Coating composition for forming an Anti-slip layer on a floor surface and method for forming an Anti-slip layer on a floor surface

A coating composition with specific components and a two-stage UV curing process forms a durable and slip-resistant layer on floors, addressing the limitations of existing technologies by enhancing adhesion and wear resistance.

KR103045582B1Active Publication Date: 2026-11-06김성준
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020250178196
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-11-21
Publication Date
2026-11-06
Estimated Expiration
2045-11-21

AI Technical Summary

Technical Problem

Existing anti-slip coating technologies for floors lack effectiveness in forming a durable and slip-resistant layer, particularly in varying construction environments and floor materials, and do not optimize the composition and curing processes for enhanced adhesion and wear resistance.

Method used

A coating composition comprising purified water, 2-propanol, methyltrimethoxysilane, siloxane, silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone, and propylene glycol methyl ether, applied in two stages with UV curing, to form a laminated anti-slip layer with ceramic balls for improved friction and durability.

Benefits of technology

The composition effectively increases surface friction, enhances adhesion, and provides excellent wear resistance and durability by forming a laminated anti-slip layer with ceramic balls, suitable for various floor materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025130891249-PAT00001_ABST
    Figure 112025130891249-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a coating composition for forming an anti-slip layer on a floor surface, comprising purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone and propylene glycol methyl ether.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a coating composition for forming an anti-slip layer on a floor surface and a method for forming an anti-slip layer on a floor surface. Background Technology

[0002] Technology for forming an anti-slip layer on a floor surface primarily involves processes such as removing contaminants from the floor, drying, applying a coating composition, and curing. Conventionally, a method is widely used in which, after cleaning the floor surface, various coating compositions are applied and cured using ultraviolet rays or heat. Such coating compositions may include purified water, alcohols, siloxanes, silicons, silane compounds, ammonium fluoride, siloxane-based polymers, glycols, etc. Additionally, a method of applying particles, such as ceramic balls, to the coating layer to enhance the anti-slip effect is also known. Such conventional technologies are primarily intended to increase surface friction or improve the durability of the coating layer. However, various variations exist regarding the composition of the coating composition, the application and curing processes, and the method of applying ceramic balls, and each technology is selectively applied depending on the characteristics of the floor surface, the construction environment, and the required anti-slip performance. The problem to be solved

[0003] The objective of one embodiment is to provide a non-slip coating composition capable of effectively forming a non-slip layer on a floor surface by providing a coating composition comprising purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone and propylene glycol methyl ether, and a method for forming a non-slip layer on a floor surface using the same. means of solving the problem

[0004] A coating composition according to one embodiment may comprise purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone and propylene glycol methyl ether as a coating composition for forming an anti-slip layer on a floor surface.

[0005] In a coating composition according to one embodiment, purified water may be 70% by weight or more and 80% by weight of the coating composition, 2-propanol may be 2% by weight or more and 5% by weight of the coating composition, and methyltrimethoxysilane may be 1% by weight or more and 4% by weight of the coating composition. Additionally, siloxane and silicon may be 2% by weight or more and 6% by weight of the coating composition, ammonium fluoride may be 1% by weight or more and 5% by weight of the coating composition, and hexamethylcyclotrisiloxane may be 1% by weight or more and 4% by weight of the coating composition. Furthermore, tetramethylsilicone may be 1% by weight or more and 4% by weight of the coating composition, and propylene glycol methyl ether may be 2% by weight or more and 6% by weight of the coating composition.

[0006] A method for forming an anti-slip layer on a floor surface according to one embodiment may include the steps of: washing the floor surface to remove contaminants; drying the floor using heat to remove moisture from the washed floor; applying a coating composition first to the dried floor surface to create a first coating layer; applying ceramic balls on the first coating layer; curing the first coating layer by irradiating ultraviolet rays; applying a coating composition second to the cured first coating layer to create a second coating layer; and curing the second coating layer by irradiating ultraviolet rays.

[0007] In a method for forming an anti-slip layer on a floor surface according to one embodiment, the coating composition may be a coating composition comprising purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone and propylene glycol methyl ether. Effects of the invention

[0008] The coating composition of the present invention comprises purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone and propylene glycol methyl ether, thereby effectively forming an anti-slip layer on a floor surface.

[0009] A coating composition according to one embodiment can improve adhesion to the floor surface and durability by optimizing the content of each component.

[0010] A method for forming an anti-slip layer according to one embodiment can simultaneously secure anti-slip performance, wear resistance, and durability by washing and drying the floor surface, applying a coating composition in the first and second stages, applying ceramic balls, and then undergoing a UV curing process.

[0011] The effects obtainable from the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by those skilled in the art from the description below. Brief explanation of the drawing

[0012] FIG. 1 is a drawing for explaining the comparison between before and after the application of an anti-slip layer according to one embodiment. FIG. 2 is a test report for a coating composition according to one embodiment. FIG. 3 is an example of a flowchart of a method for forming an anti-slip layer according to one embodiment. Specific details for implementing the invention

[0013] Specific structural or functional descriptions of the embodiments are disclosed for illustrative purposes only and may be modified and implemented in various forms. Accordingly, actual implementations are not limited to the specific embodiments disclosed, and the scope of this specification includes modifications, equivalents, or substitutions included in the technical concept described by the embodiments.

[0014] Terms such as "first" or "second" may be used to describe various components, but these terms should be interpreted solely for the purpose of distinguishing one component from another. For example, the first component may be named the second component, and similarly, the second component may be named the first component.

[0015] When it is stated that a component is "connected" to another component, it should be understood that it may be directly connected to or coupled with that other component, or that there may be other components in between.

[0016] Singular expressions include plural expressions unless the context clearly indicates otherwise. In this document, phrases such as “A or B,” “at least one of A and B,” “at least one of A or B,” “A, B or C,” “at least one of A, B and C,” and “at least one of A, B, or C” may each include any one of the items listed together with the corresponding phrase, or all possible combinations thereof. In this specification, terms such as “comprising” or “having” are intended to designate the existence of the described features, numbers, steps, actions, components, parts, or combinations thereof, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0017] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this specification.

[0018] Hereinafter, embodiments will be described in detail with reference to the attached drawings. In the description with reference to the attached drawings, identical components are given the same reference numeral regardless of the drawing number, and redundant descriptions thereof will be omitted.

[0020] FIG. 1 is a drawing for explaining the comparison between before and after the application of an anti-slip layer according to one embodiment.

[0021] Referring to FIG. 1, according to some embodiments, a first coating layer (110) and a second coating layer (120) may be sequentially applied to a floor (100) according to the following anti-slip layer formation method. A step of cleaning the floor surface is performed to remove dust, contaminants, and foreign substances present on the surface of the floor (100). Afterward, a step of sufficiently drying the floor using heat is performed to remove moisture remaining on the surface of the cleaned floor. A coating composition is applied first to the dried floor surface to form a first coating layer (110). Ceramic balls are uniformly applied on the formed first coating layer (110) to provide anti-slip performance. The first coating layer (110) with the ceramic balls applied is cured by irradiating ultraviolet (UV) light. A second coating layer (120) is formed by applying the same or similar coating composition secondarily on the cured first coating layer (110). The second coating layer (120) is also cured through ultraviolet irradiation, so that an anti-slip layer with a structure in which the first coating layer (110) and the second coating layer (120) are laminated can be completed on the floor (100).

[0022] According to some embodiments, a coating composition may be used in forming the first coating layer (110) and the second coating layer (120), and the composition of the coating composition will be described in detail below.

[0023] In one embodiment, the coating composition may be used to form an anti-slip layer (e.g., a first coating layer (110) and a second coating layer (120)) on a floor surface. The coating composition may be applied to the floor surface to increase the frictional force of the surface. The coating composition may be cured through a UV curing process to form an anti-slip layer with excellent wear resistance. For example, the coating composition may be applied to various floor materials such as tile, stone, and concrete to prevent slip accidents.

[0024] In some embodiments of the present invention, the coating composition may include purified water. Purified water can serve as the main solvent of the coating composition to aid in the uniform mixing of each component. Purified water can improve applicability by controlling the viscosity of the coating composition. For example, the content of purified water may affect the drying speed and surface smoothness of the coating composition.

[0025] In some embodiments of the present invention, the coating composition may include 2-propanol. As a volatile solvent, 2-propanol can accelerate the drying of the coating composition. 2-propanol can improve the adhesion of the coating layer by assisting in the removal of contaminants from the surface. For example, 2-propanol evaporates quickly after application, which can shorten the curing time of the coating layer.

[0026] According to some embodiments, the coating composition may include methyltrimethoxysilane. Methyltrimethoxysilane can increase the chemical bonding strength between the coating layer and the floor surface by promoting silane bonding. Methyltrimethoxysilane can improve durability by forming a siloxane network during the curing process. For example, methyltrimethoxysilane can penetrate into the micropores of the tile surface to strengthen the bonding layer.

[0027] According to some embodiments, the coating composition may include siloxane and silicon. Siloxane and silicon can impart hydrophobicity and heat resistance to the coating layer. Siloxane and silicon can increase the durability of the coating layer by forming siloxane bonds upon UV curing. For example, siloxane and silicon can provide a waterproofing effect to the surface, thereby inhibiting the adhesion of contaminants.

[0028] According to some embodiments, the coating composition may include ammonium fluoride. Ammonium fluoride can promote a chemical reaction between the floor surface and the coating composition. Ammonium fluoride can react with siloxane components to strengthen the bonding layer. For example, ammonium fluoride can induce bonding between the softened portion of the tile surface and the siloxane network.

[0029] In some embodiments of the present invention, the coating composition may include hexamethylcyclotrisiloxane. Hexamethylcyclotrisiloxane can adjust the viscosity of the coating composition to make the coating thickness uniform. Hexamethylcyclotrisiloxane can act as a curing aid to control the curing speed of the coating layer. For example, hexamethylcyclotrisiloxane can form a siloxane ring structure upon UV irradiation to increase the heat resistance of the coating layer.

[0030] In some embodiments of the present invention, the coating composition may include tetrogenic silicon. Tetrogenic silicon can act as a curing accelerator to rapidly induce the curing reaction of the coating layer. Tetrogenic silicon can improve heat resistance and wear resistance by strengthening the bonding of the siloxane-based network. For example, tetrogenic silicon can maintain the structural stability of the coating layer in high-temperature environments.

[0031] In some embodiments of the present invention, the coating composition may include propylene glycol methyl ether. Propylene glycol methyl ether can help uniform dispersion of each component by increasing solubility. Propylene glycol methyl ether can improve the adhesion of the coating layer by lowering surface tension upon application. For example, propylene glycol methyl ether can improve the applicability of the coating composition to form a thin and uniform coating layer.

[0032] According to some embodiments, purified water may be 70% by weight or more and 80% by weight of the coating composition. When the content of purified water is maintained at 70% by weight or more and 80% by weight, the viscosity of the coating composition can be appropriately controlled. The higher the proportion of purified water, the more uniformly it can spread on the surface when applied. For example, a composition with 80% by weight of purified water can be applied quickly to a large floor area.

[0033] According to some embodiments, 2-propanol may be present in an amount of 2% to 5% by weight of the coating composition. Volatility and drying speed can be optimized when the content of 2-propanol is 2% to 5% by weight. As the proportion of 2-propanol increases, residual moisture on the surface after application can evaporate quickly. For example, a composition with 3% by weight of 2-propanol can complete surface drying within 10 minutes after application.

[0034] In some embodiments of the present invention, methyltrimethoxysilane may be present in an amount of 1% to 4% by weight of the coating composition. When the content of methyltrimethoxysilane is 1% to 4% by weight, silane bond formation can be facilitated. The higher the proportion of methyltrimethoxysilane, the greater the chemical bonding strength between the coating layer and the floor surface. For example, a composition of 2% by weight of methyltrimethoxysilane can effectively penetrate into the micropores of the tile surface.

[0035] According to some embodiments, the siloxane and silicon may be present in an amount of 2% to 6% by weight of the coating composition. When the content of the siloxane and silicon is 2% to 6% by weight, the hydrophobicity and heat resistance of the coating layer may be enhanced. As the proportion of siloxane and silicon increases, the waterproofing effect of the surface after UV curing may be increased. For example, a composition containing 3% by weight of siloxane and silicon can inhibit the adhesion of external contaminants.

[0036] In some embodiments of the present invention, ammonium fluoride may be present in an amount of 1% to 5% by weight of the coating composition. Surface chemical reactions may be promoted when the content of ammonium fluoride is 1% to 5% by weight. The higher the proportion of ammonium fluoride, the stronger the formation of a bonding layer with the siloxane component. For example, a composition of 3% by weight of ammonium fluoride can induce bonding between the softened portion of the tile surface and the siloxane network.

[0037] In some embodiments of the present invention, hexamethylcyclotrisiloxane may be present in an amount of 1% to 4% by weight of the coating composition. When the content of hexamethylcyclotrisiloxane is 1% to 4% by weight, the viscosity and curing speed of the coating composition can be appropriately controlled. As the proportion of hexamethylcyclotrisiloxane increases, a siloxane ring structure can be stably formed upon UV irradiation. For example, a composition of 2.5% by weight of hexamethylcyclotrisiloxane can increase the heat resistance of the coating layer.

[0038] In some embodiments of the present invention, the tetrogenic silicon may be present in an amount of 1% to 4% by weight of the coating composition. When the content of tetrogenic silicon is 1% to 4% by weight, the curing reaction may proceed rapidly. The higher the proportion of tetrogenic silicon, the stronger the bonding of the siloxane-based network, which can improve wear resistance. For example, a composition containing 2.5% by weight of tetrogenic silicon can maintain the structural stability of the coating layer in a high-temperature environment.

[0039] According to some embodiments, propylene glycol methyl ether may be present in an amount of 2% to 6% by weight of the coating composition. When the content of propylene glycol methyl ether is 2% to 6% by weight, uniform dispersion of each component may be possible. As the proportion of propylene glycol methyl ether increases, the surface tension is lowered upon application, which can improve the adhesion of the coating layer. For example, a composition containing 4% by weight of propylene glycol methyl ether can form a thin and uniform coating layer.

[0040] According to some embodiments, the coating composition can be used to form an anti-slip layer on a floor surface. The coating composition can be applied to the floor surface to increase the frictional force of the surface. The coating composition can be cured through a UV curing process to form an anti-slip layer with excellent wear resistance. For example, the coating composition can be applied to various floor materials such as tile, stone, and concrete to prevent slip accidents.

[0041] According to some embodiments, the coating composition can be cured through a UV curing process to form an anti-slip layer with excellent wear resistance. The coating composition can improve the durability of the coating layer by forming a siloxane-based network upon UV irradiation. During the curing process, the ceramic balls of the coating composition can be fixed to the surface to continuously maintain frictional force. For example, after UV curing, the coating layer can maintain wear resistance without peeling off even under repeated walking or friction.

[0042] In some embodiments of the present invention, the coating composition can be applied to various floor materials to prevent slip accidents. The coating composition can be applied to floor materials with different surface characteristics, such as tiles, stone, and concrete. The coating composition can penetrate and bond to the surface of each material to form an anti-slip layer. For example, the coating composition can chemically bond to a softened tile surface to prevent slip accidents.

[0043] According to some embodiments, the coating composition may be applied to a floor surface to increase the frictional force of the surface. The coating composition may form an uneven structure on the surface during the curing process after application. The coating composition may provide an anti-slip effect by arranging ceramic balls so that they are exposed on the surface. For example, the coating composition may prevent slipping during walking by increasing the coefficient of friction to 0.6 or higher.

[0044] According to some embodiments, a coating composition can increase frictional force by forming surface irregularities through a structure including ceramic balls. The coating composition can form multiple irregular layers on the surface by applying ceramic balls in a first and second layer. The ceramic balls may be partially recessed and partially exposed within the coating layer to increase mechanical frictional force. For example, the diameter and distribution density of the ceramic balls can directly affect the effect of increasing frictional force.

[0045] In some embodiments of the present invention, the coating composition may provide an anti-slip effect by exposing ceramic balls to the surface after curing. The cured coating layer may maintain an uneven structure by exposing a portion of the ceramic balls to the surface. The surface with exposed ceramic balls can suppress slipping when in contact with the sole of a shoe. For example, the anti-slip effect may be maximized when the ceramic balls are distributed with a diameter of 0.1 to 1.0 mm.

[0046] In some embodiments of the present invention, the coating composition may include a silane bonding promoting component and a siloxane-based component to increase the chemical bonding strength with the floor surface. The silane bonding promoting component can penetrate into the micropores of the tile surface to form a bonding layer. The siloxane-based component can build a siloxane network upon UV curing to increase durability. For example, ammonium fluoride can strengthen the bonding layer by promoting a chemical reaction between the softened tile surface and the siloxane-based component.

[0047] In some embodiments of the present invention, the coating composition can improve wear resistance and heat resistance by forming a siloxane network upon UV curing. During the UV irradiation process, the siloxane network can bond into a three-dimensional structure, thereby increasing the wear resistance of the coating layer. The siloxane network can maintain structural stability even in high-temperature environments. For example, a coating layer formed with a siloxane network can maintain durability without being damaged by repeated friction.

[0048] According to some embodiments, the coating composition can achieve an anti-peeling effect by strengthening the bonding layer with the softened tile surface. The coating composition can penetrate the softened tile surface with UV heat of 100°C or higher to form a chemical bond. The bonding layer with the softened surface can suppress the peeling phenomenon of the coating layer. For example, the coating composition can simultaneously improve durability and adhesion through bonding with the softened layer.

[0049] In some embodiments of the present invention, the coating composition can be applied to various floor materials such as tiles, stone, and concrete. The coating composition can adjust the application thickness and curing conditions to suit the surface characteristics of each floor material. The coating composition can penetrate into micropores or uneven structures on the surface to form a bonding layer. For example, the coating composition can deeply penetrate into the porous structure of a concrete surface to stably form an anti-slip layer.

[0050] In some embodiments of the present invention, the coating composition can be applied to the surfaces of tiles, stone, and concrete to form an anti-slip layer suitable for the characteristics of each material. The coating composition can enhance adhesion through chemical bonding after a softening process on the tile surface. On the stone surface, a silane bonding-promoting component can penetrate to strengthen the bonding layer. On the concrete surface, a siloxane-based component can penetrate the porous structure to improve wear resistance and durability.

[0051] According to some embodiments, the coating composition may include various functional components to form an anti-slip layer. The coating composition can stably form an anti-slip layer on the floor surface by having each component act complementarily. Depending on the chemical properties of each component, the coating composition can impart various physical properties such as friction, wear resistance, heat resistance, and applicability. For example, siloxane and silicon can provide hydrophobicity and heat resistance, while ammonium fluoride can enhance surface bonding strength.

[0052] In some embodiments of the present invention, the coating composition can optimize the bonding strength with the floor surface, wear resistance, heat resistance, and applicability by adjusting the mixing ratio of each component. The mixing ratio of the coating composition can be adjusted according to the floor material, construction environment, and required durability. The content of each component can directly affect the curing speed of the coating layer, surface bonding strength, and the fixing strength of the ceramic balls. For example, increasing the content of purified water improves applicability, and adjusting the content of siloxane and silicon can enhance heat resistance and hydrophobicity.

[0053] In some embodiments of the present invention, the coating composition may comprise purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone, and propylene glycol methyl ether. The coating composition can achieve desired physical properties if each component is mixed within a specified weight percent range. For example, purified water may be included in an amount of 70 to 80 weight percent, 2-propanol in an amount of 2 to 5 weight percent, and methyltrimethoxysilane in an amount of 1 to 4 weight percent. Siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone, and propylene glycol methyl ether may be included in amounts of 2 to 6 weight percent, 1 to 5 weight percent, 1 to 4 weight percent, 1 to 4 weight percent, and 2 to 6 weight percent, respectively.

[0054] In some embodiments of the present invention, purified water can serve as the main solvent of the coating composition to enable uniform mixing of all components. Purified water ensures that each component is evenly dispersed, thereby ensuring the physical stability of the coating composition. Purified water can control the viscosity of the coating composition to allow it to diffuse uniformly onto the surface upon application. For example, if the content of purified water is insufficient, the viscosity of the composition increases, which may make application difficult.

[0055] According to some embodiments, purified water can improve applicability and workability by controlling the viscosity of the coating composition. By adjusting the content of purified water, the flowability of the coating composition and the mobility of the brush or roller during operation can be improved. Purified water may evaporate during the drying process after application, which may affect the thickness and uniformity of the final coating layer. For example, if the content of purified water is close to 80%, a thin and uniform coating layer can be formed over a large area.

[0056] In some embodiments of the present invention, purified water may be included in the coating composition in a range of 70 to 80 weight percent. If the weight percentage of purified water is less than 70%, the viscosity of the composition increases, making mixing and application difficult. Conversely, if it exceeds 80%, the durability of the coating layer may decrease. For example, a composition containing 75% purified water can ensure a balance between applicability and durability.

[0057] According to some embodiments, purified water can help dissolve each component and adjust the viscosity of the coating composition so that it can be applied uniformly to the floor surface. Purified water can facilitate the mixing of organic components, such as 2-propanol and methyltrimethoxysilane, and inorganic components. The viscosity-regulating function of purified water can affect the uniformity of the coating thickness and the surface smoothness. For example, when the proportion of purified water is appropriate, the coating composition can be applied using various application methods such as brushes, rollers, and sprays.

[0058] In some embodiments of the present invention, purified water may be included in the coating composition in a range of 70 to 80 weight percent. When the content of purified water is within the range of 70 to 80 weight percent, the coating composition may have a balance of applicability and durability after curing. For example, a composition containing 78% purified water can be applied quickly over a large floor area and maintain the uniformity of the coating layer even after curing.

[0059] According to some embodiments, 2-propanol can accelerate the drying speed as a volatile solvent in the coating composition. 2-propanol can evaporate rapidly after application to promote surface drying of the coating layer. 2-propanol can help dissolve other organic components and suppress the formation of bubbles on the surface during application. For example, a composition containing 2-propanol can begin surface drying within 10 minutes after application.

[0060] According to some embodiments, 2-propanol can increase work efficiency by inducing rapid drying after application of the coating composition. By adjusting the content of 2-propanol, the waiting time after application and the possibility of surface contamination before curing can be reduced. 2-propanol can suppress dust adhesion by reducing surface tackiness during the volatilization process. For example, a composition containing 3% 2-propanol can dry the surface within 15 minutes in a 20°C environment.

[0061] According to some embodiments, 2-propanol may be included in the coating composition in a range of 2 to 5 weight percent. If the content of 2-propanol is less than 2%, the drying speed may be slow, and if it exceeds 5%, volatile organic compound (VOC) emissions may increase. For example, a composition containing 4% 2-propanol can achieve a balance of rapid drying and low VOC emissions.

[0062] In some embodiments of the present invention, 2-propanol acts as a volatile solvent to accelerate the drying of the coating composition after application. 2-propanol evaporates rapidly from the applied surface and can dry the surface of the coating layer along with moisture. The volatility of 2-propanol does not remain on the surface after application, so it does not affect the transparency and durability of the cured layer. For example, a composition containing 3% 2-propanol can complete surface drying within 20 minutes.

[0063] According to some embodiments, 2-propanol may be included in the coating composition in a range of 2 to 5 weight percent. When the content of 2-propanol is within the range of 2 to 5 percent, the coating composition can simultaneously ensure rapid drying and appropriate applicability. For example, a composition containing 5 percent 2-propanol can increase work efficiency during large-area application.

[0064] According to some embodiments, methyltrimethoxysilane can increase the chemical bonding strength with the floor surface as a silane bonding promoter. Methyltrimethoxysilane can penetrate into the micropores of inorganic surfaces, such as tiles and stone, to promote silane bonding. Methyltrimethoxysilane can react with siloxane-based components to form a three-dimensional network structure. For example, a composition containing 2% methyltrimethoxysilane can strengthen the bonding layer with the tile surface.

[0065] According to some embodiments, methyltrimethoxysilane may be included in the coating composition in a range of 1 to 4 weight percent. If the content of methyltrimethoxysilane is less than 1%, the bonding strength enhancing effect may be negligible, and if it exceeds 4%, the uniformity of the cured layer may be reduced. For example, a composition containing 3% methyltrimethoxysilane can maximize adhesion to the floor surface.

[0066] In some embodiments of the present invention, methyltrimethoxysilane can penetrate into micropores on inorganic surfaces, such as tiles and stone, and promote silane bonding. Methyltrimethoxysilane can react with hydroxyl groups on the surface to form siloxane bonds. The silane bonding promoting action can contribute to preventing peeling of the coating layer and improving durability. For example, a composition containing 2% methyltrimethoxysilane can penetrate into micropores on the surface of a tile to form a bonding layer.

[0067] According to some embodiments, methyltrimethoxysilane may be included in the coating composition in a range of 1 to 4 weight percent. When the content of methyltrimethoxysilane is within the range of 1 to 4 percent, the coating composition can simultaneously ensure bonding strength with the bottom surface and uniformity of the cured layer. For example, a composition containing 1.5 percent methyltrimethoxysilane can achieve a balance of durability and adhesion.

[0068] In some embodiments of the present invention, siloxane and silicon can impart hydrophobicity and heat resistance to the coating layer. Siloxane and silicon can improve the durability of the coating layer by forming a siloxane network upon UV curing. Siloxane and silicon can enhance the heat resistance of the coating layer to maintain structural stability in high-temperature environments. For example, a composition containing 3% siloxane and silicon can suppress deformation of the coating layer even in a thermal environment of 100°C or higher.

[0069] According to some embodiments, siloxane and silicon can improve the durability of a coating layer by forming a siloxane network upon UV curing. The siloxane network can be combined into a three-dimensional structure to simultaneously increase the wear resistance and heat resistance of the coating layer. The siloxane network can prevent damage to the coating layer even under repeated friction or thermal shock. For example, a composition containing 4% siloxane and silicon can have significantly improved durability after UV curing.

[0070] In some embodiments of the present invention, siloxane and silicon may be included in the coating composition in a range of 2 to 6 weight percent. If the content of siloxane and silicon is less than 2%, the hydrophobic and heat resistance effects may be reduced, and if it exceeds 6%, the uniformity of the cured layer may be reduced. For example, a composition containing 5% siloxane and silicon can maintain durability for a long period in a high-temperature environment.

[0071] According to some embodiments, siloxane and silicon can impart hydrophobic properties to the surface of a coating layer and enable structural stability to be maintained in high-temperature environments. Siloxane and silicon can increase the contact angle to prevent water droplets from forming on the surface. The imparting of heat resistance can prevent deformation or delamination of the coating layer even in thermal environments of 100°C or higher. For example, a composition containing 3% siloxane and silicon can prevent water from seeping into the surface and maintain the coating layer even at high temperatures.

[0072] According to some embodiments, siloxane and silicon may be included in the coating composition in a range of 2 to 6 weight percent. When the content of siloxane and silicon is within the range of 2 to 6 percent, the coating composition can ensure a balance of hydrophobicity and heat resistance. For example, a composition containing 2.5 percent siloxane and silicon can simultaneously improve the hydrophobicity and heat resistance of the surface.

[0073] According to some embodiments, ammonium fluoride can promote surface chemical reactions to strengthen the bonding layer between the coating layer and the floor surface. Ammonium fluoride can promote chemical reactions between the softened tile surface and the siloxane-based component to form a bonding layer. Ammonium fluoride can contribute to preventing peeling of the coating layer and improving durability. For example, a composition containing 3% ammonium fluoride can suppress peeling by strengthening the bonding layer with the tile surface.

[0074] In some embodiments of the present invention, ammonium fluoride may be included in the coating composition in a range of 1 to 5 weight percent. If the content of ammonium fluoride is less than 1%, the chemical reaction promoting effect may be negligible, and if it exceeds 5%, the uniformity of the cured layer may be reduced. For example, a composition containing 4% ammonium fluoride can maximize the strength of the bonding layer.

[0075] In some embodiments of the present invention, ammonium fluoride can form a bonding layer by promoting a chemical reaction between a softened tile surface and a siloxane-based component. Ammonium fluoride can induce siloxane bonding by reacting with hydroxyl groups on the tile surface. Promoting surface chemical reactions can directly contribute to improving the durability and adhesion of the coating layer. For example, a composition containing 2% ammonium fluoride can form a strong bonding layer on the tile surface.

[0076] In some embodiments of the present invention, ammonium fluoride may be included in the coating composition in a range of 1 to 5 weight percent. When the content of ammonium fluoride is within the range of 1 to 5 percent, the coating composition can simultaneously ensure the strength of the bonding layer and the uniformity of the cured layer. For example, a composition containing 1.5 percent ammonium fluoride can achieve a balance of durability and adhesion.

[0077] According to some embodiments, hexamethylcyclotrisiloxane can adjust the viscosity of a coating composition and act as a curing aid. Hexamethylcyclotrisiloxane can adjust the viscosity to maintain a uniform coating thickness. Hexamethylcyclotrisiloxane can assist in the formation of a siloxane network during the UV curing process. For example, a composition containing 2.5% hexamethylcyclotrisiloxane can simultaneously ensure uniformity of coating thickness and curing speed.

[0078] According to some embodiments, hexamethylcyclotrisiloxane may be included in the coating composition in a range of 1 to 4 weight percent. If the content of hexamethylcyclotrisiloxane is less than 1%, the viscosity control effect may be negligible, and if it exceeds 4%, the uniformity of the cured layer may be reduced. For example, a composition containing 3% hexamethylcyclotrisiloxane can maximize applicability and curing assistance effects.

[0079] According to some embodiments, hexamethylcyclotrisiloxane can adjust the viscosity of the coating composition to maintain a uniform coating thickness. Hexamethylcyclotrisiloxane can control flowability during application to improve surface smoothness. The curing assist function can promote the formation of a siloxane network upon UV irradiation. For example, a composition containing 2% hexamethylcyclotrisiloxane can simultaneously ensure uniformity of coating thickness and curing speed.

[0080] According to some embodiments, hexamethylcyclotrisiloxane may be included in the coating composition in a range of 1 to 4 weight percent. When the content of hexamethylcyclotrisiloxane is within the range of 1 to 4 percent, the coating composition can simultaneously achieve viscosity control and a curing aid effect. For example, a composition containing 1.5 percent of hexamethylcyclotrisiloxane can achieve a balance of applicability and a curing aid effect.

[0081] In some embodiments of the present invention, tetroxide silicon can act as a curing accelerator and a heat resistance enhancer. Tetroxide silicon can increase the curing speed of the coating layer by promoting the UV curing reaction. Tetroxide silicon can enhance the structural stability of the coating layer in a high-temperature environment. For example, a composition containing 2.5% tetroxide silicon can suppress deformation of the coating layer even in a thermal environment of 100°C or higher.

[0082] According to some embodiments, tetroxide silicon may be included in the coating composition in a range of 1 to 4 weight percent. If the content of tetroxide silicon is less than 1%, the curing acceleration effect may be negligible, and if it exceeds 4%, the uniformity of the cured layer may be reduced. For example, a composition containing 3% tetroxide silicon can ensure a balance between curing speed and heat resistance.

[0083] According to some embodiments, tetroxide silicon can promote the UV curing reaction and enhance the heat resistance of the coating layer. Tetroxide silicon can react with siloxane-based components to strengthen the three-dimensional network structure of the cured layer. Enhanced heat resistance can prevent deformation or delamination of the coating layer in high-temperature environments. For example, a composition containing 2% tetroxide silicon can have significantly improved heat resistance after UV curing.

[0084] According to some embodiments, tetroxide silicon may be included in the coating composition in a range of 1 to 4 weight percent. When the content of tetroxide silicon is within the range of 1 to 4 percent, the coating composition can secure a balance of curing speed and heat resistance. For example, a composition containing 1.5 percent tetroxide silicon can achieve a balance of curing acceleration and heat resistance enhancement effects.

[0085] In some embodiments of the present invention, propylene glycol methyl ether can serve to improve solubility and applicability. Propylene glycol methyl ether helps to uniformly dissolve each component and allows it to diffuse uniformly onto the surface upon application. Propylene glycol methyl ether can increase the smoothness of the surface after application and maintain the transparency of the cured layer. For example, a composition containing 4% propylene glycol methyl ether can form a uniform coating layer without generating bubbles on the surface upon application.

[0086] According to some embodiments, propylene glycol methyl ether may be included in the coating composition in a range of 2 to 6 weight percent. If the content of propylene glycol methyl ether is less than 2%, the effect of improving solubility may be negligible, and if it exceeds 6%, the uniformity of the cured layer may be reduced. For example, a composition containing 5% propylene glycol methyl ether can ensure a balance of applicability and solubility.

[0087] In some embodiments of the present invention, propylene glycol methyl ether can help the uniform dissolution of each component and enable uniform diffusion on the surface upon application. Propylene glycol methyl ether can lower surface tension upon application, thereby increasing the smoothness of the coating layer. Improved solubility can contribute to the even dispersion of each component, forming a transparent and uniform coating layer after curing. For example, a composition containing 3% propylene glycol methyl ether can form a uniform coating layer without generating bubbles on the surface upon application.

[0088] In some embodiments of the present invention, propylene glycol methyl ether may be included in the coating composition in a range of 2 to 6 weight percent. When the content of propylene glycol methyl ether is within the range of 2 to 6 percent, the coating composition can ensure a balance of solubility and applicability. For example, a composition containing 2.5 percent propylene glycol methyl ether can achieve a balance of applicability and solubility.

[0089] According to some embodiments, the coating composition can achieve desired physical properties if each component is uniformly mixed within a specified weight percentage range. The coating composition may contain purified water, 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicone, and propylene glycol methyl ether in ranges of 70 to 85 weight%, 2 to 5 weight%, 1 to 4 weight%, 2 to 6 weight%, 1 to 5 weight%, 1 to 4 weight%, 1 to 4 weight%, and 2 to 6 weight%, respectively. The weight percentage of each component can directly affect the viscosity, curing speed, wear resistance, and adhesion of the coating composition. For example, if the content of purified water is close to 80%, the coating properties are improved, and if the content of siloxane and silicon is close to 6%, hydrophobicity and heat resistance can be enhanced. If the content of ammonium fluoride is close to 5%, surface bonding strength and wear resistance can be increased.

[0090] In some embodiments of the present invention, the formulation and mixing conditions of the coating composition may be adjusted according to the floor material, construction environment, and required durability. For example, for concrete floors, the content of siloxane and silicon may be adjusted close to the upper limit to increase abrasion resistance. For tile floors, the content of methyltrimethoxysilane and ammonium fluoride may be adjusted to enhance adhesion. If the construction environment is hot and humid, the content of 2-propanol may be increased to accelerate the drying speed. If high durability is required, the content of hexamethylcyclotrisiloxane and tetraxysilicone may be adjusted to enhance the heat resistance and durability of the cured layer.

[0091] According to some embodiments, the mixing order of the coating composition may proceed by sequentially adding each organic and inorganic component using purified water as the main solvent. After preparing purified water first, 2-propanol, methyltrimethoxysilane, siloxanes and silicones, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicon, and propylene glycol methyl ether may be added in order. Each component may be stirred to ensure complete dissolution and dispersion upon addition. For example, 2-propanol and methyltrimethoxysilane may be stirred for at least 5 minutes after addition to purified water to promote dissolution. Siloxanes and silicones, ammonium fluoride, etc., may be added gradually to ensure uniformity of mixing.

[0092] In some embodiments of the present invention, each component must be sufficiently stirred using a stirring device during mixing to ensure uniform dispersion and stability. The stirring device may be an impeller type, a magnetic stirrer, or a high-speed propeller stirrer. The stirring speed can be adjusted within the range of 300 to 800 rpm, and the stirring time can be set to 10 to 30 minutes depending on the change in viscosity. For example, high-viscosity compositions can promote the dispersion of fine particles through high-speed stirring. A cooling jacket may be used to prevent a rise in temperature during the stirring process.

[0093] According to some embodiments, in a water-based solvent-based mixing procedure, purified water may be prepared first, and then 2-propanol, methyltrimethoxysilane, siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicon, and propylene glycol methyl ether may be added sequentially. 70 to 85% of the total volume of purified water may be measured first and added to a mixing container. 2-propanol may be dissolved by stirring for 3 to 5 minutes after being added to the purified water. Methyltrimethoxysilane may be added after the 2-propanol is completely dispersed and stirred for at least 5 minutes. Siloxane and silicons, ammonium fluoride, hexamethylcyclotrisiloxane, tetramethylsilicon, and propylene glycol methyl ether may be added sequentially, and stirring may be performed for 3 to 10 minutes at each step to induce complete dispersion. For example, ammonium fluoride can be added after siloxane and silicon are sufficiently dispersed to promote a chemical reaction.

[0094] According to some embodiments, during the mixing process, each component may be stirred for a certain period of time until it is completely dissolved and dispersed. The mixing time can be set to a range of 30 to 60 minutes in total and can be adjusted according to viscosity and mixing uniformity. During stirring, changes in viscosity can be monitored in real time using a viscometer. For example, when the viscosity reaches a range of 100 to 300 cP, it can be determined that the mixing is complete. After the mixing is complete, impurities can be removed from the composition through a microfilter.

[0095] In some embodiments of the present invention, the coating composition may be stored at a temperature of 5 to 25°C to maintain the stability of the components. If the storage temperature is below 5°C, some components may precipitate or the viscosity may increase. If it exceeds 25°C, loss of volatile components or premature curing may occur. For example, long-term stability can be ensured by storing at an indoor temperature of 10 to 20°C.

[0096] According to some embodiments, since the coating composition may undergo premature curing or deterioration of its components when exposed to ultraviolet rays, it may be stored by sealing it in a UV-blocking container. The UV-blocking container may be made of opaque plastic or metal. Storing it in a sealed state blocks contact with outside air, thereby preventing oxidation and moisture evaporation. For example, storing the coating composition in a sealed container with a capacity of 20L facilitates on-site transport and long-term storage. During storage, the appearance of the container and the condition of the contents can be periodically inspected to check for deterioration.

[0097] In some embodiments of the present invention, the drawings may be configured to allow for a visual comparison of the difference between the floor surface before construction and the structure of the anti-slip coating layer after construction. The drawings may clearly show the roughness, contaminant distribution, and wear marks of the floor surface before construction. The drawings may specifically show the multilayer structure of the anti-slip coating layer after construction, the distribution of ceramic balls, the thickness of the coating layer, and the surface irregularities. The drawings may indicate the boundaries of each layer, the indentation and exposure of ceramic balls, and the stacking order of the coating layers as cross-sectional views or enlarged views. The drawings may also present differences in functional characteristics, such as changes in the coefficient of friction and improved wear resistance before and after construction, in numerical form or graphs.

[0098] According to some embodiments, the floor surface wear, slip risk, structural changes in the coating layer, and functional characteristics can be verified through the drawings. The drawings allow for a comparison of the degree of wear and slip resistance values ​​of the floor surface before construction. The drawings allow for visual verification of the ceramic ball distribution density, coating layer thickness, and changes in the shape of surface irregularities after the formation of the coating layer. The drawings can display slip resistance, wear resistance, and durability values ​​before and after construction in graphs or tables. The drawings allow for a detailed comparison of differences in coating layer structure and changes in functional characteristics according to floor material.

[0099] According to some embodiments, the floor surface prior to construction may contain external contaminants, dust, oil, and signs of wear. The type and distribution of contaminants on the floor surface prior to construction may vary depending on pedestrian traffic, exposure to the external environment, and cleaning frequency. If oil remains on the floor surface prior to construction, surface tension may decrease, increasing the risk of slipping. Fine scratches, cracks, and signs of wear may form on the floor surface prior to construction due to repeated friction. Contaminants on the floor surface prior to construction can be removed by the application of a cleaning agent and a high-pressure washing process.

[0100] In some embodiments of the present invention, the floor surface prior to construction may have low surface roughness and slip resistance, which may result in a high risk of slip accidents. The roughness of the floor surface prior to construction can be quantified using a surface roughness meter and may generally be at the level of Ra 0.1 to 0.3. The slip resistance of the floor surface prior to construction may be measured at a friction coefficient level of 0.3 to 0.4. A surface with low slip resistance may have a higher probability of slip accidents when water, oil, dust, etc., are present. The slip resistance of the floor surface prior to construction may be improved to 0.6 or higher after the application of the coating layer.

[0101] According to some embodiments, the floor surface prior to construction may undergo wear due to repetitive walking, friction, external impact, etc. Repetitive walking can increase smoothness by wearing away micro-irregularities on the floor surface. External impact can cause micro-cracks or gouges on the floor surface. Contaminants and moisture can easily penetrate a worn surface, which may increase the risk of slipping. The degree of wear can be measured using a surface hardness meter or an abrasion tester.

[0102] According to some embodiments, worn floor surfaces may have reduced slip resistance, which can pose a risk to pedestrian safety. The coefficient of friction of a worn surface may decrease to 0.3 or less. Surfaces with reduced slip resistance may cause frequent slip accidents while walking. The surface condition of the worn surface can be improved through a cleaning and softening process prior to the application of the coating layer. The wear reduction effect can be verified through coefficient of friction and wear resistance tests after application.

[0103] In some embodiments of the present invention, the risk of slipping may increase if moisture, contaminants, oil, etc., remain on the floor surface prior to construction. Surfaces with residual moisture may experience a decrease in surface tension, which can lead to a rapid decline in slip resistance. If contaminants and oil remain on the surface, it may result in reduced adhesion of the coating layer and a decrease in the anti-slip effect. Residual contaminants on the floor surface prior to construction can be removed through the application of a cleaning agent, high-pressure washing, and drying processes. After the removal of residual contaminants, the surface condition can be verified through visual inspection and a surface analyzer.

[0104] In some embodiments of the present invention, an anti-slip coating layer may be formed in a multilayer structure on the floor surface after construction. The anti-slip coating layer may be laminated with a primer layer, a first coating layer (110), ceramic balls, a second coating layer (120), and an exposed ceramic ball surface. The thickness and physical properties of each layer may vary depending on UV curing, heat treatment, and application processes. The multilayer structure may contribute to improving adhesion, wear resistance, and frictional force depending on the functional role of each layer. The structural characteristics of the multilayer coating layer can be visualized using cross-sectional views, enlarged views, 3D drawings, etc.

[0105] According to some embodiments, the coating layer structure may include a primer layer bonded to a floor surface, a first coating layer (110), ceramic balls, a second coating layer (120), and an exposed ceramic ball surface. The primer layer may be applied to increase adhesion to the floor surface. The first coating layer (110) may be applied on the primer layer to form a base layer for mechanical fixation of the ceramic balls. The ceramic balls may be distributed in the first coating layer (110) with some of them recessed. The second coating layer (120) may be formed to partially enclose the ceramic balls so that some of the ceramic ball surface is exposed on the outside. The exposed ceramic ball surface may serve to increase friction. The thickness of each layer, the distribution of ceramic balls, surface irregularities, etc., may be specifically represented as a cross-sectional structure in the drawing.

[0106] According to some embodiments, ceramic balls may be uniformly distributed on the first coating layer (110) with some of them recessed. The ceramic balls may be used in a spherical or polyhedral shape with a diameter in the range of 0.1 to 1.0 mm. The ceramic balls may be distributed at regular intervals on the surface of the first coating layer (110) using a dispersion device. The depth of recess of the ceramic balls may be adjusted according to the viscosity of the first coating layer (110), the thickness of the coating, and the weight of the ceramic balls. The distribution density of the ceramic balls may be adjusted to a range of 100 to 500 balls / cm².

[0107] According to some embodiments, the second coating layer (120) may be formed to partially enclose the ceramic ball so that a portion of the ceramic ball surface is exposed to the outside. The second coating layer (120) may be cured by a UV curing process after applying a UV coating composition onto the ceramic ball. The coating thickness of the second coating layer (120) may be adjusted to a range of 50 to 200 m. The second coating layer (120) may be designed to partially cover the top of the ceramic ball so that the ceramic ball surface is exposed to the outside. The exposed ceramic ball surface may contribute to improved friction and anti-slip effects.

[0108] According to some embodiments, the total thickness of the coating layer may be determined by the sum of the stacking thicknesses of the primer layer, the first coating layer (110), the ceramic ball, and the second coating layer (120). The thickness of the primer layer may be set to 10 to 30 mm, the thickness of the first coating layer (110) to 50 to 150 mm, the diameter of the ceramic ball to 0.1 to 1.0 mm, and the thickness of the second coating layer (120) to 50 to 200 mm. The total thickness of the coating layer may be adjusted to a range of 0.2 to 1.5 mm. The coating layer thickness may be customized on-site according to the purpose of construction, floor material, and required performance. The coating layer thickness can be verified using a micrometer or a cross-sectional analyzer.

[0109] In some embodiments of the present invention, the distribution density of the ceramic balls and the thickness of the coating layer can be adjusted according to the purpose of construction, the floor material, and the required anti-slip performance. For example, for indoor gymnasium floors, the distribution density of the ceramic balls can be adjusted close to the upper limit to ensure high friction. For bathroom floors with high humidity, the thickness of the coating layer can be increased to enhance wear resistance and water resistance. If the floor material is concrete, the thickness of the primer layer and the first coating layer (110) can be adjusted to increase adhesion. Depending on the required anti-slip performance, the diameter of the ceramic balls, the distribution density, and the thickness of the coating layer can be optimized to suit the site conditions.

[0110] In some embodiments of the present invention, the coating layer structure after application may have the ceramic ball surface exposed to the outside to increase friction. The exposed ceramic ball surface can increase the contact area with the shoe during walking, thereby increasing the coefficient of friction. The surface irregularities of the ceramic balls can serve to enhance slip resistance. The distribution density and exposed area of ​​the ceramic balls can directly influence the improvement of friction. The increase in friction can be quantified using a friction coefficient measuring instrument.

[0111] According to some embodiments, the coating layer structure can be designed to increase the coefficient of friction to 0.6 or higher. The coefficient of friction can be measured according to the ASTM C1028 or KS F 2374 test methods. While the coefficient of friction of the floor surface before application is at the level of 0.3 to 0.4, the coating layer structure after application can be improved to 0.6 to 0.8 or higher. Improving the coefficient of friction can contribute to preventing slip accidents and ensuring pedestrian safety. The coefficient of friction can be maintained by measuring it periodically after application.

[0112] In some embodiments of the present invention, the coating layer structure has improved wear resistance, so that damage to the coating layer can be minimized even under repeated walking and friction. Wear resistance can be measured using a Taber wear tester or a wear resistance tester. The wear resistance of the coating layer structure can be increased by mechanical fixation of ceramic balls, curing of the multilayer coating layer, and enhancement of the heat resistance of the siloxane-based composition. Damage, peeling, and cracking of the coating layer can be minimized even under repeated walking, friction, and external impact. Improved wear resistance can contribute to extending the lifespan of the coating layer and reducing maintenance costs.

[0113] In some embodiments of the present invention, the floor surface after construction exhibits significantly improved slip resistance and durability, thereby ensuring pedestrian safety. Improved slip resistance can reduce the incidence of slipping accidents while walking. Improved durability can contribute to maintaining the long-term performance of the coating layer and extending the repetitive construction cycle. The safety of the floor surface after construction can be objectively evaluated based on the results of friction coefficient, abrasion resistance, and durability tests. Ensuring pedestrian safety can be applied in various settings, such as public facilities, commercial facilities, and residential spaces.

[0114] FIG. 3 is a test report for a coating composition according to one embodiment.

[0115] FIG. 3 discloses a test report from the Korea Institute of Construction & Living Environment Testing regarding the friction coefficient of an anti-slip layer formed using a coating composition. Here, the coating composition may be a composition comprising 80 wt% purified water, 3 wt% 2-propanol, 2 wt% methyltrimethoxysilane, 3 wt% siloxane and silicons, 3 wt% ammonium fluoride, 2.5 wt% hexamethylcyclotrisiloxane, 2.5 wt% tetroxysilicone, and 4 wt% propylene glycol methyl ether.

[0117] FIG. 4 is an example of a flowchart of a method for forming an anti-slip layer according to one embodiment.

[0118] Referring to FIG. 4, in some embodiments of the present invention, the floor surface cleaning step (310) may clean the floor surface to remove contaminants. The anti-slip layer forming method may apply a cleaning agent to the floor surface to disperse and soften dust, oil, and foreign substances. The anti-slip layer forming method may use a high-pressure washer to simultaneously remove contaminants and the cleaning agent from the floor surface after applying the cleaning agent. The anti-slip layer forming method may remove traces of moisture or contaminants remaining on the floor surface after high-pressure cleaning using an absorbent cloth or a squeegee. The anti-slip layer forming method may check the degree of contaminant removal on the floor surface visually or with a surface cleanliness meter.

[0119] According to some embodiments, a contaminant removal process can be performed to effectively remove dust, oil, and foreign substances present on the floor surface. The contaminant removal process may adjust the composition and concentration of the cleaning agent according to the type of contaminant on the floor surface. The contaminant removal process may allow the contaminant and foreign substances to be sufficiently softened by leaving the cleaning agent on the surface for a certain period of time after application. The contaminant removal process may physically separate the softened contaminant by spraying it with a high-pressure washer. After cleaning, the contaminant removal process may remove any remaining moisture or residual contaminant on the surface using an absorbent cloth, a squeegee, or a vacuum suction device.

[0120] According to some embodiments, the contaminant removal process may apply a cleaning agent to the floor surface to disperse and soften contaminants and foreign substances. The application of the cleaning agent can be carried out uniformly over the entire floor surface using various application devices such as rollers, brushes, and sprays. The viscosity and amount of the cleaning agent applied can be adjusted according to the floor material and the amount of contaminants. After the application of the cleaning agent, the process of chemically dispersing and softening contaminants and foreign substances by the cleaning agent can be maintained for 5 to 30 minutes. Depending on the composition of the cleaning agent, the application of the cleaning agent can address various contaminants such as oil, dust, and inorganic substances.

[0121] According to some embodiments, the contaminant removal process can simultaneously remove contaminants and the cleaning agent from the floor surface using a high-pressure washer after applying the cleaning agent. High-pressure washing can effectively separate the cleaning agent and contaminants by spraying water at a pressure of 50 to 150 bar. High-pressure washing can remove contaminants remaining in irregularities or crevices on the floor surface. After high-pressure washing, traces of moisture or contaminants remaining on the floor surface can be removed with an absorbent cloth or a squeegee. The high-pressure washing and absorbent removal process can increase the cleanliness of the floor surface, thereby improving the adhesion of the subsequent coating process.

[0122] According to some embodiments, the contaminant removal process can remove traces of moisture or contaminants remaining on the floor surface after high-pressure washing using an absorbent cloth or a squeegee. The absorbent cloth can rapidly absorb fine moisture remaining on the floor surface. The squeegee can physically remove residual moisture and traces of contaminants by scraping the floor surface. After using the absorbent cloth or squeegee, the moisture content of the floor surface can be maintained at 1% or less. The absorbent cloth, squeegee, or vacuum suction device can shorten the drying time of the floor surface.

[0123] According to some embodiments, the method for forming an anti-slip layer may include a heating and drying step (320) to remove moisture from the floor surface. The method for forming an anti-slip layer can reduce the moisture remaining on the floor surface to 1% or less through the heating and drying step (320). The heating and drying step (320) can be performed using heat or UV depending on the material and thickness of the floor surface. For example, in the case of a tile floor, moisture can be rapidly evaporated by irradiating with UV heat of 100°C or higher for 5 to 20 minutes. The heating and drying step (320) can serve as a pretreatment process to ensure adhesion and durability of the subsequent coating layer.

[0124] According to some embodiments, the heating and drying step (320) may be performed as a pretreatment process to ensure the adhesion and durability of the subsequent coating layer. The heating and drying step (320) can increase the penetration and bonding strength of the coating composition by removing moisture even within the micropores of the floor surface. The heating and drying step (320) can set optimal drying conditions by measuring the temperature and humidity of the floor surface in real time. For example, using a humidity sensor, the process can proceed to the next step when the surface moisture content reaches 1% or less.

[0125] In some embodiments of the present invention, the heating and drying step (320) may dry the floor surface using UV heat or hot air. The heating and drying step (320) may supply heat uniformly over the entire floor surface using a UV lamp or a hot air blower. UV heat may rapidly evaporate moisture on the surface using ultraviolet wavelengths (e.g., 254 nm or 365 nm). The hot air blower may remove moisture by heating the floor surface to a temperature of 100 to 150°C. UV heat and hot air may be used alone or in combination depending on the floor material.

[0126] In some embodiments of the present invention, the heating and drying step (320) may be performed to reduce the residual moisture on the bottom surface to 1% or less. The heating and drying step (320) may determine the time when drying is completed using a sensor that measures the surface moisture content. For example, if the surface moisture measurement result is confirmed to be 1% or less, the process may be immediately switched to the next coating process. The heating and drying step (320) may ensure that residual moisture is removed in advance so as not to cause a decrease in the adhesion of the coating layer.

[0127] In some embodiments of the present invention, the heating and drying step (320) can rapidly evaporate moisture by irradiating the floor surface with UV heat of 100°C or higher. UV heat of 100°C or higher can be applied to various floor materials such as tile, concrete, and stone. The UV heat irradiation time can be adjusted to 5 to 20 minutes depending on the thickness and material of the floor surface. For example, UV heat can be irradiated for 20 minutes on a thick concrete floor and for 5 to 10 minutes on a thin tile floor. After UV heat irradiation, the surface temperature can be monitored in real time using a non-contact thermometer.

[0128] In some embodiments of the present invention, the heating and drying step (320) may be performed under conditions of irradiating heat or UV for 5 to 20 minutes depending on the material and thickness of the floor surface. The heating and drying step (320) may pre-set an optimal irradiation time for each material of the floor surface. For example, heat or UV may be irradiated for 5 to 10 minutes for ceramic tiles and 15 to 20 minutes for concrete. The heating and drying step (320) may maintain the surface moisture content at 1% or less by combining the irradiation time and temperature. After the drying is completed, the temperature and humidity of the surface may be recorded and utilized for quality control.

[0129] In some embodiments of the present invention, the first coating layer (110) formation step (330) is a core process for imparting an anti-slip function to a floor surface and may include a first application of a coating composition and a first application of ceramic balls. The first coating layer (110) formation step (330) may be performed after the softening and pretreatment processes of the floor surface are completed. The first coating layer (110) formation step (330) may lay the foundation for an anti-slip layer on the floor surface through the first application of the coating composition. The first coating layer (110) formation step (330) may form a fine irregular structure on the surface through the first application of ceramic balls. The first coating layer (110) formation step (330) may simultaneously improve friction and wear resistance through a combination of the coating composition and ceramic balls. For example, the first coating layer (110) formation step (330) can increase mechanical fixation by applying a coating composition to a tile surface softened by UV heat and then dispersing ceramic balls.

[0130] According to some embodiments, the first coating layer (110) forming step (330) is performed after softening and pre-treating the floor surface, thereby simultaneously improving the mechanical fixation force of the subsequent ceramic balls and the durability of the coating layer. In the first coating layer (110) forming step (330), the coating composition can penetrate into the micropores of the softened surface to form a chemical bonding layer. In the first coating layer (110) forming step (330), the ceramic balls can be partially embedded within the coating layer to strengthen mechanical fixation. For example, after applying the coating composition to the softened and pre-treated tile surface, if ceramic balls are dispersed, the ceramic balls can be fixed to the surface irregularities, thereby increasing the coefficient of friction.

[0131] In some embodiments of the present invention, the first application of the coating composition may be performed as a process of uniformly distributing an anti-slip UV coating composition on a softened floor surface. The first application of the coating composition may be applied to the entire floor surface with a uniform thickness using various application devices such as a spray, a roller, or a brush. The first application of the coating composition can maximize penetration into micropores by controlling the viscosity and surface tension of the composition. For example, surface bonding strength may be improved by applying a UV coating composition with a viscosity of 100 to 300 cP to a thickness of 50 to 200 m.

[0132] According to some embodiments, the first application of the coating composition may be carried out over the entire floor surface to maximize the penetration and surface bonding of the composition. The first application of the coating composition may be designed to completely cover irregularities and micropores on the floor surface. Natural diffusion and penetration may proceed for a certain period of time (e.g., 1 to 3 minutes) after the first application of the coating composition. For example, after applying the coating composition over the entire tile surface, waiting until penetration is complete may be allowed to induce the formation of a bonding layer.

[0133] According to some embodiments, the coating thickness can be adjusted within a range of about 50 to 200 mm depending on the material of the floor surface, the purpose of use, and the required durability. The coating thickness can be precisely controlled according to the viscosity of the coating composition and the spray pressure of the coating device. If the coating thickness is 50 mm or less, the surface bonding strength may be reduced, and if it is 200 mm or more, the curing time may increase. For example, the coating thickness can be adjusted to 150 to 200 mm for industrial floors requiring wear resistance, and to 70 to 120 mm for general commercial floors.

[0134] According to some embodiments, the application area can be set to cover the entire area where anti-slip functionality is required. The application area can be planned in advance by considering the floor's usage zones, pedestrian flow, and hazardous areas. The application area can be designated as a straight line, a curve, or a specific pattern according to the construction drawings. For example, it can be applied selectively only to areas with a high risk of slipping, such as stairs, doorways, and ramps.

[0135] In some embodiments of the present invention, the ceramic ball application step (340) may be performed by dispersing ceramic balls on the first coating layer (110) to increase the anti-slip effect and friction force. The ceramic balls may be evenly distributed on the surface of the coating layer using a sprayer, a vibrating disperser, or a manual dispersion tool. The ceramic balls may be applied before the coating layer hardens, i.e., while it is wet, so that the ceramic balls may be partially embedded within the coating layer. For example, the ceramic balls may be uniformly applied over the entire surface using an air pressure sprayer with a spray pressure of 0.2 to 0.5 MPa.

[0136] According to some embodiments, the method may apply ceramic balls onto a first coating layer (110). The penetration depth of the ceramic balls may be adjusted according to the viscosity and surface tension of the coating layer. The uniformity of the particle distribution may be improved by vibrating or rolling the surface immediately after application. For example, if the ceramic balls are lightly pressed with a roller after application, the particles can be stably fixed to the coating layer.

[0137] According to some embodiments, the particle size of the ceramic balls may be selected in a diameter range of 0.1 to 1.0 mm to form irregularities on the floor surface and improve friction. The particle size of the ceramic balls may be determined according to the floor usage environment and the required anti-slip performance. If the particle size is 0.1 mm or less, a fine surface roughness may be formed, making cleaning easy. If the particle size is close to 1.0 mm, the coefficient of friction may increase significantly, but the surface texture may become rough. For example, ceramic balls with a size of 0.2 to 0.5 mm may be applied to indoor commercial floors, and 0.5 to 1.0 mm may be applied to industrial floors.

[0138] In some embodiments of the present invention, the amount of ceramic balls sprayed can be adjusted to a range of about 50 to 200 g per unit area (e.g., 1 m²) to ensure a uniform distribution on the surface of the coating layer and anti-slip performance. The amount of ceramic balls sprayed can be precisely controlled according to the spraying speed and movement speed of the coating device. If the spray amount is 50 g / m² or less, the anti-slip effect may be reduced, and if it is 200 g / m² or more, the surface may become excessively rough. For example, the spray amount can be adjusted to 100 to 150 g / m² for floors of public facilities with high pedestrian traffic, and to 150 to 200 g / m² for high-risk sections such as ramps.

[0139] In some embodiments of the present invention, the first curing step (350) may be performed as a process to secure the durability and adhesion of the anti-slip layer by curing the first coating layer (110) with ultraviolet light. The first curing step (350) may induce a curing reaction within the coating composition by irradiating the first coating layer (110) with ultraviolet light using an ultraviolet light irradiation device. In the first curing step (350), the siloxane-based component of the coating composition and the tile surface may chemically bond to form a bonding layer through ultraviolet light irradiation. In the first curing step (350), the cured coating layer may mechanically fix the ceramic ball, thereby simultaneously improving friction and wear resistance. For example, the first curing step (350) may achieve complete curing of the coating layer by irradiating with an ultraviolet light intensity of 100 to 500 mW / cm² for 5 to 30 seconds.

[0140] In some embodiments of the present invention, the first curing step (350) may serve to promote chemical bonding of the coating composition and strengthen the mechanical fixation of the ceramic ball. The first curing step (350) may increase the bonding strength with the tile surface by activating reactive components in the composition, such as methyltrimethoxysilane and siloxane and silicons, through ultraviolet irradiation. The first curing step (350) may fix the ceramic ball to the surface in close contact as the coating layer shrinks during the curing process. For example, a composition containing ammonium fluoride may increase the fixation strength of the ceramic ball by promoting a surface chemical reaction upon ultraviolet irradiation.

[0141] According to some embodiments, the first curing step (350) may be performed using an ultraviolet irradiation device until the first coating layer (110) applied to the floor surface is sufficiently cured. The first curing step (350) can precisely control the degree of curing of the coating layer by adjusting the irradiation intensity and irradiation time of the ultraviolet irradiation device. The first curing step (350) can achieve uniform curing by varying the irradiation conditions according to the thickness of the coating layer and the floor material. For example, if the coating thickness is 100 m, uniform curing can be achieved by irradiating for 10 seconds with an ultraviolet intensity of 200 mW / cm².

[0142] In some embodiments of the present invention, the method may cure the first coating layer (110) by irradiating ultraviolet light. The method may irradiate ultraviolet light continuously over the entire floor by utilizing the movable structure of the ultraviolet irradiation device. The method may determine whether the curing is complete by checking the curing state visually or with a hardness meter after ultraviolet irradiation. For example, if the surface hardness of the coating layer is measured to be 2H or higher after ultraviolet irradiation, it may be determined that the curing is complete.

[0143] According to some embodiments, UV irradiation conditions can be optimized based on the curing characteristics of the coating composition, the floor material, and the coating thickness. UV irradiation conditions can be set by adjusting the irradiation intensity and time so that the reactive components of the coating composition can be sufficiently activated. The irradiation distance can be adjusted by considering the reflectance and absorption rates of the floor material. For example, since concrete floors have a higher UV absorption rate than tiles, the irradiation intensity can be set high.

[0144] According to some embodiments, the ultraviolet irradiation conditions may consist of variables such as irradiation intensity, wavelength, irradiation distance, and irradiation time. The ultraviolet irradiation conditions may induce a curing reaction using an ultraviolet lamp with a wavelength of 365 nm or 405 nm. The ultraviolet irradiation conditions may increase irradiation efficiency by adjusting the distance between the lamp and the floor surface to 5 to 20 cm. For example, the coating layer can be uniformly cured under conditions of an irradiation intensity of 300 mW / cm², a wavelength of 365 nm, an irradiation distance of 10 cm, and an irradiation time of 15 seconds.

[0145] According to some embodiments, UV irradiation conditions can be precisely controlled to ensure uniform curing of the coating layer and improvement of surface bonding strength. UV irradiation conditions can be set so that uniform energy is delivered to the entire floor surface by moving the irradiation area at a constant speed. Optimal surface bonding strength can be secured by experimentally adjusting the irradiation intensity and time. For example, irradiating the entire floor while maintaining an irradiation speed of 10 cm / s can minimize variations in the curing of the coating layer.

[0146] According to some embodiments, the irradiation intensity can be set in the range of 100 to 500 mW / cm² depending on the output of the ultraviolet lamp. The irradiation intensity can be adjusted according to the curing reaction rate of the coating composition and the reflective characteristics of the floor surface. If the irradiation intensity is 100 mW / cm² or less, curing may be insufficient, and if it is 500 mW / cm² or more, surface overheating may occur. For example, if the lamp output is 200 W, an irradiation intensity of 350 mW / cm² can be achieved by setting the irradiation distance to 10 cm.

[0147] According to some embodiments, the irradiation time can be adjusted to about 5 to 30 seconds depending on the curing speed and application thickness of the coating composition. The irradiation time can be set longer as the application thickness increases and shorter as the application thickness decreases. If the irradiation time is less than 5 seconds, curing may be incomplete, and if it exceeds 30 seconds, discoloration or thermal damage to the coating layer may occur. For example, the irradiation time can be adjusted to 10 seconds for an application thickness of 100 m and 20 seconds for an application thickness of 200 m.

[0148] According to some embodiments, the irradiation intensity and time can be experimentally determined to ensure complete curing of the coating layer and wear resistance. The optimal conditions for the irradiation intensity and time can be derived by measuring the hardness, wear resistance, and adhesion of the coating layer after curing. For example, conditions can be experimentally selected to ensure a coefficient of friction of 0.6 or higher, a hardness of 2H or higher, and an adhesion of 1.5 MPa or higher after curing.

[0149] According to some embodiments, the first coating layer (110) can be uniformly cured under conditions of an irradiation intensity of 200 mW / cm² and an irradiation time of 10 seconds. Under conditions of an irradiation intensity of 200 mW / cm² and an irradiation time of 10 seconds, surface bonding strength and wear resistance can be simultaneously secured when using a coating thickness of 100 m and a siloxane-based composition. For example, a coating layer cured under these conditions can simultaneously achieve the mechanical fixing strength of the ceramic ball and an improvement effect on the surface friction coefficient.

[0150] In some embodiments of the present invention, the step of forming a second coating layer (120) (360) may be performed as a process of reinforcing the durability and functionality of the anti-slip layer by reapplying a coating composition onto the first cured layer. The step of forming a second coating layer (120) (360) can increase resistance to external impact and wear by reapplying a coating composition on top of the cured first coating layer (110) and the ceramic ball layer. The step of forming a second coating layer (120) (360) can strengthen the structural stability of the friction force forming layer by including a second application of the coating composition and, if necessary, reapplication of the ceramic balls. For example, the step of forming a second coating layer (120) (360) can maintain durability and anti-slip performance for a long period by adjusting the application thickness and range according to the usage environment of the floor surface.

[0151] According to some embodiments, the second coating layer (120) forming step (360) may be intended to protect the ceramic ball layer formed on the bottom surface and to improve resistance to external impact and wear. The second coating layer (120) forming step (360) may prevent the ceramic balls from falling off by capturing a portion of the ceramic ball layer with a coating composition. The second coating layer (120) forming step (360) may increase the surface hardness after the coating composition is cured, thereby suppressing wear caused by repeated walking and load. For example, the second coating layer (120) forming step (360) may expose a portion of the surface of the ceramic ball layer to maintain friction, while covering and protecting the remaining portion with a coating layer.

[0152] According to some embodiments, the second coating layer (120) forming step (360) may include a second application of the coating composition and, if necessary, reapplication of ceramic balls. The second coating layer (120) forming step (360) may further disperse ceramic balls over the second-applied coating composition to ensure uniformity of surface irregularities. The second coating layer (120) forming step (360) may control surface characteristics to meet the required friction coefficient by adjusting the spray amount and particle size when reapplication of ceramic balls. For example, the second coating layer (120) forming step (360) may selectively determine whether to reapplication of ceramic balls depending on the intended use of the floor.

[0153] According to some embodiments, a second coating composition can be applied to the cured first coating layer (110) and the ceramic ball layer to form an upper reinforcing layer. The second coating composition can be applied with a uniform thickness using a sprayer or a roller. The second coating composition can increase the mechanical fixing force of the ceramic balls by allowing the applied composition to penetrate along the surface irregularities of the ceramic ball layer. For example, the second coating composition can be applied with a thickness of 100 to 200 mm to ensure the durability of the upper reinforcing layer.

[0154] In some embodiments of the present invention, the secondary application of the coating composition can be adjusted in terms of application thickness, application range, and application method according to the floor material and usage environment. The viscosity and application amount of the secondary application of the coating composition can be controlled according to various floor materials such as tile, concrete, and stone. The application range of the secondary application of the coating composition can be selectively set according to walking frequency, load distribution, and degree of external exposure. For example, a thin coating layer can be applied to indoor floors, and a thick coating layer can be applied to outdoor stairs.

[0155] According to some embodiments, the second coating composition may be the same as the first coating layer (110) or may use a composition with a composition ratio partially adjusted to improve wear resistance and adhesion. The content of siloxane, silicons, ammonium fluoride, etc. may be adjusted in the second coating composition to improve heat resistance, chemical resistance, and wear resistance. The ratio of methyltrimethoxysilane may be changed in the second coating composition to increase the curing speed and surface hardness. For example, the siloxane content of the composition for the second coating may be increased by 1 to 2% compared to the composition for the first coating to enhance durability.

[0156] According to some embodiments, the purpose of forming a reinforcing layer is to protect the ceramic ball layer from the external environment and to increase the durability and wear resistance of the coating layer. The reinforcing layer can block external impact and the penetration of contaminants by exposing a portion of the surface of the ceramic ball while covering the remaining portion with a coating composition. The reinforcing layer can extend the lifespan of the anti-slip layer by suppressing wear caused by repeated walking, equipment movement, and external loads. For example, the reinforcing layer can be designed so that the surface hardness is 2H or higher after the curing of the secondary applied coating composition.

[0157] In some embodiments of the present invention, the purpose of forming a reinforcing layer is to increase the mechanical fixing force of the ceramic ball, prevent peeling of the coating layer, and maintain long-term anti-slip performance. The reinforcing layer can fix the ceramic ball in close contact with the surface by utilizing shrinkage stress during the curing process of the coating composition. The reinforcing layer can prevent peeling of the coating layer by increasing the chemical bonding force with the bottom surface. For example, the reinforcing layer can suppress the detachment of the ceramic ball by promoting a chemical reaction between ammonium fluoride and a siloxane-based component.

[0158] In some embodiments of the present invention, the purpose of forming a reinforcing layer is to simultaneously improve the chemical bonding strength and surface hardness of the coating composition, thereby reinforcing the heat resistance and chemical resistance of the bottom surface. When the reinforcing layer is cured by UV light, siloxane and silicon can impart hydrophobic and heat resistance properties to the surface. The surface hardness of the reinforcing layer is increased by the action of methyltrimethoxysilane, thereby increasing resistance to chemicals and high-temperature environments. For example, the reinforcing layer can be designed so that discoloration and peeling do not occur when exposed to acid and alkali solutions for 24 hours during a chemical resistance test.

[0159] According to some embodiments, the ceramic ball reapplication may reinforce the friction-forming layer by additionally dispersing ceramic balls after or during the application of the second coating layer (120). The ceramic ball reapplication may form an uneven structure by uniformly spraying ceramic balls onto the surface before the second applied coating composition hardens. The ceramic ball reapplication may control the distribution density of the ceramic balls by adjusting the nozzle size and pressure of the spraying device. For example, the ceramic ball reapplication may apply particles with a diameter of 0.1 to 1.0 mm at a spraying amount of 200 g / m².

[0160] According to some embodiments, ceramic ball recoating can be performed selectively depending on the intended use of the floor, the required coefficient of friction, the uniformity of surface irregularities, etc. Ceramic ball recoating can be applied intensively to sections with a high anti-slip rating, such as indoor walkways, stairs, and ramps. To ensure uniformity of surface irregularities, the particles can be fixed by lightly pressing them with a roller after spraying. For example, ceramic ball recoating can be applied to industrial floors requiring a coefficient of friction of 0.6 or higher.

[0161] According to some embodiments, ceramic ball recoating can achieve an optimal anti-slip effect by adjusting the spray amount, particle size, and distribution density. With ceramic ball recoating, the smaller the particle size, the finer the surface roughness is formed, allowing for both walking comfort and anti-slip effects to be secured simultaneously. Although increasing the distribution density of ceramic ball recoating increases the coefficient of friction, excessive distribution can reduce surface flatness, so optimal conditions can be set experimentally. For example, ceramic ball recoating can create various uneven patterns by mixing 0.3mm particles and 0.7mm particles.

[0162] According to some embodiments, the friction reinforcement condition can be adjusted so that the coefficient of friction increases to 0.6 or higher during the secondary ceramic ball application stage. The friction reinforcement condition can satisfy standard anti-slip grades by adjusting the distribution density and application thickness of the ceramic balls. The friction reinforcement condition can measure the coefficient of friction after application and perform additional application or surface adjustment if necessary. For example, if the measurement result of the coefficient of friction is less than 0.6, additional ceramic balls can be sprayed to reinforce it.

[0163] According to some embodiments, friction reinforcement conditions can be set by experimentally optimizing the particle size, distribution density, and application method of the ceramic balls. Although friction increases as the particle size increases due to larger surface irregularities, an appropriate size can be selected to prevent a decrease in walking comfort. Since the surface uniformity of the friction reinforcement conditions varies depending on the spraying method, an air pressure or vibrating spraying device may be selectively used. For example, by applying a particle size of 0.5 mm and a distribution density of 150 g / m² for the friction reinforcement conditions, an anti-slip effect can be secured on both indoor and outdoor floors.

[0164] In some embodiments of the present invention, the friction reinforcement conditions may vary depending on the material of the floor surface, the usage environment, and the required anti-slip grade. For the friction reinforcement conditions, an optimal combination of ceramic balls can be selected for each floor material, such as tile, concrete, or stone. The application amount and particle size can be adjusted by considering the indoor and outdoor environment, humidity, and the possibility of contaminant adhesion. For example, large particles and a high distribution density may be applied to outdoor stairs, while small particles and a low distribution density may be applied to indoor floors.

[0165] In some embodiments of the present invention, the second curing step (370) may be performed as a process of curing the coating layer by irradiating ultraviolet light after the second coating layer (120) is applied. In the second curing step (370), by irradiating ultraviolet light onto the surface of the second coating layer (120), the curable component in the composition may undergo a photochemical reaction to form a polymer network. In the second curing step (370), ultraviolet light may be irradiated uniformly over the entire applied coating layer using an ultraviolet irradiation device. For example, in the second curing step (370), ultraviolet light with a wavelength of 365 nm may be irradiated for 10 to 30 seconds to simultaneously cure the surface and the interior of the coating layer.

[0166] According to some embodiments, a second curing step (370) may be included as an essential step to ensure the durability, adhesion, and wear resistance of the anti-slip layer. The second curing step (370) allows the cured second coating layer (120) to firmly fix the ceramic ball, thereby preventing the ceramic ball from falling off even with repeated walking and external impact. The second curing step (370) increases the degree of curing of the coating layer, allowing the coefficient of friction and wear resistance values ​​to be maintained for a long period. For example, the second curing step (370) can ensure a pencil hardness of at least 2H after curing by comparing the surface hardness before and after curing.

[0167] According to some embodiments, the second curing step (370) may serve to strengthen the chemical bonding of the second coating layer (120) and the mechanical fixing force of the ceramic ball. In the second curing step (370), components in the composition, such as siloxane, silicons, and methyltrimethoxysilane, may chemically bond with the tile surface by ultraviolet irradiation. In the second curing step (370), the coating layer may shrink and fix along the surface irregularities of the ceramic ball during the curing process, thereby increasing the mechanical fixing force of the ceramic ball. For example, in the second curing step (370), ammonium fluoride may be activated to form a bonding layer between the softened tile surface and the coating layer.

[0168] In some embodiments of the present invention, in step 7, the method may cure the second coating layer (120) by irradiating ultraviolet light. The ultraviolet irradiation may be performed uniformly over the entire second coating layer (120) using a UV curing device. The ultraviolet irradiation may be performed selectively over the entire floor or in parts using a mobile or stationary UV lamp. For example, the ultraviolet irradiation may be performed for 10 to 30 seconds at an irradiation intensity of 100 to 150 mJ / cm² to induce complete curing of the coating layer.

[0169] According to some embodiments, the UV re-irradiation conditions can adjust various factors, such as irradiation intensity, irradiation time, and irradiation wavelength, to suit the characteristics of the floor material and the coating composition. The UV re-irradiation conditions can adjust the irradiation intensity according to the reflectance and absorption rates of the floor material, such as tile, concrete, or stone. The UV re-irradiation conditions can adjust the irradiation time within the range of 5 to 60 seconds according to the curing speed and thickness of the coating composition. For example, the UV re-irradiation conditions can select a UV lamp with a wavelength of 365 nm or 405 nm to maximize the reaction efficiency of the photoinitiator in the composition.

[0170] In some embodiments of the present invention, the UV re-irradiation conditions may be optimized according to the thickness of the second coating layer (120), the application range, and the distribution of ceramic balls. When the thickness of the applied second coating layer (120) is 100 to 200 mm, the UV re-irradiation conditions may extend the irradiation time to 20 to 40 seconds to ensure complete curing to the interior. In areas where ceramic balls are densely packed, the UV re-irradiation conditions may increase the irradiation intensity to strengthen the bonding force between the coating layer and the ceramic balls. For example, when the application range is wide, the UV re-irradiation conditions may achieve uniform curing of the entire surface by moving the UV lamp while irradiating.

[0172] The embodiments described above may be implemented as hardware components, software components, and / or combinations of hardware and software components. For example, the devices, methods, and components described in the embodiments may be implemented using a general-purpose computer or a special-purpose computer, such as, for example, a processor, a controller, an arithmetic logic unit (ALU), a digital signal processor, a microcomputer, a field programmable gate array (FPGA), a programmable logic unit (PLU), a microprocessor, or any other device capable of executing and responding to instructions. The processing unit may execute an operating system (OS) and software applications executed on said operating system. Additionally, the processing unit may access, store, manipulate, process, and generate data in response to the execution of the software. For ease of understanding, the processing unit may be described as being used as a single unit, but those skilled in the art will understand that the processing unit may include multiple processing elements and / or multiple types of processing elements. For example, the processing unit may include multiple processors or one processor and one controller. In addition, other processing configurations, such as parallel processors, are also possible.

[0173] Software may include computer programs, code, instructions, or a combination of one or more of these, and may configure a processing unit to operate as desired or instruct the processing unit independently or collectively. Software and / or data may be stored on any type of machine, component, physical device, virtual equipment, computer storage medium, or device so as to be interpreted by the processing unit or to provide instructions or data to the processing unit. Software may be distributed over networked computer systems and may be stored or executed in a distributed manner. Software and data may be stored on computer-readable recording media.

[0174] The method according to the embodiment may be implemented in the form of program instructions that can be executed through various computer means and recorded on a computer-readable medium. The computer-readable medium may store program instructions, data files, data structures, etc., either individually or in combination, and the program instructions recorded on the medium may be those specifically designed and configured for the embodiment or those known and available to those skilled in the art of computer software. Examples of computer-readable recording media include magnetic media such as hard disks, floppy disks, and magnetic tapes; optical recording media such as CD-ROMs and DVDs; magneto-optical media such as floptical disks; and hardware devices specifically configured to store and execute program instructions, such as ROM, RAM, and flash memory. Examples of program instructions include machine code, such as that generated by a compiler, as well as high-level language code that can be executed by a computer using an interpreter, etc.

[0175] The hardware device described above may be configured to operate as one or more software modules to perform the operation of the embodiment, and vice versa.

[0176] Although the embodiments have been described above with reference to the limited drawings, those skilled in the art can apply various technical modifications and variations based thereon. For example, suitable results may be achieved even if the described techniques are performed in a different order than described, and / or if the components of the described system, structure, device, circuit, etc. are combined or assembled in a form different from described, or replaced or substituted by other components or equivalents.

[0177] Therefore, other implementations, other embodiments, and equivalents to the claims also fall within the scope of the claims set forth below.

Claims

Claim 1 A coating composition for forming an anti-slip layer on a floor surface, comprising: purified water; 2-propanol; methyltrimethoxysilane; ammonium fluoride; and hexamethylcyclotrisiloxane. A coating composition comprising: propylene glycol methyl ether; wherein the purified water is 70% by weight or more and 80% by weight or less of the coating composition; the 2-propanol is 2% by weight or more and 5% by weight or less of the coating composition; the methyltrimethoxysilane is 1% by weight or more and 4% by weight or less of the coating composition; the ammonium fluoride is 1% by weight or more and 5% by weight or less of the coating composition; the hexamethylcyclotrisiloxane is 1% by weight or more and 4% by weight or less of the coating composition; and the propylene glycol methyl ether is 2% by weight or more and 6% by weight or less of the coating composition. Claim 2 A coating composition according to claim 1, wherein the purified water is 80% by weight of the coating composition, the 2-propanol is 3% by weight of the coating composition, the methyltrimethoxysilane is 2% by weight of the coating composition, the ammonium fluoride is 3% by weight of the coating composition, the hexamethylcyclotrisiloxane is 2.5% by weight of the coating composition, and the propylene glycol methyl ether is 4% by weight of the coating composition. Claim 3 A method for forming an anti-slip layer on a floor surface using a coating composition of claim 1 or 2, wherein the method comprises: a step of washing the floor surface to remove contaminants; a step of drying the floor using heat to remove moisture from the washed floor; a step of applying the coating composition first to the dried floor surface to create a first coating layer; a step of applying ceramic balls on the first coating layer; a step of curing the first coating layer by irradiating ultraviolet rays; a step of applying the coating composition second to the cured first coating layer to create a second coating layer; and a step of curing the second coating layer by irradiating ultraviolet rays. Claim 4 delete

Citation Information

Patent Citations

  • Cleaning and Anti-slip agent for tile

    JP2008297426A

  • Aqueous coating composition

    JP2025093584A

  • Coating composition capable of both light curing and moisture curing and method for preparing the same

    KR1020240147792A