Tabernacle Method and Tabernacle Device
The film deposition method using a PECVD device with protective insulating films addresses the issue of constrictions in carbon-based films on semiconductor patterns, ensuring film integrity and shape transfer precision.
Patent Information
- Application Number
- KR1020267034032
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-27
- Filing Date
- 2025-02-21
- Publication Date
- 2026-11-10
AI Technical Summary
Existing methods for forming a carbon-based film on the top of a pattern in semiconductor devices often result in constrictions, which can lead to unintended consumption of the film during etching and hinder the transfer of desired shapes.
A film deposition method involving a PECVD device that includes a first film deposition process to form a carbon-based film vertically on a pattern, followed by a second process to deposit a protective insulating film, and a third process to further deposit the carbon-based film, with the protective film preventing etching by hydrogen active species and controlling ion energy through high-frequency power and impedance adjustment.
The method effectively suppresses the occurrence of constrictions in the carbon-based film, ensuring its integrity and enabling precise transfer of shapes during etching processes.
Smart Images

Figure PCT00014_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a tabernacle method and a tabernacle apparatus. Background Technology
[0002] In semiconductor devices, a technique is known for selectively forming a carbon-based film on the top of a pattern, such as a trench or hole, formed in a mask or an etching target film to realize more complex or fine wiring shapes. For example, in the technique described in Patent Document 1, a carbon-based film is formed on the top of a trench formed in a substrate containing silicon. Specifically, in the substrate, a fluid film, which is an amorphous carbon polymer film, is deposited mainly at the bottom of the trench, and then the fluid film at the bottom is exposed to nitrogen plasma to etch the fluid film at the bottom, and gaseous C from the fluid film x N y H z Forms a species. At this time, C regarding the fluid membrane at the bottom x N y H z C for the top of the trench where silicone is exposed, compared to the bond coefficient of the species x N y H z Because the attachment coefficient of the species is high, C x N y H z Paper is selectively redeposited at the crest of the trench. As a result, a carbonaceous film is selectively formed at the crest of the trench. Prior art literature
[0003] Japanese Patent Publication No. 2021-19199 The problem to be solved
[0004] The technology of the present disclosure suppresses the occurrence of constrictions in the first film when the first film is formed selectively and vertically on the top of the pattern. means of solving the problem
[0005] One aspect of the technology according to the present disclosure is a film deposition method comprising: housing a substrate having a pattern inside a processing chamber; generating plasma from a film deposition gas using high-frequency power to perform a film deposition treatment on said substrate, the method comprising: a first film deposition process for selectively and perpendicularly depositing a first film on the top portion of said pattern; a second film deposition process for depositing a second film covering said first film; and a third film deposition process for perpendicularly depositing the first film again after said second film is deposited. Effects of the invention
[0006] According to the technology of the present disclosure, when a first film is formed selectively and vertically on the top of a pattern, the occurrence of a constriction in the first film can be suppressed. Brief explanation of the drawing
[0007] FIG. 1 is a cross-sectional view schematically illustrating an example of the configuration of a membrane forming device according to a first embodiment of the technology related to the present disclosure. FIG. 2a is a partial enlarged cross-sectional view of an example of a pattern formed on a wafer on which a film deposition process is performed in the film deposition apparatus of FIG. 1. FIG. 2b is a partial enlarged cross-sectional view of an example of a pattern formed on a wafer on which a film deposition process is performed in the film deposition apparatus of FIG. 1. Figure 3a is a diagram illustrating an example of the distribution of hydrocarbon active species and hydrogen active species generated from plasma in a simulation model that reproduces the film formation treatment of a vertically grown carbon-based membrane at the top. Figure 3b is a diagram illustrating the distribution of hydrocarbon active species and hydrogen active species generated from plasma in a simulation model that reproduces the film formation treatment of a vertically grown carbon-based membrane at the top. Figure 4a is a partially enlarged cross-sectional view to explain an example of the difference in the shape of constriction in a vertically growing carbon-based membrane at the top depending on the presence or absence of a protective film. Figure 4b is a partially enlarged cross-sectional view to explain an example of the difference in the shape of constriction occurrence in a vertically growing carbon-based membrane at the top depending on the presence or absence of a protective film. Figure 4c is a partially enlarged cross-sectional view to explain an example of the difference in the shape of constriction occurrence in a normal vertical growth carbon-based membrane due to the presence or absence of a protective film. Figure 4d is a partially enlarged cross-sectional view to explain an example of the difference in the shape of constriction occurrence in a normal vertical growth carbon-based membrane due to the presence or absence of a protective film. Figure 5a is a partially enlarged cross-sectional view to explain an example of the difference in the shape of the constriction of a normal vertically grown carbon-based film due to the difference in thickness of the insulating film as a protective film. FIG. 5b is a partially enlarged cross-sectional view to explain an example of the difference in the shape of the constriction of a normal vertically grown carbon-based film due to the difference in thickness of the insulating film as a protective film. FIG. 5c is a partially enlarged cross-sectional view to explain an example of the difference in the shape of the constriction of a normal vertically grown carbon-based film due to the difference in thickness of the insulating film as a protective film. FIG. 5d is a partially enlarged cross-sectional view to explain an example of the difference in the shape of the constriction of a normal vertically grown carbon-based film due to the difference in thickness of the insulating film as a protective film. FIG. 6 is a flowchart showing an example of a tabernacle method according to a first embodiment. Figure 7 is a partially enlarged cross-sectional view showing one form (an example) of a normal vertically grown carbon-based membrane formed by the membrane formation method of Figure 6. FIG. 8a is a process diagram showing an example of a film formation method according to a second embodiment of the technology related to the present disclosure. FIG. 8b is a process diagram showing an example of a film formation method according to a second embodiment of the technology related to the present disclosure. FIG. 8c is a process diagram showing an example of a film formation method according to a second embodiment of the technology related to the present disclosure. FIG. 8d is a process diagram showing an example of a film formation method according to a second embodiment of the technology related to the present disclosure. FIG. 8e is a process diagram showing an example of a film formation method according to a second embodiment of the technology related to the present disclosure. FIG. 9 is a flowchart showing an example of a tabernacle method according to a second embodiment. Specific details for implementing the invention
[0008] Hereinafter, an embodiment of the technology according to the present disclosure will be described with reference to the drawings. First, a first embodiment of the technology according to the present disclosure will be described. FIG. 1 is a cross-sectional view schematically illustrating an example of the configuration of a film-forming device according to the first embodiment of the technology according to the present disclosure. This film-forming device is a PECVD (Plasma-Enhanced Chemical Vapor Deposition) device that performs film formation by generating plasma from a film-forming gas.
[0009] In FIG. 1, the film deposition device (100) is provided with a roughly cylindrical chamber (11) (processing chamber) that accommodates a wafer (W) (substrate), and in the chamber (11), plasma is generated from a film deposition gas inside, as described later. The chamber (11) has an inlet / outlet port (12) on a side wall for transporting the wafer (W) inside and out, and the inlet / outlet port (12) is opened and closed by a gate valve (13).
[0010] Inside the chamber (11), a roughly disc-shaped loading platform (14) is disposed, and the loading platform (14) loads a wafer (W). Additionally, an annular guide ring (15) is disposed on the outer edge of the loading platform (14) to surround the loaded wafer (W). The loading platform (14) is supported by a cylindrical support member (16) extending upward from the bottom of the chamber (11).
[0011] Additionally, a lower electrode (17) and a heater (18) are embedded inside the loading platform (14). The heater (18) generates heat by power supplied from the heater power source (19) to heat the loaded wafer (W). Additionally, a refrigerant passage (not shown) may be embedded inside the loading platform (14) as needed. This refrigerant passage cools the loaded wafer (W) by circulating a refrigerant supplied from the outside. Furthermore, to improve the heat transfer between the loading platform (14) and the wafer (W), a heat transfer gas may be supplied between the loading platform (14) and the wafer (W) as needed.
[0012] Additionally, an upper electrode (20) is positioned on the ceiling portion of the chamber (11) so as to face the loading platform (14), and an insulating member (21) is positioned between the chamber (11) and the upper electrode (20). The upper electrode (20) has a base member (22), a ceiling plate (23), and an intermediate member (24). The base member (22), the ceiling plate (23), and the intermediate member (24) are made of a conductive member, for example, aluminum. The ceiling plate (23), the intermediate member (24), and the base member (22) are arranged in this order from the bottom, but the ceiling plate (23) and the base member (22) are spaced apart by an intermediate member (24) that is approximately ring-shaped, forming a gas diffusion space (25) between them. Additionally, the intermediate member (24) may be omitted, in which case a concave portion is provided in the ceiling plate (23) or the base member (22) to form a gas diffusion space (25). In the base member (22), a gas introduction port (26) is installed and connected from above to the gas diffusion space (25), while in the ceiling plate (23), a plurality of gas holes (27) are installed and connected to the interior of the chamber (11) to the gas diffusion space (25).
[0013] Additionally, the film-forming device (100) is equipped with a gas supply unit (28), and the gas supply unit (28) is connected to a gas introduction port (26) via a gas pipe (29). The gas supply unit (28) has a gas source, a flow controller, or an opening / closing valve, and supplies a processing gas, such as a film-forming gas, for generating plasma. The supplied film-forming gas is introduced into a gas diffusion space (25) via the gas introduction port (26) and is also introduced into the interior of the chamber (11) by diffusion from each gas hole (27). In this way, the upper electrode (20) functions as a shower head. An insulating member (30) is placed on the upper electrode (20). Furthermore, in this embodiment, the film-forming gas supplied by the gas supply unit (28) includes only hydrocarbon gas (e.g., acetylene (C2H2) gas), argon (Ar) gas, and hydrogen (H2) gas. In addition, by using this film-forming gas, the film-forming device (100) plasma-forms the film-forming gas to generate hydrocarbon active species during the film-forming process, and forms an amorphous carbon-based film by hydrocarbon ions or hydrocarbon radicals in the hydrocarbon active species.
[0014] The membrane device (100) further comprises an exhaust device (31), and the exhaust device (31) includes, for example, a turbo molecular pump or a dry pump, and the exhaust device (31) reduces the pressure inside the chamber (11) through an exhaust pipe (36) connected to the bottom of the chamber (11).
[0015] The membrane device (100) further comprises a high-frequency power source (32), and the high-frequency power source (32) is connected to an upper electrode (20) via a matching device (33). The matching device (33) matches the load impedance of the high-frequency power source (32) to the output impedance of the high-frequency power source (32). The high-frequency power source (32) supplies high-frequency power with a frequency of 40 MHz to 460 MHz to the upper electrode (20).
[0016] Accordingly, in the film formation device (100), high-frequency power with a frequency of 40 MHz or higher is supplied to the upper electrode (20). Generally, when high-frequency power with a frequency of 40 MHz or higher is supplied to the upper electrode (20) to generate plasma, the generated plasma becomes a high-density plasma, and the electrical impedance of the plasma is reduced. As a result, the maximum value of the high-frequency power supplied to the upper electrode (20) is lower compared to the maximum value when low-frequency power (frequency: 200 kHz to 13 MHz) is supplied to the upper electrode (20). That is, when high-frequency power is supplied to the upper electrode (20), the plasma potential is reduced, and thereby, the sheath voltage that contributes to the acceleration of ions in the plasma is reduced. In addition, as the frequency of the supplied high-frequency power increases, the sheath vibrates at a high speed, so the tracking ability of the ions to the sheath voltage is reduced. As a result, the ion energy applied from the plasma to the wafer (W) loaded on the loading platform (14) is reduced.
[0017] The film deposition device (100) further comprises a control unit (34), and the control unit (34) controls each component of the film deposition device (100). The control unit (34) is a computer equipped with a processor, memory, input device, display device, or signal input / output interface, and a control program and recipe data are stored in the memory of the control unit (34). When the film deposition process is executed in the film deposition device (100), the processor of the control unit (34) executes a corresponding control program and controls each component of the film deposition device (100) according to the recipe data.
[0018] Specifically, the control unit (34) controls the gas supply unit (28) and the exhaust device (31) to adjust the internal pressure of the chamber (11) and controls the high-frequency power supply (32) to supply high-frequency power to the upper electrode (20). Additionally, the control unit (34) controls the gas supply unit (28) to diffuse and introduce the film-forming gas into the interior of the chamber (11). At this time, the film-forming gas is excited and plasmafied by the electric field generated by the high-frequency power supplied to the upper electrode (20), and active species are generated, and film-forming treatment is performed on the wafer (W) by these active species.
[0019] The membrane device (100) further comprises an impedance circuit (35). The impedance circuit (35) is placed in an electrical path (37) that connects the lower electrode (17) and ground. The impedance circuit (35) includes at least one of an inductor or a capacitor, and by connecting them in series or in parallel, the impedance between the lower electrode (17) and ground can be changed. Additionally, the inductor or capacitor included in the impedance circuit (35) may be either a fixed element or a variable element.
[0020] By changing this impedance, the electrical coupling between the upper electrode (20) and the lower electrode (17) can be weakened, thereby controlling the high-frequency current flowing through the lower electrode (17) to be further reduced. As a result, the energy of the ions incident on the wafer (W) can be controlled more precisely.
[0021] In the film deposition apparatus (100), when a film deposition gas is plasmad to generate active species and a film deposition treatment is performed on a wafer (W), an amorphous carbon-based film can be grown selectively and vertically on the top of a pattern formed on the wafer (W), for example, a trench on a groove. The reason why an amorphous carbon-based film can be grown selectively and vertically on the top of a trench is described in the specification of Japanese Patent Application No. 2023-200333 filed by the applicant. Furthermore, in the film deposition apparatus (100), this carbon-based film is formed by a film deposition treatment that is only a single process of plasmadizing the film deposition gas.
[0022] An amorphous carbon-based film (hereinafter referred to as the "vertically grown carbon-based film on the top of the pattern") that is selectively and vertically grown on the top of such a pattern can be used as an additional hard mask. For example, in the manufacture of a three-dimensional NAND-type flash memory, when forming deep trenches or deep holes by etching, the vertically grown carbon-based film on the top functions as an additional hard mask for the hard mask that has already been deposited. Therefore, there is a need to thicken the vertically grown carbon-based film on the top, and for example, to realize a vertically grown carbon-based film on the top with a thickness of about 1000 nm. Accordingly, the applicant used a deposition apparatus (100) to deposit a relatively thick vertically grown carbon-based film on the top of a pattern formed on a wafer (W).
[0023] FIGS. 2A and 2B are partial enlarged cross-sectional views of an example of a pattern formed on a wafer (W) on which a film deposition process is performed in the film deposition apparatus (100) of FIG. 1. In this wafer (W), an insulating film (39) is formed on the surface of a substrate (38) containing silicon, and a hard mask layer (40) containing amorphous carbon is formed on the insulating film (39). A pattern, for example, a groove-shaped trench (41), is formed in the hard mask layer (40). The trench (41) penetrates the hard mask layer (40), and the insulating film (39) is exposed at the bottom of the trench (41) ( FIG. 2A).
[0024] First, the applicant formed a vertically grown carbon-based film (42) with a thickness of about 200 nm on the top of the trench (41). At this time, the vertically grown carbon-based film (42) on the top did not swell or constrict (Fig. 2a).
[0025] Next, the applicant formed a vertically grown carbon-based film (42) with a thickness of about 400 nm on the top of the trench (41). At this time, the applicant confirmed that a necking of the vertically grown carbon-based film (42) was occurring near the boundary line between the hard mask layer (40) and the vertically grown carbon-based film (42) (Fig. 2b). When etching is performed using the vertically grown carbon-based film (42) as an additional hard mask, if such a necking occurs, the vertically grown carbon-based film (42) may be consumed in an unintended form during etching, and there is a risk that the desired shape cannot be transferred to the etched layer. Therefore, when forming the vertically grown carbon-based film (42) on the top of the trench (41), it is necessary to suppress the occurrence of a necking of the vertically grown carbon-based film (42).
[0026] The applicant created a simulation model that reproduces the film formation process of the vertically grown carbon-based membrane (42) at the top to find the cause of the constriction in the vertically grown carbon-based membrane (42) at the top. In addition, the applicant used the said model to simulate the film formation process when the thickness of the vertically grown carbon-based membrane (42) at the top was different, and confirmed the film formation shape of the vertically grown carbon-based membrane (42) at the top.
[0027] However, when the vertically grown carbon-based film (42) at the top is formed, hydrocarbon ions or hydrocarbon radicals among the hydrocarbon active species generated from the acetylene gas included in the film-forming gas form the carbon-based film. Meanwhile, hydrogen radicals among the hydrogen active species generated from the hydrogen gas included in the film-forming gas etch the carbon-based film. Thus, the applicant confirmed the distribution of hydrocarbon active species and hydrogen active species in the film-forming process of the vertically grown carbon-based film (42) at the top in a simulation model.
[0028] FIGS. 3a and 3b are diagrams illustrating an example of the distribution of hydrocarbon active species and hydrogen active species generated from plasma in a simulation model that reproduces the film formation process of a vertically grown carbon-based membrane (42) at the top. In the figures, hydrocarbon active species are indicated by "○" and hydrogen active species are indicated by "●". In addition, within the trench (41), hydrocarbon active species and hydrogen active species actually exist up to the bottom of the trench. However, FIG. 3 shows the distribution of hydrocarbon active species and hydrogen active species from the top of the trench (41) to near the boundary line between the hard mask layer (40) and the vertically grown carbon-based membrane (42) at the top for ease of understanding. Also, hereinafter, the "boundary line between the hard mask layer (40) and the vertically grown carbon-based membrane (42) at the top" is simply referred to as the "boundary line of the carbon-based membrane."
[0029] In the case where the thickness of the vertically grown carbon-based film (42) at the top is about 200 nm, in the simulation model, hydrocarbon active species were present without gaps from the top of the trench (41) to near the boundary line of the carbon-based film (Fig. 3a). Accordingly, it was estimated that the reason no constriction occurred in the vertically grown carbon-based film (42) at the top with a thickness of about 200 nm was that the formation of the carbon-based film was superior to the etching of the carbon-based film in the range from the top of the trench (41) to near the boundary line of the carbon-based film.
[0030] In addition, when the thickness of the vertically grown carbon-based film (42) at the top is about 400 nm, in the simulation model, within the trench (41), hydrocarbon active species were concentrated near the top of the trench (41) and were almost non-existent near the boundary of the carbon-based film. On the other hand, hydrogen active species were present not only near the top of the trench (41) but also completely near the boundary of the carbon-based film (Fig. 3b). Accordingly, it was estimated that the reason for the occurrence of a constriction in the vertically grown carbon-based film (42) at the top with a thickness of about 400 nm was that the etching of the carbon-based film was dominant over the formation of the carbon-based film near the boundary of the carbon-based film, and as a result, the vertically grown carbon-based film (42) at the top was cut away.
[0031] And as shown in FIG. 3b, when the trench (41) is deepened, the applicant has estimated the mechanism described below as the reason why hydrocarbon active species are concentrated near the upper part of the trench (41). That is, since hydrocarbon active species have a higher adhesion coefficient than hydrogen active species, many hydrocarbon active species are attached to the hard mask layer (40) near the upper part of the trench (41), and few hydrocarbon active species reach the vicinity of the carbon-based film formation. On the other hand, since hydrogen active species have a lower adhesion coefficient than hydrocarbon active species, hydrogen active species are not attached to the hard mask layer (40) near the upper part of the trench (41), and many hydrogen active species reach the vicinity of the carbon-based film formation.
[0032] From the above, the applicant has obtained the finding that the difference between the distribution of hydrocarbon active species and hydrogen active species inside the trench (41) due to the difference in adhesion coefficient is significant as the trench (41) becomes deeper, and a constriction occurs in the normal vertical growth carbon-based membrane (42).
[0033] Based on this finding, the applicant conceived of protecting the normal vertical growth carbon-based film (42) itself from etching by hydrogen active species as a means to suppress the occurrence of constrictions in the normal vertical growth carbon-based film (42). Specifically, the applicant conceived of covering the normal vertical growth carbon-based film (42) with a protective film having etching resistance before the trench (41) deepens and the etching of the carbon-based film becomes dominant over the formation of the carbon-based film near the boundary line of the carbon-based film.
[0034] Therefore, the applicant used a film deposition device (100) and compared a case (example) in which a vertically grown carbon-based film (42) on a wafer (W) is covered with a protective film, and a case (comparative example) in which a vertically grown carbon-based film (42) on a wafer (W) is not covered with a protective film. FIGS. 4a to 4d are partial enlarged cross-sectional views to explain an example of the difference in the shape of the constriction of the vertically grown carbon-based film (42) on a wafer (W) depending on the presence or absence of a protective film.
[0035] Specifically, first, as a comparative example, as shown in FIG. 4a, a vertically grown carbon-based film (42) with a thickness of about 200 nm was formed on the top of the trench (41). In this film formation process, the flow rate of acetylene gas in the film formation gas was set to 30 sccm, the flow rate of hydrogen gas was set to 30 sccm, and the flow rate of argon gas was set to 1000 sccm. In addition, the internal pressure of the chamber (11) was set to 1 Torr, and 500 W of high-frequency power was supplied to the upper electrode (20). In addition, subsequent film formation processes were also carried out under the same conditions.
[0036] After that, the normal vertical growth carbon-based film (42) was not covered with a protective film, and the film formation process was continued until the thickness of the normal vertical growth carbon-based film (42) reached about 400 nm. At this time, as shown in FIG. 4b, a constriction of the normal vertical growth carbon-based film (42) occurred near the boundary line of the carbon-based film.
[0037] Next, as an example, a vertically grown carbon-based film (42) with a thickness of about 200 nm was first formed on the top of the trench (41). Then, as shown in FIG. 4c, the vertically grown carbon-based film (42) or the hard mask layer (40) was covered with an insulating film (43) containing silicon oxide (SiO2), for example, a protective film thinner than the vertically grown carbon-based film (42). This insulating film (43) was formed by Atomic Layer Deposition (ALD) in a film formation device (100). Then, the formation of the vertically grown carbon-based film (42) was initiated again, and the film formation process was continued until the thickness of the vertically grown carbon-based film (42) reached about 400 nm. At this time, as shown in FIG. 4d, no constriction occurred in the vertically grown carbon-based film (42) even near the boundary line of the carbon-based film.
[0038] From the above, the applicant has obtained the insight that if a normal vertical growth carbon-based film (42) formed to a certain thickness is covered with a thin insulating film (43), then no constriction occurs in the normal vertical growth carbon-based film (42) during subsequent formation of the normal vertical growth carbon-based film (42). That is, the applicant has obtained the insight that if the normal vertical growth carbon-based film (42) is covered with a thin insulating film (43), the normal vertical growth carbon-based film (42) is not eroded by hydrogen active species. The technology of the present disclosure is based on this insight.
[0039] Additionally, the applicant used a film deposition device (100) to determine the thickness of the insulating film (43) required to suppress the occurrence of a constriction in the normal vertical growth carbon-based film (42) on the wafer (W). At this time, a normal vertical growth carbon-based film (42) with a thickness of about 300 nm was deposited once on the normal part of the trench (41), and then the normal vertical growth carbon-based film (42) or the hard mask layer (40) was covered with the insulating film (43). Then, the deposition of the normal vertical growth carbon-based film (42) was started again, and the film deposition process was continued until the thickness of the normal vertical growth carbon-based film (42) became about 600 nm.
[0040] In addition, the applicant first formed a vertically grown carbon-based film (42) with a thickness of about 300 nm on the top of the trench (41), then checked the shape of the vertically grown carbon-based film (42) and confirmed that no constriction occurred in the vertically grown carbon-based film (42). That is, it was confirmed that hydrocarbon active species were present without gaps even about 300 nm below the upper opening of the trench (41), and that the formation of the carbon-based film was superior to the etching of the carbon-based film.
[0041] FIGS. 5a to 5d are partial enlarged cross-sectional views to explain an example of the difference in the shape of the constriction of the normal vertical growth carbon-based film (42) due to the difference in thickness of the insulating film (43) as a protective film. In addition, in order to emphasize the shape of the normal vertical growth carbon-based film (42), the illustration of the insulating film (43) is omitted in FIG. 5.
[0042] Specifically, first, as Comparative Example 1, a normal vertical growth carbon-based film (42) was not covered with an insulating film (43), and a film formation treatment was performed twice to form a normal vertical growth carbon-based film (42) with a thickness of about 600 nm. At this time, as shown in FIG. 5a, a relatively large constriction occurred in the normal vertical growth carbon-based film (42) near the boundary line of the carbon-based film.
[0043] Next, as Comparative Example 2, a normal vertical growth carbon-based film (42) with a thickness of about 300 nm formed by the first film formation process was covered with an insulating film (43) with a thickness of about 0.4 nm. Then, a second film formation process was performed to form a normal vertical growth carbon-based film (42) with a thickness of about 600 nm. At this time as well, as shown in FIG. 5b, a constriction occurred in the normal vertical growth carbon-based film (42) near the boundary line of the carbon-based film. However, the constriction in Comparative Example 2 was slightly smaller than the constriction in Comparative Example 1.
[0044] Next, as Comparative Example 3, a normal vertical growth carbon-based film (42) with a thickness of about 300 nm formed by the first film formation process was covered with an insulating film (43) with a thickness of about 1.0 nm. Then, a second film formation process was performed to form a normal vertical growth carbon-based film (42) with a thickness of about 600 nm. At this time as well, as shown in FIG. 5c, a constriction occurred in the normal vertical growth carbon-based film (42) near the boundary line of the carbon-based film. However, the constriction in Comparative Example 3 was slightly smaller than the constriction in Comparative Example 2.
[0045] Finally, as Example 1, a normal vertical growth carbon-based film (42) with a thickness of about 300 nm formed by the first film formation process was covered with an insulating film (43) with a thickness of about 2.0 nm. Then, a second film formation process was performed to form a normal vertical growth carbon-based film (42) with a thickness of about 600 nm. At this time, as shown in FIG. 5d, no constriction occurred in the normal vertical growth carbon-based film (42) near the boundary line of the carbon-based film.
[0046] From the above, the applicant has obtained the insight that if the thickness of the insulating film (43) covering the normal vertical growth carbon-based film (42) is at least 2.0 nm or more, the occurrence of constriction in the normal vertical growth carbon-based film (42) can be suppressed.
[0047] FIG. 6 is a flowchart illustrating an example of a film formation method according to the present embodiment. The film formation method of FIG. 6 is realized by a processor of the control unit (34) executing a corresponding control program. In the film formation method according to the present embodiment, the formation of a normal vertical growth carbon-based film (42) and the formation of an insulating film (43) are performed alternately, but the formation of the normal vertical growth carbon-based film (42) is performed at least twice.
[0048] First, in a film deposition device (100), a wafer (W) having a plurality of trenches (41) formed in a hard mask layer (40) is brought into the chamber (11) of the film deposition device (100), and the wafer (W) is loaded onto a loading platform (14). Subsequently, the supply of film deposition gas containing only acetylene gas (first gas), argon gas, and hydrogen gas (second gas) into the chamber (11) is started, and high-frequency power with a frequency of 40 MHz is supplied to the upper electrode (20). By doing so, the film deposition gas is plasma-ized to generate hydrocarbon active species or hydrogen active species, and a film deposition process is performed on the wafer (W). At this time, the deposition of a carbon-based film by hydrocarbon active species (first active species) is superior to the etching of a carbon-based film by hydrogen active species (second active species). Accordingly, at the top of the trench (41), a vertically growing carbon-based film (42) (first film) is formed vertically (step S61) (first film formation process). Then, at the timing when the thickness of the vertically growing carbon-based film (42) formed vertically at the top of the trench (41) becomes 300 nm, the film formation process is temporarily stopped, and the inside of the chamber (11) is purged by the exhaust device (31).
[0049] Next, with the wafer (W) loaded on the internal loading platform (14) of the chamber (11), a silicon-containing gas or an oxygen-containing gas is alternately introduced into the chamber (11) to generate plasma from each gas. Then, an insulating film (43) (second film) is formed by ALD to cover the hard mask layer (40) or the vertically grown carbon-based film (42) on the top part (step S62) (second film formation process). Step S62 is stopped at the timing when the thickness of the insulating film (43) being formed becomes at least 2 nm, and the interior of the chamber (11) is purged by the exhaust device (31).
[0050] Next, with the wafer (W) loaded on the internal loading platform (14) of the chamber (11), the supply of film-forming gas into the chamber (11) is started again, and high-frequency power with a frequency of 40 MHz is supplied to the upper electrode (20) to perform film-forming treatment on the wafer (W). At this time, at the top of the trench (41), the formation of the carbon-based film by hydrocarbon active species becomes superior to the etching of the carbon-based film by hydrogen active species. As a result, the normal vertical growth carbon-based film (42) is again formed vertically on the already formed normal vertical growth carbon-based film (42) (step S63) (third film-forming process). Meanwhile, near the boundary line of the carbon-based film, the normal vertical growth carbon-based film (42) is protected by an insulating film (43), and the etching of the normal vertical growth carbon-based film (42) by hydrogen active species is suppressed. As a result, no constriction occurs in the normal vertical growth carbon-based film (42). Then, at the timing when the thickness of the normal vertical growth carbon-based film (42) that is vertically formed again becomes 300 nm, the film formation process is temporarily stopped, and the inside of the chamber (11) is purged by the exhaust device (31).
[0051] Next, it is determined whether the number of times the normal vertical growth carbon-based membrane (42) is formed has reached the prescribed number of times required to obtain the required thickness of the normal vertical growth carbon-based membrane (42) (Step S64). If the number of times the normal vertical growth carbon-based membrane (42) is formed has not reached the prescribed number of times, the process returns to Step S62, and Steps S62 and S63 are repeated. Meanwhile, if the number of times the normal vertical growth carbon-based membrane (42) is formed has reached the prescribed number of times, the process is terminated.
[0052] In the film deposition method of FIG. 6, the film deposition process is temporarily stopped at the timing when the thickness of the vertically grown carbon-based film (42) at the top of the vertically deposited film reaches 300 nm. Here, as described above, the deposition of the carbon-based film is superior to the etching of the carbon-based film even at a distance of about 300 nm below the upper opening of the trench (41). Therefore, when the film deposition process is temporarily stopped, no constriction occurs in the vertically grown carbon-based film (42) at the top.
[0053] Then, when step S63 is repeated, the normal vertical growth carbon-based membrane (42) formed in the earlier step moves further downward relative to the upper opening of the trench (41). However, since the normal vertical growth carbon-based membrane (42) is covered with an insulating film (43) each time it is formed, it is not eroded by hydrogen active species located below the trench (41).
[0054] Accordingly, in the membrane formation method of Fig. 6, the occurrence of constrictions in the vertically growing carbon-based membrane (42) at the top can be suppressed.
[0055] In addition, in the film deposition method of FIG. 6, the film deposition process is temporarily stopped at the timing when the thickness of the vertically growing carbon-based film (42) of the top portion that is vertically deposited becomes 300 nm, but the film deposition process may also be temporarily stopped at the timing when the thickness of the vertically growing carbon-based film (42) of the top portion that is vertically deposited becomes 200 nm. In this case, since the distance from the upper opening of the trench (41) to the boundary line of the carbon-based film is shortened, even hydrocarbon active species with a high adhesion coefficient can easily reach the vicinity of the boundary line of the carbon-based film, and the deposition of the carbon-based film can be made more certainly superior to the etching of the carbon-based film.
[0056] In addition, the film deposition process may be temporarily stopped at the timing when the thickness of the vertically grown carbon-based film (42) at the top of the film, which is formed vertically, becomes nearly 400 nm. In this case, the number of executions of step S63 required to obtain the vertically grown carbon-based film (42) at the top of the film is reduced, so throughput can be improved.
[0057] FIG. 7 is a partial enlarged cross-sectional view showing one form (example) of a normal vertical growth carbon-based film (42) formed by the film formation method of FIG. 6. In the form shown in FIG. 7, steps S62 and S63 were repeated twice. In this form, a normal vertical growth carbon-based film (42) with a thickness of about 900 nm was obtained, but no constriction occurred in the normal vertical growth carbon-based film (42). Also, because step S63 is repeated twice, the form shows three normal vertical growth carbon-based films (42) stacked as a whole, but the bottom layer and the middle normal vertical growth carbon-based film (42) are covered by an insulating film (43). And an insulating film (43) is interposed between each normal vertical growth carbon-based film (42).
[0058] Additionally, the thickness of the insulating film (43) formed in step S62 is at least 2 nm, but from the perspective of protecting the vertically grown carbon-based film (42) at the top, it is preferable for the insulating film (43) to be thick. However, the insulating film (43) covers not only the vertically grown carbon-based film (42) at the top, but also the insulating film (39) exposed at the bottom of the hard mask layer (40) or the trench (41). And if the insulating film (43) covering the insulating film (39) is thick, there is a risk that the etching of the insulating film (39) will be hindered when the hard mask layer (40) or the vertically grown carbon-based film (42) at the top is used as a hard mask to perform etching of the insulating film (39) (hereinafter referred to as "next process etching"). In addition, if the insulating film (43) covering the hard mask layer (40) (or the normal vertical growth carbon-based film (42)) is thick, the width of the trench (41) becomes narrow. Therefore, the thickness of the insulating film (43) is at least 2 nm, but it is preferable to be as close to 2 nm as possible.
[0059] Next, a second embodiment of the technology related to the present disclosure will be described. The second embodiment differs from the first embodiment in that the insulating film (43) is etched back each time the insulating film (43) is formed, and the entire insulating film (43) is removed last. Furthermore, below, descriptions of processing details and configurations identical to those of the first embodiment will be omitted, and only descriptions of processing details and configurations different from those of the first embodiment will be provided.
[0060] FIGS. 8a to 8e are process diagrams illustrating an example of a film formation method according to a second embodiment of the technology of the present disclosure, and FIG. 9 is a flowchart illustrating an example of a film formation method according to the present embodiment. The film formation method of FIG. 8 is also realized by the processor of the control unit (34) executing a corresponding control program. In addition, in the film formation method according to the present embodiment, the formation of the normal vertical growth carbon-based film (42) is performed at least twice.
[0061] First, steps S61 and S62 are performed to form a vertical growth carbon-based film (42) on the top of the trench (41) (Fig. 8a), and the vertical growth carbon-based film (42) is also covered with an insulating film (43) (Fig. 8b).
[0062] Next, after purging the interior of the chamber (11) by the exhaust device (31), the wafer (W) is loaded onto the internal loading platform (14) of the chamber (11), and a processing gas for etching back is introduced into the interior of the chamber (11) to generate plasma from each gas. The processing gas for etching back includes, for example, nitrogen trifluoride (NF3) gas or fluorocarbon (CF)-based gas. Since the etching by the plasma generated from this processing gas for etching back is strongly anisotropic, the insulating film (43) covering the top portion of the vertically grown carbon-based film (42) of the entire insulating film (43) is selectively removed (etched back) (step S91) (Fig. 8c) (film removal process). Step S91 is stopped at the timing after the insulating film (43) is removed and the top of the normal vertical growth carbon-based film (42) is exposed, and the inside of the chamber (11) is purged by the exhaust device (31).
[0063] Next, step S63 is executed to deposit a vertically growing carbon-based film (42) again vertically on the already deposited vertically growing carbon-based film (42) (Fig. 8d). Then, at the timing when the thickness of the vertically growing carbon-based film (42) deposited again vertically reaches 300 nm, the deposition process is temporarily stopped, and the interior of the chamber (11) is purged by the exhaust device (31).
[0064] Next, it is determined whether the number of times the normal vertical growth carbon-based membrane (42) is formed has reached the prescribed number of times required to obtain the required thickness of the normal vertical growth carbon-based membrane (42) (Step S64). If the number of times the normal vertical growth carbon-based membrane (42) is formed has not reached the prescribed number of times, the process returns to Step S62, and Steps S62, S91, and S63 are repeated. Meanwhile, if the number of times the normal vertical growth carbon-based membrane (42) is formed has reached the prescribed number of times, the process proceeds to Step S92.
[0065] In step S92, the wafer (W) is removed from the chamber (11), and in another substrate processing device, high-temperature heating etching (thermal etching) using, for example, a fluorine-based gas, or wet etching using hydrofluoric acid is performed on the wafer (W). At this time, the insulating film (43) covering the hard mask layer (40) or the normal vertical growth carbon-based film (42) is removed (Fig. 8e). Then, after no insulating film (43) remains inside the trench (41), the processing is terminated.
[0066] However, when an insulating film (43) is interposed between each vertically grown carbon-based film (42) of the normal portion, the vertically grown carbon-based film (42) of the normal portion is cut away during the next process etching, and the insulating film (43) is exposed. In this way, when an insulating film (43) made of a material different from that of the vertically grown carbon-based film (42) of the normal portion is exposed, the consumption rate of the hard mask changes, and after the next process etching is finished, there may be cases where more hard mask remains than necessary. And if more hard mask remains than necessary, it takes time to remove the hard mask, and there is a risk that throughput will decrease.
[0067] In this regard, in the film formation method of FIG. 8, since the insulating film (43) covering the top portion of the top portion vertically grown carbon-based film (42) is selectively removed and then the top portion vertically grown carbon-based film (42) is formed vertically again, the insulating film (43) is not interposed between each top portion vertically grown carbon-based film (42). Furthermore, the insulating film (43) covering the top portion vertically grown carbon-based film (42), etc., is finally removed so that no insulating film (43) remains inside the trench (41). Therefore, after the end of the next process etching, the hard mask does not remain in excess of what is necessary, and the next process etching is not affected by the charge of the insulating film (43). As a result, in the next process etching, a decrease in throughput can be avoided, and a trench or hole of a desirable shape can be formed.
[0068] In addition, in the membrane formation method of Fig. 8, just like in the membrane formation method of Fig. 6, the occurrence of constriction in the vertically growing carbon-based membrane (42) at the top can be suppressed.
[0069] Although preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the embodiments described above, and various modifications and changes are possible within the scope of the gist thereof.
[0070] For example, in the first embodiment, the insulating film (43) covering the hard mask layer (40) or the normal vertical growth carbon-based film (42) is not removed, but in the same way as in the second embodiment, the insulating film (43) may be removed so that the insulating film (43) does not remain inside the trench (41).
[0071] In addition, in each of the embodiments described above, an insulating film containing silicon oxide was used as the protective film, but other insulating films, such as an insulating film containing silicon nitride (SiN), may be used as long as the protective film has resistance to hydrogen active species. In addition, a film having resistance to hydrogen active species other than an insulating film may be used as the protective film. For example, a carbon film with high etching resistance, such as diamond-like carbon (DLC), or a carbon-containing film with similarly high etching resistance may be used as the protective film. In particular, since the carbon film has almost the same composition as the normal vertical growth carbon-based film (42), it does not become charged by plasma, and thus the need to remove the protective film to avoid the influence of charge during the next etching process can be eliminated. This allows for improved throughput. In addition, when using a carbon film, the carbon film coating of the thin film by ALD, etc., may be repeated frequently while growing the normal vertical growth carbon-based film (42). Accordingly, even if a small defect occurs in the normal vertical growth carbon-based film (42) due to hydrogen active species, the defect can be filled and repaired with a thin carbon film, and the normal vertical growth carbon-based film (42) can be grown. However, when using an insulating film other than one containing silicon oxide, it is preferable that the protective film be removable by thermal etching or wet etching.
[0072] However, the aforementioned constriction may occur regardless of each active species when a carbon-based film is selectively and vertically deposited on the top of a pattern using an active species with a high adhesion coefficient contributing to film deposition and an active species with a low adhesion coefficient contributing to etching. Therefore, the film deposition method of FIG. 6 or FIG. 9 is applicable even if the film selectively and vertically deposited on the top of a pattern is a film other than an amorphous carbon-based film. For example, even if the film selectively and vertically deposited on the top of a pattern is a film containing tungsten carbide, the occurrence of constrictions in the film can be suppressed by applying the film deposition method of FIG. 6 or FIG. 9. In addition, the film deposition method of FIG. 6 or FIG. 9 can be applied even when other hydrogen compound gases are used instead of acetylene gas in the film deposition gas. For example, even when forming a film selectively and vertically at the top of a pattern using silane gas, which is a hydrogen compound gas of silicon, or boran gas, which is a hydrogen compound gas of boron, the film formation method of FIG. 6 or FIG. 9 can be applied.
[0073] Additionally, as a protective film, it may have an adsorption inhibitory effect on an amorphous carbon-based film. Accordingly, for example, when vertically forming the carbon-based film (42) at the top of the trench (41) again in step S63, the carbon-based film does not actively adhere to the protective film, so the carbon-based film can be formed preferentially at the top of the trench (41). Furthermore, by preventing the carbon-based film from actively adhering to the protective film, the narrowing of the trench (41) can be suppressed.
[0074] In addition, a sacrificial layer may be used instead of a protective layer. In this case, when the normal vertical growth carbon-based film (42) is formed vertically again, the sacrificial layer is etched more actively than the normal vertical growth carbon-based film (42) by hydrogen active species. As a result, the etching of the normal vertical growth carbon-based film (42) can be suppressed, and accordingly, the occurrence of constrictions in the normal vertical growth carbon-based film (42) can be suppressed.
[0075] In addition, in each of the embodiments described above, the lower layer of the vertically grown carbon-based film (42) at the top is a hard mask layer (40) containing amorphous carbon, but the lower layer of the vertically grown carbon-based film (42) at the top is not limited to this. For example, the lower layer of the vertically grown carbon-based film (42) at the top may be silicon as a substrate, a mask containing an oxynitride film, an insulating layer in which a plurality of oxide films and a plurality of nitride films are alternately stacked, a single layer of oxide films, a single layer of nitride films, or a wiring layer containing metal.
[0076] Additionally, in each of the embodiments described above, the film formation method of FIG. 6 or FIG. 9 was applied when forming a vertical growth carbon-based film (42) vertically on the top of the trench (41). However, the film formation method of FIG. 6 or FIG. 9 may also be applied when forming a vertical growth carbon-based film (42) vertically on the top of the hole as a pattern.
[0077] In addition, the film deposition device that performs the film deposition method of FIG. 6 or FIG. 9 is not limited to the film deposition device (100) of FIG. 1. Any film deposition device capable of reducing the energy of ions incident on the wafer (W) can perform the film deposition method of FIG. 6 or FIG. 9.
[0078] The present application claims priority based on Japanese patent application No. 2024-051536 filed on March 27, 2024, and incorporates all of the contents of the application herein. Explanation of the symbols
[0079] W: Wafer 11: Chamber 41: Trench 42: Vertical growth carbon-based membrane at the top 43: Insulating film 100: Tabernacle apparatus
Claims
Claim 1 A film deposition method comprising accommodating a substrate including a pattern inside a processing chamber and generating plasma from a film deposition gas using high-frequency power to perform a film deposition treatment on the substrate, the method comprising: a first film deposition process for selectively and vertically depositing a first film on the top portion of the pattern; a second film deposition process for depositing a second film covering the deposited first film; and a third film deposition process for vertically depositing the first film again after the second film is deposited. Claim 2 A method of forming a membrane, wherein, in claim 1, the material constituting the first membrane and the material constituting the second membrane are different. Claim 3 A method for forming a film according to claim 1, wherein the material constituting the first film and the material constituting the second film both include carbon-based materials. Claim 4 A method of forming a membrane according to claim 2 or 3, wherein the second membrane forming process and the third membrane forming process are repeated. Claim 5 A method of forming a film, wherein, in paragraph 2 or 3, the second film is thinner than the first film. Claim 6 A film formation method according to claim 2 or 3, wherein the first film is formed by only one process of generating plasma from the film formation gas. Claim 7 A film formation method according to claim 2 or 3, wherein in the first film formation process and the third film formation process, a first active species generated from a first gas included in the film formation gas forms the first film, and a second active species generated from a second gas included in the film formation gas etches the first film. Claim 8 A method for forming a film according to claim 7, wherein the second film comprises etching resistance to the second active species. Claim 9 In paragraph 7, the above-mentioned first gas is a hydrocarbon gas, a method for forming a film. Claim 10 In paragraph 7, the second gas is hydrogen gas, a method for forming a membrane. Claim 11 A film formation method according to claim 2 or 3, further comprising a film removal process for removing at least the second film covering the top portion of the first film, wherein the film removal process is performed between the second film formation process and the third film formation process. Claim 12 A film formation method according to claim 2 or 3, wherein the first film is an amorphous carbon-based film and the second film is an insulating film. Claim 13 In Clause 12, the insulating film comprises silicon dioxide, a film formation method. Claim 14 A film deposition method comprising housing a substrate including a pattern inside a processing chamber and generating plasma from a film deposition gas using high-frequency power to perform a film deposition treatment on the substrate, comprising: a first film deposition process for selectively and vertically depositing a first film on the top portion of the pattern; a second film deposition process for depositing a second film covering the deposited first film; and a third film deposition process for vertically depositing the first film again after the second film is deposited, wherein in the first film deposition process and the third film deposition process, a first active species generated from a first gas included in the film deposition gas deposits the first film, and a second active species generated from a second gas included in the film deposition gas etches the first film, and the adhesion coefficient of the second active species is lower than the adhesion coefficient of the first active species. Claim 15 A method for forming a film according to claim 14, wherein the second film comprises etching resistance to the second active species. Claim 16 A film deposition device comprising a processing chamber with a reduced internal pressure, and accommodating a substrate including a pattern inside the processing chamber, and generating plasma from a film deposition gas using high-frequency power to perform a film deposition process on the substrate, further comprising a first film deposition process for selectively and vertically depositing a first film on the top portion of the pattern, a second film deposition process for depositing a second film covering the deposited first film, and a third film deposition process for vertically depositing the first film again after the second film is deposited. Claim 17 In paragraph 16, the material constituting the first membrane and the material constituting the second membrane are different, forming a membrane device. Claim 18 A film forming device according to claim 16, wherein the material constituting the first film and the material constituting the second film both comprise carbon-based materials. Claim 19 A film forming device according to claim 17 or 18, wherein the first film forming process, the second film forming process, and the third film forming process are executed inside the same processing room.