Transparent microcrystalline glass and chemically strengthened microcrystalline glass
By controlling the grain size distribution and chemical strengthening treatment in the glass-ceramics, the problem in the existing technology that the glass-ceramics cannot meet the optical performance and mechanical strength requirements at the same time is solved, and a balance between high mechanical strength and excellent optical properties is achieved, which is suitable for Screen protective glass for electronic devices.
Patent Information
- Application Number
- PCT/CN2024/077739
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-21
- Filing Date
- 2024-02-20
- Publication Date
- 2024-10-24
AI Technical Summary
When controlling the grain size and crystal composition of existing glass-ceramics, it is difficult to meet the requirements of excellent optical properties and mechanical strength at the same time, and inappropriate control of grain size will affect the mechanical strength.
By controlling the grain size distribution in the crystallized glass with lithium feldspar and lithium disilicate as the main crystal phases, it is ensured that the longest dimension of the average grains is between 16nm and 40nm, and the proportion of grains with the longest dimension of 20nm≤≤100nm is The ratio is greater than or equal to 40% and less than or equal to 90%, 10nm ≤ longest dimension < 20nm, the proportion of crystal grains is greater than 0% and less than or equal to 60%, 50nm ≤ longest dimension < 100nm, the proportion of crystal grains is less than or equal to 10%, combined with chemical strengthening treatment, to obtain excellent optical properties and mechanical strength of transparent glass-ceramics.
It achieves a balance between the high mechanical strength and excellent optical properties of glass-ceramics, further improves the optical properties and mechanical strength through chemical strengthening treatment, and is suitable for screen protection glass for electronic devices.
Smart Images

Figure CN2024077739_24102024_PF_FP_ABST
Abstract
Description
Transparent microcrystalline glass and chemically strengthened microcrystalline glass
[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office of China on February 21, 2023, with application number 202310146826.8 and invention name “A Transparent Microcrystalline Glass and Chemically Strengthened Microcrystalline Glass”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the technical field of microcrystalline glass, and in particular to a transparent microcrystalline glass and a chemically strengthened microcrystalline glass. Background Art
[0003] Glass-ceramics are typically produced by adding a certain amount of nucleating agents, such as ZrO2, P2O5, HfO2, TiO2, and Cr2O3, to a glass body. The glass is then held at a certain temperature for a period of time, inducing crystallization through the nucleating agents and precipitating the target crystalline phase. This results in the desired glass-ceramics. The production of glass-ceramics typically requires heat treatment of the base glass. By varying the heat treatment temperature and holding time, glass-ceramics with varying crystallization states can be obtained.
[0004] At present, the petalite crystal phase (LiAlSi4O 10 Glass-ceramics with primary crystalline phases of 2,4-dioxane (Li₂Si₂O₅) and lithium disilicate (Li₂Si₂O₅) have begun to be used in electronic devices. Glass-ceramics used in electronic devices, particularly as screen protectors, require not only excellent optical properties but also exceptional mechanical strength.
[0005] Summary of the Invention
[0006] In order to make microcrystalline glass meet the requirements of optical properties and mechanical strength, the common practice in the industry is to strictly control the size and crystal composition of the grains. For example, the grain size in microcrystalline glass is controlled within a certain range, such as within 100nm, and the content of crystals that are detrimental to optical properties in microcrystalline glass is strictly controlled.
[0007] However, simply controlling the grain size to less than 100 nm and controlling the crystal phase composition cannot ensure that microcrystalline glass that meets the requirements of excellent optical properties (including transmittance and b-value) and mechanical strength properties will be obtained. In addition, inappropriate grain size control will often have an adverse effect on the mechanical strength properties of microcrystalline glass.
[0008] In response to the above technical problems, we studied the relationship between the crystal phase conditions in microcrystalline glass, such as the composition of the crystal phase in microcrystalline glass, grain size and grain size distribution, and the optical properties and mechanical properties of microcrystalline glass. We then found that for microcrystalline glass with petalite and lithium disilicate as the main crystal phases, controlling the size distribution of the grains it contains will have a stronger positive effect on transmittance and mechanical strength. In particular, microcrystalline glass that meets specific grain distribution requirements can ensure high mechanical strength and excellent optical properties.
[0009] The purpose of this application is to provide a transparent glass-ceramic and chemically strengthened glass-ceramic with excellent optical properties and mechanical strength. The specific technical solutions include:
[0010] In a first aspect, a transparent glass-ceramic is provided, wherein the main crystalline phase of the transparent glass-ceramic includes a petalite crystalline phase and a lithium silicate crystalline phase; and the grains of the crystalline phase in the transparent glass-ceramic meet the following characteristics:
[0011] The average longest dimension of the grains ranges from 16 nm to 40 nm;
[0012] The number of grains with a maximum dimension of 20 nm or less and less than 100 nm accounts for greater than or equal to 40% and less than or equal to 90%.
[0013] The number of grains with a maximum dimension of 10 nm or less and a maximum dimension of 20 nm is greater than 0% and less than or equal to 60%.
[0014] The number of grains with a maximum dimension of 50 nm or less and a maximum dimension of 100 nm accounts for less than or equal to 10%.
[0015] The grain ratio refers to the proportion of grains within a certain dimensional range to the total number of grains. By ensuring that the average longest dimension of the grains meets this range, combined with ensuring that the grain distribution meets this requirement, a transparent glass-ceramic with excellent optical properties, such as high transmittance and a low b-value, as well as excellent mechanical strength, can be obtained. Furthermore, chemical strengthening treatment of the transparent glass-ceramic can yield chemically strengthened glass-ceramics with excellent optical and mechanical strength properties.
[0016] In some embodiments of the present application, the lithium silicate crystalline phase is a lithium disilicate crystalline phase, or the lithium silicate crystalline phase is a lithium monosilicate crystalline phase and a lithium disilicate crystalline phase; the lithium silicate crystalline phase is preferably a lithium disilicate crystalline phase.
[0017] In some embodiments of the present application, based on the mass of the transparent glass-ceramics, the total crystalline phase content of the transparent glass-ceramics is greater than or equal to 70 wt%, that is, the total mass of the crystalline phase accounts for at least 70 wt% of the total mass of the transparent glass-ceramics.
[0018] In some embodiments of the present application, at a thickness of 0.64 mm, the optical b value of the transparent glass-ceramics is 0.10 to 1.00, preferably 0.30 to 1.00.
[0019] In some embodiments of the present application, at a thickness of 0.64 mm, the transmittance of the transparent micro-ceramic glass for light with a wavelength of 400 nm is greater than or equal to 85%, preferably greater than or equal to 88%.
[0020] In some embodiments of the present application, at a thickness of 0.64 mm, for light in the wavelength range of 400 nm to 740 nm, the average transmittance of the transparent microcrystalline glass is greater than or equal to 86%, preferably greater than or equal to 90%.
[0021] In some embodiments of the present application, at a thickness of 0.7 mm, the single-rod static pressure strength of the transparent microcrystalline glass is greater than or equal to 250 N, preferably 250 N to 600 N, and more preferably 270 N to 600 N.
[0022] In some embodiments of the present application, the composition of the transparent microcrystalline glass includes, expressed in molar percentage of oxides: SiO2 65.00mol%-74.00mol%, Al2O3 3.00mol%-5.60mol%, Li2O 15.00mol%-23.00mol%, P2O5 0.50mol%-1.50mol%, ZrO2 0.80mol%-3.50mol%, ZnO 0.00mol%-1.00mol%, MgO 0.00mol%-1.50mol%, Na2O 0.00mol%-4.00mol%, B2O3 0.00mol%-2.00mol%, K2O 0.00mol%-1.00mol%, CaO 0.00mol%-2.00mol%, SrO 0.00mol%-0.50mol%, BaO 0.00mol%-1.00mol%.
[0023] In the present application, the transparent microcrystalline glass is obtained by heat treatment of substrate glass, and the heat treatment includes nucleation treatment and / or crystallization treatment. It should be understood that when the substrate glass is heat treated, one-step heat treatment can be performed, or two-step or multi-step heat treatment can be performed. If a one-step heat treatment is performed, it means that the nucleation treatment is not performed separately, and the nucleation and target crystal growth are directly performed in a one-step heating process, which can be understood as directly performing a crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, that is, a nucleation treatment (that is, nucleation treatment) is performed first, and then a target crystal growth treatment (that is, crystallization treatment) is performed.
[0024] It should be understood that, in this application, the composition of the substrate glass, measured in molar percentage of oxides, is the same or substantially the same as that of the transparent glass-ceramics. Forming methods for the substrate glass include, but are not limited to, float, overflow, rolling, or casting. In some embodiments of this application, a clarifier may be added to the substrate glass during preparation. The clarifier includes, but is not limited to, SnO2, Sb2O3, or NaCl. The amount of clarifier added may range from 0.01 mol% to 2.00 mol%, preferably from 0.01 mol% to 1.50 mol%, based on the mass of the substrate glass.
[0025] In a second aspect, a chemically strengthened glass-ceramics is provided, which is obtained by subjecting the transparent glass-ceramics in any embodiment of the first aspect to a chemical strengthening treatment.
[0026] In some embodiments of the present application, the salt bath for chemical strengthening treatment is a molten salt containing potassium salt and / or sodium salt, wherein the salt bath contains 0wt% to 1wt% of lithium salt; the temperature of the salt bath is 380°C to 550°C, preferably 400°C to 500°C; and the chemical strengthening treatment time is 1 to 48 hours, preferably 1 hour to 12 hours. The potassium salt includes one or more of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate; the sodium salt includes one or more of sodium nitrate, sodium sulfate, and sodium carbonate, preferably sodium nitrate; and the lithium salt includes one or more of lithium nitrate, lithium sulfate, and lithium carbonate, preferably lithium nitrate.
[0027] In some embodiments of the present application, DOL_0 of the chemically strengthened glass-ceramics is greater than or equal to 0.18t and less than or equal to 0.25t, where t is the thickness of the chemically strengthened glass-ceramics.
[0028] In some embodiments of the present application, the CS_50 of 0.7 mm thick chemically strengthened glass-ceramics is greater than 90 MPa, preferably greater than 90 MPa and less than or equal to 300 MPa, and more preferably 95 MPa to 300 MPa.
[0029] In some embodiments of the present application, the chemically strengthened microcrystalline glass with a thickness of 0.7 mm is subjected to a drop resistance test using 80-grit sandpaper, and the average sandpaper drop resistance height of the chemically strengthened microcrystalline glass is greater than or equal to 80 cm; the average sandpaper drop resistance height is based on tests of at least 10 identical chemically strengthened microcrystalline glass samples.
[0030] In some embodiments of the present application, the Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 670 kgf / mm 2 , preferably 670kgf / mm 2 Up to 800kgf / mm 2 .
[0031] In a third aspect, a glass device is provided, which is made of the transparent microcrystalline glass in any embodiment of the first aspect, or made of the chemically strengthened microcrystalline glass in any embodiment of the second aspect.
[0032] In a fourth aspect, an electronic device is provided, comprising the transparent microcrystalline glass according to any embodiment of the first aspect, or the chemically strengthened microcrystalline glass according to any embodiment of the second aspect.
[0033] In some embodiments of the present application, the electronic device includes at least one of a mobile phone, a tablet computer, a smart wearable, a display, and a television.
[0034] One or more technical solutions of this application include the following beneficial effects:
[0035] The present application provides transparent glass-ceramics whose primary crystalline phases include petalite and lithium silicate. In addition to the average grain longest dimension satisfying a range of 16 nm to 40 nm, the grain size distribution also meets specific characteristic requirements. The combination of these two conditions results in a crystalline structure that ensures the transparent glass-ceramics possess high mechanical strength and excellent optical properties. The transparent glass-ceramics provided herein that meet the specific grain size distribution requirements, when chemically strengthened through chemical strengthening treatment, also exhibit excellent optical properties and mechanical strength.
[0036] Of course, any product implementing the present application does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0038] FIG1 is a surface morphology image of the transparent glass-ceramics in Example 6 taken with a scanning electron microscope (SEM);
[0039] FIG2 is a surface morphology of the glass-ceramics in Comparative Example 2 taken with a scanning electron microscope (SEM);
[0040] FIG3 is a surface morphology of the glass-ceramics in Comparative Example 5 taken with a scanning electron microscope (SEM);
[0041] FIG4 is a graph showing the transmittance of the glass-ceramics in Example 4, Example 7, and Comparative Example 4 to light in the wavelength range of 360 nm to 740 nm;
[0042] FIG5 is a differential scanning calorimetry (DSC) test curve of the substrate glass in Example 7;
[0043] FIG6 is an XRD pattern of the transparent glass-ceramics in Example 1;
[0044] FIG7 is an XRD pattern of the transparent glass-ceramics in Example 10. DETAILED DESCRIPTION
[0045] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and examples. It is apparent that the described examples are only a portion of the embodiments of this application, rather than all of them. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.
[0046] Explanation of terms
[0047] Base glass: refers to glass that has not been subjected to nucleation, crystallization and strengthening treatments, or is also called basic glass.
[0048] Glass-ceramics, also known as glass ceramics or crystallized glass, are a type of solid composite material composed of both a glass phase and a microcrystalline / crystalline phase. These phases are produced through the targeted and controlled crystallization of a glass substrate. The microcrystalline phase is sometimes referred to as the crystalline phase or crystalline phase in other literature.
[0049] Chemically strengthened glass-ceramics are solid composite materials obtained by chemically strengthening glass-ceramics. It should be understood that during high-temperature chemical strengthening, alkali metal ions with large ionic radii (such as potassium and sodium ions) in the salt bath / molten salt / molten salt replace alkali metal ions with smaller ionic radii (such as sodium and lithium ions) in the glass-ceramics, resulting in a volume difference in the exchanged ions and compressive stress on the surface of the glass-ceramics.
[0050] The longest dimension of a grain: For a certain grain, the maximum value of the grain length in each dimension is the longest dimension of the grain.
[0051] Average longest dimension of grains: the average value of the longest dimensions of all grains contained in the glass-ceramic.
[0052] Total crystalline phase content: the percentage of the total mass of the crystalline phase in the microcrystalline glass to the total mass of the microcrystalline glass.
[0053] Optical b-value: A value used to characterize the yellow-blue color of glass-ceramics. The optical b-value in this application refers to the b-value of transmitted light. A positive optical b-value indicates a blue tint.
[0054] Single rod static pressure strength: the maximum value of the pressure that the microcrystalline glass can withstand from the extrusion rod, measured in N. When the pressure exceeds this value, the microcrystalline glass will break.
[0055] DOL_0: Depth of the compressive stress layer, also known as the depth of the compressive stress layer, refers to the distance from any main surface of the microcrystalline glass to the position close to the surface where the compressive stress is zero.
[0056] CS_50: Compressive stress at a depth of 50 μm from the main surface of the glass-ceramic. The main surface here refers to the surface with the largest surface area in the glass-ceramic brick or glass-ceramic sheet, such as the top and bottom surfaces of the glass-ceramic sheet.
[0057] In the prior art, in order to obtain a glass-ceramic, a certain amount of nucleating agent, such as ZrO2, P2O5, HfO2, TiO2, Cr2O3, etc., is usually added to the glass body (e.g., substrate glass or base glass), and then the glass is kept warm at a certain temperature for a period of time to induce crystallization of the glass through the nucleating agent. The formation and growth of crystals require overcoming certain energy barriers. Therefore, the acquisition of glass-ceramics usually requires heat treatment of the substrate glass. Since the transformation from substrate glass to glass-ceramics is a continuous non-uniform change process, and there are heat absorption and heat release phenomena in this process, glass-ceramics with different crystallization states can be obtained by changing the temperature and holding time of the heat treatment.
[0058] With the continuous deepening of research on microcrystalline glass, in order to obtain microcrystalline glass with excellent performance in various fields, it is often necessary to add some other oxides to the substrate glass system, such as alkali metal oxides, alkaline earth metal oxides, rare earth elements, etc., which makes the composition of the substrate glass more complex, resulting in the substrate glass precipitating not a single crystal, but multiple crystals during the crystallization process.
[0059] In order to obtain transparent microcrystalline glass that meets the requirements of electronic device screen protection glass, the common practice in the industry is to strictly control the size and crystal composition of the grains. 10 Taking transparent microcrystalline glass with (petalite) as the main crystal phase as an example, in order to obtain a transparent microcrystalline glass with a light transmittance greater than 85% in the 400nm to 1000nm band at a thickness of 0.64mm, the common practice in the industry is to control its grain size within 100nm, and to strictly control the content of crystal phases such as SiO2 and Li2SiO3 that are detrimental to optical properties. However, after further research, the inventors found that simply by controlling the grain size to be less than 100nm and controlling the crystal phase composition, it is not possible to ensure that a transparent microcrystalline glass that meets the requirements of excellent optical properties (including transmittance and optical b value) and mechanical strength performance is obtained, and inappropriate grain size control often affects the mechanical strength of the transparent microcrystalline glass. Therefore, how to ensure that a transparent microcrystalline glass with excellent optical properties and mechanical strength properties is obtained, containing Li2Si2O5 and LiAlSi4O 10Transparent microcrystalline glass with a main crystalline phase is a technical problem that the inventors are committed to solving.
[0060] In response to the above technical problems, the inventors studied the relationship between the crystal phase conditions in microcrystalline glass, such as the composition of the crystal phase in microcrystalline glass, grain size and grain size distribution, and the optical properties and mechanical properties of microcrystalline glass, and then found that: for microcrystalline glass with lithium feldspar and lithium disilicate as the main crystal phases, controlling the grain size distribution it contains will have a stronger positive effect on transmittance and mechanical strength. In particular, microcrystalline glass that meets specific grain distribution requirements can ensure high mechanical strength and excellent optical properties.
[0061] In some embodiments of the present application, a transparent microcrystalline glass and chemically strengthened microcrystalline glass having excellent optical properties (such as transmittance, b-value) and mechanical strength properties are provided, as well as glass devices made of transparent microcrystalline glass or chemically strengthened microcrystalline glass, and electronic devices including transparent microcrystalline glass or chemically strengthened microcrystalline glass.
[0062] In some embodiments of the present application, a transparent microcrystalline glass is provided, wherein the main crystalline phase of the transparent microcrystalline glass comprises a petalite crystalline phase (LiAlSi4O 10 ) and lithium silicate crystalline phase; the "main crystalline phase" (or also called main crystalline phase) here refers to a crystalline phase with a higher weight content than other crystalline phases present in the transparent microcrystalline glass; the grains of the crystalline phase in the transparent microcrystalline glass meet the following characteristics:
[0063] The average longest dimension of the grains ranges from 16 nm to 40 nm;
[0064] The number of grains with a maximum dimension of 20 nm ≤ < 100 nm (hereinafter referred to as grains A) accounts for greater than or equal to 40% and less than or equal to 90%;
[0065] The number of grains with a maximum dimension of 10 nm ≤ < 20 nm (hereinafter referred to as grains B) is greater than 0% and less than or equal to 60%;
[0066] The number of grains with a longest dimension of 50 nm ≤ < 100 nm (hereinafter referred to as grains C) accounts for less than or equal to 10%.
[0067] In some embodiments of the present application, in the transparent glass-ceramics, the average longest dimension L of the grains is aveIt can be 16nm, 20nm, 22nm, 25nm, 28nm, 30nm, 32nm, 35nm, 38nm or 40nm, or a numerical value within the numerical range consisting of any two of the above numerical values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. In some embodiments of the present application, the proportion of grain A can be 40%, 50%, 60%, 70%, 80%, 85%, 89% or 89.9%, or a numerical value within the numerical range consisting of any two of the above numerical values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. In some embodiments of the present application, the proportion of grain B can be 0.1%, 1%, 5%, 10%, 20%, 30%, 40%, 50% or 60%, or a numerical value within the numerical range consisting of any two of the above numerical values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. In some embodiments of the present application, the proportion of grain C can be 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, or a numerical value within the numerical range consisting of any two of the above numerical values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It is understood that in the transparent microcrystalline glass provided by the present application, in addition to grains A and grains B, it can also include grains with a longest dimension less than 10nm (hereinafter referred to as grains D) and grains with a longest dimension greater than or equal to 100nm (hereinafter referred to as grains E), and the sum of the number of grains A, grains B, grains D and grains E is 100%, wherein the number of grains D and grains E is not limited in this application, as long as the purpose of the present application can be achieved. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.
[0068] By making the average longest dimension L aveMeeting the above range requirements, combined with making the grain distribution meet the above requirements, can ensure that a transparent microcrystalline glass with excellent optical properties, such as high transmittance and low b value, and excellent mechanical strength properties are obtained. At the same time, the above transparent microcrystalline glass is chemically strengthened through a strengthening treatment to obtain a chemically strengthened microcrystalline glass with excellent optical properties and mechanical strength properties. The inventors found that: when the proportion of smaller grains in the microcrystalline glass is relatively large, although the optical properties of the microcrystalline glass are good, the mechanical strength properties cannot reach a better level; and when the proportion of larger grains in the microcrystalline glass is relatively large, the optical properties of the microcrystalline glass will deteriorate. In order to achieve a better balance between the optical properties and mechanical strength of the microcrystalline glass, the crystal grains contained in the transparent microcrystalline glass provided in this application must meet specific size distribution requirements. By regulating the proportion of grains A, B and C within a specific range, it can be ensured that the obtained transparent microcrystalline glass has excellent optical properties and mechanical strength properties.
[0069] In this application, when testing the grain length of the transparent microcrystalline glass, the surface morphology of the microcrystalline glass polished sheet is analyzed using particle size analysis software to obtain the longest dimension of each grain, and then the average grain longest dimension L is obtained. ave The particle size analysis software may include but is not limited to ImageJ software, Nano Measure software, etc.
[0070] In some embodiments of the present application, the lithium silicate crystalline phase is a lithium disilicate crystalline phase (Li2Si2O5), or the lithium silicate crystalline phase is a lithium silicate crystalline phase (Li2SiO3) and a lithium disilicate crystalline phase (Li2Si2O5); the lithium silicate crystalline phase is preferably a lithium disilicate crystalline phase.
[0071] In some embodiments of the present application, depending on the composition of the substrate glass, the primary crystalline phases include petalite and lithium silicate, but β-quartz (SiO2) and / or lithium phosphate (Li3PO4) may also be present as secondary crystalline phases. The content of the secondary crystalline phases is less than or equal to 10% based on the mass of the transparent microcrystalline glass.
[0072] In some embodiments of the present application, based on the mass of the transparent glass-ceramics, the total crystalline phase content of the transparent glass-ceramics accounts for greater than or equal to 70wt%, that is, the total mass of the crystalline phase accounts for at least 70wt% of the total mass of the transparent glass-ceramics, preferably greater than or equal to 70wt% and less than 100wt%. In some embodiments, based on the mass of the transparent glass-ceramics, the total crystalline phase content of the transparent glass-ceramics can be 70wt%, 72wt%, 74wt%, 75wt%, 76wt%, 78wt%, 80wt%, 82wt%, 84wt%, 85wt%, 86wt%, 88wt%, 90wt%, 92wt%, 95wt% or 99wt%, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. The total crystalline phase content of the transparent microcrystalline glass is within the above range, and the obtained transparent microcrystalline glass has excellent optical properties and mechanical strength properties. The obtained transparent microcrystalline glass can be chemically strengthened to prepare chemically strengthened microcrystalline glass that meets the requirements of screen protection cover of electronic equipment.
[0073] In this application, when testing the total crystalline content of glass-ceramics, the glass-ceramics are first ground into a fine powder with a maximum particle size of less than 75 μm. The fine powder is then tested to obtain XRD diffraction data. The XRD diffraction data is then fitted and calculated using analysis software to obtain the total crystalline content of the glass-ceramics. The above-mentioned analysis software may include but is not limited to Gsas, Fullprof, Maud, Jade, etc.
[0074] In some embodiments of the present application, at a thickness of 0.64 mm, the optical b value of the transparent glass-ceramics is 0.10 to 1.00, preferably 0.30 to 1.00. In some embodiments, the optical b value of the transparent glass-ceramics with a thickness of 0.64 mm can be 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90 or 1.00, or a numerical value within the numerical range consisting of any two of the above numerical values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. Thereby ensuring that the transparent glass-ceramics provided by the present application has excellent optical properties.
[0075] In some embodiments of the present application, at a thickness of 0.64 mm, for light of 400 nm wavelength, the transmittance of the transparent glass-ceramics is greater than or equal to 85%, preferably greater than or equal to 88%. In some embodiments, the transmittance of the transparent glass-ceramics with a thickness of 0.64 mm for light of 400 nm can be 85%, 86%, 87%, 88%, 89%, 90% or 91%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The transmittance of glass-ceramics for 400nm light will affect the color presented by the glass-ceramics. If the transmittance of glass-ceramics for 400nm light is too low (for example, less than 85%), even if its average transmittance for light in the visible light band (for example, 400nm to 740nm) is high (for example, greater than 90%), the glass-ceramics may still present an undesirable color for display glass, such as a bluish-purple color, thereby limiting the application of the glass-ceramics. The transparent glass-ceramics provided in this application has a transmittance of greater than or equal to 85% for 400nm light, which is conducive to presenting the colorless and transparent effect desired for display glass, and is also conducive to obtaining transparent glass-ceramics with excellent optical properties.
[0076] In some embodiments of the present application, at a thickness of 0.64 mm, for light in the wavelength range of 400 nm to 740 nm, the average transmittance of the transparent glass-ceramics is greater than or equal to 86%, preferably greater than or equal to 90%. In some embodiments, the average transmittance of the transparent glass-ceramics with a thickness of 0.64 mm for light in the wavelength range of 400 nm to 740 nm can be 86%, 87%, 88%, 89%, 90%, 91%, 92% or 93%, or a value within the range of values consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The transparent glass-ceramics provided in the present application has an excellent transparent effect.
[0077] In any of the above embodiments of the present application, at a thickness of 0.7 mm, the single-rod static pressure strength of the transparent glass-ceramics is greater than or equal to 250 N, preferably greater than or equal to 250 N and less than or equal to 600 N. In some embodiments, the single-rod static pressure strength of the transparent glass-ceramics with a thickness of 0.7 mm can be 250 N, 300 N, 350 N, 400 N, 450 N, 500 N, 550 N or 600 N, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The transparent glass-ceramics provided in the present application has excellent mechanical strength properties in addition to having excellent optical properties.
[0078] The present application has no particular restrictions on the composition of the transparent microcrystalline glass in any of the above embodiments, as long as it can meet the above-mentioned grain size distribution. In some embodiments of the present application, the composition of the transparent microcrystalline glass includes, expressed in molar percentage of oxides: SiO2 65.00mol%-74.00mol%, Al2O3 3.00mol%-5.60mol%, Li2O 15.00mol%-23.00mol%, P2O5 0.50mol%-1.50mol%, ZrO2 0.80mol%-3.50mol%, ZnO 0.00mol%-1.00mol%, MgO 0.00mol%-1.50mol%, Na2O 0.00mol%-4.00mol%, B2O3 0.00mol%-2.00mol%, K2O 0.00mol%-1.00mol%, CaO 0.00mol%-2.00mol%, SrO 0.00mol%-0.50mol%, BaO 0.00mol%-1.00mol%.
[0079] SiO2, as a forming oxide of the glass network, is an indispensable component of the glass network structure. The addition of SiO2 can increase the stability and mechanical strength of the glass-ceramics. In the present application, the content of SiO2 is between 65.00 mol% and 74.00 mol%, which is beneficial to ensure the strength and formability of the transparent glass-ceramics and increase the stability of the transparent glass-ceramics. In some embodiments, expressed as a molar percentage of oxide, the content of SiO2 in the transparent glass-ceramics can be 65.00 mol%, 66.00 mol%, 67.00 mol%, 68.00 mol%, 69.00 mol%, 70.00 mol%, 71.00 mol%, 72.00 mol%, 73.00 mol% or 74.00 mol%, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass having the desired properties of the present application can be obtained.
[0080] Al2O3 is an intermediate oxide in glass formation, which can improve the chemical stability of microcrystalline glass. At the same time, since the volume of [AlO4] tetrahedron is larger than that of [SiO4] tetrahedron, it can provide more space for ion exchange during chemical strengthening treatment, thereby promoting the progress of ion exchange. Therefore, in the present application, the content of Al2O3 is 3.00mol%-5.60mol%. In some embodiments, expressed as a molar percentage of oxide, the content of Al2O3 in the transparent microcrystalline glass can be 3.00mol%, 3.20mol%, 3.40mol%, 3.60mol%, 3.80mol%, 4.00mol%, 4.20mol%, 4.60mol%, 4.80mol%, 5.00mol%, 5.20mol%, 5.40mol% or 5.60mol%, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass having the desired properties of the present application can be obtained.
[0081] Li2O, Na2O and K2O, as the external oxides of the glass network, can provide free oxygen, destroy the network structure of the glass, thereby improving the viscosity of the glass and promoting the melting and clarification of the glass liquid. At the same time, Li2O and Na2O can also exchange ions with the molten salt bath. The content of the two is an important factor affecting the stress of microcrystalline glass. In addition, Li2O is also a lithium silicate and petalite (LiAlSi4O10 Therefore, the contents of Li2O, Na2O, and K2O in this application need to meet specific range requirements in order to obtain transparent microcrystalline glass with excellent mechanical properties.
[0082] In some embodiments, expressed as a molar percentage of oxide, the content of Li2O in the transparent glass-ceramics can be 15.00 mol%, 15.50 mol%, 16.00 mol%, 16.50 mol%, 17.00 mol%, 17.50 mol%, 18.00 mol%, 18.50 mol%, 19.00 mol%, 19.50 mol%, 20.00 mol%, 20.50 mol%, 21.00 mol%, 21.50 mol%, 22.00 mol%, 22.50 mol% or 23.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0083] In some embodiments, expressed as a molar percentage of oxide, the content of Na2O in the transparent glass-ceramics can be 0.00 mol%, 0.50 mol%, 1.00 mol%, 1.50 mol%, 2.00 mol%, 2.50 mol%, 3.00 mol%, 3.50 mol%, or 4.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0084] In some embodiments, expressed as a molar percentage of oxide, the content of KO in the transparent glass-ceramics can be 0.00 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, 0.50 mol%, 0.60 mol%, 0.70 mol%, 0.80 mol%, 0.90 mol%, or 1.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0085] B2O3 is generally used as a flux in the formation process of the substrate glass, which can reduce the high-temperature viscosity of the glass, accelerate the clarification of the glass, and reduce the crystallization ability of the glass. Therefore, the content of B2O3 in the present application is 0.00mol%-2.00mol%. In some embodiments, expressed as a molar percentage of the oxide, in the transparent microcrystalline glass, the content of B2O3 can be 0.00mol%, 0.20mol%, 0.40mol%, 0.60mol%, 0.80mol%, 0.90mol%, 1.00mol%, 1.20mol%, 1.40mol%, 1.60mol%, 1.80mol% or 2.00mol%, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained.
[0086] P2O5 can serve as a glass network forming oxide, promoting glass phase separation in the glass, thereby affecting the crystallization of the glass. In the present application, to ensure the precipitation of the target crystalline phase, the P2O5 content is 0.50mol%-1.50mol%. In some embodiments, expressed as a molar percentage of the oxide, the P2O5 content in the transparent glass-ceramics can be 0.50mol%, 0.60mol%, 0.70mol%, 0.80mol%, 0.90mol%, 1.00mol%, 1.10mol%, 1.2mol%, 1.30mol%, 1.4mol% or 1.50mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0087] ZrO2 is an intermediate oxide in glass formation that can improve the chemical stability of glass-ceramics, increase the hardness of glass-ceramics, and increase the scratch and drop resistance of glass-ceramics. At the same time, ZrO2 has a large accumulation effect on the glass structure due to its high cationic charge and strong electric field, and is often used as a nucleating agent in glass. In addition, ZrO2 can not only increase the strength and toughness of glass-ceramics, but also improve its corrosion resistance. Therefore, the content of ZrO2 in this application is 0.80mol%-3.50mol%. In some embodiments, expressed as a molar percentage of oxide, the content of ZrO2 in the transparent glass-ceramics can be 0.80mol%, 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol% or 3.50mol%, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the performance required by this application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the transparent microcrystalline glass or chemically strengthened microcrystalline glass having the desired properties of the present application can be obtained.
[0088] CaO, SrO, BaO, MgO, and ZnO, as oxides outside the glass network, help reduce the viscosity of the glass, inhibit glass crystallization during glass formation, and improve the low-temperature melting properties of the glass. In this application, the addition of appropriate amounts of CaO, SrO, BaO, MgO, and ZnO can achieve the effect of reducing the viscosity of the glass while not affecting the glass crystallization performance.
[0089] In some embodiments, expressed as a molar percentage of oxide, the ZnO content in the transparent glass-ceramics can be 0.00 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, 0.50 mol%, 0.60 mol%, 0.70 mol%, 0.80 mol%, 0.90 mol%, or 1.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0090] In some embodiments, expressed as a molar percentage of oxide, the content of MgO in the transparent glass-ceramics can be 0.00 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, 0.50 mol%, 0.60 mol%, 0.70 mol%, 0.80 mol%, 0.90 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol% or 1.50 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained.
[0091] In some embodiments, expressed as a molar percentage of oxide, the CaO content in the transparent glass-ceramics can be 0.00 mol%, 0.20 mol%, 0.40 mol%, 0.60 mol%, 0.80 mol%, 0.90 mol%, 1.00 mol%, 1.20 mol%, 1.40 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0092] In some embodiments, the SrO content in the transparent glass-ceramics, expressed as a molar percentage of the oxide, can be 0.00 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, or 0.50 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics having the desired properties of the present application can be obtained.
[0093] In some embodiments, expressed as a molar percentage of oxide, the BaO content in the transparent glass-ceramics can be 0.00 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, 0.50 mol%, 0.60 mol%, 0.70 mol%, 0.80 mol%, 0.90 mol%, or 1.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0094] In the present application, the transparent microcrystalline glass is obtained by heat treatment of substrate glass, and the heat treatment includes nucleation treatment and / or crystallization treatment. It should be understood that when the substrate glass is heat treated, one-step heat treatment can be performed, or two-step or multi-step heat treatment can be performed. If a one-step heat treatment is performed, it means that the nucleation treatment is not performed separately, and the nucleation and target crystal growth are directly performed in a one-step heating process, which can be understood as directly performing a crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, that is, a nucleation treatment (that is, nucleation treatment) is performed first, and then a target crystal growth treatment (that is, crystallization treatment) is performed.
[0095] It should be understood that, in this application, the composition of the substrate glass, measured in molar percentage of oxides, is the same or substantially the same as that of the transparent glass-ceramics. Forming methods for the substrate glass include, but are not limited to, float, overflow, rolling, or casting. In some embodiments of this application, a clarifier may be added to the substrate glass during preparation. The clarifier includes, but is not limited to, SnO2, Sb2O3, or NaCl. The amount of clarifier added may range from 0.01 mol% to 2.00 mol%, preferably from 0.01 mol% to 1.50 mol%, based on the mass of the substrate glass.
[0096] That is, in some embodiments of the present application, the composition of the substrate glass or transparent glass-ceramics may further include a clarifier. The content of the clarifier may be 0.01 mol%, 0.10 mol%, 0.20 mol%, 0.30 mol%, 0.40 mol%, 0.50 mol%, 0.60 mol%, 1.00 mol%, 1.20 mol%, 1.50 mol%, or 2.00 mol%, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. By selecting the above-mentioned clarifier and regulating the content of the clarifier, bubbles can be effectively discharged during the glass melting process (e.g., the melting process of the substrate glass).
[0097] The present application does not impose any particular restrictions on the preparation method of transparent microcrystalline glass, as long as the purpose of the present application can be achieved. In some embodiments of the present application, the preparation method of transparent microcrystalline glass may include but is not limited to the following steps: first, the raw materials are mixed, melt-molded, annealed and cooled according to the formula, and the molding methods include float, overflow, rolling or casting, etc., to obtain the substrate glass; then the substrate glass is heated to a nucleation temperature of T0, and the holding time is t0, and then the temperature is raised to a crystallization temperature of T1, and the holding time is t1, to obtain transparent microcrystalline glass. Preferably, the nucleation temperature T0 is T0'-15℃ to T0'+50℃, T0' is the temperature corresponding to the first endothermic peak in the DSC curve of the substrate glass, and the preferred holding time t0 is 180min to 300min. Preferably, the crystallization temperature T1 is T1'-60℃ to T1'+40℃, T1' is the temperature corresponding to the first exothermic peak in the DSC curve of the substrate glass, and the preferred holding time t1 is 60min to 500min. The present application does not limit the specific method of mixing and cooling, as long as the purpose of the present application can be achieved. The present application does not limit the temperature of the melting, which can be selected according to the specific formula.
[0098] In the present application, those skilled in the art can select the thickness of the transparent glass-ceramics according to their needs. Exemplarily, the thickness of the transparent glass-ceramics is 0.2 mm to 5.0 mm, preferably 0.2 mm to 2.0 mm. For example, the thickness of the transparent glass-ceramics can be 0.2 mm, 0.5 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.2 mm, 1.5 mm, 1.6 mm, 1.8 mm, 2.0 mm, 2.5 mm, 2.8 mm, 3.0 mm, 3.5 mm, 3.8 mm, 4.0 mm, 4.5 mm, 4.8 mm, or 5.0 mm, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the transparent glass-ceramics or chemically strengthened glass-ceramics having the performance required by the present application can be obtained.
[0099] In some embodiments of the present application, a chemically strengthened glass-ceramics is provided, which is obtained by subjecting the transparent glass-ceramics in any of the aforementioned embodiments to a chemical strengthening treatment.
[0100] It should be understood that due to the ion exchange that occurs during the chemical strengthening process, the transparent glass-ceramics are given specific stress characteristics. Therefore, after the chemical strengthening treatment, the mechanical properties of the transparent glass-ceramics in any of the aforementioned embodiments of the present application will be appropriately increased. However, the chemical strengthening process does not significantly affect the optical properties of the transparent glass-ceramics. Since the transparent glass-ceramics provided in this application have excellent optical properties and mechanical strength, the chemically strengthened glass-ceramics provided in this application also have excellent optical properties and mechanical strength. The above-mentioned chemical strengthening treatment is a chemical strengthening treatment known in the art, and this application is not limited thereto.
[0101] In some embodiments of the present application, the salt bath for chemical strengthening treatment is a molten salt containing potassium and / or sodium salts, wherein the salt bath contains 0 wt% to 1 wt% of a lithium salt; the potassium salt includes one or more of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate; the sodium salt includes one or more of sodium nitrate, sodium sulfate, and sodium carbonate, preferably sodium nitrate; and the lithium salt includes one or more of lithium nitrate, lithium sulfate, and lithium carbonate, preferably lithium nitrate. The temperature of the salt bath is 380°C to 550°C, preferably 400°C to 500°C. The chemical strengthening treatment time is 1 to 48 hours, preferably 1 to 12 hours. The "potassium and / or sodium salt" mentioned above refers to at least one of potassium and sodium salts. In some embodiments, the salt bath for chemical strengthening treatment is 100 wt% NaNO3. The present application does not particularly limit the content of potassium and sodium salts in the salt bath, as long as it can achieve the objectives of this application.
[0102] In some embodiments of the present application, the depth of the compressive stress layer DOL_0 of the chemically strengthened glass-ceramics is greater than or equal to 0.18t and less than or equal to 0.25t, where t is the thickness of the chemically strengthened glass-ceramics. It should be understood that in the thickness direction, the degree of ion exchange varies from the surface to the center in a gradient, and the overall Na-K and / or Li-Na exchange amount generally does not exceed 1% of the total mass of the glass-ceramics, and the difference in ion radius is at the pm (picometer) level, so the expansion effect in the thickness direction is extremely slight, and it can be approximately considered that the thickness has not changed. That is, the thickness difference before and after the chemical strengthening of the transparent glass-ceramics of the present application is very small, and the thickness of the chemically strengthened glass-ceramics is approximately equal to the thickness of the transparent glass-ceramics before strengthening.
[0103] For example, in some embodiments, the compressive stress layer depth DOL_0 of a 0.7 mm thick chemically strengthened glass-ceramics may be greater than or equal to 130 μm and less than or equal to 175 μm. For example, the compressive stress layer depth DOL_0 of a 0.7 mm thick chemically strengthened glass-ceramics may be 130 μm, 132 μm, 134 μm, 135 μm, 136 μm, 138 μm, 140 μm, 142 μm, 144 μm, 145 μm, 146 μm, 148 μm, 150 μm, 155 μm, 160 μm, 165 μm, 170 μm, or 175 μm, or a value within a numerical range consisting of any two of the above values as endpoints, as long as the chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. It should be understood that, in specific embodiments, any of the above ranges may be combined with any other ranges, as long as the chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. The compressive stress layer is sufficiently deep that, when the chemically strengthened glass-ceramics comes into contact with a sharp object, it can better prevent the resulting cracks from entering the tensile stress layer, thereby further improving the mechanical strength of the chemically strengthened glass-ceramics. In this application, the compressive stress layer depth DOL_0 was measured using an SLP-2000 stress meter.
[0104] For the chemically strengthened microcrystalline glass of the present application: a compressive stress layer with a certain depth is formed on the surface of the transparent microcrystalline glass by ion exchange, and at the same time, a tensile stress layer capable of achieving force balance with the compressive stress layer is formed inside the transparent microcrystalline glass. It should be understood that after the chemical strengthening treatment and the ion exchange process, the composition at the surface of the microcrystalline glass may be different from the composition of the newly formed microcrystalline glass (that is, the microcrystalline glass that has not undergone ion exchange). That is, in the present application, the composition of the compressive stress layer formed on the surface of the chemically strengthened microcrystalline glass by ion exchange may be different from the composition of the transparent microcrystalline glass. This is because during ion exchange, a type of alkali metal ion (for example, Li + Or Na + ) will be replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced by, such as Na in glass-ceramics + K in salt bath for chemical strengthening + Exchange, K + Replaced by, and / or, Li in glass-ceramics + and Na in the salt bath for chemical strengthening treatment + Exchange, by Na +However, in the embodiments, after chemical strengthening, the composition of the glass-ceramics at or near the center of the depth of the glass article still has the composition of the newly formed glass-ceramics. That is, in the present application, the composition of the tensile stress layer in the chemically strengthened glass-ceramics that has not undergone ion exchange still has the composition of the transparent glass-ceramics.
[0105] In some embodiments of the present application, the CS_50 of the chemically strengthened glass-ceramics with a thickness of 0.7 mm is greater than 90 MPa, preferably greater than 90 MPa and less than or equal to 300 MPa, more preferably 95 MPa to 300 MPa. In some embodiments, the CS_50 of the chemically strengthened glass-ceramics with a thickness of 0.7 mm can be 90 MPa, 95 MPa, 100 MPa, 120 MPa, 140 MPa, 150 MPa, 160 MPa, 180 MPa, 200 MPa, 220 MPa, 240 MPa, 250 MPa, 260 MPa, 270 MPa, 280 MPa or 300 MPa, or a value within the numerical range consisting of any two of the above values as endpoints, as long as the chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. This shows that the chemically strengthened glass-ceramics provided in this application has excellent mechanical properties.
[0106] In some embodiments of the present application, a 0.7 mm thick chemically strengthened glass-ceramics is subjected to a drop resistance test using 80-grit sandpaper. The average sandpaper drop resistance height h of the chemically strengthened glass-ceramics is greater than or equal to 80 cm, preferably greater than or equal to 80 cm and less than or equal to 200 cm. The average sandpaper drop resistance height is based on the test of at least 10 identical chemically strengthened glass-ceramics samples. In some embodiments, for 80-grit sandpaper, the average sandpaper drop resistance height h of the 0.7 mm thick chemically strengthened glass-ceramics can be 80 cm, 85 cm, 90 cm, 95 cm, 100 cm, 105 cm, 110 cm, 115 cm, 120 cm, 130 cm, 140 cm, 150 cm, 160 cm, 170 cm, 180 cm, 190 cm, or 200 cm, or a value within a range of values consisting of any two of the above values as endpoints, as long as the chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. This indicates that the chemically strengthened glass-ceramics provided by the present application has excellent drop resistance. The above-mentioned "same chemically strengthened glass-ceramics" refers to chemically strengthened glass-ceramics obtained using the same formula and the same preparation method.
[0107] In some embodiments of the present application, the Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 670 kgf / mm2 , preferably 670kgf / mm 2 Up to 800kgf / mm 2 In some embodiments, the Vickers hardness of the chemically strengthened glass-ceramics can be 670 kgf / mm 2 、680kgf / mm 2 、690kgf / mm 2 , 700kgf / mm 2 、710kgf / mm 2 、720kgf / mm 2 , 730kgf / mm 2 , 740kgf / mm 2 , 750kgf / mm 2 、760kgf / mm 2 、770kgf / mm 2 、780kgf / mm 2 、790kgf / mm 2 or 800kgf / mm 2 , or values within a numerical range consisting of any two of the above values as endpoints, as long as the chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. This demonstrates that the chemically strengthened glass-ceramics provided in this application have excellent mechanical strength properties.
[0108] In some embodiments of the present application, a glass device is provided, which is made from the transparent glass-ceramics described in any of the aforementioned embodiments or the chemically strengthened glass-ceramics described in any of the aforementioned embodiments. For example, the glass device may include, but is not limited to, mobile phone display screen protective cover glass, mobile phone rear cover glass, laptop screen protective cover glass, and automobile center console glass cover. The transparent glass-ceramics and chemically strengthened glass-ceramics provided herein both have excellent optical properties and mechanical strength, and thus the glass devices provided herein also have excellent optical properties and mechanical strength.
[0109] In some embodiments of the present application, an electronic device is provided, comprising the transparent glass-ceramics of any of the aforementioned embodiments or the chemically strengthened glass-ceramics of any of the aforementioned embodiments. For example, the electronic device may include, but is not limited to, a mobile phone, a tablet computer, a smart wearable device, a display, or a television. Smart wearable devices may include, but are not limited to, electronic watches, smart bracelets, smart watches, smart glasses, and the like. Displays may include, but are not limited to, high-definition displays, in-vehicle displays, and in-flight displays.
[0110] Exemplarily, an electronic device may include a housing and an electronic component partially located within the housing, the housing including a front surface, a rear surface and a side surface, the electronic component including a display device, the display device being located at the front surface of the housing or adjacent to the front surface, and the chemically strengthened microcrystalline glass provided in the present application may be applied to the front surface and / or the rear surface and / or the side surface of the housing; preferably, the electronic device may also include a covering product covering the front surface of the housing or located on the display device, and the chemically strengthened microcrystalline glass provided in the present application may be applied to the covering product.
[0111] Test method:
[0112] 1. Optical performance test
[0113] (1) A 50 mm × 50 mm × 0.64 mm glass-ceramic polished wafer was cleaned in an ultrasonic cleaner. The cleaning conditions were as follows: cleaning time 5 min, deionized water, cleaning temperature 50°C, and cleaning frequency 40 kHz.
[0114] (2) After cleaning, the transmittance and optical b-value of the polished microcrystalline glass sheet were tested using a haze meter in accordance with the test method of the national standard GB / T 7962.12-2010 "Test Methods for Colorless Optical Glass Part 12: Spectral Transmittance". The haze meter used in this application is a Konica Minolta CM-3600A spectrophotometer from Japan. The light receiving optical system is transmission, the spectroscopic method is a diffraction grating, the wavelength range is 360nm-740nm, the wavelength spacing is 10nm, the illumination light source is a pulsed xenon lamp X4, and the ambient temperature of the instrument is 24°C and the air humidity is 40%.
[0115] 2. Grain size and distribution test
[0116] (1) Select a polished glass-ceramic sheet with a length, width and thickness of 10 mm × 10 mm × 1.0 mm as the test sample.
[0117] (2) The microcrystalline glass polishing sheet selected in (1) is immersed in a 5wt% hydrofluoric acid solution at 20°C for 40s, and then the microcrystalline glass polishing sheet is taken out, ultrasonically cleaned and dried. After the hydrofluoric acid solution is immersed and corroded, the glass phase on the surface of the microcrystalline glass polishing sheet will be removed, and the grains will be clearly visible. After that, gold is sprayed on the surface of the dried microcrystalline glass polishing sheet, and a JEOL cold field emission scanning electron microscope (SEM) model JSM-7500F is used to obtain the surface morphology of the microcrystalline glass polishing sheet with clear grain boundaries. The magnification of the photograph after taking is 100KX. The "hydrofluoric acid solution" here refers to a hydrofluoric acid aqueous solution.
[0118] (3) Use the particle size distribution software ImageJ to process the surface morphology image taken in (2). Select the grains in the 1000nm×1000nm area in the surface morphology image as samples, mark them with the longest dimension of the grains, and the software will automatically record the longest dimension of each grain in the area. The average value of the longest dimension of all recorded grains in the area is defined as the average grain longest dimension L. ave .
[0119] In the selected area,
[0120] D1 is the percentage of the number of grains with the longest dimension greater than or equal to 10nm and less than 20nm in the total number of grains (i.e., the total number of grains); D2 is the percentage of the number of grains with the longest dimension greater than or equal to 20nm and less than 30nm in the total number of grains; D3 is the percentage of the number of grains with the longest dimension greater than or equal to 30nm and less than 40nm in the total number of grains; D4 is the percentage of the number of grains with the longest dimension greater than or equal to 40nm and less than 50nm in the total number of grains; D5 is the percentage of the number of grains with the longest dimension greater than or equal to 50nm and less than 60nm in the total number of grains; D6 is the percentage of the number of grains with the longest dimension greater than or equal to 6 D7 is the percentage of the number of grains with the longest dimension being greater than or equal to 70 nm and less than 80 nm in the total number of grains; D8 is the percentage of the number of grains with the longest dimension being greater than or equal to 80 nm and less than 90 nm in the total number of grains; D9 is the percentage of the number of grains with the longest dimension being greater than or equal to 90 nm and less than 100 nm in the total number of grains; D10 is the percentage of the number of grains with the longest dimension being greater than or equal to 100 nm and less than 200 nm in the total number of grains; there are no grains with the longest dimension greater than 200 nm in the transparent microcrystalline glass of the present application.
[0121] 3. Single rod static pressure strength test
[0122] Place the glass-ceramic sample to be tested (a polished glass-ceramic sheet with a length, width, and thickness of 50mm × 50mm × 0.7mm is used as the glass-ceramic sample to be tested in this application) on the bottom ring of the tensile testing machine (LT_850A). Start the test software and set the movement speed of the extrusion rod (rod diameter 8mm, indenter arc radius 10mm) to 10mm / min. Click to start the test. The extrusion rod will apply force to the center of the glass-ceramic sheet to be tested (i.e., the glass-ceramic sample to be tested) at the set movement speed until the glass-ceramic sheet cracks and breaks. The test software will automatically read the force (N) when the glass-ceramic sheet breaks as the test result.
[0123] Take 10 glass-ceramic samples in the same state for testing, and take the average value of the test results as the single-rod static pressure strength of the glass-ceramic sample.
[0124] 4. Stress testing
[0125] Using a stress meter SLP-2000 from Japan's Orihara, we conducted tests based on the national standard GB-T 18144-2008, "Glass Stress Test Method," to measure the compressive stress layer depth DOL_0 and the compressive stress at a depth of 50 μm (denoted as C5_50). For this stress test, we tested chemically strengthened glass-ceramics samples measuring 50 mm x 50 mm x 0.7 mm.
[0126] During testing, a light source wavelength of 518nm, SOC = 25.0 (nm / cm) / MPa, refractive index = 1.54, and exposure time: 300usec were selected. When testing surface CS_50 and DOL_0, conductive fluid was applied to the stress gauge. A chemically strengthened glass-ceramic sample was then wiped clean and placed on the test path to measure the values. The SLP-2000 uses a conductive fluid with a refractive index of 1.51.
[0127] SOC: Photoelastic coefficient. Photoelasticity refers to the anisotropic birefringence of transparent materials when subjected to stress. By measuring the photoelastic coefficient and birefringence, the residual stress (MPa) within the material can be determined.
[0128] 5. Drop test
[0129] Average sandpaper drop height h: refers to the ratio of the sum of the sandpaper drop heights of multiple identical glass-ceramic samples measured for each sample to the number of tested glass-ceramic samples, which is used to characterize the drop resistance of the glass-ceramic.
[0130] Take at least 10 pieces of the same glass-ceramic samples for testing each time, and the average height of the sandpaper drop resistance
[0131] Where n is the number of glass-ceramic samples tested in each batch, and hi is the sandpaper drop resistance height of a single sample tested.
[0132] Among them, the test method for a single sample's resistance to sandpaper drop height is:
[0133] Step 1: Apply 80-grit sandpaper to the bottom surface of a 160g model machine and place the model machine on a green figure LT-SKDL-CD drop machine.
[0134] Step 2: Place a chemically strengthened glass-ceramic sample to be tested with a length, width and thickness of 50mm×50mm×0.7mm directly below the model machine, with the chemically strengthened glass-ceramic sample to be tested facing the sandpaper. Make the model machine fall from a certain drop height to impact the chemically strengthened glass-ceramic sample to be tested directly below the model machine. If the glass-ceramic sample does not break, then increase the drop height of the model machine in a certain pattern, and continue to impact the model machine and fall, impacting the chemically strengthened glass-ceramic sample directly below the model machine until the chemically strengthened glass-ceramic sample breaks. For example, the drop height of the model machine starts from 40cm, and the chemically strengthened glass-ceramic sample to be tested is dropped once. If the chemically strengthened glass-ceramic sample does not break, then increase the drop height of the model machine by 10cm, and drop again, and repeat the above process until the chemically strengthened glass-ceramic sample breaks.
[0135] Step 3: The last drop height of the chemically strengthened glass-ceramic sample when it breaks is recorded as its sandpaper drop height. For example, if the drop height is increased by 10 cm each time, when the drop height of the chemically strengthened glass-ceramic sample when it breaks is 50 cm, the sandpaper drop height of the chemically strengthened glass-ceramic sample is 40 cm.
[0136] 6. Vickers hardness test
[0137] The Vickers hardness of chemically strengthened glass-ceramics was tested using a digital low-load Vickers hardness tester (VTD405, Beijing Wowei Technology Co., Ltd.) in accordance with the national standard GB / T 37900-2019, "Test method for hardness and fracture toughness of ultra-thin glass - Low-load Vickers hardness indentation method." The Vickers hardness test was conducted on chemically strengthened glass-ceramics samples measuring 50 mm x 50 mm x 0.7 mm.
[0138] 7. Crystal phase test
[0139] The glass-ceramics were ground into a fine powder using a grinding mill. The maximum particle size of the fine powder was less than 75 μm. The powder was then tested using an X-ray diffractometer (Shimadzu XRD-6100) within a diffraction angle range of 2θ = 10°-80°, a scanning speed of 6° / min, an operating voltage of 40 kV, and an operating current of 30 mA to obtain the XRD diffraction peak curve. The XRD diffraction data was then analyzed using the professional processing software Jade to identify the crystalline phases in the glass-ceramics. The XRD diffraction peak curve of the glass-ceramics was also fitted to determine the total crystalline phase content in the glass-ceramics.
[0140] Specifically, the total crystalline content is determined by importing the RAW X-ray diffractometer test result file into Jade, the Rietveld refinement software for X-ray diffraction data, and performing fitting and calculation to obtain the total crystalline content in the glass-ceramics. The ratio of the fitted crystalline phase peak area to the total fitted peak area is the total crystalline content, also known as the crystallinity.
[0141] 8.DSC test:
[0142] The substrate glass to be tested was crushed, ground, and passed through a 200-mesh sieve to obtain the sample to be tested. Then, 20 mg of the sample to be tested was weighed and heated from room temperature to 1100°C at a heating rate of 10°C / min using a differential thermal analyzer under a nitrogen atmosphere to obtain a DSC curve of the sample. The differential thermal analyzer used in this application was a Mettler-Toledo TGA / DSC3+ thermogravimetric and simultaneous thermal analyzer. The instrument was placed in an ambient temperature of 24°C and an air humidity of 40%. The standard substance used in the test was α-Al2O3 powder, and the sample container was a platinum crucible.
[0143] In the above test method, the glass-ceramic tiles in the examples and comparative examples are shaped, cut, and polished to obtain glass-ceramic samples of the desired size (e.g., polished glass-ceramic sheets). These samples are then tested. For example, polished glass-ceramic sheets with a length, width, and thickness of 50 mm × 50 mm × 0.7 mm, 10 mm × 10 mm × 1.0 mm, or 50 mm × 50 mm × 0.64 mm can be obtained. In this application, a micrometer is used to test the thickness of the transparent glass-ceramic.
[0144] Example 1
[0145] <Preparation of Base Glass>
[0146] According to the design of formula 1 in Table 1, it is converted into glass production raw materials for batching, with a total mass of 1000 g, and then mixed in a V-type mixer for 30 minutes. After mixing, W1 = 0.30wt% (based on the total mass of the raw materials) of the clarifier SnO2 is added and mixed evenly. Then, it is transferred to a platinum crucible, melted in a 1650°C lifting furnace for 5 hours, poured into a forming mold for forming and cooling, cooled to 900°C, and then placed in a 500°C annealing furnace for annealing for 24 hours, and then cooled to room temperature with the furnace to obtain the substrate glass.
[0147] <Preparation of Glass-Ceramics>
[0148] The substrate glass prepared above is heated to a nucleation temperature T0 of 552°C and a holding time t0 of 240 minutes, and then heated to a crystallization temperature T1 of 670°C and a holding time t1 of 100 minutes to obtain a glass-ceramic brick. After the glass-ceramic brick is shaped, cut, and polished, a glass-ceramic sample of the desired size is obtained. The glass-ceramic samples processed in this application are all polished glass-ceramic sheets. The glass-ceramic bricks or glass-ceramic samples obtained through the above steps refer to the transparent glass-ceramic mentioned above in this application.
[0149] <Preparation of Chemically Strengthened Glass-Ceramics>
[0150] The obtained glass-ceramics sample was treated in a 100 wt% NaNO3 salt bath at 450°C for 10 h to obtain chemically strengthened glass-ceramics.
[0151] Example 2 to Example 13
[0152] Except for adjusting the raw materials and related preparation parameters according to Table 1, Table 2 and Table 3, the rest is the same as Example 1.
[0153] Comparative Examples 1 to 10
[0154] Except for adjusting the raw materials and related preparation parameters according to Table 1, Table 2 and Table 3, the rest is the same as Example 1. Among them, the micro-ceramic glass samples in Example 10, Example 12 and Comparative Examples 1 to Comparative Examples 4 were not subjected to strengthening treatment.
[0155] The formulations and preparation parameters of the embodiments and comparative examples are shown in Tables 1 to 3.
[0156] Referring to Table 2 and Table 3, the main crystalline phases of the glass-ceramics in Examples 1 to 13 of the present application all include lithium disilicate Li2Si2O5 and petalite LiAlSi4O 10, the crystal phase composition may also include lithium silicate Li2SiO3, β-quartz and / or Li3PO4, and the proportions of grains A, B and C are all within the scope of the present application, while the glass-ceramics in Comparative Examples 1 to 10 have similar crystal phases to the embodiments, but the proportion of at least one of grains A, B and C is not within the scope of the present application. The glass-ceramics obtained in the embodiments of the present application also has a low optical b value, a high transmittance of 400nm light and an average transmittance of light from 400nm to 740nm, and a large single-rod static pressure strength, indicating that the glass-ceramics provided by the present application has both excellent optical properties and mechanical strength properties. However, the optical properties or mechanical strength of the glass-ceramics in the comparative examples are poor, so that both optical properties and mechanical strength properties cannot be achieved. At the same time, the chemically strengthened microcrystalline glass obtained in the examples of the present application has higher C5_50, DOL_0, Vickers hardness and average sandpaper drop resistance height, indicating that the chemically strengthened microcrystalline glass provided by the present application has excellent mechanical strength properties; while the microcrystalline glass in the comparative example cannot have both optical properties and mechanical strength properties, and the chemically strengthened microcrystalline glass prepared therefrom cannot have both optical properties and mechanical strength properties.
[0157] Specifically, as shown in Figures 1 and 2, and in combination with the data in Tables 2 and 3, the base glass composition of Comparative Example 2 (Figure 2) is the same as that of Example 6 (Figure 1), but due to different heat treatment processes, the grain distribution of the glass-ceramics obtained in Comparative Example 2 and Example 6 is different. The small-sized grains in Comparative Example 2 are significantly more, and the distribution of its grain size is not within the scope of this application. Therefore, although the glass-ceramics of Comparative Example 2 has excellent optical properties, its mechanical strength is poor and does not reach the expected level. As shown in Figures 1 and 3, and in combination with the data in Tables 2 and 3, the number of large-sized grains in the glass-ceramics of Comparative Example 5 (Figure 3) is significantly more, and the optical properties of the glass-ceramics of Comparative Example 5 deteriorate. This further shows that the glass-ceramics and chemically strengthened glass-ceramics that meet the specific grain distribution requirements provided by the present application can have excellent optical properties and mechanical strength properties at the same time, but do not meet the specific grain distribution requirements defined in this application. Even if the average longest dimension of the grains meets the requirements, it is difficult to have both excellent optical properties and mechanical strength properties.
[0158] Figure 4 is a test chart of the transmittance of the microcrystalline glass in Example 4, Example 7 and Comparative Example 4 to light in the 360nm to 740nm band. It can be seen from the figure that at any wavelength, the transmittance of the microcrystalline glass in the examples is higher than that of the comparative example.
[0159] Figure 5 is the DSC curve of the microcrystalline glass in Example 7. The first endothermic peak and the first exothermic peak can be determined from the figure. Specifically, the temperature T0' corresponding to the first endothermic peak in Figure 5 is 540°C, and the temperature T1' corresponding to the first exothermic peak is 702°C. Furthermore, the nucleation temperature T0 and the crystallization temperature T1 can be determined.
[0160] FIG6 is an XRD pattern of the transparent glass-ceramics in Example 1. It can be seen from the figure that the transparent glass-ceramics in Example 1 contains crystalline phases of Li2Si2O5, LiAlSi4O 10 , Li2SiO3, SiO2, Li3PO4. Figure 7 is the XRD pattern of the transparent microcrystalline glass in Example 10. It can be seen from the figure that the transparent microcrystalline glass in Example 10 contains crystalline phases Li2Si2O5, LiAlSi4O 10 、Li3PO4。
[0161] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0162] Each embodiment in this specification is described in a related manner. The same or similar parts between the embodiments can be referred to each other. Each embodiment focuses on the differences from other embodiments.
[0163] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A transparent glass-ceramic, It is characterized in that The main crystalline phase of the transparent microcrystalline glass comprises a petalite crystalline phase and a lithium silicate crystalline phase; the grains of the crystalline phase in the transparent microcrystalline glass satisfy the following characteristics: The average longest dimension of the grains is 16nm to 40nm; The number of grains with a maximum dimension of 20 nm ≤ < 100 nm accounts for greater than or equal to 40% and less than or equal to 90%, The number of grains with a maximum dimension of 10 nm ≤ < 20 nm accounts for more than 0% and less than or equal to 60%, The number of grains with a maximum dimension of 50 nm ≤ and less than 100 nm accounts for less than or equal to 10%.
2. The transparent glass-ceramic according to claim 1, in, The lithium silicate crystal phase is a lithium disilicate crystal phase, or the lithium silicate crystal phase is a lithium silicate crystal phase and a lithium disilicate crystal phase; the lithium silicate crystal phase is preferably a lithium disilicate crystal phase.
3. The transparent glass-ceramics according to claim 1 or 2, in, Based on the mass of the transparent microcrystalline glass, the total crystalline content of the transparent microcrystalline glass accounts for greater than or equal to 70wt%.
4. The transparent glass-ceramic according to any one of claims 1 to 3, in, At a thickness of 0.64 mm, the optical b value of the transparent microcrystalline glass is 0.10 to 1.00, preferably 0.30 to 1.
00.
5. The transparent glass-ceramic according to any one of claims 1 to 4, in, At a thickness of 0.64 mm, for light with a wavelength of 400 nm, the transmittance of the transparent microcrystalline glass is greater than or equal to 85%, preferably greater than or equal to 88%.
6. The transparent glass-ceramic according to any one of claims 1 to 5, in, At a thickness of 0.64 mm, for light in a wavelength range of 400 nm to 740 nm, an average transmittance of the transparent microcrystalline glass is greater than or equal to 86%, preferably greater than or equal to 90%.
7. The transparent glass-ceramic according to any one of claims 1 to 6, in, At a thickness of 0.7 mm, the single-rod static pressure strength of the transparent microcrystalline glass is greater than or equal to 250N, preferably 250N to 600N, and more preferably 270N to 600N.
8. The transparent glass-ceramic according to any one of claims 1 to 7, in, Expressed in terms of molar percentage of oxides, the composition of the transparent glass-ceramics includes: SiO 2 65.00mol%-74.00mol%、Al 2 O 3 3.00mol%-5.60mol%、Li 2 O 15.00mol%-23.00mol%、P 2 O 5 0.50mol%-1.50mol%、ZrO 2 0.80mol%-3.50mol%、ZnO 0.00mol%-1.00mol%、MgO 0.00mol%-1.50mol%、Na 2 O 0.00mol%-4.00mol%、B 2 O 3 0.00mol%-2.00mol%、K 2 O 0.00mol%-1.00mol%、CaO 0.00mol%-2.00mol%、SrO 0.00mol%-0.50mol%、BaO 0.00mol%-1.00mol%。 9. A chemically strengthened glass-ceramic, It is characterized in that The transparent microcrystalline glass is obtained by chemically strengthening the transparent microcrystalline glass according to any one of claims 1 to 8.
10. The chemically strengthened glass-ceramics according to claim 9, in, The salt bath for the chemical strengthening treatment is a molten salt containing potassium salt and / or sodium salt, wherein the salt bath contains 0wt% to 1wt% of lithium salt; the temperature of the salt bath is 380°C to 550°C, preferably 400°C to 500°C; the time for the chemical strengthening treatment is 1 to 48h, preferably 1h to 12h.
11. The chemically strengthened glass-ceramics according to claim 9 or 10, in, The DOL_0 of the chemically strengthened glass-ceramics is greater than or equal to 0.18t and less than or equal to 0.25t, where t is the thickness of the chemically strengthened glass-ceramics.
12. The chemically strengthened glass-ceramics according to any one of claims 9 to 11, in, The CS_50 of 0.7 mm thick chemically strengthened microcrystalline glass is greater than 90 MPa, preferably greater than 90 MPa and less than or equal to 300 MPa, and more preferably 95 MPa to 300 MPa.
13. The chemically strengthened glass-ceramics according to any one of claims 9 to 12, in, The 0.7 mm thick chemically strengthened glass-ceramics is subjected to a drop resistance test using 80-mesh sandpaper, and the average sandpaper resistance drop height of the chemically strengthened glass-ceramics is greater than or equal to 80 cm.
14. The chemically strengthened glass-ceramics according to any one of claims 9 to 13, in, The Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 670 kgf / mm 2 , preferably 670kgf / mm 2 Up to 800kgf / mm 2 . 15 . A glass device, which is made of the transparent glass-ceramics according to claim 1 or the chemically strengthened glass-ceramics according to claim 9 . 16 . An electronic device comprising the transparent glass-ceramics according to claim 1 or the chemically strengthened glass-ceramics according to claim 9 .
17. The electronic device according to claim 16, in, The electronic device includes at least one of a mobile phone, a tablet computer, a smart wearable, a display and a television.