Interference-resistant solid-state reference electrode
By integrating a solid ion exchange material to immobilize interfering ions, the reference electrode maintains stable potentials and withstands challenging analyte conditions, addressing interference and miniaturization issues in conventional electrodes.
Patent Information
- Application Number
- JP2022526134
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-08
- Filing Date
- 2020-11-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-11-06
AI Technical Summary
Conventional solid state reference electrodes are susceptible to interference from ionic species in the analyte, leading to unstable reference potentials due to competitive redox reactions, and are difficult to miniaturize and maintain.
Incorporation of a solid ion exchange material containing non-interfering ions between the electrode surface and the reference element, which immobilizes interfering ions through ion exchange, maintaining a stable reference potential.
The solution effectively reduces the impact of interfering ions on the reference potential, providing long-term stability and resistance to degradation, allowing for miniaturization and improved performance in challenging analyte environments.
Smart Images

Figure 0007595661000004 
Figure 0007595661000005 
Figure 0007595661000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid reference electrode. In particular, the electrode comprises a reference element in ionic communication with a polymer composite loaded with an inorganic salt containing a reference anion, and a solid ion exchange material located between the electrode surface and the reference element. In use, the solid ion exchange material immobilizes interfering ions present in an analyte by exchange with non-interfering ions present in the material. The present invention also relates to a system for electrochemical analysis of an analyte comprising the solid reference electrode, and a method for electrochemical analysis of an analyte using the solid reference electrode. [Background technology]
[0002] Electroanalytical techniques such as potentiometry and voltammetry rely on both an indicator and a reference electrode, the performance of which are equally important to the accuracy of the measurement. It is therefore important that the reference electrode provides a stable and reproducible potential that is substantially independent of the concentration of species in the analyte, including the analyte of interest.
[0003] To provide a constant reference potential, reference electrodes traditionally contain a reference element immersed in a bath of liquid or gel electrolyte of known salt concentration contained within a casing. Silver / silver chloride (Ag / AgCl) and calomel (Hg / Hg2Cl2) reference electrodes in potassium chloride (KCl) electrolyte are common. Although the electrolyte is effectively isolated from the analyte by the casing, a liquid junction (salt bridge) is required between the analyte and the internal electrolyte to allow ion exchange and complete the electrochemical cell. This liquid junction usually consists of a small opening or porous plug in the casing.
[0004] Although traditional reference electrodes are suitable for many applications, they also have significant drawbacks. For example, electrolyte can leak from the liquid junction, contaminating the analyte with the reference electrolyte salt, and analyte can migrate into the internal electrolyte solution, affecting the electrolyte salt concentration and introducing foreign species that can interfere with the reference half-cell reaction. While the junction or electrolyte can be engineered to mitigate these concerns, there is essentially a trade-off between minimizing liquid contact between the electrolyte and the analyte and maintaining an acceptable junction potential that can cause errors in the analytical measurement. Furthermore, traditional electrodes are difficult to miniaturize due to the electrolyte volume and complex structure, and are typically position-dependent, fragile, expensive, and require maintenance.
[0005] Many previous efforts have been made to address one or more of these challenges using solid reference electrodes that do not have a liquid electrolyte reservoir and a corresponding liquid-liquid junction. Vonau et al., DE10305005, describe a sintered Ag / AgCl reference element embedded in a solidified melt of KCl. The KCl is encapsulated within a ceramic layer and an outer casing, with small openings in the casing exposing the ceramic, forming a junction to regulate ionic communication and limit KCl dissolution into the analyte. These electrodes rely on a porous junction between the internal salt and the analyte, resulting in fragile and complex structures.
[0006] One promising approach is to embed the reference element in a composite in the form of a water-permeable polymer matrix loaded with an inorganic salt constituting the reference anion. When immersed in an aqueous analyte, the complex is hydrated until a saturating concentration of the reference anion is supplied to the reference element. Thus, for example, Vonau et al., DE19533059, report a reference electrode comprising an Ag / AgCl reference element embedded in a polyester resin composite loaded with KCl. Mousavi et al., Analyst 2013(138)5216 and Journal of Solid State Electrochemistry 2014(18)607, prepared a reference electrode comprising an Ag / AgCl reference element embedded in a polyvinyl acetate (PVAc) homopolymer loaded with particulate KCl. If properly designed, the polymer matrix prevents rapid leaching of the salt while at the same time allowing sufficient ionic conduction between the reference element and the analyte.
[0007] However, in many applications, the analyte contains components that degrade the composite or interfere with the long-term stability of the measured reference potential. For example, highly acidic or abrasive analytes can degrade polymer composite electrodes to the extent that dimensional stability is lost and inorganic salts are leached out. In Applicant's co-filed PCT application published as WO2018 / 201200, this was addressed by using a composite with a cross-linked vinyl polymer matrix.
[0008] However, solid reference electrodes containing polymer composites loaded with reference salts remain susceptible to interference from soluble ionic species that can participate in competing redox reactions in the reference element. These undesirable reactions cause drift away from the expected electrode potential. In particular, anionic species such as sulfide, bromide, iodide, and cyanide can interfere with reference electrodes that have chloride or sulfate as the reference anion.
[0009] Thus, there is a continuing need to provide a solid-state reference electrode that at least partially addresses one or more of the above-mentioned shortcomings or provides a useful alternative.
[0010] Any reference in this specification to a patent document or other matter indicated as prior art should not be construed as an admission that the document or matter was known at the priority date of any of the claims or that the information it contains was part of the general public knowledge. Summary of the Invention
[0011] The inventors have found that a polymer composite reference electrode having increased resistance to redox interference by ionic species present in the analyte can be obtained by incorporating a solid ion exchange material having exchangeable non-interfering ions. During use, the solid ion exchange material blocks one or more interfering ions that diffuse from the analyte to the electrode, thereby reducing the probability of undesired redox reactions in the reference element. The ion exchange reaction immobilizes the interfering ions and releases the non-interfering ions that do not substantially affect the measured reference potential.
[0012] According to a first aspect, the present invention provides a solid reference electrode comprising: a reference element in ionic communication with a composite comprising a water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion; an electrode surface for contacting an analyte; and a solid ion exchange material located between the electrode surface and the reference element, the solid ion exchange material comprising one or more non-interfering ions, such that in use, when interfering ions are present in a solution of the analyte, the solid ion exchange material immobilizes the one or more interfering ions by exchange with the non-interfering ions.
[0013] In some embodiments, the solid ion exchange material comprises a metal salt or an ion exchange resin. In some embodiments, the solid ion exchange material comprises a metal salt that has a lower water solubility than a solid inorganic salt.
[0014] In some embodiments, one or more of the non-interfering ions are non-interfering anions and one or more of the interfering ions are interfering anions. The non-interfering anions may constitute the reference anions. In some embodiments, the solid ion exchange material comprises a metal salt comprising a cation selected from the group consisting of silver, mercury, and lead. In some embodiments, the solid ion exchange material comprises a metal salt comprising a metal present in the reference element. In some embodiments, the interfering anion is selected from the group consisting of sulfide, iodide, bromide, and cyanide. In some embodiments, the interfering anion comprises sulfide.
[0015] In some embodiments, the solid ion exchange material is a particulate material.
[0016] In some embodiments, the solid ion exchange material is loaded into the polymer matrix of the composite, or into a further polymer composite located between the electrode surface and the reference element, the further polymer composite comprising a solid anion exchange material dispersed in a hydratable polymer.
[0017] In some embodiments, the solid ion exchange material is loaded into the polymer matrix of the composite. The solid ion exchange material may be present in an amount of at least 1% by weight of the composite, such as at least 3% by weight.
[0018] In some embodiments, the solid ion exchange material is packed into a water-permeable layer of an additional polymer composite located between the electrode surface and the composite.
[0019] In some embodiments, the reference anion is a chloride ion, hi some embodiments, the reference element is selected from the group consisting of Ag / AgCl and calomel.
[0020] In some embodiments, the water-permeable polymer group comprises a vinyl polymer of a vinyl monomer containing a heteroatom. The vinyl polymer may be crosslinked. The crosslinked vinyl polymer may be a copolymer of i) at least one vinyl monomer selected from the group consisting of vinyl esters, vinyl amides, and acrylates, and ii) at least two crosslinkers containing copolymerizable vinyl functional groups. If a hydratable polymer is present, it may also be a vinyl polymer of a vinyl monomer containing a heteroatom.
[0021] In some embodiments, the complex comprises at least 30% by weight of a solid inorganic salt.
[0022] According to a second aspect, the present invention provides a system for the electrochemical analysis of an analyte, the system comprising a solid reference electrode according to any embodiment of the first aspect; a second electrode selected from an ion selective electrode and a working electrode; and means for measuring the potential difference between the second electrode and the reference electrode.
[0023] According to a third aspect, the present invention provides a method for the electrochemical analysis of an analyte, the method comprising contacting the analyte with i) a solid reference electrode according to any embodiment of the first aspect and ii) a second electrode selected from an ion selective electrode and a working electrode; and measuring the difference in electrochemical potential between the second electrode and the reference electrode.
[0024] In some embodiments, the analyte comprises one or more interfering ions in solution. In some such embodiments, the interfering ions are interfering anions. The interfering anions may be selected from the group consisting of sulfide, iodide, bromide, and cyanide. In some embodiments, the interfering anion comprises sulfide.
[0025] When the terms "comprise", "comprises" and "comprising" are used in this specification (including the claims), they are to be interpreted as specifying stated features, integers, steps or components, but not as excluding the presence of one or more other features, integers, steps or components, or groups thereof.
[0026] As used herein, the terms "first," "second," "third," etc., in connection with various features of the disclosed devices are assigned arbitrarily and are intended merely to distinguish between two or more such features that the devices may incorporate in various embodiments. The terms do not, in themselves, indicate a particular orientation or order. Moreover, it will be understood that the presence of a "first" feature does not imply the presence of a "second" feature, the presence of a "second" feature does not imply the presence of a "first" feature, etc.
[0027] Further aspects of the invention appear below in the detailed description of the invention. [Brief description of the drawings]
[0028] Embodiments of the present invention are herein described, by way of example only, with reference to the accompanying drawings.
[0029] FIG. 1 shows a schematic diagram of a solid reference electrode according to one embodiment of the present invention, in which a solid ion exchange material is dispersed in a composite.
[0030] FIG. 2 shows a schematic diagram of a printed solid reference electrode according to another embodiment of the present invention, in which a solid ion exchange material is dispersed in a printed composite layer.
[0031] FIG. 3 is a schematic diagram of a solid reference electrode according to another embodiment of the invention, in which the solid ion exchange material is in a water-permeable layer located between the electrode surface and the composite.
[0032] FIG. 4 is a plot of the potential response of an electrode containing AgCl as a solid ion exchange material and a reference electrode lacking a solid ion exchange material when exposed to an analyte containing sulfide anion for 140 days as measured in Example 2.
[0033] FIG. 5 is a plot of the potential response of an electrode containing chloride-loaded ion exchange resin particles as the solid ion exchange material and a reference electrode without a solid ion exchange material when exposed to an analyte containing sulfide anions, as measured in Example 3.
[0034] FIG. 6 is a plot of the potential response of an electrode containing AgCl as a solid ion exchange material and a reference electrode lacking a solid ion exchange material when exposed to a strongly acidic analyte containing sulfide anion, as measured in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] solid reference electrode The present invention relates to a solid reference electrode. The electrode comprises a reference element in ionic communication with a complex. The complex comprises a water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion. The electrode has an electrode surface for contacting an analyte, and a solid ion exchange material is disposed between the electrode surface and the reference element. The solid ion exchange material comprises one or more non-interfering ions. In use, when interfering ions are present in a solution of the analyte, the solid ion exchange material immobilizes the one or more interfering ions by exchanging them for the non-interfering ions.
[0036] Reference Element A solid reference electrode comprises a reference element, which as used herein is a conductive body that contains or develops in situ a redox couple that can provide a reference potential when exposed to a reference electrolyte in use.
[0037] The reference element may be any suitable reference element capable of providing a stable potential when contacted with a reference electrolyte having a constant concentration of a reference anion. Such reference elements include those having silver chloride (Ag / AgCl), calomel (Hg / Hg2Cl2), silver sulfate (Ag / Ag2SO4), and mercury sulfate (Hg / Hg2SO4) redox couples. In some embodiments, the reference element is an Ag / AgCl or calomel reference element that provides a reference potential when exposed to a reference electrolyte containing a stable chloride concentration. Ag / AgCl reference elements are particularly preferred, at least in part, for environmental and safety reasons.
[0038] Ag / AgCl reference elements may include silver wires or other silver metal bodies that are typically coated with silver chloride by electrochemical or chemical oxidation. In some embodiments, the reference element includes a meshed or braided metal structure to improve the surface area in contact with the composite. Ag / AgCl reference elements can also be made by a variety of other methods, such as sintering a mixture of Ag and AgCl powders. Printed Ag / AgCl reference elements can be obtained by printing a layer of silver on a substrate and chemically oxidizing the layer with a chlorinating agent such as hypochlorite. Alternatively, an ink containing both Ag and AgCl particles in a carrier can be used.
[0039] In use, the reference element is electrically connected to other electrodes through an external circuit. As such, the reference element is typically provided with a suitable electrical termination for connection to the circuit. For example, in the case of a silver wire reference electrode, the electrical termination may be the bare end of the wire.
[0040] The reference potential relative to the sensing electrode is measured by electrical conduction through the conductive body of the reference electrode. Because reference electrodes are configured for potentiometric, voltammetric, and amperometric electrochemical analysis, the potential of the reference element must be measured without significant impedance between the active redox couple on the reference element and the potentiometer. Thus, electrodes are generally configured for low impedance measurement of the reference potential, with the electrode's overall impedance being primarily due to limitations in ionic conductance between the reference element and the analyte, as opposed to limitations in electrical conductance through the reference element. Notably, the electrode does not include a resistor coupled to the reference element at which the reference potential is measured. It will also be appreciated that electrodes are generally configured to provide a single reference potential for the measurement, as opposed to electrodes that determine a reference potential by combining ion-sensitive potentials established at two different electrode sections separated by a resistor.
[0041] Complex The reference element is in ionic communication with the complex. The role of the complex is to provide a substantially stable solution concentration of the reference anion at the reference element when the electrode is in contact with an aqueous analyte and hydrated, while allowing sufficient ionic conductivity between the reference element and the analyte. The reference element will preferably be in ionic communication with the complex when in contact with or in close proximity to the electrolyte, provided that these criteria are met in use. In some embodiments, the reference element is in direct contact with the complex. In some embodiments, the complex is at least partially disposed between the electrode surface and the reference element.
[0042] The complex comprises a water-permeable polymer matrix loaded with a solid inorganic salt containing the reference anion. Thus, the complex is generally a solid material without an internal liquid electrolyte reservoir. However, it is necessary that the complex is sufficiently permeable to water to allow hydration of the complex during use and provide a satisfactory ionic conductivity between the reference element and the analyte. Furthermore, it is preferable that the inorganic salt has a low elution rate into the analyte. In some applications, it is also preferable that the complex is not easily degraded by highly acidic or abrasive analytes.
[0043] The composite is preferably dimensionally stable in the intended aqueous analyte for the required life of the device (one week or more, or one month or more). Dimensional stability is an important mechanical requirement in many applications. Thus, in some embodiments, the composite does not undergo significant swelling when immersed in an aqueous analyte, which would result in leaching of solid inorganic salts. Any swelling may be less than about 10% of the initial volume.
[0044] The composite can define the physical body of the solid reference electrode. In some embodiments, however, the reference electrode constitutes a casing around the composite. The casing may be made of an insulating and durable material suitable for the envisaged application, such as poly(methyl methacrylate). If used, the casing will generally include a window for exposing the composite to the analyte, which can be exposed directly or through an intermediate water-permeable layer as described below.
[0045] The polymer matrix of the complex is loaded with a solid inorganic salt constituting the reference anion. The inorganic salt is sufficiently soluble in water that the hydration of the complex results in a constant saturated solution concentration of the reference anion in the reference element. The solid inorganic salt may be dispersed in the polymer matrix, typically as a particulate solid. The solid inorganic salt is typically dispersed throughout the polymer matrix, although it is not excluded that a non-uniform distribution of the inorganic salt exists in the complex. In some embodiments, the distribution of the inorganic salt is due to gravimetric settling of particulate salt in the monomer mixture prior to polymerization.
[0046] High loading of solid inorganic salt is considered to be beneficial because it can extend the life of the reference electrode. In some embodiments, the composite comprises at least 10% by weight of solid inorganic salt, preferably at least 30% by weight, more preferably at least 50% by weight of solid inorganic salt. However, the loading should not be so high that the physical integrity of the composite is compromised. A suitable loading can be achieved by gravimetrically precipitating the inorganic salt in the form of a particulate solid (i.e., powder) into the monomer mixture before polymerization.
[0047] TIFF0007595661000001.tif22108 The solid inorganic salt comprises a reference anion. As used herein, a reference anion is an anion that participates in the desired redox half-reaction in the reference element. For example, Ag / AgCl reference electrode and Ag / Ag2SO4 reference electrode require chloride and sulfate reference anions, respectively. In use, the reference anion needs to be provided in a constant solution concentration in the complex to obtain a constant reference potential. This is evident, for example, from the fact that the half-life potential of an Ag / AgCl reference electrode is given by the applicable Nernst equation (1): where E is the half-cell reduction potential, E 0 is the standard half-cell reduction potential, R is the universal gas constant, T is temperature, a Cl - is the activity of chloride ions (correlated with their concentration).
[0048] In some embodiments, the solid inorganic salt is a sulfate salt, such as potassium sulfate for an Ag / Ag2SO4 reference electrode. In other embodiments, the solid inorganic salt is a chloride salt, such as potassium chloride (KCl), sodium chloride (NaCl), or lithium chloride (LiCl), preferably KCl. A chloride reference anion is required when the reference electrode is, for example, an Ag / AgCl or calomel electrode.
[0049] In some embodiments, the inorganic salt consists of an inorganic cation and an inorganic anion, i.e., it lacks ligands or other organic components. The inorganic salt is not covalently bound to the polymer matrix of the composite, since the polymer matrix and the inorganic salt are chemically distinct components of the composite. In contrast, an ionic polymer charge-balanced with a reference ion is not an inorganic salt-loaded composite, and by itself provides an insufficient amount of readily soluble reference ion to establish a long-term, constant saturated solution concentration in the reference element.
[0050] The inorganic salt may be a particulate solid. In some embodiments, the particulate solid has an average particle size of less than 1 mm, preferably less than 500 microns. The particles may be large enough to form a well-dispersed distribution throughout the polymer matrix.
[0051] The complex comprises a water-permeable polymer matrix loaded with an inorganic salt containing a reference anion, and in some embodiments also a solid ion exchange material. As used herein, the polymer matrix is the polymer phase of the complex in which the inorganic salt is loaded. In at least some embodiments, the complex comprises the polymer matrix as a continuous phase and the inorganic salt as a discontinuous phase. Thus, it is preferred that the polymer of the polymer matrix has an appropriate hydrophobic-hydrophilic balance. The water permeability should be sufficient to allow hydration of the complex and provide ionic conduction through the polymer matrix between the reference element and the analyte. Thus, the impedance of the electrode is acceptably low and the electrode can achieve a stable potential (i.e., become conditioned) in an acceptable time when placed in the analyte. However, it is also preferred that the complex is not too hydrophilic, as this may result in substantial swelling of the polymer, loss of physical integrity of the electrode body, and / or rapid leaching of the inorganic salt and / or solid ion exchange material into the analyte. The polymer matrix is generally electrically insulating, and in particular is not composed of an inherently conductive polymer (such as polypyrrole). The reference substance and the ion exchange material are therefore electrically isolated from each other in use.
[0052] The type of polymer is not considered to be limited, so long as the polymer substrate is adequately water permeable in view of the above considerations. Thus, the polymer may be a vinyl polymer, an epoxy resin, a polyester resin, a polysiloxane, a polyurethane, a polysaccharide, in some embodiments. Specific examples of suitable polymers include propoxylate diglycidyl ether, methyl methacylate glycidyl-methacrylate tetrahydrofurfuryl acrylate copolymer, cellulose acetate, ethyl cellulose, and cellulose, etc., as disclosed in WO2012074356A1; silicone rubber, polyvinyl chloride, polystyrene, polyhydroxyethyl-methacrylate, polyvinylidene chloride, and polyurethane, as disclosed in WO1996035116A1; cellulose acetate, cellulose acetate butyrate, cellulose triacetate, nitrocellulose, and combinations thereof, as disclosed in US6793789B2; and vinyl fluoride polymers, as disclosed in US4908117A. These may include hexafluoropropylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, epichlorohydrin epoxy resins as disclosed in DE102010050481A1, polymers such as polymethacrylic acid, polyacrylonitrile, polybutyl acrylate as disclosed in US8486246B2, N-acrylamides as disclosed in DE10354100A1, acrylate polymers as disclosed in WO2006032284A1, polymers or copolymers of N-acryloylaminoethoxyethanol as disclosed in US7790323B2, copolymers of cationic and anionic monomers containing quaternary amines as disclosed in DE102011089707A1, and the like.
[0053] In some embodiments, the polymer matrix of the composite comprises a vinyl polymer. As used herein, a vinyl polymer is an addition polymer of one or more vinyl monomers that contain an extended alkane (...-CCCC-...) backbone chain. A wide range of vinyl polymers are believed to be suitable, although an appropriate combination of monomer(s), crosslinking groups, and degree of crosslinking in the polymer matrix may be required to provide excellent chemical resistance and mechanical stability while achieving an optimal hydrophobic-hydrophilic balance for low impedance and high electrochemical stability, as will be further described.
[0054] The vinyl polymer may be a polymer of at least one vinyl monomer containing a heteroatom, and may optionally contain two or more heteroatoms. The heteroatom or heteroatoms may be selected from oxygen and nitrogen. Such heteroatom-containing vinyl monomers may impart hydrophilicity to the polymer backbone, allowing for hydration and ionic conduction through the complex. In some embodiments, the vinyl monomer containing a heteroatom is selected from the group consisting of vinyl esters, vinyl amides, acrylates, acrylonitrile, and vinyl ethers. In some embodiments, the vinyl monomer contains a carbonyl group and may be selected from the group consisting of vinyl esters, vinyl amides, and acrylates. Suitable vinyl monomers may include vinyl acetate, vinyl caprolactam, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hexyl (meth)acrylate.
[0055] In some embodiments, the vinyl polymer comprises a vinyl monomer containing a heteroatom as the only monofunctional monomer. In other embodiments, the vinyl polymer is a copolymer of a vinyl monomer containing a heteroatom and a less polar vinyl monomer lacking a heteroatom. The monomer composition suitable for the vinyl polymer can be selected without undue burden by those skilled in the art in view of the principles disclosed herein.
[0056] In some embodiments, the vinyl polymer is a crosslinked vinyl polymer. Such a polymer can be obtained, for example, by copolymerizing a mixture containing a vinyl monomer containing a heteroatom and a copolymerizable crosslinker. Crosslinking of the vinyl polymer can, in some embodiments, increase the resistance of the electrode to degradation as a result of chemical attack, for example, under highly acidic and / or high temperature use conditions. In some embodiments, crosslinking can enhance the resistance of the electrode to mechanical degradation, for example, under abrasive use conditions.
[0057] In some embodiments, the vinyl polymer is crosslinked with a hydrophilic crosslinking group. As used herein, a hydrophilic crosslinking group is a group that imparts hydrophilicity to the polymer matrix. A hydrophilic crosslinking group is generally an organic linking group that includes one or more hydrophilic functional groups, such as carboxyl groups, ether groups, amide groups, amine groups, etc., and is preferably a carboxyl group and / or an ether group. In other embodiments, the vinyl polymer is crosslinked with a more hydrophobic crosslinking group. In this case, it will be understood that a more hydrophilic backbone may be desirable to achieve the required overall hydrophilic-hydrophobic balance.
[0058] The crosslinked vinyl polymer may be a copolymer of a vinyl monomer containing a heteroatom and a crosslinker having at least two copolymerizable vinyl functional groups, such as an acrylate or methacrylate. The crosslinker may be a hydrophilic crosslinker, such as, for example, ethylene glycol di(meth)acrylate, oligoethylene glycol di(meth)acrylate, or polyethylene glycol di(meth)acrylate. In other embodiments, the crosslinker may have hydrophobic properties, such as the aliphatic crosslinker 1,6-hexanediol di(meth)acrylate.
[0059] In some embodiments, the crosslinking agent is ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol dimethacrylate (e.g., Mn=330 to 20,000), polyethylene glycol diacrylate (e.g., Mn=250 to 20,000), N,N'-methylenebisacrylamide, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di (meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A glycerolate di(meth)acrylate, diurethane di(meth)acrylate, divinylbenzene, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerol propoxylate triacrylate (e.g., Mn=428), trimethylolpropane estoxylate triacrylate, and trimethylolpropane propoxylate triacrylate. As used herein, "(meth)acrylate" refers to either acrylate or methacrylate. In some embodiments, the crosslinker is selected from the group consisting of ethylene glycol di(meth)acrylate, poly(ethylene glycol) di(meth)acrylate.
[0060] The crosslinked vinyl polymer comprises an appropriate crosslink density. If the crosslink density is too low, the resistance to chemical and / or mechanical degradation or the long-term stability of the reference electrode may be lower than desired. However, if the crosslink density is too high, the permeability or mechanical properties of the polymer may be unsatisfactory. In an embodiment where the vinyl polymer is a copolymer of a vinyl monomer containing a heteroatom and a crosslinker, the vinyl polymer may comprise 0.5-7% by weight of the crosslinker, for example 1-4% by weight of the crosslinker, or 1.5-3.5% by weight of the crosslinker.
[0061] Solid Ion Exchange Materials A solid reference electrode comprises a solid ion exchange material containing one or more non-interfering ions. This material is located between the electrode surface for contacting the analyte and a reference element. In use, the solid ion exchange material immobilizes one or more interfering ions present in the analyte solution by exchanging them with non-interfering ions. The role of the solid ion exchange material is therefore to sacrificially react by ion exchange with interfering ions penetrating the electrode, thereby immobilizing the interfering ions and preventing, inhibiting or retarding them from reaching the reference element. The ions released in the ion exchange reaction are non-interfering anions, and therefore have little adverse effect on the potential stability of the electrode.
[0062] As used herein, an interfering ion is capable of participating in a competing redox reaction with the reference element that causes a deviation from the expected electrode potential. In contrast, a non-interfering ion is one that does not significantly affect the measured electrode potential.
[0063] In some embodiments, the solid ion exchange material contains non-interfering anions. Thus, the ion exchange material may protect the electrode from one or more interfering anions present in the analyte by anion exchange. Without wishing to be bound by any theory, the inventors believe that interfering anions may be probabilistically distinguished from non-interfering anions for a given electrode system by comparing the standard reduction potentials of the relevant redox reactions predicted at the reference electrode. Taking the Ag / AgCl reference electrode as an example, the standard reference reduction potentials (25° C., 1 atm) for several anions are shown in Table 1. Anions that react with the reference element at a standard reference potential more negative than the reaction of the reference electrode are expected to interfere with the measured potential. On the other hand, anions that react at the same or more positive standard potentials as the standard electrode reaction are expected not to interfere with the measured potential. [Table 1-1]
[0064] Anionic species such as sulfide, bromide, iodide, and cyanide can interfere with reference electrodes that rely on chloride or sulfate as the reference anion. Chloride can also be an interfering anion when sulfate is the reference anion. Sulfide in particular has been found to be a significant concern for the long-term stability of composite reference electrodes, consistent with the large differences between the standard reduction potentials of redox reactions involving sulfide compared to those using chloride or sulfate.
[0065] The range of suitable non-interfering anions that the ion exchange material may contain will depend on the redox couple upon which the reference potential measurement is based. In the case of Ag / AgCl or saturated calomel reference elements, the solid ion exchange material may contain anions selected from chloride, sulfate, or nitrate.
[0066] In some embodiments, the solid ion exchange material contains the reference anion itself as the exchangeable anion. This is particularly preferred since the resulting ion exchange reaction simply releases additional reference anions into the environment already in solution. Thus, in the case of Ag / AgCl or saturated calomel reference elements, the solid ion exchange material preferably contains exchangeable chlorides. In the case of Ag / Ag2SO4 reference elements, the solid ion exchange material may contain exchangeable sulfates.
[0067] In some embodiments, the solid ion exchange material comprises non-interfering cations capable of ion exchange with one or more interfering cations present in the analyte.
[0068] The solid ion exchange material may generally be any solid material capable of immobilizing interfering anions and releasing non-interfering ions by ion exchange mechanism. In some embodiments, the solid ion exchange material comprises a metal salt or an ion exchange resin. The solid ion exchange material may be a particulate material having an average particle size of, for example, less than 10 mm, or less than 5 mm, or less than 1 mm, or less than 500 microns. Thus, the particulate ion exchange material may be dispersed throughout the polymer matrix of the composite or in an additional protective layer between the composite and the electrode surface, so as to provide a good protective effect.
[0069] Metal salts as solid ion exchange materials. In some embodiments, the solid ion exchange material is a metal salt. The metal salt does not need to be completely insoluble in water, but preferably has a lower solubility in water than the solid inorganic salt that constitutes the reference anion. It is therefore less likely to dissolve from the complex during the useful life of the electrode. Furthermore, the product salt is expected to be relatively insoluble as well, so the relative insolubility may help immobilize interfering ions during use.
[0070] As mentioned above, the present invention may be used to protect an electrode from one or more interfering anions, and therefore the metal salt may be a metal salt of a suitable non-interfering anion. Most preferably, the metal salt comprises the reference anion itself.
[0071] Since the goal is to precipitate the product salt of the ion exchange reaction as an insoluble salt, the choice of metal for the metal salt may depend on the expected interfering anions of the analyte. Furthermore, the metal salt preferably has a strong affinity for the interfering anion, thereby providing good selectivity and fast ion exchange kinetics in the salt metathesis reaction. For immobilization of sulfide anions, salts containing a wide range of metal cations may be suitable, since most metals, except for certain alkali and alkaline earth metals, form insoluble sulfides. For other interfering anions, such as bromide, iodide, and chloride, the range of metals that form insoluble salts is narrower and includes, for example, silver, mercury, and lead.
[0072] In some embodiments, the metal salt comprises a metal that is present in the reference element and participates in the reference redox reaction. Thus, any dissolution of the metal salt inside the electrode does not release metal species that participate in competing redox reactions in the reference element. In some embodiments, the metal salt comprises a cation selected from silver and mercury and an anion selected from chloride and sulfate. In particular, AgCl may be the preferred ion-exchange metal salt for Ag / AgCl reference elements, Ag2SO4 may be the preferred ion-exchange metal salt for Ag / Ag2SO4 reference elements, and Hg2Cl2 may be the preferred ion-exchange metal salt for saturated calomel reference elements.
[0073] Ion exchange resins as solid ion exchange materials In some embodiments, the solid ion exchange material is an ion exchange resin, which is believed to exchange interfering ions with ions of the exchange resin in a manner similar to that of metal salts, thereby immobilizing the interfering ions and preventing them from interacting with the reference element.
[0074] Ion exchange resins are polymers, such as cross-linked polystyrene, that have ionic functional groups whose charge is balanced by exchangeable ions. Both cation and anion exchange resins are known and can be selected depending on whether blocking and immobilization of cationic or anionic interfering ions is desired. In some embodiments, the ion exchange resin is an anion exchange resin, such as a strong or weak basic ion exchange resin. Basic ion exchange resins typically contain pendant quaternized amine functional groups, with exchangeable anions that balance the charge of the cationic amine groups. Thus, the ion exchange resin included in the electrode can be initially loaded with a suitable non-interfering anion (e.g., chloride). Basic ion exchange resins may have a lower affinity for the initially loaded non-interfering anions than for the interfering anions present in the analyte, which favors immobilization of the interfering anions on the resin.
[0075] It is preferable to use a resin whose exchanged ions match those of the redox couple of the reference element. For an Ag / AgCl reference, chloride-based exchange resins such as Amberjet 4200Cl, Amberlite IRA410Cl, Dowex 1X8 chloride form, and Dowex Marathon A chloride form are good candidates.
[0076] Location of solid ion exchange material At least a portion of the solid ion exchange material is disposed between the analyte contact surface of the electrode and the reference element. As mentioned above, the role of the solid ion exchange material is to intercept and immobilize interfering anions as they diffuse to the electrode, thus reducing the probability of undesired interactions with the reference element. The solid ion exchange material must therefore be disposed and distributed in the electrode in a manner suitable to perform this function.
[0077] It will also be apparent to one skilled in the art that the ion exchange material actually involved in the sacrificial ion exchange reaction should not be in electrical communication with the reference element, otherwise the reaction will adversely affect the measured reference potential. Thus, at least the sacrificially reacting portion of the solid ion exchange material is physically separated from the reference element, for example by the insulating polymer matrix of the composite. The reference element is electrically insulated from at least the sacrificially reacting portion of the solid ion exchange material.
[0078] The solid ion exchange material may be loaded into a polymer composite within the electrode. It may be loaded into the polymer matrix of the same composite in which the solid inorganic salt is loaded, or it may be loaded into another polymer composite, e.g., a discrete electrode layer, located between the electrode surface and the reference element. Loading both the solid ion exchange material and the solid inorganic salt into a polymer composite, e.g., the same composite, within the electrode may provide many advantages, such as ease of manufacture, control of electrode hydration, efficient blocking and immobilization of interfering ions, etc. Also, the solid components may provide superior electrode life and reliability, including with abrasive or corrosive analytes, since they may be embedded and optionally dispersed throughout a polymer matrix (or substrate) whose compatibility with such analytes can be tailored. This structure also provides an opportunity to renew used electrodes, e.g., electrodes with fouled surfaces, by removing the surface layer of the composite electrode without losing the electrode's protective capabilities.
[0079] In some embodiments, the solid ion exchange material is present in the polymer matrix of the same composite in which the solid inorganic salt is loaded. Thus, the solid ion exchange material and the solid inorganic salt constituting the reference anion may be co-dispersed in the polymer matrix, for example as particulate material. The solid ion exchange material may be present in an amount of at least 1% by weight, for example at least 3% by weight, of the composite.
[0080] In such a configuration, the complex may be exposed, for example, through a window in the electrode casing, thereby forming an electrode surface for contacting the analyte. In use, the electrode is immersed in the analyte and hydrated by the penetration of water into the complex. Interfering ions that diffuse into the complex undergo an ion exchange reaction with the solid ion exchange material and are immobilized in the complex before reaching the reference element. The inventors have found through experiments that sulfide anions are immobilized in a thin layer on the surface of a complex containing 5 or 10% by weight AgCl dispersed in a matrix, and do not penetrate deep enough to interfere with the reference element. Thus, the reference element should be placed deep enough on the surface of the complex to be immobilized before the interfering ions arrive, while ensuring sufficient ionic conductivity between the reference element and the analyte. In some embodiments, the reference element is between 1 mm and 10 mm from the surface.
[0081] One such embodiment of the invention is depicted in FIG. 1. The electrode 100 includes a reference element 102 embedded in a composite 104. The reference element 102 includes a silver wire coated with silver chloride and having a proximal end 106 in contact with the composite 104. A distal end 108 extends from the composite and is therefore electrically connectable to a potentiometer. The composite 104 includes a matrix of polyvinyl acetate crosslinked with about 2% ethylene glycol dimethacrylate (EGDMA) by weight. The matrix is loaded with particulate potassium chloride (KCl) present in an amount greater than 50% by weight of the composite, and particulate silver chloride (AgCl) present in an amount of about 5% by weight of the composite. The particulate components are dispersed throughout the composite. An impermeable polymer casing 110 surrounds the composite, except for a window 112 at which a surface 114 of the composite is exposed for contact with the analyte.
[0082] In use, electrode 100 is immersed in an aqueous analyte containing one or more analytes and one or more interfering anions, including sulfide. The complex becomes hydrated through window 112, dissolving a portion of the KCl and establishing a saturation concentration of chloride ions in reference element 102. Electrode 100 thus provides a stable Ag / AgCl reference potential against which the potential of an ion-selective electrode or working electrode can be measured, as described in more detail below.
[0083] Interfering anions present in the analyte will infiltrate the complex during initial hydration and, by diffusion, during continued use of the reference electrode. However, in accordance with the principles disclosed herein, the interfering anions are immobilized on particulate AgCl particles located between surface 114 and reference element 102, e.g., at location 116. The ion exchange reaction believed to immobilize sulfide anions is a salt metathesis reaction shown by Equation 2: S 2- (aq)+2AgCl(s) → Ag2S(s)+2Cl - (aq)(2)
[0084] Considering that the interior of the composite 104 already has a saturated concentration of chloride and that the reference element is electrically isolated from the AgCl particles that intercept and immobilize the sulfide ions, the release of chloride anions due to the ion exchange reaction does not affect the measured reference potential.
[0085] Another embodiment is depicted in FIG. 2. The electrode 200 is a printed electrode, formed on a substrate 201 by a printing technique such as screen printing or inkjet printing. The substrate 201 may be any of a wide range of substrates including polymer substrates (e.g., polyethylene terephthalate, polyimide), paper substrates, glass substrates, ceramic substrates, or any of these with a film coating including indium tin oxide. The reference element 202 is a printed layer including silver and silver chloride, which may be printed with a commercially available Ag / AgCl ink. A layer of composite 204 is printed over the reference element, except for the distal end 208, which remains exposed, and thus electrically connectable to a potentiometer. The composite 204 includes a polymer matrix, such as polyvinyl acetate (PVAc), in which particles of both KCl and AgCl are dispersed. This layer may be printed with an ink including PVAc and particles dispersed in acetone, and cured after printing. The composite 204 may also include multiple printed layers. A surface 214 of the composite is exposed for contact with the analyte. Optionally, electrode 200 may further include an insulating printed layer (not shown) over a portion of composite 204, while leaving a portion of composite surface 214 exposed for contact with the analyte. During use, the complex is hydrated through surface 214, thus establishing a reference potential as described herein for electrode 100. However, interfering anions such as sulfide are immobilized on AgCl particles in the polymer matrix by an ion exchange reaction before reaching reference element 202.
[0086] In other embodiments, the solid ion exchange material is present in a water-permeable composite layer located between the electrode surface and the solid inorganic salt loaded composite. The water-permeable layer may comprise a solid ion exchange material dispersed in a hydratable polymer. The water-permeable layer may optionally comprise a solid inorganic salt that constitutes the reference anion, although this is not believed to be necessary for the function or protective effect of the electrode.
[0087] It will be apparent that similar considerations regarding the properties of the hydratable polymer apply to the polymer matrix of the complex, since hydration of the complex and ionic conductivity between the reference element and the analyte are provided through the water-permeable layer. The hydratable polymer should therefore exhibit a suitable hydrophilic-hydrophobic balance to allow for rapid conditioning and low impedance, but also provide dimensional stability and retention of the solid ion exchange material. The hydratable polymer may therefore be the same or different as in the polymer matrix of the complex, but its composition may generally be as described herein for the appropriate complex polymer matrix. The water-permeable layer should have a thickness sufficient to allow for blocking and immobilization of interfering anions, but not excessively thick as this may increase impedance. In some embodiments, the thickness of the water-permeable layer is between 1 and 5 mm.
[0088] In embodiments where the solid ion exchange material is present in the water permeable layer, the complex is generally not directly exposed to the analyte. Rather, it is covered by the water permeable layer entirely, or at least at the locations where contact with the analyte is expected, such as the window area of the electrode casing. The exposed surface of the water permeable layer can be the electrode surface for contact with the analyte. In use, the electrode is immersed in the analyte and hydrated by the penetration of water from the water permeable layer into the complex. Interfering ions that diffuse through the water permeable layer are immobilized in the water permeable layer by ion exchange reaction with the solid ion exchange material before reaching the complex or reference element.
[0089] It is of course not excluded that a further water-permeable layer may be present between the inorganic salt-loaded composite and the layer comprising the solid ion exchange material, or as an outer layer forming the analyte-contacting surface of the electrode.
[0090] An embodiment of the invention is depicted in FIG. 3, in which like numbered items are as described herein for electrode 100 depicted in FIG. 1. In electrode 300, reference element 102 is embedded in a composite 304 comprising an EGDMA cross-linked polyvinyl acetate matrix and particulate KCl dispersed therein. However, the particulate ion exchange material is not present in the composite, but instead in a water-permeable layer 318 disposed directly against composite 304. Layer 318 is comprised of an EGDMA cross-linked polyvinyl acetate matrix having particulate AgCl dispersed therein and has a thickness of about 1-5 mm. A surface 314 of the water-permeable layer is exposed for contact with the analyte within window 112 of casing 110.
[0091] In use, the electrode 300 is immersed in an aqueous analyte containing one or more analyte species and one or more interfering anions, including sulfide. The water-permeable layer and the complex are hydrated through the window 112, dissolving a portion of the KCl and establishing a saturation concentration of chloride ions in the reference element 108. The electrode 100 thus provides a stable Ag / AgCl reference potential. Interfering anions present in the analyte will infiltrate the water-permeable layer during initial hydration and, by diffusion, during continued use of the reference electrode. However, in accordance with the principles disclosed herein, the interfering anions are immobilized on particulate AgCl particles located in the water-permeable layer, for example at positions 316 between the surface 314 and the reference element 102.
[0092] Method for producing a solid reference electrode It is apparent from the above discussion that many different electrode configurations fall within the scope of the present invention. Accordingly, the methods for fabricating the solid reference electrode also vary.
[0093] The method generally involves preparing a composite comprising a water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion. In some embodiments, a solid ion exchange material is also dispersed in the polymer matrix. The solid inorganic salt and the solid ion exchange material have been previously described herein.
[0094] In some embodiments, the solid inorganic salt and optionally the solid ion exchange material are combined with a polymer precursor, such as a polymerizable composition comprising one or more monomers, crosslinkable polymers, or curable resins. The polymer precursor is then polymerized, crosslinked, and / or cured to form a water-permeable polymer matrix loaded with the inorganic salt and optionally the solid ion exchange material.
[0095] When the water-permeable polymeric substrate comprises a vinyl polymer, the method may include combining the solid inorganic salt and optionally the solid ion-exchange material with a polymerizable composition comprising one or more vinyl monomers. The polymerizable composition may optionally include a cross-linking agent comprising at least two copolymerizable vinyl functional groups. Suitable vinyl monomers and cross-linking agents have been previously described herein. The composite is then prepared by polymerizing the composition, typically in the presence of a free radical initiator or catalyst. The polymerizable composition may thus include a photoinitiator such as 2,2-dimethoxy-2-phenylacetophenone. The method may then include irradiating the mixture with UV light for a time sufficient to initiate and sufficiently complete the polymerization. Alternatively, the mixture may include a thermally activated initiator such as 2,2'-azobis(2-methylpropionitrile). The method may then include heating the mixture at a temperature and for a time sufficient to initiate and sufficiently complete the polymerization. It is also envisioned to prepare a composite having a cross-linked polymeric substrate by combining the solid inorganic salt and optionally the solid ion-exchange material with an uncross-linked vinyl polymer and then cross-linking the polymer.
[0096] The composite is prepared to be in ionic contact with the reference element. Suitable reference elements have also been described. Thus, in some embodiments, the reference element is contacted with the polymer precursor containing an inorganic salt and, optionally, a solid ion exchange material before the completion of polymerization, crosslinking or curing. For example, the reference element may be inserted into the polymer precursor, or the polymer precursor may be cast or printed onto the reference element. Polymerization or curing may then be initiated to create an electrode in which the reference element is in contact with or attached to the composite.
[0097] In embodiments in which the solid ion exchange material is dispersed in the composite, the method may include providing a surface of the composite as an electrode surface for contacting the analyte in use. For example, if a polymer precursor is polymerized or cured within the casing, then a window of appropriate size may be formed in the casing to expose the surface of the composite.
[0098] In the embodiment in which the solid ion exchange material is present in the water-permeable layer of the polymer composite located between the electrode surface and the composite loaded with the solid inorganic salt constituting the reference ion, the method of the present invention may include providing this water-permeable layer. The water-permeable layer may be provided such that the solid ion exchange material, and optionally also the solid inorganic salt constituting the reference anion, are dispersed in a hydratable polymer. Hydrateable polymers have already been described herein. It may therefore be produced in a similar manner to the polymer matrix of the composite, for example by dispersing the solid ion exchange material in a polymer precursor and polymerizing, crosslinking or curing the precursor to form a water-permeable layer with the required properties.
[0099] A water-permeable layer may be formed on the composite. This may involve either forming a composite on the water-permeable layer or forming a water-permeable layer on the composite. As an example of the first option, the electrode 300 depicted in FIG. 3 may be manufactured by placing a mixture of vinyl acetate, EGDMA, particulate AgCl and a free radical initiator as a layer on the bottom of the casing 110 (before the window 112 is opened). This mixture is then polymerized to form a water-permeable layer 318 comprising cross-linked polyvinyl acetate with AgCl dispersed therein. The mixture of vinyl acetate, EGDMA, particulate KCl and free radical initiator is then transferred into the casing and the reference element 102 is inserted to the required depth in the mixture. The mixture is then polymerized to form a composite 304 on top of the water-permeable layer. Finally, a window 112 is formed in the casing to expose the surface 314.
[0100] In a second alternative example, a printed electrode can be fabricated on a substrate by successively printing and curing i) a conductive reference element layer comprising Ag and AgCl, ii) a composite layer comprising KCl dispersed in a water-permeable polymer matrix on a portion of the reference element, and ii) a water-permeable layer comprising AgCl dispersed in a hydratable polymer covering the composite layer.
[0101] In embodiments in which the solid ion exchange material is dispersed in a water-permeable layer, the method may include providing a surface of the water-permeable layer as an electrode surface for contacting the analyte in use. For example, if the electrode is provided in a casing, a window of appropriate size may be provided in the casing to expose the surface of the water-permeable layer.
[0102] Systems and methods for electrochemical analysis of analytes - Patents.com The solid reference electrode of the present invention may be used in electrochemical analyses including potentiometric, voltage, and amperometric measurements. In potentiometric analyses, the potential difference between an ion-sensitive electrode in contact with the analyte and a reference electrode is passively measured. In three-electrode voltammetric analyses, a working electrode and a counter electrode are contacted with the analyte, the potential between these electrodes is changed according to a predetermined pattern, and the current transfer to the analyte is measured. The reference electrode is coupled to the working electrode so that the working potential can be measured and controlled during the analysis. A similar arrangement is used in amperometric analyses, except that the current flow is controlled and the resulting potential difference between the working and reference electrodes is measured.
[0103] Thus, the present invention relates to a system for the electrochemical analysis of an analyte, comprising a solid reference electrode as described herein, an ion-selective electrode or working electrode (depending on the type of analysis to be performed), and means for measuring the potential difference between the ion-selective or working electrode and the reference electrode, such as a voltmeter or potentiostat.
[0104] In some embodiments, the system is a potentiometric system for determining the concentration of an ion in an analyte, the system including a solid reference electrode as described herein, an ion-selective electrode, and a means for measuring the potential difference between the ion-selective electrode and the reference electrode, such as a voltmeter or potentiostat.
[0105] The present invention also relates to a method for electrochemical analysis of an analyte. The method comprises contacting a solid reference electrode as described herein and an ion-selective electrode or counter electrode with the analyte and measuring the difference in electrochemical potential between the reference electrode and the ion-selective electrode or working electrode. The two electrodes may be contacted by immersion in the analyte. The analyte may be an aqueous analyte. The difference in electrochemical potential may be measured using a voltmeter or potentiostat.
[0106] In some embodiments, the method is a method for determining an ion concentration in an analyte, the method comprising contacting a solid reference electrode and an ion-selective electrode as described herein with the analyte and measuring the difference in electrochemical potential between the ion-selective electrode and the reference electrode.
[0107] In the system and method for determining ion concentration, the ion selective electrode is not considered to be particularly limited and will depend on the intended application. For example, the ion selective electrode may be a pH, oxidation-reduction potential (ORP), cyanide, metal ion, or potentiometric sensor of a biosensor. In some embodiments, the ion selective electrode is sensitive to hydrogen ions such that the system is a pH meter. In some embodiments, the ion selective electrode is a solid electrode, for example, a polymer composite electrode. An example of such an electrode is a composite hydrogen ion selective sensor comprising a mixture of Ta2O5 and RuO2 dispersed in a polymer matrix, as described in WO2016 / 033632.
[0108] Interfering ions are expected in analytes of electrochemical analysis in many applications, including environmental monitoring, process monitoring in the mining and chemical industries, oil and gas related monitoring systems, biological systems, wastewater treatment and pipelines.
[0109] In some embodiments, the analyte is an acidic and / or abrasive analyte where interfering ions present additional challenges for maintaining a stable reference potential. Examples of such analytes are found in the mining and mineral processing industries. In some embodiments, the analyte is, for example, leachate and leach slurries from heap leaching operations, or acid mine drainage streams.
[0110] In some embodiments, the analyte includes one or more interfering ions. The interfering ions may be interfering anions, such as sulfide, iodide, bromide, and cyanide. In some embodiments, the analyte includes sulfide.
[0111] Working Example The invention will now be described with reference to the following examples, which are understood to be illustrative and not limiting of the invention described herein.
[0112] material All starting materials were purchased from Sigma-Aldrich or other commercial suppliers. The KCl used was of analytical quality (VWR AnalaR) to avoid shifts in the reference potential due to any inorganic contaminants. Monomers, crosslinkers, and initiators were of 98% purity or higher. Silver particles (99.9%, 5–8 μm) and silver chloride coarse powder (99.997%) were purchased from Alfa Aesar. AmberjetTM 4200 Cl, a strongly basic (type I) ion exchange resin in the chloride form (particle size 600–800 μm), was commercially sourced.
[0113] Example 1. Preparation of electrodes Silver wires (1.5 mm thick, 99.95% Ag) were polished with fine sandpaper and washed with ethanol. Each wire was inserted into a 1M KCl solution and connected to a potentiostat. A small current (7 mA, 100 s) was passed between the silver electrode (anode) and the platinum counter electrode (cathode) to coat the wires with silver chloride.
[0114] A mixture of vinyl acetate and ethylene glycol dimethacrylate (EGDMA), with EGDMA present as 2% by weight of the total monomers, was prepared and a small amount of 2,2'-azobis(2-methylpropionitrile) (≤2% by weight) was added as a thermal initiator.
[0115] Dry KCl powder was added to each mixture, and the settled slurry was transferred by pipette to glass vials (volume 1–10 mL) so that the vials were filled with KCl powder and the monomer mixture filled the voids between the particles. Solid particulate additives (either AgCl, Ag metal particles or AmberjetTM4200Cl ion exchange resin) were dispersed in some of the mixtures as shown in Table 1. Small amounts (0.1–0.5 mL) of additional monomer mixture were transferred to the vials to form a salt-free sealed layer on the top of the vial during subsequent polymerization. The mass ratio of KCl to monomer was approximately 2:1 in the mixtures.
[0116] A silver chloride-coated silver wire (2-5 cm long, depending on vial size) was then inserted into each vial and the vials were sealed. The mixture was heated to approximately 50 °C for approximately 18 h to copolymerize the monomers. After polymerization was complete, the bottom of the vial was polished off to expose a solid composite containing a matrix of EGDMA-crosslinked polyvinyl acetate (PVAc) loaded with both solid KCl and solid particulate additives. The electrodes were then ready for use. [Table 1-2]
[0117] Example 2. Electrochemical testing of electrodes with metal salt additives The electrochemical performance of electrodes E1-E5 (1.5 mL vial volume) prepared in Example 1 was evaluated in 1 g / liter Na2S solution in pH 9 buffer. The potential response of the electrodes was measured against a saturated calomel electrode (SCE) obtained from Koslow Scientific Company (which was regularly maintained during electrochemical testing to ensure stable performance). A multichannel potentiostat (Biologic VMP3 potentiostat) was used to record the open circuit potential (OCP) signal of the electrodes.
[0118] Figure 4 shows the potential response of the electrodes. The control electrode E1 was initially stable to the SCE potential but began to drift after approximately 30 days of exposure to the analyte. After being on-line for 120 days, the potential was -132 mV vs. SCE compared to a theoretical potential of -45 mV vs. SCE. The periods marked with "X" in Figure 4 correspond to periods where the SCE failed to be maintained.
[0119] In contrast, the inclusion of 5% (E2) or 10% (E3) by weight AgCl particles dispersed throughout the composite resulted in a stable reference potential throughout the experiment, despite the presence of sulfide anions in the analyte. After 120 days online, the potential was -44 mV vs SCE, compared to a theoretical potential of -45 mV vs SCE. Throughout the experiment, the potential was virtually the same for electrodes E2 and E3. After the experiment, a discolored layer was observed at the composite-analyte interface, but no discoloration was observed deeper in the composite.
[0120] The protection of the electrode potential is believed to be due to the immobilization of sulfide anions in this layer, preventing them from diffusing through the complex to reach the Ag / AgCl wire. The sulfide anions exchange with chloride anions on the AgCl particles, forming insoluble Ag2S and releasing free chloride anions.
[0121] The inclusion of 5% (E4) or 10% (E5) by mass of Ag metal particles was not effective in protecting the electrodes from drift due to interference from sulfide anions. The potential of electrode E4, which contained 5% by mass of Ag metal particles, was stable for the first 20 days, but then a severe drift was observed.
[0122] Example 3. Electrochemical testing of electrodes with ion exchange resin additives The electrochemical performance of electrodes E1 and E6 (1.5 mL vial volume) prepared in Example 1 was evaluated in triplicate in 1 g / liter Na2S solution in pH 9 buffer. The potential response of the electrodes was measured against a saturated calomel electrode (SCE) obtained from Koslow Scientific Company, which was regularly maintained during electrochemical testing to ensure stable performance. A multichannel potentiostat (Biologic VMP3 potentiostat) was used to record the open circuit potential (OCP) signal of the electrodes.
[0123] FIG. 5 shows the potential response of the electrodes, and the potentials shown are the average of the three electrodes. The control electrode E1 without additive and electrode E6 with ion exchange resin additive initially showed very similar results, leveling off at a level close to the theoretical potential of -45 mV vs SCE. At about day 30, there was some indication that the standard electrode E1 was drifting due to interference from sulfide ions, as was also seen at this time in Example 2. In contrast, electrode E6 containing ion exchange resin loaded with chloride ions continued to show a very stable potential.
[0124] One E1 electrode and one E6 electrode were removed after 24 days online, the casing removed, and the electrodes cut lengthwise with a razor blade. Visual inspection of the inside of the electrodes confirmed that the ion exchange resin beads were dispersed inside the composite. The electrodes were then subjected to X-ray fluorescence analysis. Elemental maps (20mmx10mm) of the dried cross sections were collected in air at 20mbar using a Bruker M4 Tornado high performance μXRF spectrometer equipped with a Rh X-ray tube, polycapillary optics, and a silicon drift detector. The polycapillary optics allowed the collection of maps with a spot size of 25μm diameter for MoKα. The mapping was performed with a pixel spacing of 25μm and a 20ms pixel resolution. -1 The acquisition time was 100 s. The X-ray generator was operated at 50 kV and 599 μA with a 12.5 μM Al filter. XRF images revealed that sulfur selectively accumulated on the resin beads dispersed in the E6 electrode composite. On the other hand, no sulfur accumulation was observed in the D1 electrode composite.
[0125] Example 4. Accelerated poisoning test Electrodes E1 (no additive) and E2 (5 wt. % AgCl additive) were placed in an aqueous solution of 1 mmol / l sodium sulfide (Na2S) and 1 mmol / l sodium bromide (NaBr) buffered at pH 9 and maintained at a pressure of 8 bar or higher for 7 weeks. The electrodes were then cross-sectioned and analyzed by XRF using the same method as used in Example 3. Elemental mapping suggested that the penetration of sulfur and bromine into the interior of the E1 electrode was less than that of the E2 electrode.
[0126] Example 5. Electrochemical testing of metal salt-added electrodes under strongly acidic conditions The electrochemical performance of electrodes E1 (no additive) and E2 (5 wt% AgCl additive) prepared in Example 1 was evaluated in 1000 ppm Na2S aqueous solution acidified to pH 2.6. Five identical electrodes of each type were tested in parallel. The potential response of the electrodes was measured against a commercial Ag / AgCl reference electrode with 3 mol / liter KCl internal electrolyte (which was regularly maintained during the electrochemical test to ensure stable performance).
[0127] Figure 6 shows the potential response of the electrodes. Three of the control electrodes E1 showed an initial response close to the theoretical potential difference of -9 mV, but all failed after 7 days online. On the other hand, all five AgCl-containing electrodes E2 remained stable for nearly 50 days. Thereafter, their performance changed, with two fluctuating significantly, but three continued to provide reliable reference potentials even after more than 200 days online.
[0128] Those skilled in the art will appreciate that the invention described herein may be susceptible to variations and modifications other than those specifically described, and it is understood that the invention includes all such variations and modifications which fall within the spirit and scope of the invention.
Claims
1. a reference element in ionic communication with the complex, an electrode surface for contacting the analyte, and a solid ion exchange material located between the electrode surface and the reference element; the composite includes an electrically insulating, water-permeable polymer matrix loaded with a solid inorganic salt comprising a reference anion, the solid inorganic salt being a particulate solid dispersed in the polymer matrix, the solid inorganic salt being sufficiently soluble in water such that hydration of the composite results in a constant saturated solution concentration of the reference anion in the reference element, and the reference anion is capable of participating in a desired redox half-reaction in the reference element to provide a reference potential; the solid ion exchange material comprises one or more non-interfering anions; the reference element is electrically insulated from the solid ion exchange material; A solid reference electrode, wherein in use, when interfering anions are present in the analyte solution, the solid ion exchange material immobilizes one or more of the interfering anions by exchange with the non-interfering anions.
2. 2. The solid reference electrode of claim 1, wherein the solid ion exchange material comprises a metal salt or an ion exchange resin.
3. 3. The solid reference electrode of claim 1 or 2, wherein the solid ion exchange material comprises a metal salt having a lower water solubility than the solid inorganic salt.
4. The solid reference electrode of any one of claims 1 to 3, wherein the non-interfering anion comprises the reference anion.
5. The solid reference electrode of any one of claims 1 to 4, wherein the solid ion exchange material comprises a metal salt comprising a cation selected from the group consisting of silver, mercury, and lead.
6. A solid reference electrode according to any one of claims 1 to 5, wherein the solid ion exchange material comprises a metal salt comprising a metal present in the reference element.
7. The solid reference electrode according to any one of claims 1 to 6, wherein the interfering anions are selected from the group consisting of sulfide, iodide, bromide, and cyanide ions.
8. A solid reference electrode according to any one of claims 1 to 7, wherein the solid ion exchange material is a particulate material.
9. 9. The solid reference electrode according to claim 1, wherein the solid ion exchange material is loaded into the polymer matrix of the composite or into a further polymer composite located between the electrode surface and the reference element.
10. 10. The solid reference electrode of claim 9, wherein the further polymer composite comprises the solid ion exchange material dispersed in a hydratable polymer.
11. 10. The solid reference electrode of claim 9, wherein the solid ion exchange material is loaded into the polymer matrix of the composite.
12. 12. The solid reference electrode of claim 11, wherein the solid ion exchange material is present in an amount of at least 1% by weight of the composite.
13. 11. A solid reference electrode according to claim 9 or 10, wherein the solid ion exchange material is packed in a water-permeable layer of the further polymer composite located between the electrode surface and the composite.
14. A solid reference electrode according to any one of claims 1 to 13, wherein the reference anion is a chloride ion.
15. 15. The solid reference electrode of claim 14, wherein the reference element is selected from the group consisting of Ag / AgCl and calomel.
16. A solid reference electrode according to any one of claims 1 to 15, wherein the water-permeable polymer matrix comprises a vinyl polymer of a vinyl monomer containing a heteroatom.
17. 17. The solid reference electrode of claim 16, wherein the vinyl polymer is crosslinked.
18. 18. The solid reference electrode of claim 17, wherein the crosslinked vinyl polymer is a copolymer of i) at least one vinyl monomer selected from the group consisting of vinyl esters, vinyl amides, and acrylates, and ii) a crosslinker containing at least two copolymerizable vinyl functional groups.
19. The solid reference electrode according to any one of claims 1 to 18, wherein the composite comprises at least 30% by mass of the solid inorganic salt.
20. 1. A system for the electrochemical analysis of an analyte, the system comprising: A solid reference electrode according to any one of claims 1 to 19. a second electrode selected from an ion selective electrode and a working electrode; and means for measuring a potential difference between said second electrode and said reference electrode.
21. 1. A method for the electrochemical analysis of an analyte, the method comprising: i) a solid reference electrode according to any one of claims 1 to 19, and ii) contacting a second electrode selected from an ion selective electrode and a working electrode with the analyte; and measuring an electrochemical potential difference between the second electrode and the reference electrode.
22. 22. The method of claim 21 , wherein the analyte comprises one or more interfering anions in solution, the one or more interfering anions being capable of participating in a competing redox reaction with a reference element that causes a deviation from an expected electrode potential.
23. 23. The method of claim 22, wherein the interfering anions are selected from the group consisting of sulfide, iodide, bromide, and cyanide.
24. 23. The method of claim 22, wherein the interfering anion comprises a sulfide ion.
25. 25. The method of any one of claims 22 to 24, wherein the solid ion exchange material immobilizes one or more of the interfering anions by exchange with the non-interfering anions.
Citation Information
Patent Citations
Reference electrode
JP1984190650A
Comparison electrode
JP2003262606A
All-solid state reference electrode
WO1996035116A1
Solid state reference electrode
WO2018201200A1