Composite active material for secondary battery, and secondary battery
Patent Information
- Application Number
- JP2024515881
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-08
- Filing Date
- 2023-11-02
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-11-02
AI Technical Summary
Existing silicon-based active materials for lithium-ion batteries suffer from insufficient control of the surface layer structure, leading to volume expansion and contraction during charging and discharging, which causes particle collapse, decreased coulombic efficiency, and poor cycle characteristics due to excessive electrolyte reaction.
A composite active material comprising silicon particles with a silicon nitride and/or silicon carbide phase and a matrix phase containing a transition metal element, which stabilizes the silicon particle surface by forming a catalytic film-like or particulate layer to control the surface structure and suppress oxidation.
The composite active material enhances chemical durability, maintaining high charge/discharge performance with improved capacity retention rate and initial coulombic efficiency by stabilizing the silicon particle surface.
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite active material for a secondary battery, and a secondary battery including the composite active material for a secondary battery. [Background technology]
[0002] In response to environmental concerns about energy demand, the use of lithium-ion batteries (LIBs) is expanding as their use in electric vehicles (EVs) is rapidly progressing. Graphite, the mainstream LIB anode material, has a low theoretical capacity density (372 mAh / g), and in order to improve battery capacity, active development of high-capacity active materials using silicon, tin, and oxides is being actively carried out. However, these materials have a problem in that the volume expansion and contraction of the materials is large when they absorb and release lithium ions, and the active materials become pulverized by repeated charging and discharging, which deteriorates the charge and discharge characteristics.
[0003] Patent Document 1 describes a negative electrode material for a non-aqueous electrolyte secondary battery that comprises silicon nanoparticles and a coating layer that coats the silicon nanoparticles, the coating layer comprising an amorphous silicon oxide and a silicon carbide phase, and at least a portion of the silicon carbide phase being present on the surface of the silicon nanoparticles.
[0004] Patent Document 2 describes that in carbon-coated silicon particles, at least a portion of the surface is coated with carbon, at least a portion of the interface between the carbon coating and the silicon particle has a layer of silicon carbide, and the ratio of powder X-ray diffraction analysis is below a certain level.
[0005] Patent Document 3 describes a silicon negative electrode active material that includes a double clamping layer having a silicon core containing silicon particles, a silicon carbide layer on the silicon core, and a silicon oxide layer between the silicon core and the silicon carbide layer. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2015-60776 [Patent Document 2] Japanese Patent Application Publication No. 2014-75325 [Patent Document 3] Japanese Patent Publication No. 2020-181820 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the case of the silicon particles and active materials containing them described in Patent Documents 1 to 3, the control of the surface layer structure (form of oxide film, silicon nitride or silicon carbide) on the silicon particles is insufficient. As a result, the repeated volume expansion and contraction of the silicon particles due to repeated charging and discharging is not sufficiently suppressed, so that the silicon particles may collapse. In addition, the electrochemical reaction between the silicon particles and the electrolyte proceeds vigorously, so that the solid electrolyte interface layer (SEI layer) continues to be formed on the surface of the silicon particles, and there is a problem that both the initial coulombic efficiency and the charge and discharge capacity are reduced due to the large consumption of lithium ions. Therefore, further improvement is required for the cycle characteristics and initial coulombic efficiency of the battery.
[0008] An object of the present invention is to provide a composite active material for a secondary battery that can suppress the collapse of silicon particles as described above and can maintain high charge / discharge performance, such as capacity retention rate and initial coulombic efficiency, when used in a secondary battery, and a secondary battery that contains the composite active material for a secondary battery in its negative electrode. [Means for solving the problem]
[0009] The present inventors considered that the silicon particles described in Patent Documents 1 to 3 and active materials containing them have difficulty in controlling the surface layer structure on the silicon particles, and therefore the charge / discharge performance of the secondary battery is insufficient, and investigated a method for stabilizing the structure of the silicon particle surface in the active material. As a result, the present inventors found that in a composite active material having a structure of silicon particles having a silicon nitride phase and / or silicon carbide phase and a matrix phase containing the silicon particles, by including a transition metal element, a film-like or particulate silicon nitride or silicon carbide phase can be imparted to the silicon particle surface by its catalytic action, thereby improving the chemical durability of the silicon particle surface and controlling the surface layer structure on the silicon particles.
[0010] The present invention has the following aspects. [1] A composite active material for a secondary battery comprising silicon particles, a silicon nitride phase and / or a silicon carbide phase, and a matrix phase encapsulating the silicon particles, wherein at least one phase selected from the group consisting of the silicon nitride phase, the silicon carbide phase, and the matrix phase contains a transition metal element. [2] The composite active material for a secondary battery according to [1], wherein at least a portion of the silicon nitride phase and / or silicon carbide phase is present on the surface of the silicon particles. [3] The composite active material for a secondary battery according to [1] or [2], wherein the silicon nitride phase and / or the silicon carbide phase are contained in a higher concentration on or in the vicinity of the surface of the silicon particles than in the matrix phase. [4] The composite active material for a secondary battery according to any one of [1] to [3], wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La. [5] The composite active material for a secondary battery according to any one of [1] to [4], wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cu, and La. [6] The composite active material for a secondary battery according to any one of [1] to [5], wherein the content of the transition metal element is 0.01 atm % to 5 atm % based on the total amount of silicon present in the silicon particles. [7] The composite active material for a secondary battery according to any one of [1] to [6], wherein the matrix phase contains carbon. [8] The composite active material for a secondary battery according to any one of [1] to [7], wherein the matrix phase has a composition represented by SiOx (1 < x < 2). [9] The composite active material for a secondary battery according to any one of [1] to [8], wherein the matrix phase has silicon oxycarbide.
[10] The composite active material for a secondary battery according to any one of [1] to [9], wherein the average particle diameter of the silicon particles is in the range of 10 nm to 300 nm.
[11] The composite active material for a secondary battery according to any one of [1] to
[10] , wherein the transition metal element is in the range of 0.001 atm% to 5 atm% with respect to the total amount of silicon.
[12] The composite active material for a secondary battery according to any one of [1] to
[11] , wherein a carbon layer exists on the surface.
[13] The composite active material for a secondary battery according to any one of [1] to
[12] , which contains Li and / or Mg.
[14] A secondary battery including the composite active material for a secondary battery according to any one of [1] to
[13] in a negative electrode.
Advantages of the Invention
[0011] The composite active material for a secondary battery of the present invention can improve the chemical durability of the surface of silicon particles and control the surface layer structure on the silicon particles, and can maintain high charge and discharge performance such as the capacity retention rate and the initial Coulomb efficiency in a secondary battery.
Brief Description of the Drawings
[0012] [Figure 1] FIG. 1 is a diagram showing the HADDF-STEM image and the results of elemental EDS mapping analysis of the composite active material for a secondary battery obtained in Example 1.
Modes for Carrying Out the Invention
[0013] The present invention will be described below, but the present invention is not limited to the examples in the following description. In this specification, the term "to" indicating a numerical range includes the upper and lower limits. Note that "A and / or B" means either A or B, or both. In addition, in this specification, a ratio based on mass (percentage, etc.) is the same as a ratio based on weight (percentage, etc.).
[0014] [Composite active material for secondary batteries] The composite active material for secondary batteries of the present invention has silicon particles, a matrix phase encapsulating the silicon particles, and a silicon nitride phase and / or a silicon carbide phase, and contains a transition metal element in at least one phase selected from the group consisting of the silicon nitride phase, the silicon carbide phase, and the matrix phase.
[0015] The composite active material for secondary batteries of the present invention has a structure having silicon particles, a matrix phase surrounding the silicon particles, and a silicon nitride phase and / or a silicon carbide phase, and a transition metal element is supported in at least one phase selected from the group consisting of the silicon nitride phase, the silicon carbide phase, and the matrix phase. Note that "silicon nitride phase and / or silicon carbide phase" means either one or both of the silicon nitride phase and the silicon carbide phase.
[0016] In this embodiment, the silicon nitride phase and / or silicon carbide phase may be present inside the silicon particles, on the surface of the silicon particles, in the matrix phase, or in all of these. Among these, in this embodiment, it is preferable that at least a part of the silicon nitride phase and / or silicon carbide phase is present on the surface of the silicon particles. That is, it is preferable that the silicon particles are partially or entirely covered with the silicon nitride phase and / or silicon carbide phase. By having at least a part of the silicon nitride phase and / or silicon carbide phase present on the surface of the silicon particles, oxidation of the silicon surface during high-temperature firing of the active material is suppressed, thereby improving the initial coulombic efficiency. Furthermore, by improving the chemical durability of the silicon particle surface, the capacity retention rate in the secondary battery can be improved. In addition, at this time, the matrix phase is present so as to further cover the silicon particles covered with the silicon nitride phase and / or silicon carbide phase.
[0017] In this embodiment, it is particularly preferable that a silicon nitride phase and / or silicon carbide phase is present at a high concentration on or near the surface of the silicon particles rather than in the matrix phase. Specifically, the silicon nitride phase and / or silicon carbide phase is present on or near the surface of the silicon particles, and for example, the silicon nitride phase and / or silicon carbide phase is present at a high concentration as shown in Fig. 1. This embodiment efficiently prevents the oxidation reaction between oxygen and Si during high-temperature firing of the active material. Here, the vicinity of the surface of the silicon particle refers to a region preferably within 10 nm from the surface of the silicon particle toward the outside of the silicon particle.
[0018] The transition metal element has a catalytic action and is preferably at least one selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La, from the viewpoint of effectively generating a silicon nitride phase or a silicon carbide phase, and is particularly preferably at least one selected from the group consisting of Fe, Mn, Ni, Cu, and La. The transition metal element in the present invention is considered to be present in the form of metal ions in at least one phase selected from the group consisting of a silicon nitride phase, a silicon carbide phase, and a matrix phase. In other words, when the transition metal element is Mn, Mn 2+ It is thought to exist as
[0019] The content of the transition metal element is preferably 0.01 atm% to 5 atm%, more preferably 0.1 atm% to 4 atm%, and even more preferably 0.2 atm% to 3 atm%, based on the total amount of silicon (Si element) present in the silicon particles in the composite active material for secondary batteries of the present invention. The content of the transition metal element is preferably 0.001 atm% to 5 atm%, more preferably 0.003 atm% to 4 atm%, and even more preferably 0.005 atm% to 3 atm%, based on the total amount of silicon in the composite active material for secondary batteries of the present invention. When the content of the transition metal element is within the above range, the silicon nitride phase or silicon carbide phase generated by catalytic action becomes an appropriate amount for improving the charge / discharge performance of the composite active material. The content of transition metal elements can be measured by various quantitative analyses of element content, such as ICP mass (inductively coupled plasma mass) analysis, energy dispersive X-ray fluorescence (EDX) analysis, X-ray fluorescence (XRF) analysis, EPMA (electron probe microanalyzer) analysis, X-ray photoelectron spectroscopy (XPS), etc. The location of transition metal elements can be identified by HADDF-STEM analysis and EDX element mapping analysis.
[0020] The silicon nitride phase is an inorganic compound represented by the chemical formula SiNx (0.1≦x≦1.33), and has electrochemical reactivity with lithium ions, as well as excellent fracture toughness, high-temperature properties, and thermal shock resistance. The Si3N4 crystal is an example of the silicon nitride phase (x=1.33), and may be either the α-phase or the β-phase. The silicon nitride phase is a structure that is generated by a solid-phase reaction at high temperatures (for example, 1200°C or higher), but can be easily formed at lower temperatures due to the catalytic effect of transition metal ions. The components and crystalline state of the silicon nitride phase can be appropriately controlled by changing the type and amount of transition metal ions added, the conditions of the solid-phase reaction, and the like.
[0021] The range of x can be easily controlled by adjusting the amount of transition metal element added as a catalyst and the high-temperature reaction conditions (temperature, time, atmosphere), etc. This SiNx (0.1≦x≦1.33) can easily react with Li ions, and therefore has a certain electrochemical reaction activity. On the other hand, silicon nitride phases are widely used as gas barrier materials and have the function of blocking oxygen diffusion. In the present invention, when a silicon nitride phase is formed on the surface of silicon particles during high-temperature sintering in the production of a composite active material, the diffusion of oxygen into the inside of the silicon particles is prevented, and the oxidation reaction of silicon is effectively suppressed.
[0022] In addition, it is common for a natural oxide film to exist on silicon particles, and during high-temperature firing, transition metal ions can diffuse through the natural oxide film, causing a catalytic effect that greatly promotes the nitridation reaction of silicon. As a result, silicon nitride crystals are formed between the surface oxide film and the silicon crystals in the center of the silicon particles, blocking contact between the silicon crystals and oxygen from outside the silicon or the surrounding area, suppressing the oxidation reaction on the silicon particle surface.
[0023] Silicon carbide in the silicon carbide phase is represented by the chemical formula SiC and is a compound of carbon and silicon in a 1:1 ratio. It has properties intermediate between diamond and silicon, and has extremely excellent hardness characteristics, heat resistance, and chemical stability.
[0024] The silicon nitride phase and / or silicon carbide phase may have, for example, a film-like or particulate shape. In the present invention, there is no particular limitation on the structure of the silicon nitride phase or silicon carbide phase, and both crystalline and amorphous structures are applicable. The silicon nitride phase or silicon carbide phase may be in a crystalline or amorphous state, and the presence of the silicon nitride phase or silicon carbide phase is considered to be a solid. 29 This can be confirmed by Si-NMR spectrum. 29In a Si-NMR spectrum, peak A in the chemical shift range of 0 ppm to -20 ppm, which is assigned to a silicon carbide phase, peak B in the chemical shift range of -30 ppm to -60 ppm, which is assigned to a silicon nitride phase, and peak C in the chemical shift range of -70 ppm to -100 ppm, which is assigned to silicon, are detected, and it is preferable that the area ratio R of the above peaks calculated by the following formula (1) is in the range of 0.1 to 1.0. R = (A + B) / C ‥(1) The peaks A and B are non-zero valent Si elements such as SiO4 and SiO2, and the peak C is zero valent Si. The area ratio R of each peak calculated by formula (1) being in the above range means that the proportion of Si (zero valent) is greater than Si (non-zero valent), which indicates that oxidation is not advanced (low oxidation state) in the silicon particles constituting the composite active material for secondary batteries of the present invention. In this way, the silicon particles are in a low oxygen state, which can effectively improve the initial coulombic efficiency of the composite active material. Furthermore, it is particularly preferable that a silicon nitride phase or a silicon carbide phase is present on the surface of the silicon particles, since this increases the chemical stability of the silicon particles and improves the cycle characteristics during charging and discharging.
[0025] The silicon nitride phase and silicon carbide phase can also be measured by a Fourier transform infrared spectrophotometer (FT-IR). Specifically, when the stretching absorption peaks of the Si-N bond (900 cm-1) and the Si-C bond (800 cm-1) are detected in the FT-IR measurement results, it can be determined that the silicon nitride phase and the silicon carbide phase are formed.
[0026] Also, if the silicon nitride phase or silicon carbide phase is in a crystalline state, it can be confirmed by XRD (X-ray diffraction, CuKα light source) measurement or TEM observation. For example, when XRD measurement is performed, if X-ray diffraction peaks that match α-Si3N4 (PDF#41-0360), β-Si3N4 (PDF#33-1160), α-SiC (PDF#49-1430), and β-SiC (PDF#29-1129) are detected within the range of 2θ=10° to 80°, it is determined that various crystal structures of the silicon nitride phase or silicon carbide phase are present.
[0027] The silicon particles preferably have a peak at about 2θ=28.4° in XRD (X-ray diffraction) measurement. When this peak is detected, it is understood that Si crystals having a main crystal face (111) are present. The Si crystal has the property of being able to highly exhibit charge / discharge performance, particularly in secondary batteries, such as charge / discharge capacity and initial coulombic efficiency.
[0028] As described above, at least a part of the silicon nitride phase and silicon carbide phase is preferably present on the surface of the silicon particles. When the silicon nitride phase and silicon carbide phase are present on the surface of the silicon particles, the total thickness of the silicon nitride phase and silicon carbide phase is preferably 0.1 nm to 10 nm, more preferably 0.3 nm to 8 nm, and even more preferably 0.5 nm to 6 nm. When the thickness is within this range, the silicon particle surface can be given very excellent fracture toughness, high temperature characteristics, thermal shock resistance, and chemical stability, and the collapse of the silicon particles due to charging and discharging can be suppressed. The thickness of the silicon nitride phase and silicon carbide phase can be measured by cutting with a focused ion beam (FIB) and observing the cross section with FE-SEM, or by slicing the sample and observing the cross section of the silicon particles with TEM observation.
[0029] The average particle size of the silicon particles is preferably in the range of 10 nm to 300 nm, more preferably 30 nm to 250 nm, and further preferably 50 nm to 200 nm. When the average particle size of the silicon particles is in this range, the collapse of the silicon particles is suppressed, and the charge / discharge performance such as the capacity maintenance rate and the initial coulombic efficiency in the secondary battery tends to be maintained at a high level. In addition, in this specification, the "average particle size" is the value of D50 that can be measured using a laser diffraction particle size analyzer or the like. That is, in the particle size distribution, when a volume cumulative distribution curve is drawn from the small diameter side, the particle size at which the cumulative 50% is reached is the average particle size. The average particle size can be measured by a dynamic light scattering method using a laser particle size analyzer or the like.
[0030] The specific surface area of the silicon particles is set to 50 m from the viewpoints of charge / discharge capacity, initial coulombic efficiency, and cycle characteristics. 2 / g~400m 2 / g is preferred, and 100m 2 / g~300m 2 / g is more preferable, and 150m 2 / g~230m 2 / g is more preferable. In this specification, the "specific surface area" is a value determined by the BET method, and can be determined by nitrogen gas adsorption measurement, for example, by using a specific surface area measuring device. In addition, in order to remove organic deposits on the silicon particles, it is preferable to perform a heat treatment at 500°C for 2 hours in a nitrogen atmosphere before measuring the specific surface area.
[0031] The shape of the silicon particles may be any of granular, needle-like, and flake-like, but is preferably crystalline. When the silicon particles are crystalline, it is preferable from the viewpoint of initial coulombic efficiency and cycle characteristics that the crystallite diameter obtained from the diffraction peak attributed to Si (111) in X-ray diffraction is in the range of 5 nm to 14 nm. The crystallite diameter is more preferably 12 nm or less, and even more preferably 10 nm or less.
[0032] From the viewpoint of charge / discharge performance when used as a secondary battery, the silicon particles preferably have a length in the long axis direction of 30 nm to 300 nm and a thickness of 1 nm to 60 nm. From the viewpoint of charge / discharge performance when used as a secondary battery, a needle-like or flake-like shape with an aspect ratio, which is the ratio of thickness to length, of 0.5 or less is preferable. The shape of silicon particles can be measured by dynamic light scattering to measure the average particle size, but the aspect ratio of a sample can be more easily and precisely identified by using an analytical means such as a transmission electron microscope (TEM) or a field emission scanning electron microscope (FE-SEM). In the case of silicon particles, the sample can be cut with a focused ion beam (FIB) and the cross section can be observed with an FE-SEM, or the sample can be sliced and the state can be identified by TEM observation. The aspect ratio of silicon particles is a calculation result based on the main part of 50 particles of the sample within the field of view of the TEM image.
[0033] The above silicon particles preferably have an amorphous oxide film on their outer surface. When a silicon nitride phase and / or a silicon carbide phase exists on the surface of the silicon particles, it is preferable that an amorphous oxide film further exists on the outer surface of the silicon nitride phase and / or the silicon carbide phase. The amorphous oxide film is an amorphous oxide film, preferably an oxide film of silicon (Si), particularly preferably an SiO2 film. When such an amorphous oxide film exists, excellent fracture toughness, high-temperature characteristics, thermal shock resistance, and chemical stability can be imparted to the surface of the silicon particles as long as the charge-discharge performance (capacity, initial Coulomb efficiency) is not significantly affected, and the disintegration of the silicon particles due to charge-discharge can be suppressed. The amorphous oxide film preferably exists on at least a part of the outer surface of the silicon particles and may exist on the entire surface. The amorphous oxide film can be formed on the surface of the silicon particles by an oxidation reaction during high-temperature firing.
[0034] From the viewpoint of improving the balance of the effects (positive and negative) derived from the amorphous oxide film, the thickness of the amorphous oxide film is preferably 8 nm or less, more preferably 1 nm to 7 nm, and particularly preferably 2 nm to 6 nm. When the thickness of the amorphous oxide film is within this range, the decrease in the charge-discharge performance (capacity and initial Coulomb efficiency) of the silicon particles can be minimized, and the cycle characteristics can be improved by suppressing the disintegration of the silicon particles during charge-discharge.
[0035] The above matrix phase in the composite active material for the secondary battery of the present invention preferably contains carbon. By containing carbon in the matrix phase, the conductivity of the composite active material can be improved.
[0036] Also, it is preferable that the above matrix phase has a composition represented by SiOx (1 < x < 2). By having a composition represented by SiOx (1 < x < 2) in the matrix phase, the chemical stability of the composite active material can be improved.
[0037] The matrix phase preferably contains a silicon-based material. This silicon-based material contains silicon, carbon, and oxygen elements, and has a three-dimensional network structure of a silicon-oxygen-carbon skeleton. The silicon-based material preferably further contains carbon (carbonaceous phase). The three-dimensional network structure of a silicon-oxygen-carbon skeleton has relatively high chemical stability, and by forming a composite structure with carbon (carbonaceous phase), the volume change due to the absorption and release of lithium can be reduced. The silicon-based material may contain a nitrogen element in addition to silicon, carbon, and oxygen.
[0038] The matrix phase preferably contains a silicon oxycarbide (SiOC) structure, which can improve the chemical stability of the matrix.
[0039] The composite active material for secondary batteries preferably has a carbon layer on the surface, that is, has a carbon coating on at least a part of the surface. The carbon layer (carbon coating) is preferably a coating made of low-crystalline carbon. Unlike graphitic carbon materials, low-crystalline carbon refers to a carbon material in an amorphous state in which lattice periodic regular structures are hardly observed or only short-period structures are present in small amounts. From the viewpoint of improving chemical stability and thermal stability, the amount of the carbon layer (carbon coating) is preferably 0.1% by mass or more and 30% by mass or less, more preferably 1% by mass or more and 25% by mass or less, and even more preferably 5% by mass or more and 20% by mass or less, based on 100% by mass of the composite active material for secondary batteries. The amount of the carbon layer (carbon coating) can be measured by thermal analysis.
[0040] From the viewpoint of improving chemical stability and thermal stability, the average thickness of the carbon coating is preferably 10 nm or more and 300 nm or less. The composite active material for secondary batteries has a carbon layer (carbon coating) on a part of the surface, and from the viewpoint of improving chemical stability and thermal stability, the carbon layer (carbon coating) is preferably present on 1% or more of the surface of the composite active material, and more preferably on 10% or more. The composite active material for secondary batteries may have a carbon layer (carbon coating) on its surface continuously or discontinuously. The carbon layer (carbon coating) is preferably present on the surface of the composite active material by chemical vapor deposition.
[0041] From the viewpoint of improving the initial coulombic efficiency when used in a secondary battery, the composite active material for secondary batteries preferably further contains Li and / or Mg. The total content (molar ratio) of Li and Mg is preferably 0.5 mol% to 10.0 mol%, more preferably 1.0 mol% to 7.0 mol%, and further preferably 2.0 mol% to 6.0 mol%, based on the total Si content of the composite active material for secondary batteries. The content of Li and Mg can be measured by various quantitative analyses of element content, such as ICP mass (inductively coupled plasma mass) analysis, energy dispersive X-ray fluorescence (EDX) analysis, X-ray fluorescence (XRF) analysis, and EPMA (electron probe microanalyzer) analysis. Li and Mg are present in the composite active material for secondary batteries as metal ions (Li + and Mg 2+ ) is thought to exist.
[0042] The true density of the composite active material for secondary batteries is preferably 1.6 g / cm 3 More than 2.0g / cm 3 When the true density is within the above range, the energy density of the resulting secondary battery can be improved. 3 More preferably, 1.80 g / cm 3 The above is more preferable. The true density is a value measured using a true density measuring device.
[0043] The average particle size of the composite active material for secondary batteries is preferably 2 μm or more and 15 μm or less. If the average particle size of the composite active material for secondary batteries is 2 μm or more, a significant increase in the specific surface area can be suppressed, and when the material is used as a secondary battery, the generation of SEI during charging and discharging can be suppressed, and a decrease in the reversible charge and discharge capacity per unit volume can be suppressed. Furthermore, if the average particle size is 15 μm or less, peeling from the current collector during the preparation of the electrode film can be suppressed. The average particle size of the composite active material for secondary batteries is more preferably 2.5 μm or more, and even more preferably 3.0 μm or more. Furthermore, the average particle size of the composite active material for secondary batteries is more preferably 12 μm or less, and even more preferably 10 μm or less.
[0044] The specific surface area of the composite active material for secondary batteries is 0.3 m 2 / g or more 10m 2 / g or less. The specific surface area is preferably 0.5 m 2 / g or more is more preferable, and 1m 2 When the specific surface area is in the above range, the amount of solvent absorbed during electrode production can be kept appropriate, and the amount of binder used to maintain binding properties can also be kept appropriate.
[0045] [Method of manufacturing composite active material for secondary batteries] The method for producing a composite active material for secondary batteries of the present invention includes at least a step of wet-pulverizing raw silicon under a dispersant-added condition (wet-pulverizing step), a step of supporting a transition metal element-containing compound on the surface of the pulverized raw silicon (transition metal element supporting step), a step of uniformly mixing a polysiloxane compound, a carbon source resin, and the silicon slurry obtained in the wet-pulverizing step, and then removing the solvent and drying the mixture (homogenizing step), and a step of performing a high-temperature treatment in a non-oxidizing atmosphere at a temperature range of 900 to 1300°C (high-temperature treatment step). The homogenizing step may be performed either before or after the transition metal element supporting step. The composite active material for secondary batteries of the present invention described above is not limited to that obtained by the method for producing a composite active material for secondary batteries of the present invention.
[0046] <Wet grinding process> In the wet grinding step, the raw silicon is dispersed in a solvent such as an organic solvent to obtain a silicon slurry, which is a dispersion of the raw silicon. The silicon slurry is obtained by adjusting the raw silicon while grinding it in a wet grinding device. In this embodiment, a dispersant is added to the organic solvent to promote grinding of the raw silicon. Examples of the wet grinding device include a roller mill, a high-speed rotary grinder, a container-driven mill, and a bead mill. The preferred average particle size of the ground raw silicon in the obtained silicon slurry is the same as the average particle size of the silicon particles described in the above [Composite active material for secondary batteries].
[0047] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; alcohols such as ethanol, methanol, normal propyl alcohol, and isopropyl alcohol; and aromatics such as benzene, toluene, and xylene.
[0048] The above-mentioned dispersant can be of aqueous or non-aqueous type, and non-aqueous dispersant is preferred.The non-aqueous dispersant can be of polymer type such as polyether type, alcohol type, polyalkylene polyamine type, polycarboxylic acid partial alkyl ester type, polyhydric alcohol ester type, alkyl polyamine type, and inorganic type such as polyphosphate type.The concentration of the solid content of raw silicon in the silicon slurry is not particularly limited, but is preferably in the range of 5% by mass to 40% by mass, more preferably 10% by mass to 30% by mass, with the total amount of organic solvent, dispersant, and raw silicon being 100% by mass.
[0049] <Transition metal element supporting step> In the transition metal element supporting step, a transition metal element-containing compound is added to the silicon slurry obtained in the wet grinding step, and the mixture is stirred, and the solvent is removed and then dried. This results in a pulverized raw silicon material containing a transition metal element. The transition metal element-containing compound is preferably at least one salt of a transition metal element selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La. Examples of the salt include inorganic salt compounds such as sulfates, hydrochlorides, and carbonates, and also organic salt compounds such as anhydrous acetates and acetylacetonate ligand compounds. That is, examples of the transition metal element-containing compound include manganese chloride (II), anhydrous manganese acetate (II), manganese sulfate (II), manganese acetate (II), and manganese (II, III) acetylacetonate when the transition metal element is manganese (Mn). The metal element-containing compound may be added by dispersing it in an organic solvent (polar or non-polar).
[0050] The stirring can be performed with a stirrer equipped with stirring blades, and the stirring time is, for example, 5 minutes to 2 hours, preferably 10 minutes to 1 hour. The stirring can be performed at room temperature, or while heating to about 30 to 50°C. The solvent can be removed by a common method such as filtration. The drying can be performed with, for example, a dryer, a reduced pressure dryer, a spray dryer, or the like. The drying temperature is preferably 80°C or higher, and 120°C or lower. Drying can be performed while reducing pressure.
[0051] <Uniformization process> In the homogenization step, the matrix phase, which is a three-dimensional network structure of silicon-oxygen-carbon skeleton, is mixed with the pulverized raw material silicon to homogenize it, and then the solvent is removed and the mixture is dried to obtain a composite active material precursor. This matrix phase is formed from a polysiloxane compound and a carbon source resin.
[0052] The polysiloxane compound may be a resin containing at least one of a polycarbosilane structure, a polysilazane structure, a polysilane structure, and a polysiloxane structure. It may be a resin containing only these structures, or a composite resin having at least one of these structures as a segment and chemically bonded to other polymer segments. The form of the composite may be graft copolymerization, block copolymerization, random copolymerization, alternating copolymerization, etc. For example, a composite resin having a graft structure in which a polysiloxane segment is chemically bonded to the side chain of a polymer segment, a composite resin having a block structure in which a polysiloxane segment is chemically bonded to the end of a polymer segment, etc. may be mentioned.
[0053] In this embodiment, the polysiloxane segment is preferably a polysiloxane compound having a structural unit represented by the following general formula (S-1) and / or the following general formula (S-2): In particular, the polysiloxane compound more preferably has a carboxy group, an epoxy group, an amino group, or a polyether group on the side chain or terminal of the siloxane bond (Si-O-Si) main skeleton.
[0054] [ka]
[0055] [ka]
[0056] In the above general formulas (S-1) and (S-2), R 1 R represents an aromatic hydrocarbon group, an alkyl group, an epoxy group, a carboxy group, or the like, which may have a substituent. 2 and R 3 each independently represents an alkyl group, a cycloalkyl group, an aryl group, an aralkyl group, an epoxy group, a carboxy group, or the like.
[0057] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, a 1-ethyl-1-methylpropyl group, etc. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, etc.
[0058] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.
[0059] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.
[0060] Examples of polymer segments other than the polysiloxane segment contained in the polysiloxane compound include vinyl polymer segments such as acrylic polymers, fluoroolefin polymers, vinyl ester polymers, aromatic vinyl polymers, and olefin polymers, as well as polymer segments such as urethane polymer segments, ester polymer segments, and ether polymer segments. Among these, vinyl polymer segments are preferred.
[0061] The polysiloxane compound may be a composite resin in which a polysiloxane segment and a polymer segment are bonded in a structure represented by the following structural formula (S-3), or may have a three-dimensional network polysiloxane structure.
[0062] [ka]
[0063] In the above formula (S-3), the carbon atom is a carbon atom that constitutes a polymer segment, and the two silicon atoms are silicon atoms that constitute a polysiloxane segment.
[0064] The polysiloxane segment of the polysiloxane compound may have a functional group capable of reacting by heating, such as a polymerizable double bond, in the polysiloxane segment. By subjecting the polysiloxane compound to heat treatment before thermal decomposition, a crosslinking reaction progresses and the compound is solidified, which makes it easy to carry out the thermal decomposition treatment.
[0065] Examples of the polymerizable double bond include a vinyl group and a (meth)acryloyl group. The number of polymerizable double bonds in the polysiloxane segment is preferably 2 or more, more preferably 3 to 200, and even more preferably 3 to 50. In addition, by using a composite resin having two or more polymerizable double bonds as the polysiloxane compound, the crosslinking reaction can be easily promoted.
[0066] The polysiloxane segment may have a silanol group and / or a hydrolyzable silyl group. Examples of the hydrolyzable group in the hydrolyzable silyl group include a halogen atom, an alkoxy group, a substituted alkoxy group, an acyloxy group, a phenoxy group, a mercapto group, an amino group, an amide group, an aminooxy group, an iminoxy group, and an alkenyloxy group. The hydrolyzable silyl group becomes a silanol group by hydrolysis of these groups. In parallel with the thermosetting reaction, a hydrolysis condensation reaction proceeds between the hydroxyl group in the silanol group and the hydrolyzable group in the hydrolyzable silyl group, thereby obtaining a solid polysiloxane compound.
[0067] The silanol group in the present invention is a silicon-containing group having a hydroxyl group directly bonded to a silicon atom. The hydrolyzable silyl group in the present invention is a silicon-containing group having a hydrolyzable group directly bonded to a silicon atom, and specifically includes, for example, a group represented by the following general formula (S-4).
[0068] [ka]
[0069] In the above formula (S-4), R 4 R represents a monovalent organic group such as an alkyl group, an aryl group, or an aralkyl group. 5 is a halogen atom, an alkoxy group, an acyloxy group, an allyloxy group, a mercapto group, an amino group, an amido group, an aminooxy group, an iminoxy group or an alkenyloxy group, and b is an integer of 0 to 2.
[0070] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, and a 1-ethyl-1-methylpropyl group.
[0071] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.
[0072] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.
[0073] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0074] Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, and a tert-butoxy group.
[0075] Examples of the acyloxy group include a formyloxy group, an acetoxy group, a propanoyloxy group, a butanoyloxy group, a pivaloyloxy group, a pentanoyloxy group, a phenylacetoxy group, an acetoacetoxy group, a benzoyloxy group, and a naphthoyloxy group.
[0076] Examples of the allyloxy group include a phenyloxy group and a naphthyloxy group.
[0077] Examples of the alkenyloxy group include a vinyloxy group, an allyloxy group, a 1-propenyloxy group, an isopropenyloxy group, a 2-butenyloxy group, a 3-butenyloxy group, a 2-pentenyloxy group, a 3-methyl-3-butenyloxy group, and a 2-hexenyloxy group.
[0078] Examples of the polysiloxane segment having a structural unit represented by the above general formula (S-1) and / or the above general formula (S-2) include those having any of the structures of the following formulae (1) to (8).
[0079] [ka]
[0080] [ka]
[0081] [ka]
[0082] The polymer segment may have various functional groups as necessary within the scope of not impairing the effects of the present invention. Examples of such functional groups include a carboxyl group, a blocked carboxyl group, a carboxylic anhydride group, a tertiary amino group, a hydroxyl group, a blocked hydroxyl group, a cyclocarbonate group, an epoxy group, a carbonyl group, a primary amide group, a secondary amide group, a carbamate group, and a functional group represented by the following structural formula (S-5).
[0083] [ka]
[0084] The polymer segment may also have a polymerizable double bond such as a vinyl group or a (meth)acryloyl group.
[0085] The polysiloxane compound is preferably produced, for example, by the following methods (1) to (3).
[0086] (1) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment, and this polymer segment is mixed with a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond to carry out a hydrolysis condensation reaction.
[0087] (2) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment. A polysiloxane is also prepared in advance by subjecting a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond to a hydrolysis and condensation reaction. The polymer segment and the polysiloxane are then mixed together to carry out a hydrolysis and condensation reaction.
[0088] (3) A method of mixing a polymer segment, a silane compound having a silanol group and / or a hydrolyzable silyl group, and a polymerizable double bond, and a polysiloxane, and carrying out a hydrolysis condensation reaction, which produces a polysiloxane compound.
[0089] Examples of polysiloxane compounds include the Ceranate (registered trademark) series (organic / inorganic hybrid coating resin; manufactured by DIC Corporation) and the Compoceran SQ series (silsesquioxane hybrid; manufactured by Arakawa Chemical Industries, Ltd.).
[0090] The carbon source resin has good miscibility with polysiloxane compounds, and is carbonized by high-temperature baking in an inert non-oxidizing atmosphere, and can be used as the carbon material in the present invention. The carbon source resin or the resin contained in the carbon source resin composition is not particularly limited, and may include a molecular structure having a benzene ring or an aromatic functional group. Examples of the resin include thermosetting resins; thermoplastic resins; petroleum-based or coal-based tar or pitch, such as petroleum-based tar or pitch by-produced during ethylene production, coal tar produced during coal dry distillation, heavy components or pitch obtained by distilling and removing low-boiling components of coal tar, and tar or pitch obtained by liquefying coal; and further, the above tar or pitch that has been crosslinked; and the like. One or more of these can be used in combination.
[0091] The thermosetting resin is not particularly limited, and examples thereof include phenolic resins such as novolac-type phenolic resins and resol-type phenolic resins; epoxy resins such as bisphenol-type epoxy resins and novolac-type epoxy resins; melamine resins; urea resins; aniline resins; cyanate resins; furan resins; ketone resins; unsaturated polyester resins; and urethane resins. Modified versions of these resins modified with various components can also be used. When using a thermosetting resin, a curing agent for the resin can be used in combination.
[0092] Furthermore, the thermoplastic resin is not particularly limited, and examples thereof include polyethylene, polystyrene, polyacrylonitrile, acrylonitrile-styrene (AS) resin, acrylonitrile-butadiene-styrene (ABS) resin, polypropylene, vinyl chloride, methacrylic resin, polyethylene terephthalate, polyamide, polycarbonate, polyacetal, polyphenylene ether, polybutylene terephthalate, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyetherimide, polyamideimide, polyimide, and polyphthalamide.
[0093] The resin or resin composition used as the raw material of the carbon material in the present invention preferably contains nitrogen-containing resins as the main resin component from the viewpoint of promoting the formation of silicon nitride. By carbonizing such a resin, the catalytic action of transition metal ions on the formation of nitrogen compounds is enhanced, and a carbon material containing nitrogen can also be obtained. When nitrogen is contained in carbon, the electronegativity of nitrogen can impart suitable electrical properties to the carbon (carbon material for lithium ion secondary batteries). This can promote the absorption and release of lithium ions and impart high charge and discharge properties.
[0094] Examples of the nitrogen-containing resins include the following: Thermosetting resins include melamine resins, urea resins, aniline resins, cyanate resins, urethane resins, as well as phenolic resins and epoxy resins modified with nitrogen-containing components such as amines.
[0095] Furthermore, when a nitrogen-containing compound is used as a component other than the main component resin, the type of the compound is not particularly limited. For example, hexamethylenetetramine, which is a curing agent for novolac-type phenolic resin, aliphatic polyamines, aromatic polyamines, dicyandiamide, and the like, which are curing agents for epoxy resins, as well as nitrogen-containing compounds such as amine compounds, ammonium salts, nitrates, and nitro compounds that do not function as curing agents, can be used in addition to the curing agent components.
[0096] The nitrogen-containing compound may be used alone or in combination of two or more kinds, whether or not the main component resin contains nitrogen-containing resins. The method for preparing the resin composition used as the raw material of the carbon material in the present invention is not particularly limited. For example, the above-mentioned main component resin and other components are blended in a predetermined ratio, and these components are dissolved in a solvent and mixed. Alternatively, the precursor of the composite active material of the present invention can be prepared by mixing these components with the above-mentioned silicon slurry.
[0097] <High temperature treatment process> In the high-temperature treatment step, the precursor of the composite active material after drying in the homogenization step is fired in a non-oxidizing atmosphere. The apparatus used for the high-temperature treatment can be appropriately selected from among a fluidized bed reactor, a rotary furnace, a vertical moving bed reactor, a tunnel furnace, a batch furnace, a rotary kiln, and the like, depending on the purpose. The high-temperature treatment is carried out according to a firing program that is defined by the heating rate, the holding time at a constant temperature, and the like. The firing temperature is preferably, for example, in the range of 900°C to 1300°C, with the maximum reaching temperature. This allows the composite active material for secondary batteries of the present invention to be obtained.
[0098] The non-oxidizing atmosphere during the high-temperature firing means an atmosphere with an oxygen concentration of 100 ppm or less. There is no particular limitation on the type of gas used as the non-oxidizing atmosphere, and examples include nitrogen, argon, hydrogen, and nitrogen-hydrogen mixed gas. Among these, the use of nitrogen gas is preferred from the viewpoint of promoting the formation of the silicon nitride phase.
[0099] Furthermore, the sintered product obtained in the high-temperature treatment step is pulverized and classified as necessary to obtain a composite active material with a desired particle size. The pulverization may be performed in one step or in several steps until the composite active material has a desired particle size. If the composite active material after sintering is a mass or aggregate having a particle size of 10 mm or more, the composite active material may be coarsely pulverized using a jaw crusher, roll crusher, etc., and then pulverized using a glow mill, ball mill, etc., and further pulverized using a bead mill, jet mill, etc. The particle size is the average particle size and is the D50 value.
[0100] In addition, when the composite active material produced by pulverization contains coarse particles, it is preferable to perform classification in order to remove the coarse particles and adjust the particle size distribution by removing fine powders. The classifier used may be an air classifier, a wet classifier, or the like, depending on the purpose, but when removing coarse particles, a classification method that passes through a sieve is preferable because it can reliably achieve the purpose.
[0101] When the composite active material for secondary batteries further has carbon (carbon coating) on the surface, the obtained composite active material is coated with a carbon coating in a chemical vapor deposition apparatus in a flow of a pyrolytic carbon source gas and a carrier inert gas at a temperature range of 700°C to 1000°C. Examples of pyrolytic carbon source gases include acetylene, ethylene, acetone, alcohol, propane, methane, and ethane. Examples of inert gases include nitrogen, helium, and argon, and nitrogen is usually used.
[0102] [Secondary battery] The secondary battery of the present invention is characterized in that it contains the composite active material for secondary batteries of the present invention in the negative electrode. The secondary battery of the present invention is not particularly limited as long as it contains the composite active material for secondary batteries in the negative electrode, but may also contain other components such as an organic binder and a conductive assistant.
[0103] The secondary battery of the present invention can be produced by applying a slurry containing an organic binder and, if necessary, other components such as a conductive assistant, in the form of a thin film onto a copper foil current collector. A carbon material such as graphite can also be added to the slurry to produce a negative electrode. Examples of the carbon material include natural graphite, artificial graphite, and amorphous carbon such as hard carbon or soft carbon.
[0104] For example, the negative electrode material can be obtained by kneading the composite active material for secondary batteries and the binder, which is an organic binding material, together with a solvent using a dispersing device such as a stirrer, a ball mill, a super sand mill, or a pressure kneader to prepare a negative electrode material slurry, which is then applied to a current collector to form a negative electrode layer. Alternatively, the negative electrode material can be obtained by forming the paste-like negative electrode material slurry into a sheet, pellet, or other shape and integrating it with a current collector.
[0105] Examples of the organic binder include styrene-butadiene rubber copolymers (hereinafter also referred to as "SBR"); ethylenically unsaturated carboxylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, (meth)acrylonitrile, and hydroxyethyl (meth)acrylate, and unsaturated carboxylic acid copolymers such as (meth)acrylic copolymers composed of ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; and polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamideimide, and carboxymethylcellulose (hereinafter also referred to as "CMC").
[0106] Depending on their physical properties, these organic binders may be dispersed or dissolved in water, or dissolved in an organic solvent such as N-methyl-2-pyrrolidone (NMP), etc. The content of the organic binder in the negative electrode layer of the secondary battery is preferably 1% by mass to 30% by mass, more preferably 2% by mass to 20% by mass, and even more preferably 3% by mass to 15% by mass.
[0107] When the content of the organic binder is 1% by mass or more, the adhesion is better and the destruction of the negative electrode structure due to the expansion and contraction during charging and discharging is more suppressed, whereas when the content of the organic binder is 30% by mass or less, the increase in the electrode resistance is more suppressed.
[0108] In addition, the negative electrode material slurry may be mixed with a conductive assistant as necessary. Examples of the conductive assistant include carbon black, graphite, acetylene black, and oxides and nitrides that exhibit conductivity. The amount of the conductive assistant used may be, for example, 1% by mass to 15% by mass with respect to the composite active material of the present invention.
[0109] The material and shape of the current collector may be, for example, a strip of copper, nickel, titanium, stainless steel, etc. in the form of foil, perforated foil, mesh, etc. Also, porous materials such as porous metal (foamed metal) and carbon paper can be used.
[0110] Examples of methods for applying the negative electrode material slurry to the current collector include metal mask printing, electrostatic coating, dip coating, spray coating, roll coating, doctor blade, gravure coating, screen printing, etc. After application, it is preferable to perform rolling treatment using a flat plate press, a calendar roll, etc. as necessary.
[0111] The negative electrode material slurry may be formed into a sheet or pellet shape, and this may be integrated with a current collector by, for example, rolling, pressing, or a combination of these.
[0112] The negative electrode layer formed on the current collector or the negative electrode layer integrated with the current collector is preferably heat-treated according to the organic binder used. The temperature of the heat treatment is not particularly limited, but for example, when a water-based styrene-butadiene rubber copolymer (SBR) or the like is used, the heat treatment may be performed at 100 to 130°C, and when an organic binder having a polyimide or polyamideimide as the main skeleton is used, the heat treatment is preferably performed at 150 to 450°C.
[0113] This heat treatment removes the solvent, hardens the binder, and increases the strength, improving the adhesion between the particles and between the particles and the current collector. It is preferable to carry out these heat treatments in an inert atmosphere such as helium, argon, or nitrogen, or in a vacuum atmosphere, in order to prevent oxidation of the current collector during the treatment.
[0114] In addition, it is preferable to subject the negative electrode to pressure treatment after the heat treatment. 3 from 1.8 g / cm 3 and preferably 1.1 g / cm 3 to 1.7 g / cm 3More preferably, it is 1.2 g / cm 3 from 1.6 g / cm 3 It is more preferable that the electrode density is higher. The higher the electrode density, the more the adhesion and the volumetric capacity density of the electrode tend to improve. On the other hand, if the electrode density is too high, the voids in the electrode are reduced, which weakens the effect of suppressing the volumetric expansion of silicon and the like, and the capacity retention rate may decrease. Therefore, the optimum range of the electrode density is selected.
[0115] The secondary battery of the present invention includes the composite active material for secondary batteries of the present invention. As the secondary battery including the composite active material for secondary batteries, non-aqueous electrolyte secondary batteries and solid electrolyte secondary batteries are preferred, and the composite active material for secondary batteries exhibits excellent performance particularly when used as the negative electrode of the non-aqueous electrolyte secondary battery.
[0116] When the secondary battery of the present invention is used as a wet electrolyte secondary battery, for example, the secondary battery can be constructed by disposing a positive electrode and a negative electrode containing the composite active material for a secondary battery of the present invention opposite each other with a separator interposed therebetween and injecting an electrolytic solution.
[0117] The positive electrode can be obtained by forming a positive electrode layer on the surface of a current collector in the same manner as the negative electrode. In this case, the current collector can be a strip of a metal or alloy such as aluminum, titanium, or stainless steel in the form of a foil, a perforated foil, a mesh, or the like.
[0118] There are no particular limitations on the positive electrode material used in the positive electrode layer. When preparing a lithium ion secondary battery among non-aqueous electrolyte secondary batteries, for example, a metal compound, metal oxide, metal sulfide, or conductive polymer material capable of doping or intercalating lithium ions may be used. For example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), and composite oxides thereof (LiCoxNiyMnzO2, x+y+z=1), lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13, VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (wherein M is Co, Ni, Mn, or Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene, porous carbon, etc. can be used alone or in combination.
[0119] As the separator, for example, a nonwoven fabric, cloth, microporous film, or a combination thereof, mainly composed of polyolefin such as polyethylene or polypropylene can be used. Note that if the positive electrode and the negative electrode of the nonaqueous electrolyte secondary battery to be produced are not in direct contact with each other, there is no need to use a separator.
[0120] As the electrolyte, for example, a so-called organic electrolyte can be used in which a lithium salt such as LiClO4, LiPF6, LiAsF6, LiBF4, or LiSO3CF3 is dissolved in a non-aqueous solvent such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, or ethyl acetate, or a mixture of two or more components.
[0121] The structure of the secondary battery of the present invention is not particularly limited, but usually, the positive electrode, the negative electrode, and a separator provided as necessary are wound into a flat spiral shape to form a wound electrode plate group, or these are stacked in a flat plate shape to form a stacked electrode plate group, and these electrode plate groups are generally sealed in an exterior body. Note that the half cell used in the examples described below has a negative electrode mainly composed of the composite active material for secondary batteries of the present invention, and a simplified evaluation was performed using metallic lithium as the counter electrode, but this is for the purpose of more clearly comparing the cycle characteristics of the active material itself.
[0122] The secondary battery of the present invention is not particularly limited, and can be used as a paper-type battery, a button-type battery, a coin-type battery, a laminated battery, a cylindrical battery, a square battery, etc. The above-mentioned composite active material for a secondary battery of the present invention can also be applied to general electrochemical devices that use insertion and desorption of lithium ions as a charge / discharge mechanism, such as hybrid capacitors and solid lithium secondary batteries. EXAMPLES
[0123] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the present examples, [%] and [parts] represent "mass%" and "mass parts" unless otherwise specified. Silicon slurries, polysiloxane compounds, and curable resin compositions were prepared by the following methods, and the composite active materials for secondary batteries of Examples 1 to 20 and Comparative Examples 1 and 2 were produced using these, and secondary battery evaluations were also performed.
[0124] "Synthesis Example 1: Preparation of silicon slurry (Si1-Si5)" Zirconia beads (particle size range: 0.1 mm to 0.2 mm) and 100 ml of methyl ethyl ketone solvent (MEK) were placed in a container (150 ml) of a small bead mill device at a filling rate of 60%, and then raw silicon (average particle size 5 μm) and cationic dispersant liquid (BYK Japan Co., Ltd., BYK145) were added as shown in Table 1 below, and wet grinding was performed using a bead mill under each of the conditions shown in Table 1 below to obtain dark brown liquid silicon slurry (solid concentration 30 mass%; Si1 to Si5). The average particle size (D50) of the raw silicon after crushing was measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000), and the D50 of the raw silicon after crushing was confirmed by TEM observation. The average particle size (D50) of the raw silicon after crushing is shown in Table 1.
[0125] [Table 1]
[0126] "Synthesis Example 2: Preparation of polysiloxane compound (synthesis of methyltrimethoxysilane condensation product)" First, 1,421 parts of methyltrimethoxysilane (hereinafter referred to as MTMS) was charged into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, and the temperature was raised to 60°C. Next, a mixture of 0.17 parts of iso-propyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 207 parts of deionized water was dropped into the reaction vessel over 5 minutes, and then the mixture was stirred at a temperature of 80°C for 4 hours to cause a hydrolysis condensation reaction. The condensate obtained by this hydrolysis condensation reaction was distilled at a temperature of 40 to 60°C and a reduced pressure of 40 to 1.3 kPa (referring to a condition in which the reduced pressure condition at the start of distillation of methanol is 40 kPa, and the pressure is reduced to 1.3 kPa at the end), and methanol and water generated during the reaction were removed, thereby obtaining 1,000 parts by mass of a liquid (active ingredient 70% by mass) containing a condensate of MTMS having a number average molecular weight of 1,000 to 5,000. The active ingredient is calculated by dividing the theoretical yield (parts by mass) when all the methoxy groups of a silane monomer such as MTMS undergo a condensation reaction by the actual yield (parts by mass) after the condensation reaction (theoretical yield (parts by mass) when all the methoxy groups of a silane monomer undergo a condensation reaction / actual yield (parts by mass) after the condensation reaction).
[0127] (Production of Curable Resin Composition (1)) First, 150 parts by mass of butanol (hereinafter referred to as BuOH), 105 parts by mass of polytetramethoxysilane (hereinafter referred to as PTMS), and 277 parts by mass of dimethoxydimethylsilane (hereinafter referred to as DMDMS) were placed in a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, and the temperature was raised to 80°C. Next, at the same temperature, a mixture containing 21 parts by mass of methyl methacrylate (hereinafter referred to as MMA), 4 parts by mass of butyl methacrylate (hereinafter referred to as BMA), 3 parts by mass of butyl acrylate (hereinafter referred to as BA), 2 parts by mass of (3-mercaptopropyl)triethoxysilane (hereinafter referred to as MPTS), 3 parts by mass of BuOH, and 0.6 parts by mass of tert-butylperoxy-2-ethylhexanoate (hereinafter referred to as TBPEH) was added dropwise into the reaction vessel over 6 hours, and after completion of the addition, the mixture was allowed to react at the same temperature for a further 20 hours to obtain an organic solvent solution of a vinyl polymer (a2-1) having a number average molecular weight of 10,000 and having a hydrolyzable silyl group. Next, a mixture of 0.04 parts by mass of Phoslex A-3 and 112 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis and condensation reaction, thereby obtaining a liquid containing a composite resin in which the hydrolyzable silyl group of the vinyl polymer (a2-1) was bonded to the hydrolyzable silyl group and silanol group of the polysiloxane derived from the above-mentioned PTMS and DMDMS. To this liquid were added 472 parts by mass of the MTMS condensate (a1) obtained in Synthesis Example 2 and 80 parts by mass of deionized water, and the mixture was stirred at the same temperature for 10 hours to cause a hydrolysis and condensation reaction. The mixture was distilled under the same conditions as in Synthesis Example 2 to remove the produced methanol and water, and then 250 parts by mass of BuOH was added to obtain 1,000 parts by mass of a curable resin composition (1) having a non-volatile content of 60.1% by mass.
[0128] (Production of Curable Resin Composition (2)) First, 150 parts by mass of BuOH, 249 parts by mass of PTMS, and 263 parts by mass of DMDMS were placed in a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet, and the temperature was raised to 80°C. Next, at the same temperature, a mixture containing 18 parts by mass of MMA, 14 parts by mass of BMA, 7 parts by mass of BA, 1 part by mass of acrylic acid (AA), 2 parts by mass of MPTS, 6 parts by mass of BuOH, and 0.9 parts by mass of TBPEH was added dropwise into the reaction vessel over 5 hours, and after completion of the addition, the mixture was allowed to react at the same temperature for a further 10 hours to obtain an organic solvent solution of a vinyl polymer (a2-2) having a hydrolyzable silyl group and a number average molecular weight of 20,100. Next, a mixture of 0.05 parts by mass of Phoslex A-3 and 147 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis and condensation reaction, thereby obtaining a liquid containing a composite resin in which the hydrolyzable silyl group of the vinyl polymer (a2-2) was bonded to the hydrolyzable silyl group and silanol group of the polysiloxane derived from PTMS and DMDMS. Next, 76 parts by mass of 3-glycidoxypropyltrimethoxysilane, 231 parts by mass of the MTMS condensate (a1) obtained in Synthesis Example 2, and 56 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 15 hours to cause a hydrolysis and condensation reaction. The mixture was distilled under the same conditions as in Synthesis Example 1 to remove the produced methanol and water, and then 250 parts by mass of BuOH was added to obtain 1,000 parts by mass of a curable resin composition (2) having a non-volatile content of 60.0% by mass.
[0129] Example 1 To 100g of silicon slurry (Si2 in Synthesis Example 1, average particle size D50 = 100nm, Si content = 16.7% by mass), an appropriate amount of manganese (III) acetylacetonate solution (concentration 5% by mass; solvent ethanol) was added in accordance with Mn / Si (molar ratio) = 0.005 / 100, and the mixture was stirred at room temperature for 1 hour. The polysiloxane compound (curable resin composition (1): average molecular weight 3500) and phenolic resin (average molecular weight 3000) prepared in Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 50 / 20 / 30, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature in a nitrogen atmosphere at 1100 ° C for 2 hours, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. The Fourier transform infrared spectrophotometer (FT-IR) measurement results showed that the Si-N bond (900 cm -1 ) and Si-C (800cm -1 ) bond stretching absorption peak was detected. TEM observation of the cross section of the FIB-processed composite active material particle revealed a structure that appeared to be a SiNx / SiC crystal on the silicon particle surface. HADDF-STEM images and elemental EDS mapping images confirmed that Mn elements were detected around the Si particles, and that a large amount of N elements was distributed around the area where Mn elements were present (Figure 1).
[0130] A slurry was prepared by mixing 80 parts by mass of the composite active material powder obtained above with 10 parts by mass of acetylene black as a conductive assistant and 10 parts by mass of a mixture of CMC and SBR as a binder. The obtained slurry was formed into a film on a copper foil. After drying under reduced pressure at 110°C, a coin-type lithium-ion battery was fabricated as a half cell with Li metal foil as the counter electrode. The charge and discharge characteristics of the fabricated half cell were evaluated at 25°C using a secondary battery charge and discharge tester (manufactured by Hokuto Co., Ltd.). The cutoff voltage range was 0.005 to 1.5 V. The charge and discharge measurement results showed that the initial charge / discharge capacity was 1953 mAhg -1 / 1650mAhg -1 The initial coulombic efficiency was 84.5%. For the evaluation of the full cell, a positive electrode film was prepared using a single-layer sheet of LiCoO2 as the positive electrode active material and aluminum foil as the current collector, and a negative electrode film was prepared by mixing graphite powder and active material powder with a discharge capacity design value of 450mAh / g. A non-aqueous electrolyte solution in which lithium hexafluorophosphate was dissolved at a concentration of 1mol / L in a 1 / 1 (volume ratio) mixture of ethylene carbonate and diethyl carbonate was used as the non-aqueous electrolyte, and a coin-type lithium ion secondary battery was prepared using a 30μm-thick polyethylene microporous film as the separator. The laminated lithium ion secondary battery was charged at a constant current of 1.2mA (0.25c based on the positive electrode) at room temperature until the voltage of the test cell reached 4.2V, and after reaching 4.2V, the current was reduced to keep the cell voltage at 4.2V and charging was performed, and the discharge capacity was calculated. The capacity retention rate after 100 cycles at 45° C. was 86% (see Table 2 below).
[0131] Examples 2 to 6 To 100 g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100 nm, Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (concentration 5 mass%; solvent ethanol) was added in accordance with the Mn / Si (molar ratio) of 0.05 / 100 (Example 2); 0.5 / 100 (Example 3); 1.0 / 100 (Example 4); 2.0 / 100 (Example 5); 5.7 / 100 (Example 6), respectively, and the mixture was stirred at room temperature for 1 hour. The other operations were carried out under the same conditions as in Example 1. The obtained analysis results and the results of the charge / discharge evaluation of the half cell are shown in Table 2.
[0132] Examples 7 to 10 100 g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100 nm, Si content = 16.7 mass%) was added to an appropriate amount of manganese (III) acetylacetonate solution (concentration 5 mass%; solvent ethanol) with a Mn / Si (molar ratio) adjusted to 0.5 / 100, and various metal ion solutions (Fe 3+ , Ni + , Cu 2+ ,La 3+ ) was added under the conditions described below, and the mixture was stirred at room temperature for 1 hour. Example 7: Mn / Si (molar ratio) = 0.5 / 100 (using manganese (III) acetylacetonate solution); Fe / Si (molar ratio) = 0.1 / 100 (using iron (II) acetate anhydride solution, solvent ethanol) Example 8: Mn / Si (molar ratio) = 0.5 / 100 (using manganese (III) acetylacetonate solution); Ni / Si (molar ratio) = 0.1 / 100 (using nickel acetate anhydride solution, solvent: methanol) Example 9: Mn / Si (molar ratio) = 0.5 / 100 (using manganese (III) acetylacetonate solution); Cu / Si (molar ratio) = 0.1 / 100 (using copper (II) acetate anhydride solution, solvent ethanol) Example 10: Mn / Si (molar ratio) = 0.5 / 100 (using manganese (III) acetylacetonate solution); La / Si (molar ratio) = 0.1 / 100 (using lanthanum (III) acetate anhydride solution, solvent ethanol) Other operations were carried out under the same conditions as in Example 1. The obtained analytical results and the results of the charge / discharge evaluation of the half-cell are shown in Table 2.
[0133] Example 11 To 100g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100nm, Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) was added according to Mn / Si (molar ratio) = 0.2 / 100, and the mixture was stirred at room temperature for 1 hour. The polysiloxane compound (curable resin composition (1): average molecular weight 3500) and phenolic resin (average molecular weight 3000) prepared as in Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 50 / 10 / 40, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature in a nitrogen atmosphere at 1100 ° C for 2 hours, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. Then, 25g of the above sample powder was placed in the reaction vessel of a chemical vapor deposition apparatus (CVD, disk rotary kiln, Takasago Industrial Co., Ltd.) and carbon coating was performed under the conditions of 850℃ / 1 hour in a mixed gas flow of acetylene (flow rate: 0.3L / min) and nitrogen (flow rate: 0.7L / min). According to the thermal analysis results, the amount of carbon coating was 2 mass% relative to 100 mass% of the composite active material. Various evaluation results are shown in Table 2.
[0134] Example 12 To 100 g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100 nm, Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) was added according to Mn / Si (molar ratio) = 0.2 / 100, and the mixture was stirred at room temperature for 1 hour. The polysiloxane compound (curable resin composition (2): average molecular weight 3500) and phenolic resin (average molecular weight 3000) prepared as in Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 50 / 2 / 48, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature under conditions of 1100 ° C for 2 hours in a nitrogen atmosphere, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. The results of various evaluations are shown in Table 2.
[0135] Example 13 To 100 g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100 nm, Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) was added according to Mn / Si (molar ratio) = 0.2 / 100, and the mixture was stirred at room temperature for 1 hour. After that, methyl polysilicate silane (M silicate 51, Tama Chemical Industry Co., Ltd.) was added to the product after high-temperature firing so that the composition mass ratio Si / SiOx / C = 50 / 10 / 40 was obtained, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature under conditions of 1100 ° C for 2 hours in a nitrogen atmosphere, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. The results of various evaluations are shown in Table 2.
[0136] Example 14 To 100 g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100 nm, Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) was added according to Mn / Si (molar ratio) = 0.2 / 100, and the mixture was stirred at room temperature for 1 hour. The polysiloxane compound (curable resin composition (2): average molecular weight 3500) and phenolic resin (average molecular weight 3000) prepared as in Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 40 / 30 / 30, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature under conditions of 1100 ° C for 2 hours in a nitrogen atmosphere, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. The results of various evaluations are shown in Table 2.
[0137] Examples 15-16 100g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100nm, Si content = 16.7 mass%) was added with an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) according to Mn / Si (molar ratio) = 0.2 / 100, and further added lithium ion compound and magnesium ion compound under the following conditions, and stirred at room temperature for 1 hour. The polysiloxane compound (curable resin composition (1): average molecular weight 3500) and phenolic resin (average molecular weight 3000) of Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 50 / 10 / 40, and after thorough mixing in a stirrer, it was dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature in a nitrogen atmosphere under conditions of 1100 ° C for 2 hours, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. Various evaluation results are shown in Table 2. Example 15: Li / Si molar ratio = 0.1, lithium acetate anhydride (10% by mass, solvent: ethanol) Example 16: Mg / Si molar ratio = 0.1, anhydrous magnesium acetate (10% by mass, solvent: ethanol)
[0138] Examples 17 to 20 100g of silicon slurry (Example 17: Synthesis Example 1 Si5 / average particle size D50 = 15nm; Example 18: Synthesis Example 1 Si1 / average particle size D50 = 57nm; Example 19: Synthesis Example 1 Si3 / average particle size D50 = 250nm; Example 20: Synthesis Example 1 Si4 / average particle size D50 = 400nm) was added with an appropriate amount of manganese (III) acetylacetonate solution (5 mass%; solvent ethanol) adjusted to Mn / Si (molar ratio) = 0.2 / 100, and stirred at room temperature for 1 hour. Then, the polysiloxane compound (curable resin composition (1): average molecular weight 3500) and phenol resin (average molecular weight 3000) prepared as in Synthesis Example 2 above were added to the product after high-temperature firing so that the composition mass ratio Si / SiOC / C = 50 / 10 / 40, and the mixture was thoroughly mixed in a stirrer and then dried under reduced pressure at 110°C. The dried material was sintered at high temperature in a nitrogen atmosphere at 1100℃ for 2 hours, and then crushed and classified (average particle size D50 = about 5μm) to obtain a powder of the composite active material.
[0139] Comparative Example 1 100g of silicon slurry (Si2 of Synthesis Example 1, average particle size D50 = 100nm, Si content = 16.7 mass%), polysiloxane compound of Synthesis Example 2 (curable resin composition (1): average molecular weight 3500) and phenolic resin (average molecular weight 3000) were mixed so that the composition mass ratio in the product after high-temperature firing was Si / SiOC / C = 50 / 10 / 40, and after thorough stirring, dried under reduced pressure at 110 ° C. The dried product was fired at a high temperature under conditions of 1100 ° C for 2 hours in a nitrogen atmosphere, and then crushed and classified (average particle size D50 = about 5 μm) to obtain a powder of a composite active material. The measurement results of a Fourier transform infrared spectrophotometer (FT-IR) did not detect the stretching absorption peaks of Si-N bond (900 cm-1) and Si-C (800 cm-1) bond. TEM observation of the cross section of the composite active material particle processed by FIB showed that no structure that could be considered to be a SiNx / SiC crystal was observed on the silicon particle surface. Other operations were carried out under the same conditions as in Example 1, and the results of various evaluations are shown in Table 2.
[0140] Comparative Example 2 Commercially available nanosilicon particles (average particle size 100 nm or less, manufactured by Sigma-Aldrich), a polysiloxane compound (curable resin composition (1): average molecular weight 3500), and a phenolic resin (average molecular weight 3000) were mixed so that the product after high-temperature sintering would have a composition mass ratio of Si / SiOC / C = 50 / 10 / 40, and after thorough stirring, the product was dried under reduced pressure at 110°C. The dried product was sintered at high temperature under conditions of 1100°C for 2 hours in a nitrogen atmosphere, and then crushed and classified (average particle size D50 = approximately 5 μm) to obtain a powder of a composite active material. Measurement results using a Fourier transform infrared spectrophotometer (FT-IR) showed that the Si-N bond (900 cm -1 ) and Si-C (800cm -1 The other operations were carried out under the same conditions as in Example 1, and the results of the various evaluations are shown in Table 2.
[0141] [Table 2]
[0142] From Table 2 above, it can be seen that the composite active material for secondary batteries of the present invention (Examples 1 to 20) has a higher capacity retention rate and initial (coulombic) efficiency when used in a secondary battery than the composite active material not containing a transition metal element (Comparative Examples 1 and 2). Therefore, it was shown that the composite active material for secondary batteries of the present invention can improve the chemical durability of the silicon particle surface and can maintain high charge / discharge performance such as the capacity retention rate and initial coulombic efficiency in a secondary battery.
[0143] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2022-178741) filed on November 8, 2022, the contents of which are incorporated herein by reference.
Claims
1. The silicon oxide film has silicon particles, a silicon nitride phase and / or a silicon carbide phase, and a matrix phase containing the silicon particles, The matrix phase comprises carbon, The composite active material for a secondary battery contains a transition metal element in at least one phase selected from the group consisting of the silicon nitride phase, the silicon carbide phase, and the matrix phase.
2. 2. The composite active material for a secondary battery in accordance with claim 1, wherein at least a part of the silicon nitride phase and / or silicon carbide phase is present on the surface of the silicon particles.
3. 2. The composite active material for a secondary battery according to claim 1, wherein a higher concentration of the silicon nitride phase and / or the silicon carbide phase is contained on or in the vicinity of the surface of the silicon particles than in the matrix phase.
4. The composite active material for secondary batteries according to any one of claims 1 to 3, wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La.
5. 4. The composite active material for a secondary battery according to claim 1, wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cu, and La.
6. 4. The composite active material for a secondary battery according to claim 1, wherein the content of the transition metal element is 0.01 atm % to 5 atm % based on the total amount of silicon present in the silicon particles.
7. 4. The composite active material for a secondary battery according to claim 1, wherein the matrix phase has a composition represented by SiOx (1<x<2).
8. 4. The composite active material for a secondary battery according to claim 1, wherein the matrix phase comprises silicon oxycarbide.
9. 4. The composite active material for a secondary battery according to claim 1, wherein the silicon particles have an average particle size in the range of 10 nm to 300 nm.
10. 4. The composite active material for a secondary battery according to claim 1, wherein the transition metal element is in the range of 0.001 atm % to 5 atm % based on the total amount of silicon.
11. 4. The composite active material for a secondary battery according to claim 1, wherein a carbon layer is present on a surface thereof.
12. 4. The composite active material for a secondary battery according to claim 1, further comprising Li and / or Mg.
13. A secondary battery comprising the composite active material for secondary batteries according to any one of claims 1 to 3 in a negative electrode.