x The effect of fluctuations in the current derived from the NO x Therefore, the current Ip2 (second pump current) flowing through the Ip2 cell 130 is measured, and the NO concentration in the exhaust gas is calculated based on the current value. x The concentration is detected.

[0082] Next, a method for manufacturing the above-mentioned gas sensor element 10 will be described with reference to Fig. 7 to Fig. 11. Fig. 7 is a flow chart showing each step in the method for manufacturing the gas sensor element. As shown in Fig. 7, the method for manufacturing the gas sensor element of this embodiment includes a placement step S101, a first formation step S102, a second formation step S103, a lamination step S104, and a firing step S105.

[0083] The setting step S101 is a step of forming, on a first green sheet 121sU for forming the first ceramic structure 100A, an unsintered gas inlet portion 151U made of a material for forming the first porous body (gas inlet portion) 151, and an opening 150aU corresponding to the space 150a inside the unsintered peripheral wall portion 141U made of a material for forming the peripheral wall portion 141. Fig. 8 is a plan view showing a part of the first laminate L1 obtained in the setting step S101.

[0084] The first green sheet 121sU is for forming the insulating layer 121s of the first ceramic structure 100A. On the surface of the first green sheet 121sU, the unsintered peripheral wall portion 141U is formed by printing. The unsintered peripheral wall portion 141U is made of a part of the unsintered insulator 140U made of the material for forming the insulator 140. The unsintered peripheral wall portion 141U (unsintered insulator 140U) contains alumina as a main component.

[0085] The non-burned gas introduction section 151U contains alumina as a main component, and also contains a first burnable powder (for example, carbon powder) that is burned in the firing step S105 described below. The shape of the first burnable powder is preferably irregular, not spherical.

[0086] The green gas introduction section 151U of this embodiment is formed in advance in a peelable state on a separately prepared support sheet, and the green gas introduction section 151U on the sheet is transferred to a predetermined location of the first green sheet 121sU (a notch formed in the green insulator 140U), thereby forming the green gas introduction section 151U at the predetermined location of the first green sheet 121sU. Note that in other embodiments, the green gas introduction section 151U may be formed by printing.

[0087] In the first laminate L1, members made of various materials for forming the solid electrolyte body 121e, the Vs-electrode 122, etc. are appropriately laminated.

[0088] The first forming step S102 is a step in which the unsintered buffer layer 300U made of a material having a lower shrinkage start temperature than the unsintered gas inlet 151U is formed so as to overlap the inner end 151bU corresponding to the other end 151b arranged on the opening 150aU side of the unsintered gas inlet 151U. Fig. 9 is a plan view showing a part of the first laminate L1 in a state in which the unsintered buffer layer 300U is formed on the inner end 151bU of the unsintered gas inlet 151U in the first forming step S102.

[0089] As described above, the unsintered buffer layer 300U is made of a material having a lower shrinkage start temperature than the unsintered gas inlet 151U. Examples of such an unsintered buffer layer 300U include a layer that contains zirconia as a main component and a second burnable powder (e.g., carbon powder) that is burned in the firing step S105 described later.

[0090] In addition, it is preferable that the second burnable powder has a larger particle size than the first burnable powder. When the particle size of the second burnable powder is larger than that of the first burnable powder, the unsintered buffer layer 300U can be easily adjusted to have a lower shrinkage start temperature than the unsintered gas inlet 151U, and the decrease in the gas flow rate (diffusion rate) in the first porous body (gas inlet) 151 of the finally obtained buffer layer 300 is suppressed.

[0091] In addition, the content of the second burnable powder in the unsintered buffer layer 300U is preferably lower than the content of the first burnable powder in the unsintered gas inlet 151U. When the content of the second burnable powder in the unsintered buffer layer 300U is thus low, the unsintered buffer layer 300U can be easily adjusted to have a lower shrinkage start temperature than the unsintered gas inlet 151U, and the decrease in the gas flow rate (diffusion rate) in the first porous body (gas inlet) 151 of the finally obtained buffer layer 300 is suppressed.

[0092] In addition, the second burnable powder is preferably spherical. If the second burnable powder is spherical, the buffer layer 300 finally obtained does not have a structure that easily diffuses gas, so that a decrease in the flow rate (diffusion rate) of gas in the first porous body (gas inlet portion) 151 is suppressed.

[0093] In the first formation step S102, the unsintered buffer layer 300U is formed on the inner end 151bU so as not to cover the end face 151b2U facing the opening 150aU of the inner end 151bU. Therefore, the finally obtained buffer layer 300 is prevented from decreasing the flow rate (diffusion rate) of the gas in the first porous body (gas inlet portion) 151.

[0094] As shown in Fig. 9, the unsintered buffer layer 300U has an elongated shape in the front-rear direction (longitudinal direction) of the gas sensor element 10. The unsintered buffer layer 300U is formed by printing using a printing device. Taking into consideration printing misalignment and the like, an end 300Ua on the front side (upper side in Fig. 9) of the unsintered buffer layer 300U is formed on the unsintered peripheral wall portion 141U disposed in front of the unsintered gas inlet portion 151U. An end 300Ub on the rear side (lower side in Fig. 9) of the unsintered buffer layer 300U is formed on the unsintered peripheral wall portion 141U disposed in rear of the unsintered gas inlet portion 151U.

[0095] The second formation process S103 is a process in which a burnt portion 500U made of a paste material (e.g., carbon paste) containing a burnt material (e.g., carbon powder) is printed to fill the opening 150aU on the first green sheet 121sU and overlap the unsintered buffer layer 300U with the end portion 501U protruding toward the unsintered gas inlet portion 151U outside the opening 150aU.

[0096] FIG. 10 is a plan view showing a part of the first laminate L1 in a state where the burnt portion 500U is formed in the second forming step S104 so that the end portion 501U overlaps the unsintered buffer layer 300U.

[0097] The burnt portion 500U is made of a paste material (e.g., carbon paste) containing a burnt material (e.g., carbon powder). That is, a known paste material generally used for forming an opening is used as the burnt portion 500U. Note that the burnt portion 500U is filled into the opening 150aU so that its end (periphery) protrudes from the opening 150a, taking into account printing misalignment and the like.

[0098] The burnt portion 500U has a lower shrinkage start temperature than the unsintered buffer layer 300U and the unsintered gas inlet portion 151U, and therefore, among them, shrinkage starts earliest in the firing step S105 described later. The end portion 501U of the burnt portion 500U is the part most susceptible to the influence of shrinkage. If the end portion 501U of the burnt portion 500U is formed so as to directly overlap the unsintered gas inlet portion 151U, the difference between the shrinkage start temperature of the burnt portion 500U and the shrinkage start temperature of the unsintered gas inlet portion 151U is too large, so that when the burnt portion 500U shrinks, the end portion 501U pulls the unsintered gas inlet portion 151U, and there is a risk of defects such as cracks occurring in the unsintered gas inlet portion 151U.

[0099] In this embodiment, in order to prevent the above-mentioned defects from occurring in the unsintered gas inlet 151U, the end 501U of the burnt portion 500U is formed so as to be in direct contact with the unsintered buffer layer 300U formed to be overlaid on the unsintered gas inlet 151U, rather than with the unsintered gas inlet 151U. Since the shrinkage start temperature of the unsintered buffer layer 300U is lower than that of the unsintered gas inlet 151U, when the end 501U of the burnt portion 500U shrinks, the unsintered buffer layer 300U that is in direct contact with the end 501U can follow the movement of the shrinking end 501U faster than the unsintered gas inlet 151U.

[0100] Even if the green buffer layer 300U is formed on the green gas inlet portion 151U, normally, the green buffer layer 300U does not cause defects in the green gas inlet portion 151U due to shrinkage of the green buffer layer 300U.

[0101] 10, even if the part of the burnt-out section 500U closer to the center than the end 501U comes into direct contact with the non-burnt gas inlet 151U, that part (the part on the center side) usually does not affect the non-burnt gas inlet 151U when the burnt-out section 500U contracts. Therefore, in order to achieve the object of the present invention, the part of the burnt-out section 500U other than the end 501U may come into direct contact with the non-burnt gas inlet 151U.

[0102] The lamination step S104 is a step in which the first green sheet 121sU on which the burnt portion 500U is formed and the second green sheet 111sU for forming the second ceramic structure 100B are laminated together.

[0103] In this lamination step S104, the first laminate L1 including the first green sheet 121sU on which the burnt portion 500U is formed and the second laminate L2 including the second green sheet 111sU for forming the second ceramic structure 100B are laminated together. The second green sheet 111sU is a sheet for forming the insulating layer 111s of the second ceramic structure 100B. The first laminate L1, the second laminate L2, and the like are laminated to obtain an unfired laminate L for forming the gas sensor element 10. FIG. 11 is a cross-sectional view that shows a schematic configuration of the unfired laminate L for forming the gas sensor element 10. FIG. 11 shows the laminate L at a portion corresponding to the cross-sectional configuration of the gas sensor element 10 shown in FIG.

[0104] As shown in FIG. 11, the first laminate L1 includes a first green sheet 121sU, an unsintered gas inlet portion 151U, an unsintered buffer layer 300U, a burned portion 500U, and the like.

[0105] The second laminate L2 includes the second green sheet 111sU, the unfired alumina insulating layer 119U for forming the alumina insulating layer 119, the unfired reinforcing layer 192U for forming the reinforcing layer 192, the unfired adhesive layer 193U for forming the adhesive layer 193, and the burnt portion 600U used together with the burnt portion 500U for forming the opening 150aU. The burnt portion 600U is made of the same composition as the burnt portion 500U described above, and is filled in the opening 150aU by being overlapped on the burnt portion 500U. The burnt portion 600U is formed at a predetermined position of the second green sheet 111sU by using printing. The burnt portion 600U has approximately the same size as the burnt portion 500U in a plan view.

[0106] The unsintered buffer layer 300U is formed on the surface 151b1U of the inner end 151bU. This surface 151b1U will eventually become the opposing surface 151b1. As shown in Fig. 11, the unsintered buffer layer 300U is formed on the surface 151b1U of the inner end 151bU so as not to cover the end surface 151b2U facing the opening 150aU of the inner end 151bU.

[0107] In the lamination step S104, furthermore, unfired sheets or the like necessary for manufacturing the gas sensor element 10 are appropriately laminated on the first laminate L1, the second laminate L2, or the like.

[0108] The firing step S105 is a step of firing the laminate L obtained after the lamination step S104. In the firing step S105, the laminate L is fired under a predetermined temperature condition to obtain the gas sensor element 10. When the laminate L is fired, the burnt portions 500U, 600U disappear, and a space (main space) 150a used as the first measurement chamber 150 and a gap 150b connected to the space 150a are formed. [Explanation of symbols]

[0109] Reference Signs List 1...gas sensor, 10...gas sensor element, 100A...first ceramic structure, 100B...second ceramic structure, 100C...third ceramic structure, 110...pump cell, 111e...second solid electrolyte body, 112, 113...pump electrodes, 120...detection cell, 121e...first solid electrolyte body, 122, 123...detection electrodes, 141...peripheral wall portion, 150a...space (main space), 150b...gap, 150b1...outer edge of gap, 151b1...opposing surface, 200...frame-shaped body, 300...buffer layer

Claims

1. A gas sensor element in which a plurality of plate-shaped ceramic structures are laminated, a first ceramic structure having a detection cell including a first solid electrolyte body and a pair of detection electrodes provided on both sides of the first solid electrolyte body; a second ceramic structure including a pump cell including a second solid electrolyte body and a pair of pump electrodes provided on both sides of the second solid electrolyte body, the second ceramic structure being disposed in a stacking direction while maintaining a gap with respect to the first ceramic structure; a layered structure having a frame-shaped body disposed between the first ceramic structure and the second ceramic structure and surrounding a space formed between the first ceramic structure and the second ceramic structure, the frame-shaped body having one end disposed on an exterior side and the other end disposed on the space side, the frame body comprising: a gas inlet portion made of porous ceramic for introducing an external detection target gas into the space while passing the external detection target gas from the one end side to the other end side; and a peripheral wall portion made of dense ceramic and surrounding the space together with the gas inlet portion; a gap communicating with the space is formed between a surface of the other end of the gas inlet portion facing the second ceramic structure and the second ceramic structure, a gas sensor element made of a ceramic material having a lower shrinkage start temperature than a material for forming the gas introduction portion, the gas sensor element including a buffer layer formed on the opposing surface so as to overlap with the boundary between the outer edge of the gap and the second ceramic structure when viewed from the stacking direction.

2. 2. The gas sensor element according to claim 1, wherein the buffer layer is made of a porous ceramic containing pores larger than pores contained in the gas inlet portion.

3. 3. The gas sensor element according to claim 1, wherein the buffer layer is formed on the opposing surface so as not to cover an end face of the other end of the gas inlet portion that faces the space.

4. The second ceramic structure is A plate-shaped main body including the pump cell; an adhesive layer formed of a dense ceramic layer and disposed between the plate-shaped main body and the third ceramic structure; 4. The gas sensor element according to claim 1, further comprising a reinforcing layer disposed between the plate-shaped main body portion and the adhesive layer and shaped to surround the space when viewed from the stacking direction.

5. The material for forming the buffer layer contains zirconia as a main component, 5. The gas sensor element according to claim 1, wherein a material for forming the gas inlet portion contains alumina as a main component.

6. A gas sensor comprising the gas sensor element according to any one of claims 1 to 5.

7. a first ceramic structure having a detection cell including a first solid electrolyte body and a pair of detection electrodes provided on both sides of the first solid electrolyte body; a second ceramic structure having a pump cell including a second solid electrolyte body and a pair of pump electrodes provided on both sides of the second solid electrolyte body and disposed in a stacking direction while maintaining a gap with respect to the first ceramic structure; and a third ceramic structure having a layered structure having a frame-shaped body disposed between the first ceramic structure and the second ceramic structure and surrounding a space formed between the first ceramic structure and the second ceramic structure, the frame-shaped body having one end disposed on an exterior side and the other end disposed on the space side, the frame-shaped body including a gas inlet portion made of porous ceramic that introduces an external detection target gas into the space while passing the gas from the one end side to the other end side, and a peripheral wall portion made of dense ceramic and surrounding the space together with the gas inlet portion, an installation step in which an unsintered gas inlet portion made of a material for forming the gas inlet portion and an unsintered peripheral wall portion made of a material for forming the peripheral wall portion are installed on a first green sheet for forming the first ceramic structure, and openings corresponding to the space are formed on the inside of the unsintered gas inlet portion and the unsintered peripheral wall portion; a first forming step in which an unsintered buffer layer made of a material having a lower shrinkage start temperature than the unsintered gas inlet is formed so as to overlap an inner end portion corresponding to the other end portion arranged on the opening side of the unsintered gas inlet; a second forming step of forming a burnt-out portion made of a paste material containing a burnt-out material by printing so as to fill the opening on the first green sheet and overlap the unsintered buffer layer while an end of the burnt-out portion protrudes toward the unsintered gas inlet portion located outside the opening; a lamination step of laminating the first green sheet having the burnt portion formed therein and a second green sheet for forming the second ceramic structure on each other; and a firing step of firing the laminate obtained after the lamination step.

8. The unfired gas inlet contains a first burnable powder that is burned in the firing step, 8. The method for manufacturing a gas sensor element according to claim 7, wherein the unsintered buffer layer contains a second burnable powder that is burned in the firing step and has a particle size larger than that of the first burnable powder.

9. 9. The method for manufacturing a gas sensor element according to claim 8, wherein a content of said second burnable powder in said unsintered buffer layer is lower than a content of said first burnable powder in said unsintered gas inlet portion.

10. 10. The method for manufacturing a gas sensor element according to claim 8, wherein the second burnable powder has a spherical shape, and the first burnable powder has an irregular shape.

11. The unsintered buffer layer contains zirconia as a main component, 11. The method for manufacturing a gas sensor element according to claim 7, wherein the unsintered gas inlet portion contains alumina as a main component.

12. 12. The method for manufacturing a gas sensor element according to claim 7, wherein in the first formation step, the unsintered buffer layer is formed on the inner end portion so as not to cover an end face of the inner end portion facing the opening portion.

Citation Information

Patent Citations

  • Manufacture of oxygen sensor

    JP1996114571A

  • Sensor substrate and gas sensor element equipped therewith

    JP2003156468A

  • Stacked gas sensor element, its manufacturing method, and gas sensor

    JP2003294690A

  • Method for manufacturing ceramic laminate

    JP2010286473A

  • Method for manufacturing ceramic laminated body and ceramic laminated body obtained thereby

    JP2011219310A