Substrate treating methods
By replacing unstable Si-H bonds in silicon films with Si-D bonds through immersion in liquid heavy water and microwave irradiation, the method addresses hydrogen-related defects, improving the stability and reliability of semiconductor components.
Patent Information
- Application Number
- KR1020220045065
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-12
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-04-12
AI Technical Summary
The shrinking size of semiconductor components exacerbates the impact of small defects, particularly hydrogen-related issues in silicon films, leading to performance degradation.
A substrate treatment method involving forming a silicon film, immersing it in liquid heavy water (D2O), and irradiating it with microwaves to replace unstable Si-H bonds with Si-D bonds, maintaining stable OH bonds.
Improves the stability and reliability of silicon films by removing unstable hydrogen bonds and enhancing the performance of semiconductor devices.
Smart Images

Figure 112022038905137-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a substrate processing method. Background Technology
[0003] Due to the recent trend toward high integration of semiconductor devices, the size of the components constituting these devices is shrinking. As the size of these components becomes increasingly smaller, small defects occurring within them are having an increasingly significant impact on the performance or characteristics of the semiconductor devices. The problem to be solved
[0005] One of the technical problems that the technical concept of the present invention aims to solve is to provide a substrate processing method that improves the stability of a silicon film. means of solving the problem
[0007] A substrate treatment method according to exemplary embodiments may include the step of forming a silicon film on a substrate; the step of soaking the substrate on which the silicon film is formed in liquid heavy water (D2O); and the first microwave irradiation step of irradiating microwaves onto the silicon film immersed in the liquid heavy water.
[0008] A substrate treatment method according to exemplary embodiments may include the steps of: forming a silicon film on a substrate; irradiating the silicon film with microwaves; and immersing the silicon film in liquid heavy water (D2O).
[0009] A substrate processing method according to exemplary embodiments may include the step of forming a first material layer on a substrate; and the step of forming a second material layer by irradiating the first material layer with microwaves in an environment of liquid heavy water (D2O). The first material layer may comprise a first compound of Formula 1 below, and the second material layer may comprise a second compound of Formula 2 below.
[0010] [Chemical Formula 1]
[0011] Si x Oy H z (x, y, z are real numbers greater than or equal to 0 and less than 1, and x+y+z=1)
[0012] [Chemical Formula 2]
[0013] Si a O b H c D d (a, b, c, d are real numbers greater than or equal to 0 and less than 1, and a+b+c+d=1) Effects of the invention
[0015] According to embodiments of the technical concept of the present invention, a substrate treatment method can be provided to improve the stability of a silicon film by removing hydrogen unstably bonded to silicon or replacing it with deuterium, and bonding deuterium to silicon unsaturated bond sites.
[0016] The various and beneficial advantages and effects of the present invention are not limited to those described above and will be more easily understood in the process of explaining specific embodiments of the present invention. Brief explanation of the drawing
[0018] FIG. 1 is a process flow diagram schematically illustrating a substrate processing method according to exemplary embodiments. FIG. 2a is a schematic diagram showing a substrate processing method according to exemplary embodiments, and FIG. 2b is a chart showing a microwave irradiation state according to exemplary embodiments. FIG. 3 is a schematic diagram showing the chemical structure of a silicon film before and after a substrate processing method according to exemplary embodiments is performed. FIG. 4a is a graph showing the infrared absorption spectrum of a silicon film before the substrate processing method according to exemplary embodiments is performed, and FIG. 4b is a graph showing the infrared absorption spectrum of a silicon film after the substrate processing method according to exemplary embodiments is performed. FIG. 5 is a process flow diagram schematically illustrating a substrate processing method according to exemplary embodiments. FIG. 6 is a schematic diagram illustrating a substrate processing method according to exemplary embodiments. FIG. 7 is a schematic diagram showing the chemical structure of a silicon film before and after a substrate processing method according to exemplary embodiments is performed. FIG. 8a is a graph showing the infrared absorption spectrum of a silicon film before the substrate treatment method according to exemplary embodiments is performed, and FIG. 8b is a graph showing the infrared absorption spectrum of a silicon film after the substrate treatment method according to exemplary embodiments is performed. FIG. 9 is a process flow diagram schematically illustrating a substrate processing method according to exemplary embodiments. Specific details for implementing the invention
[0019] Hereinafter, preferred embodiments of the present invention will be described as follows with reference to the attached drawings.
[0021] FIG. 1 is a process flow diagram schematically illustrating a substrate processing method (10) according to exemplary embodiments.
[0022] FIG. 2a is a schematic diagram showing a substrate processing method (10) according to exemplary embodiments, and FIG. 2b is a chart showing a microwave irradiation state according to exemplary embodiments.
[0023] FIG. 3 is a schematic diagram showing the chemical structure of a silicon film before and after the substrate processing method (10) according to exemplary embodiments is performed.
[0025] Referring to FIGS. 1, FIGS. 2a, FIGS. 2b and FIGS. 3, a substrate processing method (10) according to exemplary embodiments may include a first step (S10) of forming a silicon film on a substrate, a second step (S11) of immersing the substrate on which the silicon film is formed in liquid heavy water (D2O), and a third step (S12) of irradiating microwaves onto the silicon film immersed in the liquid heavy water (D2O). A substrate processing method according to exemplary embodiments may further include a fourth step (S13) of performing a subsequent process on the substrate.
[0027] In the first step (S10), a silicon film, for example, a polycrystalline silicon film, can be formed on a substrate. The method of forming the silicon film on the substrate is not limited. In exemplary embodiments, the silicon film can be formed using Atomic Layer Deposition (ALD), Chemical Vapor Deposition (CVD), etc.
[0028] Referring together with FIG. 2a, FIG. 2a illustrates a silicon film forming process according to exemplary embodiments. A silicon film (3) can be formed on a substrate (2) in a first chamber (A). A silicon film forming apparatus may include a first electrode (E1) and a second electrode (E2) positioned opposite each other, and a gas supply unit (G) that supplies gas into the first chamber (A). The silicon film forming apparatus may further include a power supply unit (not shown) that applies power to the first electrode (E1) and the second electrode (E2). The power supply unit may apply high-frequency power to the second electrode (E2) to form plasma.
[0029] A silicon film (3) can be formed on a substrate (2) using the silicon film forming device described above. A substrate (2) on which a silicon film is to be formed can be loaded onto a first electrode (E1). When the substrate (2) is loaded onto the first electrode (E1), a gas for forming a silicon film (e.g., silane (SiH4), hydrogen (H2), etc.) can be supplied into the first chamber (A) through a gas supply unit (G), and a high-frequency power source can be applied to the first electrode (E1). When the high-frequency power source is applied to the first electrode (E1), a discharge occurs between the first electrode (E1) and the second electrode (E2), and free electrons generated by the discharge gain energy and can collide with silane (SiH4) and hydrogen (H2). Due to this collision, ions and radicals of silane (SiH4) and hydrogen (H2) are formed, and a silicon film (3) can be formed on the substrate (2) loaded onto the first electrode (E1). However, the silicon film forming method and the silicon film forming device are not limited to those described above, and various methods may be used.
[0030] In exemplary embodiments, the silicon film (3) may be applied to the channel layer, gate electrode layer, substrate, and wiring layer that applies a signal to the circuit of a semiconductor device. The silicon film (3) may be, for example, a polycrystalline silicon film, but is not limited thereto. The silicon film (3) may be a single-crystal silicon film or an amorphous silicon film. In other embodiments, the silicon film (3) may be an insulating film comprising silicon (Si) and oxygen (O) as main materials. The silicon film (3) may further comprise hydrogen (H). The silicon film (3) may be applied to the gate insulating layer, tunnel insulating layer, etc. of a semiconductor device.
[0032] The silicon film (3) formed on the substrate (2) may contain defects. For example, the silicon film may contain dangling bonds, which are unpaired electrons that are not bonded to other atoms on the surface. In the case of polycrystalline silicon, dangling bonds may also be present at grain boundaries between crystals. In addition, the silicon film may contain defects, vacancies formed by the loss of atoms, etc., at the interface between the silicon film and other semiconductor materials.
[0033] Defects contained in the silicon film can cause degradation of the silicon film. For example, if hydrogen (H) is bonded to defect sites in the silicon film, the performance of the semiconductor device containing the silicon film may decrease. Since hydrogen bonded to silicon lattice defect sites has a desorption activation energy of only about 1.86 eV, it can be desorbed by a subsequent heat treatment process after the formation of the silicon film and outgasted as hydrogen gas (H2). As an example of a subsequent process, a heat treatment process may be applied to remove impurities from conductive materials such as titanium (Ti), titanium nitride (TiN), and tungsten (W) that are deposited after the formation of the silicon film. If hydrogen atoms bonded to the silicon film are desorbed and outgasted as hydrogen gas (H2) by such a heat treatment process, the defect density of the silicon film may increase. Furthermore, the characteristics of the semiconductor device may degrade due to damage to the film caused by outgassing or the influx of impurities into other layers.
[0034] A substrate treatment method (10) according to exemplary embodiments may replace unsaturated bonds of a silicon film with Si-D by bonding heavy hydrogen (D) to defect sites of a silicon film, or replace unstable Si-H bonds of a silicon film with Si-D bonds. This will be described in detail in subsequent steps (S11, S12).
[0036] In the second step (S11), the substrate on which the silicon film is formed may be immersed in liquid heavy water (D2O). The liquid heavy water (D2O) may be a deuterium source that supplies deuterium (D) to the silicon film.
[0037] Referring together with FIG. 2a, a bath (4) containing liquid heavy water (5) may be provided in the second chamber (B). The substrate (2) on which the silicon film (3) is formed in the first step (S10) may be received in the bath (4) of the second chamber (B) and immersed in the liquid heavy water (5).
[0038] Liquid heavy water (D2O) is more stable than gaseous heavy water as a source of deuterium. As an example of a gaseous source of deuterium, deuterated silane (SiD4) has the characteristic of spontaneously igniting in air without an ignition source. Consequently, when using a gaseous source of deuterium, the source must be equipped with a separate safety device, and the supply environment must be precisely controlled. In contrast, liquid heavy water (D2O) is less reactive and stable at room temperature, making it easier to supply deuterium compared to gaseous sources and allowing it to be applied to various process conditions.
[0040] In the third step (S12), microwaves can be irradiated onto a silicon membrane immersed in liquid heavy water.
[0041] Referring together with FIG. 2a, microwaves (8) can be irradiated onto a silicon film (3) immersed in liquid heavy water (5) in a third chamber (C). The third chamber (C) may include a microwave generator (7). In exemplary embodiments, the microwave generator (7) may be a magnetron. Microwaves (8) emitted from the microwave generator (7) may be irradiated onto the silicon film (3) on the substrate (2). The microwave generator (7) may be positioned at the top of the third chamber (C) so as to irradiate microwaves (8) onto the silicon film (3) immersed in liquid heavy water (5). However, the placement location, number, etc. of the microwave generator (7) are not limited to those depicted.
[0042] In FIG. 2a, the second chamber (B) for performing the second step (S11) and the third chamber (C) for performing the third step (S12) are depicted as separate chambers, but are not limited thereto. In other embodiments, the second step (S11) and the third step (S12) may be performed in the same chamber, in which case a transfer means for moving the bath (4) within the chamber may be provided.
[0044] In exemplary embodiments, the third step (S12) may include a step of irradiating a silicon film with microwaves (S121) and a step of stopping microwave irradiation on the silicon film (S122). The step of irradiating with microwaves (S121) and the step of stopping microwave irradiation (S122) may be performed once or multiple times as a cycle. Referring together with FIG. 2b, when the cycle is repeated n times, microwaves may be irradiated on the silicon film for a time of tn1 to tn2, and microwave irradiation may be stopped for a time of tn2 to t(n+1)1. n may be, for example, between 1 and 15.
[0045] In each cycle, the step of irradiating the silicon film with microwaves (S121) may be sustained for a first time, and the step of stopping the microwave irradiation of the silicon film (S122) may be sustained for a second time that is longer than the first time. For example, the first time may be about 10 seconds to about 20 seconds, and the second time may be about 40 seconds to about 50 seconds. However, the microwave irradiation pattern is not limited thereto. The first time may be the same as the second time or longer than the second time. According to the embodiments, the first time and the second time may be maintained constant for each cycle or may change according to the cycle.
[0046] In the third step (S12), the temperature of the liquid heavy water may be increased. For example, in the third step (S12), the temperature of the liquid heavy water (D2O) may be increased to approximately 320K to 373K. By irradiating the liquid heavy water with microwaves so that it has the above temperature, the Si-H bonds and unsaturated bonds of Si in the silicon film can be sufficiently replaced with Si-D bonds. In exemplary embodiments, when a polycrystalline silicon film is used as the silicon film, the degree of temperature increase in the third step (S12) is greater than when an amorphous silicon film is used, so the deuterium substitution reaction may be further promoted. However, the silicon film to which the substrate processing method (10) can be applied is not limited to a polycrystalline silicon film and can also be applied to an amorphous silicon film.
[0048] The third step (S12) may further include a step (S123) for determining whether the microwave irradiation step (S121) has been performed a predetermined number of times. If it is determined that the step of irradiating microwaves onto the silicon film (S121) has been performed fewer than the desired number of times, a cycle including the step of irradiating microwaves (S121) and the step of stopping microwave irradiation (S122) may be performed again. If it is determined that the step of irradiating microwaves onto the silicon film (S121) has been performed a desired number of times, the fourth step (S13) may be performed.
[0050] In the third step (S12), the Si-H bonds of the silicon film may be replaced with Si-D bonds, or the Si unsaturated bonds may be replaced with Si-D bonds.
[0051] Referring to FIG. 3, FIG. 3 is a schematic diagram showing the chemical structure of a silicon film before and after a substrate processing method is performed. The arrow to the left of FIG. 3 illustrates the chemical structure of the silicon film formed in the first step (S10). The arrow to the right of FIG. 3 illustrates the chemical structure of the silicon film after performing the second and third steps (S11, S12) on the silicon film formed in the first step (S10). FIG. 3 illustrates the chemical structure of a silicon film according to exemplary embodiments, and the chemical structure of the silicon film is not limited to that illustrated.
[0052] As illustrated in FIG. 3, unstable Si-H bonds present in the silicon film can be replaced with Si-D bonds by deuterium (D) contained in liquid deuterium (D2O). Although not illustrated in FIG. 3, deuterium can also be bonded to Si unsaturated bonds or vacancies present in the silicon film. However, stable OH bonds can be maintained without being replaced by deuterium. That is, the substrate processing method comprising the first to third steps (S10, S11, S12) can selectively replace only unstable Si-H bonds or Si unsaturated bonds with Si-D.
[0053] In this way, microwaves irradiated onto a silicon film enable selective deuterium substitution. Microwaves irradiated onto a silicon film can selectively vibrate unpaired electrons. Since Si unsaturated bonds and vacancies contain unpaired electrons, they can be vibrated by microwaves. Unstable Si-H bonds, where hydrogen ions and silicon unpaired electrons are bonded by electrical attraction, can also be vibrated by microwaves. Thus, deuterium can be selectively substituted only for the unpaired electrons vibrating by microwaves. Deuterium may not be substituted for the remaining stable bonds, such as OH bonds. Consequently, while maintaining stable OH bonds, deuterium can be selectively substituted only for unstable Si-H bonds, Si unsaturated bonds, and vacancy sites.
[0055] In the fourth step (S13), a subsequent process can be performed on the substrate (2). Since unstable Si-H bonds, etc., have been replaced with stable Si-D bonds by the preceding steps, hydrogen (H2) outgassing, etc., may not occur even if a high-temperature process such as heat treatment is performed in the fourth step (S13). As a result, the operating characteristics and reliability of the semiconductor device can be improved.
[0057] The above-described substrate processing method can be applied without limitation to the manufacturing process of a semiconductor device including a silicon film, and specific process conditions may vary depending on the equipment, etc. For example, in FIG. 2a, the first step (S10), the second step (S11), and the third step (S12) are shown to be performed in the first chamber (A), the second chamber (B), and the third chamber (C), respectively, but are not limited thereto. In other embodiments, the bath (4) and the microwave generator (7) are provided in a single chamber, so that the second step (S11) and the third step (S12) can be performed in a single chamber. In this case, the chamber may further include a separate transfer means between the bath (4) and the microwave generator (7).
[0059] Next, specific embodiments will be described with reference to FIGS. 4a and 4b. The process conditions of the present invention are not limited to the following embodiments.
[0060] Referring together with FIG. 1, FIG. 4a is a graph showing the infrared absorption spectrum of a silicon film formed by the first step (S10), and FIG. 4b is a graph showing the infrared absorption spectrum of a silicon film after performing the first to third steps (S10, S11, S12).
[0061] In the second step (S11), the silicon membrane may be immersed in liquid heavy water (D2O). In the third step (S12), while the silicon membrane is immersed in liquid heavy water (D2O), microwaves may be irradiated onto the silicon membrane. In the third step (S12), the step of irradiating microwaves onto the silicon membrane (S121) lasted for 15 seconds, and the step of stopping microwave irradiation onto the silicon membrane (S122) lasted for 45 seconds. In the step of irradiating microwaves (S211), microwaves were irradiated onto the silicon membrane under conditions of a frequency of 2.45 GHz, a wavelength of 0.122 m, and a power of 700 W. The step of irradiating microwaves (S121) and the step of stopping microwave irradiation (S122) were performed alternately, and each was repeated 10 times.
[0063] Referring to FIG. 4a, before the deuterium (D) substitution reaction by microwave irradiation in liquid heavy water (D2O), 2,280 cm -1 to 2,050cm -1 and 3,400cm -1 to 3,200cm -1 An absorption peak appears at [location]. In the silicon film prior to the deuterium (D) substitution reaction, Si-H bonds (2,280 cm⁻¹) appear. -1 to 2,050cm -1 ) and OH bonds (3,400 cm -1 to 3,200 cm -1 It can be seen that ) exists.
[0065] Referring to FIG. 4b, after the deuterium (D) substitution reaction by microwave irradiation in liquid heavy water (D2O), 2,280 cm -1 to 2,050cm -1 The absorption peak at decreases, and at 1,639 cm⁻¹ -1 An absorption peak is observed at 3,400 cm⁻¹. -1 to 3,200cm -1 The absorption peak at is maintained. Accordingly, the Si-H bond (2,280 cm⁻¹) -1 to 2,050cm -1) decreases, and Si-D bonding (1,639 cm -1 ) is formed, and OH bonds (3,400 cm -1 to 3,200cm -1 It can be seen that ) is maintained. Deuterium substitution by microwave irradiation can selectively replace Si-H bonds with Si-D bonds. Thus, while maintaining stable OH bonds, unstable Si-H can be selectively replaced with stable Si-D bonds.
[0067] In exemplary embodiments, the silicon film of FIG. 4a is Si x O y H z It can have the chemical formula (where x, y, and z are real numbers greater than or equal to 0 and less than 1, and x+y+z=1). The silicon film of Fig. 4b is Si a O b H c D d It may have a chemical formula of (where a, b, c, and d are each real numbers greater than or equal to 0 and less than 1, and a+b+c+d=1). The hydrogen atoms in the chemical formula of FIG. 4a may include both hydrogen derived from Si-H bonds and hydrogen derived from OH bonds. The deuterium atoms in the chemical formula of FIG. 4b may be deuterium derived from Si-D bonds formed by the substitution of Si-H bonds. Therefore, the following Equations 1 to 4 may be satisfied.
[0069] [Equation 1]
[0070] x=a
[0071] [Equation 2]
[0072] y=b
[0073] [Equation 3]
[0074] z>c
[0075] [Equation 4]
[0076] z=c+d
[0078] The chemical formulas described above are exemplary examples, and the chemical formulas of the silicon film are not limited thereto. For example, the silicon film may further include other elements or impurities in addition to hydrogen (H), oxygen (O), and silicon (Si).
[0080] A silicon film formed by the substrate processing method (10) according to exemplary embodiments may include both Si-D bonds and OH bonds. If Si-D bonds are detected while OH functional groups are preserved by infrared absorption spectrum analysis, etc., it can be determined that the substrate processing method according to the present invention has been applied.
[0082] Next, a substrate processing method (20) according to exemplary embodiments will be described with reference to FIGS. 5 to 7.
[0083] FIG. 5 is a process flow diagram schematically illustrating a substrate processing method (20) according to exemplary embodiments. FIG. 6 is a schematic diagram schematically illustrating a substrate processing method (20) according to exemplary embodiments. FIG. 7 is a schematic diagram showing the chemical structure of a silicon film before and after the substrate processing method (20) according to exemplary embodiments is performed.
[0084] In Fig. 6, the same drawing numbers as in the preceding Fig. 2a are used to describe the same configuration, and redundant descriptions are omitted.
[0086] The substrate processing method (20) of FIG. 5 may include a first step (S20) of forming a silicon film on a substrate, a second step (S21) of irradiating the silicon film with microwaves, and a third step (S22) of immersing the substrate in liquid heavy water (D2O). The substrate processing method (20) of FIG. 5 may further include a fourth step (S23) of performing a subsequent process on the substrate. The substrate processing method (20) of FIG. 5 differs from the substrate processing method (10) of FIG. 1 described above in that microwaves are first irradiated onto the silicon film, and then the substrate is immersed in liquid heavy water.
[0088] In the first step (S20), a silicon film, for example, a polycrystalline silicon film, can be formed on a substrate. The silicon film can be formed using Atomic Layer Deposition (ALD) or Chemical Vapor Deposition (CVD), and the method of formation is not limited thereto. As an exemplary embodiment, referring together with FIG. 6, a substrate (2) can be loaded onto a first electrode (E1) in a first chamber (A'), and a high-frequency power supply can be applied to the first and second electrodes (E1, E2) while supplying gas through a gas supply unit (G) to form a silicon film (3) on the substrate (2). For the method of forming the silicon film (3) in the first chamber (A'), refer to the description of FIG. 2a above.
[0090] In the second step (S21), microwaves can be irradiated onto the silicon film on the substrate. Referring together with FIG. 6, the substrate (2) can be loaded onto the substrate holder (6) in the second chamber (C'). The substrate (2) can be loaded onto the substrate holder (6) such that the silicon film (3) faces the microwave generator (7). The microwave generator (7) facing the silicon film (3) can irradiate microwaves (8) onto the silicon film (3). The substrate processing method (20) of FIG. 5 differs from the substrate processing method (10) of FIG. 1 in that microwaves are irradiated first before the silicon film is immersed in deuterium.
[0091] The second step (S21) may include a step of irradiating a silicon film with microwaves (S211) and a step of stopping microwave irradiation on the silicon film (S212). The step of irradiating with microwaves (S211) and the step of stopping microwave irradiation (S212) may each be sustained for a certain period of time, as described in FIG. 2b above. For example, the step of irradiating with microwaves (S211) may be sustained for 10 to 20 seconds, and the step of stopping microwave irradiation (S212) may be sustained for 40 to 50 seconds. The step of irradiating with microwaves (S211) and the step of stopping microwave irradiation (S212) may constitute a cycle, and said cycle may be repeated once or multiple times. For example, said cycle may be performed at least once and no more than 15 times.
[0092] In the second step (S21), the temperature of the silicon film can be raised to approximately 423K to approximately 443K. By irradiating microwaves so that the temperature of the silicon film is within the above range, impurities adsorbed on the substrate can be desorbed, and the Si-H bonds of the silicon film can be sufficiently removed in the third step (S22) described later. In exemplary embodiments, when a polycrystalline silicon film is used as the silicon film, the degree of temperature rise in the second step (S21) is greater than when an amorphous silicon film is used, so the reaction to remove Si-H bonds can be further promoted. However, the silicon film to which the substrate treatment method (20) can be applied is not limited to a polycrystalline silicon film and can also be applied to an amorphous silicon film.
[0094] The second step (S21) may further include a step (S213) for determining whether microwave irradiation has been performed a predetermined number of times. If it is determined that the step of irradiating microwaves onto the silicon film (S211) has been performed fewer than the desired number of times, a cycle including the step of irradiating microwaves (S211) and the step of stopping microwave irradiation (S212) may be performed again. If it is determined that the step of irradiating microwaves onto the silicon film (S211) has been performed a desired number of times, the third step (S22) may be performed.
[0096] In the third step (S22), the substrate can be immersed in liquid heavy water (D2O). The silicon film on the substrate can be immersed in liquid heavy water (D2O) while irradiated with microwaves. Referring together with FIG. 6, a bath (4) containing liquid heavy water (5) can be provided within the third chamber (B'). The silicon film (3) irradiated with microwaves in the second step (S21) can be immersed in liquid heavy water (5) by being contained in the bath (4) of the third chamber (B').
[0098] By the second and third steps (S21, S22), the Si-H bonds of the silicon film can be removed. Referring together to FIG. 7, FIG. 7 is a schematic diagram showing the chemical structure of the silicon film before and after the substrate processing method is performed. The arrow to the left of FIG. 7 illustrates the chemical structure of the silicon film of exemplary embodiments formed by the first step (S20). The arrow to the right of FIG. 7 illustrates the chemical structure of the silicon film after performing the second and third steps (S21, S22) on the silicon film formed by the first step (S20). FIG. 7 illustrates the chemical structure of the silicon film according to exemplary embodiments, and the chemical structure of the silicon film is not limited to that illustrated.
[0099] As illustrated in FIG. 7, unstable Si-H bonds are selectively removed by the second and third steps (S21, S22), while stable OH bonds can be maintained. By irradiating microwaves onto the silicon film in the second step (S21), the unpaired electrons scattered in the silicon film become excited, and the temperature of the silicon film can rise, for example, to about 423K to about 443K. This allows for the desorption of impurities adsorbed on the silicon film. However, in order to desorb hydrogen (H) from silicon (Si) in a silicon film in a gas (e.g., air), a temperature higher than the above-described temperature may be required. For example, in the case of Si-H2 bonds present in a silicon film in a gas, hydrogen can be desorbed in the range where the surface temperature of the silicon film is about 640K to about 700K. In addition, in the case of Si-H bonds present in the silicon film in the gas, hydrogen can be desorbed in the range where the surface temperature of the silicon film is about 720K to about 800K. Hydrogen may not be sufficiently desorbed from silicon by irradiating the silicon film in the gas with microwaves in the second step (S21).
[0100] In the subsequent third step (S22), Si-H bonds can be removed by immersing the silicon film, heated by microwave irradiation, in liquid heavy water (D2O). Specifically, when the silicon film, heated to a temperature of about 423K to about 443K in the second step (S21), is immersed in liquid heavy water at room temperature in the third step (S22), the Si-H bonds of the silicon film can react with the liquid heavy water to generate gaseous vapor (HOD). As a result, the Si-H bonds of the silicon film are removed, and as the temperature of the silicon film decreases, the silicon (Si) atoms in the surface layer can undergo surface reorganization. This can reduce the unsaturated bonds on the surface of the silicon film. In the third step (S22), the liquid heavy water may be a reactant that causes the redox reaction of the Si-H bonds of the silicon film. Liquid heavy water can also serve as a refrigerant to lower the temperature of the silicon film and prevent water vapor (H2O) from the air from adsorbing onto the surface of the silicon film.
[0101] Thus, the second and third steps (S21, S22) enable selective hydrogen removal. Microwaves irradiated onto the silicon film can selectively vibrate unpaired electrons. Unstable Si-H bonds, formed by the electrical attraction between hydrogen ions and silicon unpaired electrons, vibrate due to microwaves and can react with liquid heavy water. The remaining stable bonds, such as OH bonds, may not vibrate due to microwaves. In this way, stable OH bonds can be maintained, while only unstable Si-H bonds can be selectively removed.
[0103] Subsequently, a subsequent process can be performed on the substrate in the fourth step (S23). Since unstable Si-H bonds have been removed by the preceding steps, even if a high-temperature process such as heat treatment is performed in the fourth step (S23), phenomena such as hydrogen (H) being desorbed from silicon (Si) and outgassing into hydrogen gas (H2) do not occur, thereby improving the operating characteristics and reliability of the semiconductor device.
[0105] Next, specific embodiments will be described with reference to FIGS. 8a and 8b. The process conditions of the present invention are not limited to the following embodiments.
[0106] Referring together with FIG. 5, FIG. 8a is a graph showing the infrared absorption spectrum of a silicon film formed by the first step (S20), and FIG. 8b is a graph showing the infrared absorption spectrum of a silicon film after performing the first to third steps (S20, S21, S22).
[0107] In the second step (S21), microwaves may be irradiated onto the silicon film. In the third step (S22), the silicon film irradiated with microwaves may be immersed in liquid heavy water. In the second step (S21), the step of irradiating microwaves onto the silicon film (S211) lasted for 15 seconds, and the step of stopping microwave irradiation onto the silicon film (S212) lasted for 45 seconds. In the step of irradiating microwaves (S211), microwaves were irradiated onto the silicon film under conditions of a frequency of 2.45 GHz, a wavelength of 0.122 m, and a power of 700 W. The step of irradiating microwaves (S211) and the step of stopping microwave irradiation (S212) were performed alternately, and each was repeated 10 times.
[0109] Referring to Fig. 8a, before the Si-H bond removal reaction, 2,280 cm -1 to 2,050cm -1 and 3,400cm -1 to 3,200cm -1An absorption peak appears at [location]. In the silicon film prior to the Si-H bond removal reaction, Si-H bonds (2,280 cm⁻¹) appear. -1 to 2,050cm -1 ) and OH bonds (3,400 cm -1 to 3,200 cm -1 It can be seen that ) exists.
[0111] Referring to Fig. 8b, after the Si-H bond removal reaction, 2,280 cm -1 to 2,050cm -1 The absorption peak at decreases, but at 3,400 cm -1 to 3,200cm -1 The absorption peak at is maintained. Accordingly, the Si-H bond (2,280 cm⁻¹) -1 to 2,050cm -1 ) decreases, and OH bonds (3,400 cm -1 to 3,200cm -1 It can be seen that ) is maintained. Unlike the embodiments of FIGS. 4a and 4b, the Si-D bond (1,639 cm -1 ) is not observed. Through this, it can be confirmed that the Si-H bond is removed instead of being substituted with Si-D.
[0113] In exemplary embodiments, the silicon film of FIG. 8a is Si x O y H z It can have the chemical formula (where x, y, and z are real numbers greater than or equal to 0 and less than 1, and x+y+z=1). The silicon film of Fig. 8b is Si p O q H rIt may have a chemical formula of (where p, q, and r are real numbers greater than or equal to 0 and less than 1, and p+q+r=1). The hydrogen atoms in the chemical formula of FIG. 8a may include both hydrogen originating from Si-H bonds and hydrogen originating from OH bonds. In the silicon film of FIG. 8a, the Si-H bonds formed by stable covalent bonds are maintained, and the unstable Si-H bonds electrically bonded to the unpaired electrons of silicon are removed, thereby forming the silicon film of FIG. 8b. Therefore, the ratio of hydrogen atoms in the chemical formula of FIG. 8b may be smaller than the ratio of hydrogen atoms in the chemical formula of FIG. 8a, and the following Equations 5 to 7 may be satisfied.
[0115] [Equation 5]
[0116] x <p
[0117] [Equation 6]
[0118] y
[0119] [Equation 7]
[0120] z>r
[0122] The chemical formulas described above are exemplary examples and may further include elements or impurities other than hydrogen (H), oxygen (O), and silicon (Si).
[0124] FIG. 9 is a process flow diagram schematically illustrating a substrate processing method (30) according to exemplary embodiments.
[0126] The substrate processing method (30) of FIG. 9 may include a first step (S30) of forming a silicon film on a substrate, a second step (S31) of irradiating microwaves onto the silicon film, a third step (S32) of immersing the substrate in liquid heavy water, and a fourth step (S33) of irradiating microwaves onto the silicon film immersed in liquid heavy water. The substrate processing method (30) of FIG. 9 may further include a fifth step (S34) of performing a subsequent process on the substrate.
[0127] The substrate processing method (30) of FIG. 9 differs from the substrate processing method (20) of FIG. 5 above in that it performs a second step (S31) of irradiating microwaves onto a silicon film and a third step (S32) of immersing the substrate in liquid heavy water, followed by a fourth step (S31) of irradiating microwaves onto a silicon film. That is, the substrate processing method (30) of FIG. 9 may include steps (S31, S33) of irradiating microwaves onto a silicon film before and after the step (S32) of immersing the substrate in liquid heavy water. The second step (S31) of irradiating microwaves onto a silicon film may be performed in air, and the fourth step (S33) of irradiating microwaves onto a silicon film may be performed in an environment of liquid heavy water.
[0129] In the second step (S31), by irradiating the silicon film with microwaves first, the silicon film can be raised to a temperature of, for example, about 423K to 443K. By doing so, impurities adsorbed on the silicon film can be desorbed.
[0130] In the third step (S32), by immersing the heated silicon film in liquid heavy water at room temperature, unstable Si-H bonds of the silicon film can be removed, and unsaturated bonds can be reduced through the rearrangement (surface organization) of the surface Si layer.
[0131] In the fourth step (S33), by irradiating a silicon film immersed in liquid heavy water with microwaves a second time, Si-H bonds that did not react with the first microwave irradiation in the second step (S31) can be replaced with Si-D bonds. Additionally, silicon (Si) atoms having unsaturated bonds can be oxidized to have Si-O-Si bonds. By doing so, unstable bonds present in the silicon film can be removed or replaced with stable bonds, thereby improving the driving characteristics and reliability of the semiconductor device.
[0133] The present invention is not limited by the embodiments described above and the attached drawings, but is intended to be limited by the appended claims. Accordingly, various substitutions, modifications, changes, and combinations of embodiments may be made by those skilled in the art without departing from the technical spirit of the invention as described in the claims, and such are also to be considered to fall within the scope of the present invention. Explanation of the symbols
[0135] E1: First electrode E2: Second electrode G: Gas supply unit 2: Substrate 3: Silicone membrane 4: Bath 5: Liquid heavy water 6: Second substrate holder 7: Microwave generator 8: Microwave
Claims
Claim 1 A substrate processing method comprising: a step of forming a silicon film on a substrate; a step of soaking the substrate on which the silicon film is formed in liquid heavy water (D2O); and a first microwave irradiation step of irradiating microwaves onto the silicon film immersed in the liquid heavy water, wherein the Si-H bonds of the silicon film are replaced with Si-D bonds by the first microwave irradiation step. Claim 2 A substrate processing method according to claim 1, wherein the first microwave irradiation step comprises the step of irradiating microwaves to the silicon film for a first time period and the step of stopping microwave irradiation to the silicon film for a second time period. Claim 3 A substrate processing method according to claim 1, wherein the first microwave irradiation step is performed at least once and no more than 15 times. Claim 4 A substrate processing method according to claim 1, further comprising a second microwave irradiation step performed between the step of forming the silicon film and the step of immersing the substrate in liquid heavy water, wherein the silicon film is irradiated with microwaves. Claim 5 A substrate treatment method comprising the steps of: forming a silicon film on a substrate; irradiating the silicon film with microwaves; and immersing the silicon film in liquid heavy water (D2O), wherein the Si-H bonds of the silicon film are replaced with Si-D bonds by the step of irradiating the silicon film with microwaves. Claim 6 A substrate processing method according to claim 5, wherein the step of immersing the silicon film in liquid heavy water is performed after the step of irradiating the silicon film with microwaves. Claim 7 A substrate processing method according to claim 6, wherein, in the step of irradiating the silicon film with microwaves, the silicon film has a temperature of 423K to 443K. Claim 8 A method for treating a substrate, comprising: a step of forming a first material layer on a substrate; and a step of irradiating the first material layer with microwaves in an environment of liquid heavy water (D2O) to form a second material layer, wherein the first material layer comprises a first compound of Formula 1 below, the second material layer comprises a second compound of Formula 2 below, the first material layer comprises a Si-H functional group, and by irradiating with microwaves, the Si-H functional group is substituted with a Si-D functional group, and the second material layer comprises the Si-D functional group. [Formula 1] Si x O y H z (x, y, z are real numbers greater than or equal to 0 and less than 1, and x+y+z=1)[Chemical Formula 2]Si a O b H c D d (a, b, c, d are real numbers greater than or equal to 0 and less than 1, and a+b+c+d=1) Claim 9 A substrate processing method satisfying z=c+d; x=a; and y=b in claim 8. Claim 10 A substrate treatment method according to claim 8, wherein the first material layer further comprises an OH functional group and the second material layer further comprises an OH functional group.
Citation Information
Patent Citations
Manufacture of semiconductor
JP1996316483A
Semiconductor device and method of manufacturing thesame
KR1020040048361A
Heating device and method for assisting cement test piece in solidification
CN105196409A
Method for improving interface reactions at semiconductor surfaces
WO2008020403A2