Optical laminate, image display panel, and image display device

The optical laminate with an adhesive sheet and antistatic layer addresses static electricity-induced display defects in image display devices by maintaining low surface resistivity, enhancing performance in low-temperature environments.

WO2024190847A1PCT designated stage expired Publication Date: 2024-09-19NITTO DENKO CORP

Patent Information

Application Number
PCT/JP2024/009899
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-13
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

Image display devices, such as liquid crystal and organic electroluminescence (EL) displays, experience display defects due to static electricity, particularly in low-temperature environments, where existing optical laminates fail to adequately suppress these issues.

Method used

An optical laminate comprising an adhesive sheet with a polymer and antistatic agent, providing a surface resistivity of 1.0×10^10 Ω/□ or less at -15°C, and an antistatic layer with surface resistivity of 3.0×10^8 Ω/□ or less at 25°C, to mitigate static electricity-induced display defects.

Benefits of technology

The optical laminate effectively suppresses display defects in image display devices by maintaining low surface resistivity across temperature variations, ensuring reliable performance even in low-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009899_19092024_PF_FP_ABST
    Figure JP2024009899_19092024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an optical laminate more suitable for suppressing display defects. The optical laminate comprises an adhesive sheet, a static electricity prevention layer, and an optical film. The adhesive sheet is formed from an adhesive composition containing a polymer (A) and an antistatic agent. The surface resistivity at -15°C on the adhesive sheet side of the optical laminate is 1.0×1010 Ω / □ or less. The surface resistivity at 25°C of the static electricity prevention layer may be 3.0×108 Ω / □ or less.
Need to check novelty before this filing date? Find Prior Art

Description

Optical laminate, image display panel, and image display device

[0001] The present invention relates to an optical laminate, an image display panel, and an image display device.

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices and inorganic EL display devices), have rapidly become widespread. These various image display devices have a laminated structure of, for example, an image display cell, such as a liquid crystal cell or an EL light-emitting element, and an optical laminate including a polarizing plate and a pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet is mainly used for bonding between films included in the optical laminate or for bonding between the image display cell and the optical laminate.

[0003] In an image display device, static electricity is generated during its production, for example, when an optical laminate is bonded to an image display cell via an adhesive sheet, or during use, for example, when a user touches the image display device. If the image display device becomes charged by this static electricity, problems such as display defects can occur.

[0004] Patent Documents 1 and 2 disclose a laminated structure including a polarizing film and a conductive layer containing a conductive polymer.

[0005] JP 2016-39132 A JP 2015-509615 A

[0006] According to the studies of the present inventors, there is room for improvement in the optical laminate from the viewpoint of sufficiently preventing display defects in image display devices. Therefore, an object of the present invention is to provide an optical laminate that is more suitable for suppressing display defects.

[0007] The present inventors have found that image display devices are prone to display defects in low-temperature environments, and have completed the present invention based on this finding.

[0008] The present invention provides an optical laminate including a pressure-sensitive adhesive sheet, an antistatic layer, and an optical film, wherein the pressure-sensitive adhesive sheet is formed from a pressure-sensitive adhesive composition containing a polymer (A) and an antistatic agent, and the surface resistivity of the pressure-sensitive adhesive sheet side of the optical laminate at −15° C. is 1.0×10 10 The present invention provides an optical laminate having a resistivity of Ω / □ or less.

[0009] The present invention further provides an image display panel comprising the above optical laminate.

[0010] The present invention further provides an image display device comprising the above image display panel.

[0011] According to the present invention, an optical laminate that is more suitable for suppressing display defects in a low-temperature environment can be provided.

[0012] Fig. 1 is a cross-sectional view schematically showing an example of an optical laminate according to the present embodiment. Fig. 2 is a cross-sectional view schematically showing another example of an optical laminate according to the present embodiment. Fig. 3 is a cross-sectional view schematically showing an example of an image display panel according to the present embodiment. Fig. 4 is a cross-sectional view schematically showing another example of an image display panel according to the present embodiment. Fig. 5 is a cross-sectional view schematically showing another example of an image display panel according to the present embodiment.

[0013] An optical laminate according to a first aspect of the present invention is an optical laminate including a pressure-sensitive adhesive sheet, an antistatic layer, and an optical film, wherein the pressure-sensitive adhesive sheet is formed from a pressure-sensitive adhesive composition containing a polymer (A) and an antistatic agent, and the surface resistivity of the pressure-sensitive adhesive sheet side of the optical laminate at −15° C. is 1.0×10 10 Ω / □ or less.

[0014] In the second aspect of the present invention, for example, in the optical laminate according to the first aspect, the surface resistivity of the antistatic layer at 25° C. is 3.0×10 8 Ω / □ or less.

[0015] In a third aspect of the present invention, for example, in the optical laminate according to the first or second aspect, the surface resistivity of the antistatic layer at 25° C. is 1.0×10 7 Ω / □ or more 1.0×10 8 Ω / □ or less.

[0016] In a fourth aspect of the present invention, for example, in the optical layered body according to any one of the first to third aspects, the polymer (A) is a (meth)acrylic polymer.

[0017] In a fifth aspect of the present invention, for example, in the optical layered body according to any one of the first to fourth aspects, the polymer (A) has a polyether structure.

[0018] In a sixth aspect of the present invention, for example, in the optical laminate according to any one of the first to fifth aspects, the polymer (A) has a constituent unit derived from a monomer represented by the following formula (1):

[0019]

[0020] In the formula (1), R 1 is a hydrogen atom or a methyl group, and R 2 is an alkyl group which may be linear or branched, and n is an integer of 1 to 15.

[0021] In a seventh aspect of the present invention, for example, in the optical layered body according to any one of the first to sixth aspects, the polymer (A) has a constituent unit derived from an aromatic ring-containing monomer.

[0022] In an eighth aspect of the present invention, for example, in the optical laminate according to any one of the first to seventh aspects, in the pressure-sensitive adhesive composition, the amount of the antistatic agent blended is less than 10 parts by weight per 100 parts by weight of the polymer (A).

[0023] In a ninth aspect of the present invention, for example, in the optical layered body according to any one of the first to eighth aspects, the glass transition temperature of the polymer (A) calculated from the FOX formula is −40° C. or lower.

[0024] In a tenth aspect of the present invention, for example, in the optical laminate according to the ninth aspect, the glass transition temperature is −45° C. or lower.

[0025] An image display panel according to an eleventh aspect of the present invention includes the optical laminate according to any one of the first to tenth aspects.

[0026] An image display device according to a twelfth aspect of the present invention includes the image display panel according to the eleventh aspect.

[0027] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form without departing from the gist of the present invention.

[0028] The optical laminate according to this embodiment includes a pressure-sensitive adhesive sheet, an antistatic layer, and an optical film. The pressure-sensitive adhesive sheet is formed from a pressure-sensitive adhesive composition containing a polymer (A) and an antistatic agent. The surface resistivity of the pressure-sensitive adhesive sheet side of the optical laminate at −15° C. is 1.0×10 10 Ω / □ or less.

[0029] [Optical laminate] Fig. 1 is a cross-sectional view schematically showing an example of an optical laminate according to this embodiment. The optical laminate 10A includes an adhesive sheet 1, an antistatic layer 2, and an optical film 3. The optical laminate 10A has a structure in which the adhesive sheet 1, the antistatic layer 2, and the optical film 3 are laminated in this order, for example. The optical laminate 10A can be attached to an object (e.g., an image display panel) via the adhesive sheet 1.

[0030] The adhesive sheet 1 is formed on the antistatic layer 2. The adhesive sheet 1 and the antistatic layer 2 are laminated together. The adhesive sheet 1 is formed in contact with the antistatic layer 2. The adhesive sheet 1 is formed on one main surface of the antistatic layer 2. In FIG. 1 , the adhesive sheet 1 is formed over the entire one main surface of the antistatic layer 2. However, the adhesive sheet 1 may be formed on only a portion of one main surface of the antistatic layer 2. In this specification, the "main surface" means the surface of the film or layer having the largest area.

[0031] The antistatic layer 2 is formed on the optical film 3. The antistatic layer 2 and the optical film 3 are laminated together. The antistatic layer 2 is formed in contact with the optical film 3. The antistatic layer 2 is formed on one main surface of the optical film 3. Specifically, the optical film 3 is formed on the main surface of the antistatic layer 2 on which the adhesive sheet 1 is not formed. In FIG. 1 , the optical film 3 is formed on the entire one main surface of the antistatic layer 2. However, the optical film 3 may be formed on only a part of one main surface of the antistatic layer 2.

[0032] [Adhesive Sheet] The surface resistivity R of the adhesive sheet 1 side of the optical laminate 10A at −15° C. is 1.0×10 10 The optical laminate 10A has a resistivity of 1.0×10 10 By providing the adhesive sheet 1 having a surface resistivity R of Ω / □ or less, display defects due to charging of the image display device can be suppressed even in a low-temperature environment.

[0033] The surface resistivity R is 5.0 × 10 9 Ω / □ or less, 4.0×10 9 Ω / □ or less, 3.0×10 9 Ω / □ or less, 2.0×10 9 Ω / □ or less, 1.0×10 9 Ω / □ or less, 5.0×10 8 Ω / □ or less, 1.0×10 8 Ω / □ or less, 8.0×10 7 Ω / □ or less, and even 6.0×10 7 The lower limit of the surface resistivity R may be, for example, 1.0 × 10 6 Ω / □, 1.0×10 7 However, when the optical laminate 10A is used in an image display panel having a built-in touch sensing function, the surface resistivity R is set to 5.0×10 6 Ω / □ or more is preferable, and 1.0×10 7 The surface resistivity R can be measured, for example, using a high resistance resistivity meter (for example, the Hiresta series manufactured by Mitsubishi Chemical Analytech Co., Ltd.) under conditions of an applied voltage of 250 V and an application time of 10 seconds.

[0034] After the optical laminate 10A was subjected to a weather resistance test, the surface resistivity R′ of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A at −15° C. was, for example, 1.5×10 10 Ω / □ or less, and 1.2×10 10 Ω / □ or less, 1.0×10 10 Ω / □ or less, 9.0×10 9 Ω / □ or less, 8.0×10 9 Ω / □ or less, 7.0×10 9 Ω / □ or less, 6.0×10 9Ω / □ or less, 5.0×10 9 Ω / □ or less, 1.0×10 9 Ω / □ or less, 5.0×10 8 Ω / □ or less, 1.0×10 8 Ω / □ or less, 8.0×10 7 Ω / □ or less, and even 6.0×10 7 The lower limit of the surface resistivity R' may be, for example, 1.0 x 10 6 Ω / □, 1.0×10 7 The surface resistivity R' may be 5.0×10 8 Ω / □ or less, and even 1.0×10 8 When the resistance is Ω / □ or less, display defects can be further suppressed.

[0035] The weather resistance test was carried out in an environment of a temperature of 40° C. and a humidity of 20% RH, by irradiating light of a wavelength of 300 to 700 nm from the optical film 3 side of the optical laminate 10A at an illuminance of 500 W / m 2 The weather resistance test can be carried out by continuously irradiating the test piece with ultraviolet light for 500 hours. The weather resistance test can be carried out using, for example, an ultraviolet fade meter (for example, U48HB manufactured by Suga Test Instruments Co., Ltd.).

[0036] The optical laminate 10A is unlikely to change, for example, in surface resistivity R' at -15°C on the pressure-sensitive adhesive sheet 1 side before and after a weather resistance test. The ratio R' / R of the surface resistivity R' (Ω / □) at -15°C on the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A after the weather resistance test to the surface resistivity R (Ω / □) at -15°C on the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A before the weather resistance test is, for example, 7.0 or less, and may be 6.0 or less, 5.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, 1.4 or less, 1.3 or less, or even 1.2 or less. The lower limit of the ratio R' / R is, for example, 0.25, 0.5, or even 0.75. When the ratio R' / R is 1.5 or less, display defects can be further suppressed.

[0037] Before the weather resistance test, the surface resistivity R of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A at 25°C is, for example, 1.0 × 10 10 The surface resistivity R is, for example, 1.0 × 10 9 Ω / □ or less, and 8.0 × 108 Ω / □ or less, 5.0×10 8 Ω / □ or less, 3.0×10 8 Ω / □ or less, 2.0×10 8 Ω / □ or less, 1.0×10 8 Ω / □ or less, 8.0×10 7 Ω / □ or less, 5.0×10 7 Ω / □ or less, and even 2.0×10 7 The lower limit of the surface resistivity R may be, for example, 1.0 × 10 6 Ω / □, 1.0×10 7 It may be Ω / □.

[0038] The optical laminate 10A is less likely to have an increase in surface resistivity on the pressure-sensitive adhesive sheet 1 side, even in a low-temperature environment, for example. Before a weather resistance test, the ratio R / R1 of the surface resistivity R (Ω / □) of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A at -15°C to the surface resistivity R1 (Ω / □) of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A at 25°C is, for example, 50.0 or less, and may be 40.0 or less, 30.0 or less, 20.0 or less, 15.0 or less, 10.0 or less, 8.0 or less, 7.0 or less, or even 5.0 or less. The lower limit of the ratio R / R1 is, for example, 0.1, and may be 0.5 or even 1.0. When the ratio R / R1 is 50.0 or less, display defects can be further suppressed.

[0039] The ratio R' / R1 of the surface resistivity R' (Ω / □) at -15 ° C. of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A after the weather resistance test to the surface resistivity R1 (Ω / □) at 25 ° C. of the pressure-sensitive adhesive sheet 1 side of the optical laminate 10A before the weather resistance test is, for example, 60.0 or less, 55.0 or less, 50.0 or less, 45.0 or less, 40.0 or less, 35.0 or less, 30.0 or less, 25.0 or less, 20.0 or less, 15.0 or less, 10.0 or less, or even 5.0 or less. The lower limit of the ratio R' / R1 is, for example, 0.25, and may be 0.5, 0.75, or even 1.0. When the ratio R' / R1 is 25.0 or less, 10.0 or less, or even 5.0 or less, display defects can be further suppressed.

[0040] The pressure-sensitive adhesive sheet 1 is formed from a pressure-sensitive adhesive composition (I) containing a polymer (A) and an antistatic agent.

[0041] <Polymer (A)> Examples of the polymer (A) include a (meth)acrylic polymer, a urethane polymer, a silicone polymer, and a rubber polymer. The polymer (A) may have a polyether structure. The polymer (A) is preferably a (meth)acrylic polymer. In other words, the pressure-sensitive adhesive composition (I) may contain a (meth)acrylic polymer as a main component. In other words, the pressure-sensitive adhesive composition (I) may be an acrylic pressure-sensitive adhesive composition. The main component refers to the component with the largest content by weight in the composition. The content of the main component may be, for example, 50% by weight or more, 60% by weight or more, 70% by weight or more, 75% by weight or more, or even 80% by weight or more. In this specification, "(meth)acrylic polymer" refers to a polymer having a structural unit derived from a (meth)acrylic monomer such as (meth)acrylate. The content of structural units derived from (meth)acrylic monomers in a (meth)acrylic polymer is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. The (meth)acrylic polymer may be composed solely of structural units derived from (meth)acrylic monomers. "(Meth)acrylic" means acrylic and methacrylic. "(Meth)acrylate" means acrylate and methacrylate.

[0042] The polymer (A) may have a polyether structure. The polyether structure is a structure containing at least two ether groups (—O—). The polyether structure may be linear or branched. An example of the polyether structure contains an alkyl group, which may be linear or branched, and at least two ether groups. The polymer (A) may have the polyether structure in its main chain or in its side chain, preferably in its side chain. The polymer (A) may be a (meth)acrylic polymer having a polyether structure in its side chain.

[0043] The polymer (A) may have a structural unit having a polyether structure. In the structural unit, the polyether structure may be located in the main chain or in a side chain, preferably in the side chain. The polymer (A) may have a structural unit derived from a (meth)acrylic monomer having a polyether structure in the side chain.

[0044] The polymer (A) having a polyether structure in its side chain has, for example, a structural unit derived from a monomer (A1) represented by the following formula (1): R in formula (1) 1 is a hydrogen atom or a methyl group. 2 is an alkyl group which may be linear or branched, and is preferably a linear alkyl group. The number of carbon atoms in the alkyl group may be 1 to 10, or even 1 to 4. 2 Examples of R are a methyl group and an ethyl group. n is an integer of 1 to 15, preferably an integer of 1 to 10, and more preferably an integer of 1 to 5. When n is 1, the monomer (A1) contains two ether groups, including the "-O-" of the COO group. The monomer (A1) is a type of (meth)acrylic monomer, more specifically, a type of (meth)acrylate monomer. The R at the end of the side chain 2 When the O group is taken into consideration, the monomer (A1) is also a type of alkoxy group-containing (meth)acrylate monomer. The structural unit derived from the monomer (A1) has a polyether structure in the side chain.

[0045]

[0046] Examples of the monomer (A1) are 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate, and preferably 2-methoxyethyl acrylate (MEA). The structural units derived from the monomer (A1) can particularly contribute to a decrease in the surface resistivity of the PSA sheet formed from the PSA composition (I).

[0047] The polymer (A) may have both a structural unit derived from the monomer (A1) and a structural unit derived from the monomer (A2) described below. The polymer (A) having both structural units can contribute to improving the durability of the adhesive strength of the pressure-sensitive adhesive sheet 1.

[0048] The content of the structural unit having a polyether structure (e.g., a structural unit derived from the monomer (A1)) in the polymer (A) may be, for example, 0% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, 35% by weight or more, 40% by weight or more, 45% by weight or more, or even 50% by weight or more. The upper limit of the content may be, for example, 100% by weight or less, 90% by weight or less, 80% by weight or less, 70% by weight or less, 65% by weight or less, 60% by weight or less, or even less than 60% by weight.

[0049] The polymer (A) may have one or more structural units derived from the following monomer (A2). The monomer (A2) shown below can be copolymerized with the monomer (A1).

[0050] Examples of the monomer (A2) are (meth)acrylic monomers having an alkyl group of 1 to 30 carbon atoms on the side chain. The alkyl group may be linear or branched. Examples of the (meth)acrylic monomers having an alkyl group on the side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The content of the structural unit derived from the (meth)acrylic monomer having an alkyl group on the side chain in the polymer (A) is, for example, 80% by weight or less, and may be 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, or even 5% by weight or less, or may even be 0% by weight (no such structural unit is present).

[0051] Another example of the monomer (A2) is a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a hydroxyl group-containing (meth)acrylic monomer. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate, as well as (4-hydroxymethylcyclohexyl)-methyl acrylate. From the viewpoint of improving the durability of the pressure-sensitive adhesive sheet formed from the pressure-sensitive adhesive composition (I), 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, and 4-hydroxybutyl (meth)acrylate is more preferred. The content of the structural units derived from the hydroxyl group-containing monomer in the polymer (A) is, for example, 1 to 5% by weight, and may be 3% by weight or less, or even 2% by weight or less. The polymer (A) may not necessarily have any structural units derived from the hydroxyl group-containing monomer.

[0052] The monomer (A2) may be an aromatic ring-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, or an amide group-containing monomer.

[0053] The aromatic ring-containing monomer may be an aromatic ring-containing (meth)acrylic monomer. Examples of aromatic ring-containing monomers include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, hydroxyethylated β-naphthol (meth)acrylate, and biphenyl (meth)acrylate. During the production and / or use of an image display device including the optical laminate 10A, birefringence may occur in the pressure-sensitive adhesive sheet due to misalignment. This may cause problems with the image display device, such as light leakage and display unevenness. By including a structural unit derived from an aromatic ring-containing monomer in the polymer (A), birefringence caused by misalignment of the pressure-sensitive adhesive sheet can be reduced. This can further reduce light leakage and display unevenness in the image display device.

[0054] The aromatic ring-containing monomer may be a structural unit derived from the monomer (A3) shown in the following formula (2): R in formula (2) 3 is a hydrogen atom or a methyl group. 4 is a phenyl group in which a hydrogen atom may be substituted, preferably a phenyl group. The substituent of the hydrogen atom is, for example, a linear or branched alkyl group having 1 to 10 carbon atoms, or even 1 to 4 carbon atoms, and an alkoxy group having 1 to 4 carbon atoms. n is an integer of 1 to 15, preferably an integer of 1 to 10, and more preferably an integer of 1 to 5. When n is 1, the monomer (A3) contains two ether groups, including the "-O-" of the COO group. The monomer (A3) is a type of (meth)acrylic monomer, more specifically, a type of (meth)acrylate monomer. The R at the side chain terminal 4 When the O group is taken into consideration, the monomer (A3) is also a type of alkoxy group-containing (meth)acrylate monomer. The structural unit derived from the monomer (A3) has a polyether structure in the side chain.

[0055]

[0056] An example of the monomer (A3) is phenoxyethyl (meth)acrylate.

[0057] The polymer (A) having a structural unit derived from the monomer (A3) can further improve the durability of the optical laminate 10A. In addition, the polymer (A) having a structural unit derived from the monomer (A3) tends to prevent misalignment at the edges of the optical laminate 10A even when the optical film 3 shrinks due to heating. Therefore, the optical laminate 10A using the pressure-sensitive adhesive sheet 1 is less likely to suffer from appearance defects such as light leakage caused by shrinkage of the optical film 3, even in a high-temperature environment, for example.

[0058] Examples of carboxyl group-containing monomers are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of amino group-containing monomers are N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. Examples of the amide group-containing monomer include acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propane(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl group-containing lactam-based monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam.

[0059] Monomer (A2) may be a polyfunctional monomer. Examples of polyfunctional monomers include polyfunctional acrylates such as hexanediol di(meth)acrylate (1,6-hexanediol di(meth)acrylate), butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; and divinylbenzene. Preferred polyfunctional acrylates are 1,6-hexanediol diacrylate and dipentaerythritol hexa(meth)acrylate.

[0060] The total content of structural units derived from aromatic ring-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, amide group-containing monomers, and polyfunctional monomers in polymer (A) is preferably 20% by weight or less, more preferably 15% by weight or less, even more preferably 10% by weight or less, and particularly preferably 8% by weight or less. When polymer (A) contains these structural units, the total content may be, for example, 0.01% by weight or more, 1% by weight or more, 2% by weight or more, or even 3% by weight or more. Polymer (A) may not have these structural units. In particular, the content of structural units derived from carboxyl group-containing monomers in polymer (A) may be less than 0.1% by weight, or even 0% by weight (i.e., the polymer does not have these structural units).

[0061] Examples of the other monomer (A2) include nitrile group-containing (meth)acrylates such as acrylic acid and (meth)acrylonitrile; epoxy group-containing monomers such as glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate; sulfonic acid group-containing monomers such as sodium vinyl sulfonate; phosphoric acid group-containing monomers; (meth)acrylic acid esters having an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; vinyl esters such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene and vinyltoluene; olefins or dienes such as ethylene, propylene, butadiene, isoprene and isobutylene; vinyl ethers such as vinyl alkyl ether; and vinyl chloride.

[0062] The total content of the structural units derived from the other monomer (A2) in the polymer (A) is, for example, 30% by weight or less, and may be 10% by weight or less, and is preferably 0% by weight (no such structural units are present).

[0063] The polymer (A) preferably has a glass transition temperature (Tg h ) in the range of −55° C. or higher, and more preferably, hPreferably, the polymer has a constitutional unit derived from a (meth)acrylic monomer having a Tg h It has a constitutional unit derived from a (meth)acrylic monomer having a Tg h The polymer (A) has a structural unit derived from a (meth)acrylic monomer having a Tg in the range of -10°C or higher. Examples of such structural units are a structural unit derived from the monomer (A3) and a structural unit derived from a (meth)acrylic monomer having an alkyl group of 1 to 3 carbon atoms on the side chain. The polymer (A) may have at least one selected from the group consisting of a structural unit derived from the monomer (A3) and a structural unit derived from a (meth)acrylic monomer having an alkyl group of 1 to 3 carbon atoms on the side chain. h When the polymer (A) has a structural unit derived from a (meth)acrylic monomer having a temperature in the range of −55° C. or higher, the durability of the optical laminate 10A can be further improved.

[0064] The polymer (A) can be formed by polymerizing one or more of the above-mentioned monomers using a known method. A monomer and a partial polymer of the monomer may also be polymerized. The polymerization can be carried out, for example, by solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, or active energy ray polymerization. From the viewpoint of forming a pressure-sensitive adhesive sheet with excellent optical transparency, solution polymerization and active energy ray polymerization are preferred. The polymerization is preferably carried out while avoiding contact between the monomer and / or the partial polymer and oxygen. For this purpose, for example, polymerization in an inert gas atmosphere such as nitrogen, or polymerization in a state where oxygen is blocked by a resin film or the like, can be employed. The polymer (A) formed may be in any form, such as a random copolymer, a block copolymer, or a graft copolymer.

[0065] The polymerization system for forming the polymer (A) may contain one or more polymerization initiators. The type of polymerization initiator can be selected depending on the polymerization reaction, and may be, for example, a thermal polymerization initiator or a photopolymerization initiator.

[0066] Examples of solvents used in solution polymerization include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. However, the solvent is not limited to the above examples. The solvent may be a mixed solvent of two or more solvents.

[0067] Examples of polymerization initiators used in solution polymerization include azo polymerization initiators, peroxide polymerization initiators, and redox polymerization initiators. Examples of peroxide polymerization initiators include dibenzoyl peroxide and t-butyl permaleate. Among these, the azo polymerization initiators disclosed in JP-A-2002-69411 are preferred. Examples of such azo polymerization initiators include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, and 4,4'-azobis-4-cyanovaleric acid. However, the polymerization initiator is not limited to the above examples. The amount of the azo polymerization initiator used is, for example, 0.05 to 0.5 parts by weight, or may be 0.1 to 0.3 parts by weight, per 100 parts by weight of the total amount of monomers.

[0068] The active energy rays used in the active energy ray polymerization include, for example, ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, as well as ultraviolet rays. The active energy ray is preferably ultraviolet rays. Polymerization by irradiation with ultraviolet rays is also called photopolymerization. The polymerization system for the active energy ray polymerization typically contains a photopolymerization initiator. The polymerization conditions for the active energy polymerization are not limited as long as the polymer (A) is formed.

[0069] Examples of the photopolymerization initiator include a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, and a thioxanthone-based photopolymerization initiator, although the photopolymerization initiator is not limited to the above examples.

[0070] Examples of benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride. An example of a photoactive oxime-based photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. An example of a benzoin-based photopolymerization initiator is benzoin. An example of a benzyl-based photopolymerization initiator is benzil. An example of a benzophenone-based photopolymerization initiator is benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, or α-hydroxycyclohexyl phenyl ketone. An example of a ketal-based photopolymerization initiator is benzil dimethyl ketal. An example of a thioxanthone-based photopolymerization initiator is thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, or dodecylthioxanthone.

[0071] The amount of the photopolymerization initiator used is, for example, 0.01 to 1 part by weight, and may be 0.05 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomers.

[0072] The weight average molecular weight (Mw) of the polymer (A) is, for example, 1,000,000 to 3,000,000, and preferably 1,800,000 to 3,000,000. When the weight average molecular weight of the polymer (A) is 1,000,000 to 3,000,000, cracking of the PSA sheet can be suppressed, and an increase in viscosity and the occurrence of gelation tend to be suppressed. The weight average molecular weight (Mw) of the polymer in this specification is a value (polystyrene equivalent) based on measurement by GPC (gel permeation chromatography).

[0073] The content of the polymer (A) in the PSA composition (I) is, for example, 50% by weight or more, and may be 60% by weight or more, 70% by weight or more, 75% by weight or more, or even 80% by weight or more, in terms of solid content. The upper limit of the content may be, for example, 99% by weight or less, 97% by weight or less, or even 95% by weight or less.

[0074] <Antistatic Agent> The pressure-sensitive adhesive composition (I) contains an antistatic agent. The pressure-sensitive adhesive composition (I) may contain one or more antistatic agents. Examples of the antistatic agent include an ionic compound such as a salt. The ionic compound may be an ionic liquid that is liquid at room temperature (25°C).

[0075] Examples of ionic compounds include inorganic cation salts and organic cation salts. Examples of inorganic cation salts are inorganic cation-anion salts. Examples of cations contained in inorganic cation salts are alkali metal ions. Examples of alkali metal ions include lithium ions, sodium ions, and potassium ions, and preferably lithium ions. The inorganic cation salt may be a lithium salt.

[0076] Examples of anions contained in inorganic cation salts are Cl - ,Br - , I - , AlCl - , Al2Cl7 - , BF4 - , PF6 - , ClO - , NO3 - , CH3COO - , CF3COO - , CH3SO3 - , CF3SO3- , (CF3SO2)3C - , AsF6 - , SbF6 - , NbF6 - , TaF6 - , (CN)2N - , C4F9SO3 - , C3F7COO - , (CF3SO2)(CF3CO)N - , - O3S(CF2)3SO3 - and anions represented by the following general formulas (a) to (d): (a) (C n F 2n+1 SO2)2N - (n is an integer from 1 to 10) (b) CF2(C m F 2m SO2)2N - (m is an integer from 1 to 10) (c) - O3S(CF2) l SO3 - (l is an integer from 1 to 10) (d) (C p F 2p+1 SO2)N - (C q F 2q+1 SO2) (p and q are each independently an integer from 1 to 10)

[0077] The anion contained in the inorganic cation salt is preferably a fluorine-containing anion, more preferably a fluorine-containing imide anion. An example of the fluorine-containing imide anion is an imide anion having a perfluoroalkyl group. A more specific example of the fluorine-containing imide anion is (CF3SO2)(CF3CO)N - or an anion represented by the above general formula (a), (b) or (d), preferably (CF3SO2)2N - , (C2F5SO2)2N - and more preferably (CF3SO2)2N. - An example of a preferred inorganic cation salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0078] An example of an organic cation salt is an organic cation-anion salt. An example of a cation contained in the organic cation salt is an organic onium containing an organic group. Examples of oniums contained in the organic onium are nitrogen-containing oniums, sulfur-containing oniums, and phosphorus-containing oniums, and preferably nitrogen-containing oniums and sulfur-containing oniums. Examples of nitrogen-containing oniums are ammonium cation, piperidinium cation, pyrrolidinium cation, pyridinium cation, cations having a pyrroline skeleton, cations having a pyrrole skeleton, imidazolium cation, tetrahydropyrimidinium cation, dihydropyrimidinium cation, pyrazolium cation, and pyrazolinium cation. An example of a sulfur-containing onium is a sulfonium cation. An example of a phosphorus-containing onium is a phosphonium cation. Examples of organic groups contained in the organic onium are alkyl groups, alkoxyl groups, and alkenyl groups. Specific examples of preferred organic oniums are tetraalkylammonium cations (e.g., tributylmethylammonium cation), alkylpiperidinium cations, and alkylpyrrolidinium cations.

[0079] Examples of the anions contained in the organic cation salt are the same as the examples of the anions contained in the inorganic cation salt. Examples of preferred organic cation salts are 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (EMI-FSI) and trimethylbutylammonium bis(trifluoromethanesulfonyl)imide.

[0080] The antistatic agent may be a combination of an inorganic cationic salt and an organic cationic salt, and preferably contains an organic cationic salt.

[0081] The amount of the antistatic agent in the pressure-sensitive adhesive composition (I) is, for example, 0.5 parts by weight or more, and may be 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, or even 4 parts by weight or more, relative to 100 parts by weight of the polymer (A). The upper limit of the amount may be, for example, less than 10 parts by weight, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or even 6 parts by weight or less, relative to 100 parts by weight of the polymer (A). By appropriately adjusting the amount of the antistatic agent in the pressure-sensitive adhesive composition (I), the durability of the pressure-sensitive adhesive sheet 1 can be further improved.

[0082] <Radical Scavenger> The PSA composition (I) may further contain a radical scavenger. Examples of the radical scavenger include various antioxidants such as hindered phenols, hindered amines, phosphites, phenols, thioethers, and blends of these antioxidants.

[0083] Types of antioxidants are, for example, radical chain inhibitors and peroxide decomposers.

[0084] The antioxidant may be at least one selected from hindered phenol-based, hindered amine-based, and phosphite-based antioxidants.

[0085] The hindered phenolic antioxidant may have a structure in which a tertiary butyl group is bonded to at least one carbon atom adjacent to the carbon atom on the aromatic ring to which the phenolic OH group is bonded. Examples of the hindered phenolic antioxidant include dibutylhydroxytoluene (BHT); Irganox 1010, Irganox 1010FF, Irganox 1035, Irganox 1035FF, Irganox 1076, Irganox 1076FD, Irganox 1076DWJ, Irganox 1098, Irganox 109 ... Irganox 1135, Irganox 1330, Irganox 1726, Irganox 1425WL, Irganox 1520L, Irganox 245, Irganox 245FF, Irganox 259, Irganox 3114, Irganox 565 and Irganox 295 (all of which are trade names manufactured by BASF).

[0086] The hindered amine antioxidant may have at least one hindered piperidine group in one molecule. Examples of the hindered amine antioxidant include Adeka STAB LA-63, Adeka STAB LA-63P, Adeka STAB LA-52, and Adeka STAB LA-57 (all of which are trade names, manufactured by ADEKA Corporation).

[0087] Examples of the phosphite antioxidants are triphenyl phosphite, diphenyl isodecyl phosphite, and phenyl diisodecyl phosphite; and Adeka STAB 2112, Adeka STAB 2112RG, Adeka STAB 1178, and Adeka STAB 3010 (all of which are trade names, manufactured by ADEKA Corporation).

[0088] Examples of the phenolic antioxidants include monophenolic antioxidants, bisphenolic antioxidants, and polymeric phenolic antioxidants. Examples of the monophenolic antioxidants include 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, and stearin-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. Examples of the bisphenol antioxidant are 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), and 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-tetraoxaspiro[5,5]undecane. Examples of the polymeric phenolic antioxidant are 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis-(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, 1,3,5-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, and tocopherol.

[0089] Examples of thioether-based antioxidants are Adekastab AO-503 and Adekastab AO-26 (both are trade names, manufactured by ADEKA Corporation).

[0090] The molecular weight of the radical scavenger (e.g., antioxidant) may be 1,000 or less, 900 or less, 850 or less, 800 or less, 700 or less, 600 or less, 500 or less, 450 or less, or even 400 or less. The lower limit of the molecular weight is, for example, 100 or more. According to studies by the present inventors, radical scavengers having a molecular weight within the above range are particularly suitable for suppressing the amount of radicals generated in a pressure-sensitive adhesive sheet formed from the pressure-sensitive adhesive composition (I).

[0091] The radical scavenger (eg, antioxidant) may be a liquid at 25°C.

[0092] The amount of the radical scavenger in the pressure-sensitive adhesive composition (I) may be, for example, 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, or even 0.5 parts by weight or more, relative to 100 parts by weight of the polymer (A). The upper limit of the amount may be, for example, 15 parts by weight or less, 10 parts by weight or less, 7 parts by weight or less, 5 parts by weight or less, less than 5 parts by weight, 4 parts by weight or less, 3 parts by weight or less, or even 2 parts by weight or less, relative to 100 parts by weight of the polymer (A).

[0093] <Additives> The pressure-sensitive adhesive composition (I) may further contain materials other than the polymer (A), the antistatic agent, and the radical scavenger. Examples of such materials are additives. Examples of additives include crosslinking agents, silane coupling agents, colorants such as pigments and dyes, UV absorbers, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, rework improvers, softeners, polymerization inhibitors, rust inhibitors, inorganic fillers, organic fillers, powders such as metal powders, particles, and foil-like materials. The additives can be blended in a total amount of, for example, 10 parts by weight or less, preferably 5 parts by weight or less, and more preferably 3 parts by weight or less, per 100 parts by weight of the polymer (A).

[0094] Examples of the crosslinking agent include an organic crosslinking agent and a polyfunctional metal chelate. Examples of the organic crosslinking agent include an isocyanate crosslinking agent, a peroxide crosslinking agent, an epoxy crosslinking agent, and an imine crosslinking agent. The organic crosslinking agent and the polyfunctional metal chelate can be used for both the solvent-based and active energy ray-curable pressure-sensitive adhesive composition (I). When the pressure-sensitive adhesive composition (I) is a solvent-based pressure-sensitive adhesive composition, the crosslinking agent is preferably a peroxide crosslinking agent or an isocyanate crosslinking agent. A peroxide crosslinking agent and an isocyanate crosslinking agent may be used in combination. The pressure-sensitive adhesive composition (I) may contain an isocyanate crosslinking agent, a peroxide crosslinking agent, or both an isocyanate crosslinking agent and a peroxide crosslinking agent.

[0095] Examples of isocyanate-based crosslinking agents include aromatic isocyanate compounds such as tolylene diisocyanate, chlorophenylene diisocyanate, diphenylmethane diisocyanate, xylene diisocyanate, and polymethylene polyphenyl isocyanate; alicyclic isocyanate compounds such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and isophorone diisocyanate; and aliphatic isocyanate compounds such as butylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate. The isocyanate-based crosslinking agent may be a compound (adduct) obtained by adding the above isocyanate compound to a polyhydric alcohol compound such as trimethylolpropane; a compound obtained by addition reaction of the above isocyanate compound with a polyol such as polyether polyol, polyester polyol, acrylic polyol, polybutadiene polyol, and polyisoprene polyol; or a derivative of the above isocyanate compound, such as an isocyanurate. Specific examples of the derivatives include a trimethylolpropane / tolylene diisocyanate trimer adduct (e.g., Coronate L, manufactured by Tosoh Corporation), a trimethylolpropane / hexamethylene diisocyanate trimer adduct (e.g., Coronate HL, manufactured by Tosoh Corporation), and an isocyanurate of hexamethylene diisocyanate (e.g., Coronate HX, manufactured by Tosoh Corporation).

[0096] When the pressure-sensitive adhesive composition (I) contains an isocyanate-based crosslinking agent, the amount thereof is, for example, 0.1 to 10 parts by weight, or may be 0.2 to 5 parts by weight, 0.25 to 3 parts by weight, 0.3 to 1 part by weight, or even 0.3 to 0.5 parts by weight, relative to 100 parts by weight of the polymer (A).

[0097] Examples of peroxide-based crosslinking agents include di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, benzoyl peroxide, t-butylperoxyisobutyrate, and 1,1-di(t-hexylperoxy)cyclohexane. The peroxide-based crosslinking agent may be benzoyl peroxide because of its excellent crosslinking reaction efficiency.

[0098] When the pressure-sensitive adhesive composition (I) contains a peroxide-based crosslinking agent, the blending amount thereof is, for example, 0.005 to 5 parts by weight, and may also be 0.01 to 3 parts by weight, 0.05 to 2 parts by weight, 0.07 to 1 part by weight, 0.07 to 0.5 parts by weight, 0.07 to 0.3 parts by weight, or even 0.07 to 0.2 parts by weight, relative to 100 parts by weight of the polymer (A).

[0099] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.

[0100] When the pressure-sensitive adhesive composition (I) contains a silane coupling agent, the blending amount thereof is, for example, 5 parts by weight or less, and may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the polymer (A). The pressure-sensitive adhesive composition (I) does not have to contain a silane coupling agent.

[0101] The type of the pressure-sensitive adhesive composition (I) is, for example, an emulsion type, a solvent type (solution type), an active energy ray curable type (photocurable type), or a hot melt type (hot melt type). From the viewpoint of being able to form a pressure-sensitive adhesive sheet with excellent durability, the pressure-sensitive adhesive composition (I) may be a solvent type or an active energy ray curable type, or may be a solvent type. The solvent-type pressure-sensitive adhesive composition (I) may not contain a photocuring agent such as an ultraviolet curing agent.

[0102] The pressure-sensitive adhesive composition (I) can be used, for example, for an optical laminate. In other words, the pressure-sensitive adhesive composition (I) may be used for an optical laminate. However, the use of the pressure-sensitive adhesive composition (I) is not limited to the above examples.

[0103] In this embodiment, when polymer (A) is synthesized from the above-described group of monomers, the glass transition temperature Tg of the polymer (A) calculated from the FOX formula may be −40°C or lower. The glass transition temperature Tg of the polymer (A) tends to correlate with the glass transition temperature of the pressure-sensitive adhesive sheet 1. When the glass transition temperature Tg of the polymer (A) is, for example, −40°C or lower, the polymer (A) contained in the pressure-sensitive adhesive sheet is less likely to have a small free volume, even in a low-temperature environment. When the free volume of the polymer (A) is less likely to be small, spaces in the pressure-sensitive adhesive sheet 1 through which the antistatic agent can migrate are more likely to be generated. This facilitates the movement of the antistatic agent within the pressure-sensitive adhesive sheet 1, thereby further suppressing an increase in surface resistivity. In addition, when the glass transition temperature Tg of the polymer (A) is, for example, −40°C or lower, the optical laminate 10A can further suppress an increase in the surface resistivity of the pressure-sensitive adhesive sheet 1, for example, even in a low-temperature environment. In other words, the ratio R / R1 can be made smaller.

[0104] The glass transition temperature Tg is, for example, -40°C or lower, -44°C or lower, or even -45°C or lower, and may be -50°C or lower. The lower limit of the glass transition temperature Tg is, for example, -70°C, or may be -60°C. The FOX formula is expressed by the following formula: 1 / Tg=w1 / Tg1+w2 / Tg2+...+w m / Tg m

[0105] In the above formula, Tg is the glass transition temperature [K] of the polymer (A). m are the weight fractions of each monomer in the monomer group. m and Tg are the glass transition temperatures [K] of a single polymer of each monomer. m is a positive integer. As an example, w1 is the weight fraction of a first monomer in the monomer group, and Tg1 is the glass transition temperature [K] of a single polymer of the first monomer. The glass transition temperature Tg [°C] of polymer (A) can be calculated by calculating the glass transition temperature [K] of polymer (A) from the above formula and converting the unit.

[0106] [Antistatic Layer] The antistatic layer 2 is a layer containing a conductive material. The conductive material may be a material other than ITO, such as a conductive polymer, a complex of a conductive polymer and a dopant, an ionic surfactant, conductive fine particles, or an ionic compound.

[0107] Examples of conductive polymers include polythiophene, polyaniline, polypyrrole, polyquinoxaline, polyacetylene, polyphenylene vinylene, polynaphthalene, and derivatives thereof. The conductive material may contain one or more of these conductive polymers. Preferred conductive polymers include polythiophene, polyaniline, and derivatives thereof, with polythiophene derivatives being particularly preferred. Polythiophene, polyaniline, and derivatives thereof function as, for example, water-soluble or water-dispersible conductive polymers. When the conductive polymer is water-soluble or water-dispersible, the antistatic layer 2 can be prepared using an aqueous solution or dispersion of the conductive polymer. In this case, there is no need to use a non-aqueous organic solvent to prepare the antistatic layer 2, thereby suppressing deterioration of the optical film 3, etc., due to the organic solvent.

[0108] The conductive polymer may have a hydrophilic functional group. Examples of the hydrophilic functional group include a sulfone group, an amino group, an amide group, an imino group, a hydroxyl group, a mercapto group, a hydrazino group, a carboxyl group, a sulfate ester group, a phosphate ester group, and salts thereof (e.g., quaternary ammonium salt groups). When the conductive polymer has a hydrophilic functional group, the conductive polymer tends to be easily soluble in water, or the fine particle-shaped conductive polymer tends to be easily dispersed in water.

[0109] From the viewpoints of conductivity and chemical stability, the conductive polymer is preferably poly(3,4-disubstituted thiophene). Examples of poly(3,4-disubstituted thiophene) include poly(3,4-alkylenedioxythiophene) and poly(3,4-dialkoxythiophene), and poly(3,4-alkylenedioxythiophene) is preferred. Poly(3,4-alkylenedioxythiophene) has, for example, a structural unit represented by the following formula (I):

[0110]

[0111] In formula (I), R 1 is, for example, an alkylene group having 1 to 4 carbon atoms. The alkylene group may be linear or branched. Examples of the alkylene group include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1-methyl-1,2-ethylene group, a 1-ethyl-1,2-ethylene group, a 1-methyl-1,3-propylene group, and a 2-methyl-1,3-propylene group, of which a methylene group, a 1,2-ethylene group, or a 1,3-propylene group is preferred, and a 1,2-ethylene group is more preferred. The conductive polymer is preferably poly(3,4-ethylenedioxythiophene) (PEDOT).

[0112] Examples of dopants include polyanions. When the conductive polymer is polythiophene (or a derivative thereof), the polyanion forms an ion pair with the polythiophene (or a derivative thereof), allowing the polythiophene (or a derivative thereof) to be stably dispersed in water. The polyanion is not particularly limited, and examples include carboxylic acid polymers such as polyacrylic acid, polymaleic acid, and polymethacrylic acid; sulfonic acid polymers such as polystyrene sulfonic acid, polyvinyl sulfonic acid, and polyisoprene sulfonic acid; and the like. The polyanion may be a copolymer of vinyl carboxylic acids or vinyl sulfonic acids with other monomers. Examples of other monomers include (meth)acrylate compounds; and aromatic vinyl compounds such as styrene and vinyl naphthalene. The polyanion is particularly preferably polystyrene sulfonic acid (PSS). Examples of composites of conductive polymers and dopants include composites of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid (PEDOT / PSS).

[0113] Examples of ionic surfactants include cationic surfactants such as quaternary ammonium salts, phosphonium salts, and sulfonium salts; anionic surfactants such as carboxylic acid, sulfonate, sulfate, phosphate, and phosphite; amphoteric surfactants such as sulfobetaines, alkylbetaines, and alkylimidazolium betaines; and nonionic surfactants such as polyhydric alcohol derivatives, β-cyclodextrin inclusion compounds, sorbitan fatty acid monoesters, sorbitan fatty acid diesters, polyalkylene oxide derivatives, and amine oxides.

[0114] Examples of conductive fine particles include metal oxide fine particles such as tin oxide, antimony oxide, indium oxide, and zinc oxide, with tin oxide fine particles being preferred. Examples of materials for tin oxide fine particles include tin oxide, antimony-doped tin oxide, indium-doped tin oxide, aluminum-doped tin oxide, tungsten-doped tin oxide, a titanium oxide-cerium oxide-tin oxide composite, and a titanium oxide-tin oxide composite. The average particle size of the conductive fine particles is, for example, 1 to 100 nm, and preferably 2 to 50 nm. The average particle size of the conductive fine particles refers to the particle size (d50) corresponding to 50% cumulative volume in a particle size distribution measured, for example, by a laser diffraction particle sizer.

[0115] As the ionic compound, for example, the ionic compounds explained above in the section <Antistatic Agent> can be used.

[0116] Other examples of conductive materials include carbon materials such as acetylene black, ketjen black, natural graphite, artificial graphite, and carbon nanotubes (CNT); titanium black; homopolymers of monomers having a cationic conductive group such as a quaternary ammonium salt, an amphoteric conductive group such as a betaine compound, an anionic conductive group such as a sulfonate, or a nonionic conductive group such as glycerin, or copolymers of such monomers with other monomers (e.g., polymers having ionic conductivity such as polymers having structural units derived from acrylate or methacrylate having a quaternary ammonium salt group); and alloys (permanent antistatic agents) of hydrophilic polymers such as copolymers of ethylene and methacrylate with acrylic resins or the like.

[0117] From the viewpoints of transparency, total light transmittance, appearance, antistatic effect, and stability of the antistatic effect under high-temperature or high-humidity environments, the antistatic layer 2 preferably contains at least one selected from the group consisting of conductive polymers and carbon materials, and more preferably contains a carbon material. Carbon materials are resistant to decomposition under high-temperature and high-humidity environments and / or ultraviolet irradiation. Therefore, by including a carbon material in the antistatic layer 2, weather resistance can be improved. In addition, by including a carbon material in the antistatic layer 2, the optical laminate 10A can further suppress an increase in the surface resistivity on the pressure-sensitive adhesive sheet 1 side, even under low-temperature environments, for example. In other words, the ratio R / R1 can be made smaller.

[0118] The antistatic layer 2 may further contain other materials such as a binder in addition to the conductive material. The binder tends to improve, for example, the film-forming properties of the conductive material and the adhesion and bonding strength (anchoring strength) of the antistatic layer 2 to the optical film 3. Examples of binders include oxazoline group-containing polymers, polyurethane resins, polyester resins, acrylic resins, polyether resins, cellulose resins, polyvinyl alcohol resins, epoxy resins, polyvinylpyrrolidone, polystyrene resins, polyethylene glycol, and pentaerythritol. Preferred are oxazoline group-containing polymers, polyurethane resins, polyester resins, and acrylic resins, with polyurethane resins being particularly preferred. The antistatic layer 2 may contain one or more of these binders. The binder content in the antistatic layer 2 is, for example, 1% by weight to 90% by weight, and preferably 10% by weight to 80% by weight.

[0119] In the optical laminate 10A, the surface resistivity of the antistatic layer 2 at 25°C is, for example, 3.0 × 10 8 The surface resistivity of the antistatic layer 2 at 25° C. is, for example, 3.0×10 8 By having a resistivity of Ω / □ or less, display defects due to charging of a liquid crystal display device including the optical laminate 10A can be more effectively prevented, even in an environment where static electricity is likely to occur. The surface resistivity of the antistatic layer 2 can be determined by the following method. First, a laminate is prepared in which the surface of the antistatic layer 2 is exposed to the outside. An example of such a laminate is a laminate L1 consisting of an optical film 3 and an antistatic layer 2. Next, the surface resistivity of the surface of the antistatic layer 2 in the prepared laminate is measured. The surface resistivity of the antistatic layer 2 can be measured using a Hiresta MCP-HT800 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) in accordance with the method specified in JIS K6911:1995.

[0120] The surface resistivity of the antistatic layer 2 is preferably 2.0×10 8 Ω / □ or less, and more preferably 1.0×10 8Ω / □, and more preferably less than 7.0×10 7 Ω / □ or less, and particularly preferably 5.0×10 7 The lower limit of the surface resistivity of the antistatic layer 2 is, for example, 1.0×10 2 Ω / □, and 1.0×10 5 Ω / □, especially 1.0×10 7 When the optical laminate 10A is used in a liquid crystal display device equipped with a touch sensor or a touch panel, the surface resistivity of the antistatic layer 2 is set to 1.0×10 in order to ensure sufficient sensitivity of the touch sensor or the touch panel provided in the liquid crystal display device. 7 It may be larger than Ω / □.

[0121] The thickness of the antistatic layer 2 is, for example, 5 nm to 180 nm, preferably 150 nm or less, more preferably 140 nm or less, and in some cases 100 nm or less. The thickness of the antistatic layer 2 may be 10 nm or more, 20 nm or more, 50 nm or more, or even 55 nm or more. In order to suppress an increase in surface resistivity in the low temperature range, the thickness may be 70 nm or more, and in some cases, may be 100 nm or more. By appropriately adjusting the thickness of the antistatic layer 2, the antistatic effect can be further improved. In addition, by appropriately adjusting the thickness of the antistatic layer 2, the value of the ratio R / R1 in the optical laminate 10A can be further reduced.

[0122] [Optical Film] The optical film 3 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The optical film 3 may be a laminated film including a polarizing film and / or a retardation film. The optical film 3 may include a glass film.

[0123] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is, for example, disposed in contact with a main surface of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0124] The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which has been uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; etc. A polarizer typically comprises a polyvinyl alcohol film (polyvinyl alcohol films include an ethylene-vinyl acetate copolymer partially saponified film) and a dichroic substance such as iodine.

[0125] The thickness of the polarizer is not particularly limited and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.

[0126] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0127] The thickness of the protective film can be determined as appropriate, but is generally about 10 to 200 μm in view of strength, workability such as handling, thinness, and the like.

[0128] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing plate adhesives exhibit suitable adhesive properties for various protective films. The adhesive may contain a metal compound filler.

[0129] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0130] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.

[0131] The polarizing film may be a circular polarizing film.

[0132] The retardation film may be a film obtained by stretching a polymer film or a film obtained by aligning and fixing a liquid crystal material. The retardation film has birefringence, for example, in the in-plane and / or thickness direction.

[0133] Examples of the retardation film include anti-reflection retardation films (see JP 2012-133303 A,

[0221] ,

[0222] ,

[0228] ), viewing angle compensation retardation films (see JP 2012-133303 A,

[0225] ,

[0226] ), and tilted orientation retardation films for viewing angle compensation (see JP 2012-133303 A,

[0227] ).

[0134] The retardation film is not particularly limited in terms of, for example, retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, etc., as long as it substantially has the above-mentioned functions, and a known retardation film can be used.

[0135] The thickness of the retardation film is preferably 20 μm or less, more preferably 10 μm or less, still more preferably 1 to 9 μm, and particularly preferably 3 to 8 μm.

[0136] The retardation film is composed of, for example, two layers of a quarter-wave plate and a half-wave plate in which a liquid crystal material is oriented and fixed.

[0137] [Method for manufacturing optical laminate] The optical laminate 10A includes, for example, producing a laminate L2 consisting of a substrate and an adhesive sheet 1, producing a laminate L1 consisting of an optical film 3 and an antistatic layer 2, and transferring the adhesive sheet 1 of the laminate L2 onto the antistatic layer 2 of the laminate L1.

[0138] (Method for manufacturing laminate L1) First, a solution or dispersion of a conductive material is prepared. The solvent for the solution or dispersion is, for example, water, and may further contain a water-soluble organic solvent. Examples of water-soluble organic solvents include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol.

[0139] Next, a solution or dispersion of a conductive material is applied to the surface of the optical film 3. The resulting coating is dried to form an antistatic layer 2 on the optical film 3. In this way, a laminate L1 consisting of the optical film 3 and the antistatic layer 2 is obtained.

[0140] (Method for producing laminate L2) The pressure-sensitive adhesive sheet 1 is formed from the pressure-sensitive adhesive composition (I). The pressure-sensitive adhesive sheet 1 contains, for example, a crosslinked product of a (meth)acrylic polymer. The pressure-sensitive adhesive sheet 1 is formed from the pressure-sensitive adhesive composition (I) by the following method.

[0141] The method for producing the pressure-sensitive adhesive sheet 1 includes, for example, applying the pressure-sensitive adhesive composition (I) to a substrate to form a coating film, and drying the resulting coating film. By drying the coating film, the pressure-sensitive adhesive sheet 1 is formed on the substrate. In this way, a laminate L2 consisting of the substrate and the pressure-sensitive adhesive sheet 1 is obtained.

[0142] The substrate may be, for example, a release film. The pressure-sensitive adhesive sheet 1 formed on the release film may be transferred to, for example, an optical film. The substrate may be an optical film.

[0143] After the adhesive sheet 1 is transferred to the antistatic layer 2, the release film can be used as a release liner until the adhesive sheet 1 is put to practical use, thereby simplifying the process.

[0144] Examples of materials constituting the release film include suitable thin sheets such as porous materials such as plastic film, paper, cloth, and nonwoven fabric, nets, foam sheets, metal foils, and laminates thereof, but plastic film is preferably used because of its excellent surface smoothness.

[0145] The plastic film is not particularly limited, and examples thereof include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polybutylene terephthalate film, polyurethane film, and ethylene-vinyl acetate copolymer film.

[0146] The thickness of the release film is usually 5 to 200 μm, and preferably about 5 to 100 μm. The release film is subjected to a release treatment, for example, a silicone-based, fluorine-based, or long-chain alkyl-based treatment. The release film may be subjected to a release and antifouling treatment using a fatty acid amide-based release agent, silica powder, or the like, or an antistatic treatment such as a coating-type, kneading-type, or vapor deposition-type.

[0147] A solution (adhesive solution) containing the adhesive composition (I) may be applied to the substrate. The solids concentration of the adhesive solution is, for example, 5 to 50 wt %, preferably 10 to 40 wt %. The adhesive solution can be prepared by appropriately adding the same solvent as the polymerization solvent or a different solvent to the adhesive composition (I) depending on the polymerization form of the (meth)acrylic polymer (A).

[0148] Various methods can be used to apply the pressure-sensitive adhesive composition (I) to a substrate, including, for example, roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and extrusion coating using a die coater, etc. The amount of pressure-sensitive adhesive composition (I) to be applied can be adjusted appropriately depending on the desired thickness of the pressure-sensitive adhesive sheet 1.

[0149] By drying the coating film, the coating film hardens, forming the pressure-sensitive adhesive sheet 1. The drying temperature of the coating film is, for example, 130°C or lower, preferably 125°C or lower, more preferably 120°C or lower, even more preferably 110°C or lower, and particularly preferably 100°C or lower. The drying temperature of the coating film may be 60°C or higher, or may be 80°C or higher. When the drying temperature is 60°C or higher, for example, the reaction of the isocyanate-based crosslinking agent proceeds smoothly, the cohesive strength of the pressure-sensitive adhesive sheet 1 can be improved, and display unevenness of the image display device tends to be reduced. When the drying temperature is 130°C or lower, for example, the reaction rate of the isocyanate-based crosslinking agent can be appropriately adjusted, and transparency tends to be ensured.

[0150] The drying time of the coating film can be adjusted appropriately depending on the composition of the pressure-sensitive adhesive composition (I), and is preferably 30 to 300 seconds, more preferably 40 to 240 seconds, and particularly preferably 60 to 180 seconds.

[0151] The thickness of the pressure-sensitive adhesive sheet 1 is not particularly limited and may be 2 to 150 μm, 2 to 100 μm, or 5 to 50 μm. By appropriately adjusting the thickness of the pressure-sensitive adhesive sheet 1, it is possible to improve the adhesion between the pressure-sensitive adhesive sheet 1 and the antistatic layer 2. In addition, by appropriately adjusting the thickness of the pressure-sensitive adhesive sheet 1, it is possible to prevent the pressure-sensitive adhesive sheet 1 from peeling off from an adherend such as glass or an image display device.

[0152] The pressure-sensitive adhesive sheet 1 of the laminate L2 obtained above is transferred onto the antistatic layer 2 of the laminate L1, thereby obtaining an optical laminate 10A consisting of the optical film 3, the antistatic layer 2, and the pressure-sensitive adhesive sheet 1.

[0153] Figure 2 is a cross-sectional view schematically showing another example of the optical laminate according to this embodiment. As shown in Figure 2, the optical laminate 10B has a laminated structure in which a release liner 4, a pressure-sensitive adhesive sheet 1, an antistatic layer 2, and an optical film 3 are laminated in this order. After peeling off the release liner 4, the optical laminate 10B can be used by being attached to, for example, an image display cell. The following examples may be combined with each other as long as there is no technical contradiction.

[0154] Examples of materials that can be used to form the release liner 4 include plastic films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester film; porous materials such as paper, cloth, and nonwoven fabric; and appropriate thin sheets such as nets, foam sheets, metal foils, and laminates of these. However, plastic films are preferred because of their excellent surface smoothness.

[0155] The plastic film is not particularly limited as long as it is a film that can protect the adhesive sheet 1, and examples include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polybutylene terephthalate film, polyurethane film, ethylene-vinyl acetate copolymer film, etc.

[0156] The thickness of the release liner 4 is usually 5 to 200 μm, and preferably about 5 to 100 μm. If necessary, the release liner 4 may be subjected to a release and antifouling treatment using a silicone-based, fluorine-based, long-chain alkyl-based or fatty acid amide-based release agent, silica powder, or the like, or an antistatic treatment such as a coating-type, kneading-type or vapor deposition-type. In particular, by appropriately subjecting the surface of the release liner 4 to a release treatment such as silicone treatment, long-chain alkyl treatment or fluorine treatment, the releasability from the PSA sheet 1 can be further improved.

[0157] As described above, the release film used when producing the pressure-sensitive adhesive sheet 1 may also be used as the release liner 4 .

[0158] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate. The optical laminate of this embodiment is suitable for use in image display devices used in environments where static electricity is particularly likely to occur, particularly in vehicle displays. Examples of vehicle displays include panels for car navigation devices, cluster panels, and mirror displays. Cluster panels are panels that display the vehicle's traveling speed, engine rotation speed, etc.

[0159] [Embodiment of Image Display Panel] Fig. 3 is a cross-sectional view schematically showing an example of an image display panel according to this embodiment. As shown in Fig. 3, the image display panel 11A includes an optical laminate 10A and further includes, for example, an image display cell 30A. In detail, the optical laminate 10A is bonded to the image display cell 30A via an adhesive sheet 1.

[0160] The image display cell 30A includes, for example, an image forming layer 32, a first transparent substrate 31, and a second transparent substrate 33. The image forming layer 32 is disposed, for example, between the first transparent substrate 31 and the second transparent substrate 33, and is in contact with each of the first transparent substrate 31 and the second transparent substrate 33. The pressure-sensitive adhesive sheet 1 of the optical laminate 10A is in contact with, for example, the first transparent substrate 31 of the image display cell 30A.

[0161] The image forming layer 32 is, for example, a liquid crystal layer containing liquid crystal molecules that are homogeneously aligned in the absence of an electric field. A liquid crystal layer containing such liquid crystal molecules is suitable for an IPS (In-Plane-Switching) mode. However, the liquid crystal layer may also be used for a TN (Twisted Nematic) type, an STN (Super Twisted Nematic) type, a π type, a VA (Vertical Alignment) type, or the like. In this specification, an image display cell including a liquid crystal layer may be referred to as a liquid crystal cell, and an image display panel including a liquid crystal cell may be referred to as a liquid crystal panel. The image forming layer 32 may also be an EL light-emitting layer.

[0162] The thickness of the image forming layer 32 is, for example, 1.5 μm to 4 μm.

[0163] Examples of materials for the first transparent substrate 31 and the second transparent substrate 33 include glass and polymer. In this specification, a transparent substrate made of a polymer may be referred to as a polymer film. Examples of polymers that make up a transparent substrate include polyethylene terephthalate, polycycloolefin, and polycarbonate. The thickness of a transparent substrate made of glass is, for example, 0.1 mm to 1 mm. The thickness of a transparent substrate made of a polymer is, for example, 10 μm to 200 μm.

[0164] The image display cell 30A may further include layers other than the image forming layer 32, the first transparent substrate 31, and the second transparent substrate 33. Examples of such layers include a color filter, an easy-adhesion layer, and a hard coat layer. The color filter is, for example, arranged on the viewing side of the image forming layer 32, and is preferably located between the first transparent substrate 31 and the pressure-sensitive adhesive sheet 1 of the optical laminate 10A. The easy-adhesion layer and the hard coat layer are, for example, arranged on the surface of the first transparent substrate 31 or the second transparent substrate 33.

[0165] The image display panel 11A may further include other components in addition to the optical stack 10A and the image display cell 30A. For example, the image display panel 11A may further include a conductive structure (not shown) electrically connected to the side surface of the optical stack 10A. Connecting the conductive structure to earth makes it easier to prevent the optical stack 10A from being charged with static electricity. The conductive structure may cover the entire side surface of the optical stack 10A, or may cover only a portion of the side surface of the optical stack 10A. The ratio of the area of ​​the side surface of the optical stack 10A covered by the conductive structure to the entire area of ​​the side surface of the optical stack 10A is, for example, 1% or more, and preferably 3% or more.

[0166] Examples of materials for the conductive structure include conductive pastes made of metals such as silver and gold, conductive adhesives, and other conductive materials. The conductive structure may be wiring extending from the side surfaces of the optical laminate 10A.

[0167] The image display panel 11A may further include other optical films in addition to the optical film 3. Examples of other optical films include films used in image display devices, such as polarizing plates, reflectors, anti-transmission plates, viewing angle compensation films, and brightness enhancement films. The image display panel 11A may include one or more of these other optical films.

[0168] When the other optical film is a polarizing plate, the polarizing plate is bonded to the second transparent substrate 33 of the image display cell 30A via, for example, an adhesive sheet. This polarizing plate has, for example, the configuration described above for the optical film 3. In the polarizing plate as the other optical film, the transmission axis (or absorption axis) of the polarizer is, for example, perpendicular to the transmission axis (or absorption axis) of the polarizer in the polarizing plate. As the material of the adhesive sheet for bonding the polarizing plate and the second transparent substrate 33, those described above for the adhesive sheet 1 can be used. The thickness of this adhesive sheet is not particularly limited and is, for example, 1 to 100 μm, preferably 2 to 50 μm, more preferably 2 to 40 μm, and even more preferably 5 to 35 μm.

[0169] FIG. 4 is a cross-sectional view schematically illustrating another example of an image display panel according to this embodiment. As shown in FIG. 4, the image display panel 11B further includes a conductive layer 40 disposed between the optical laminate 10A and the image display cell 30A. However, the image display panel is preferably the image display panel 11A that does not include the conductive layer 40. The image display panel 11B provided with the conductive layer 40 tends to have high reflectivity, which may reduce the visibility of the display. The image display panel 11A that does not include the conductive layer 40 preferably has a conductive portion (the above-described conductive structure) adjacent to the adhesive sheet 1. For example, a conductive silver paste is used as the conductive portion. After bonding the optical laminate 10A to the image display cell 30A, a conductive silver paste or the like is applied to the side surface of the adhesive sheet 1 to form a conductive portion, which is then electrically connected to other wiring or the housing of the image display device, thereby improving the antistatic properties of the image display panel.

[0170] The conductive layer 40 is, for example, a layer containing a conductive agent. Examples of the conductive agent that can be used include metal oxides, conductive polymers, and those described above for the adhesive sheet 1 and the antistatic layer 2. The thickness of the conductive layer 40 is, for example, 5 nm to 180 nm. The surface resistivity of the conductive layer 40 is, for example, 1.0×10 6 Ω / □ to 1.0 x 10 10 Ω / □, preferably 1.0×10 8 Ω / □ to 1.0 x 10 9 It is Ω / □.

[0171] The image display panel of this embodiment may be an image display panel having a built-in touch sensing function. FIG. 5 shows an example of an image display panel having a built-in touch sensing function. FIG. 5 is a cross-sectional view schematically showing another example of the image display panel according to this embodiment. As shown in FIG. 5, the image display panel 11C includes an image display cell 30B further including a touch sensing electrode unit 35. In the image display cell 30B, the touch sensing electrode unit 35 is disposed between a first transparent substrate 31 and a second transparent substrate 33. The touch sensing electrode unit 35 has touch sensor and touch drive functions. The image display panel 11C is a so-called in-cell image display panel, and the image display cell 30B is a so-called in-cell image display cell. However, in the image display cell 30B, the touch sensing electrode unit 35 may be disposed closer to the viewer than the first transparent substrate 31. That is, the image display panel 11C may be a so-called on-cell image display panel, and the image display cell 30B may be a so-called on-cell image display cell.

[0172] The touch sensing electrode unit 35 includes, for example, a touch sensor electrode 36 and a touch drive electrode 37. The touch sensor electrode 36 refers to a (receiving) electrode for touch detection. The touch sensor electrode 36 and the touch drive electrode 37 can be independently formed in various patterns. For example, when the image display cell 30B is flat, the touch sensor electrode 36 and the touch drive electrode 37 can be independently provided in the X-axis direction and the Y-axis direction, respectively, and can be formed in a pattern in which they intersect at right angles. In FIG. 5 , in the touch sensing electrode unit 35, the touch sensor electrode 36 is disposed closer to the viewing side than the touch drive electrode 37. However, the touch drive electrode 37 may also be disposed closer to the viewing side than the touch sensor electrode 36. In the touch sensing electrode unit 35, the touch sensor electrode 36 and the touch drive electrode 37 may be integrated.

[0173] 5, the touch sensing electrode unit 35 is disposed between the image forming layer 32 and the first transparent substrate 31 (on the viewing side of the image forming layer 32). However, the touch sensing electrode unit 35 may also be disposed between the image forming layer 32 and the second transparent substrate 33 (on the lighting system side of the image forming layer 32).

[0174] In the touch sensing electrode unit 35, the touch sensor electrode 36 and the touch drive electrode 37 do not need to be in contact with each other. For example, the touch sensor electrode 36 may be disposed between the image forming layer 32 and the first transparent substrate 31, and the touch drive electrode 37 may be disposed between the image forming layer 32 and the second transparent substrate 33.

[0175] The drive electrode (touch drive electrode 37 or an electrode in which the touch sensor electrode 36 and the touch drive electrode 37 are integrated) in the touch sensing electrode portion 35 can also serve as a common electrode that controls the image forming layer 32.

[0176] The touch sensor electrode 36 (capacitive sensor), the touch drive electrode 37, or an electrode formed by integrating these electrodes, which constitute the touch sensing electrode unit 35, function as a transparent conductive layer. The material of this transparent conductive layer is not particularly limited, and examples include metals such as gold, silver, copper, platinum, palladium, aluminum, nickel, chromium, titanium, iron, cobalt, tin, magnesium, and tungsten, as well as alloys thereof. The material of the transparent conductive layer may be an oxide of a metal such as indium, tin, zinc, gallium, antimony, zirconium, or cadmium. Specific examples of such oxides include indium oxide, tin oxide, titanium oxide, cadmium oxide, and mixtures thereof. The material of the transparent conductive layer may also be a metal compound such as copper iodide. The material of the transparent conductive layer is preferably indium oxide (ITO) containing tin oxide or tin oxide containing antimony, with ITO being particularly preferred. When the material of the transparent conductive layer is ITO, it is preferable that the content of indium oxide in the transparent conductive layer is 80 to 99% by weight and the content of tin oxide is 1 to 20% by weight.

[0177] The electrodes constituting the touch sensing electrode unit 35 (the touch sensor electrodes 36, the touch drive electrodes 37, or an electrode formed by integrating these) can be formed as a transparent electrode pattern between the first transparent substrate 31 and the second transparent substrate 33 by a conventional method. This transparent electrode pattern is electrically connected, for example, to wiring lines formed at the ends of the transparent substrates. The wiring lines are connected, for example, to a controller IC. The shape of the transparent electrode pattern can be any shape depending on the application, such as a comb shape, a stripe shape, or a diamond shape. The thickness of the transparent electrode pattern is, for example, 10 nm to 100 nm. The width of the transparent electrode pattern is, for example, 0.1 mm to 5 mm.

[0178] [Embodiment of Image Display Device] The image display device of this embodiment includes, for example, an image display panel 11A and an illumination system. Note that the image display panels 11B and 11C shown in FIGS. 4 and 5 may also be used instead of the image display panel 11A. In the image display device, the image display panel 11A is disposed, for example, closer to the viewing side than the illumination system. The illumination system includes, for example, a backlight or a reflector, and irradiates light onto the image display panel 11A.

[0179] The image display device may be an organic EL display or a liquid crystal display. However, the image display device is not limited to these examples. The image display device may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device can be used for home appliances, in-vehicle applications, public information displays (PID), and the like, and is preferably an in-vehicle display.

[0180] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0181] <Weight-average molecular weight of (meth)acrylic polymer> The weight-average molecular weight (Mw) of the (meth)acrylic polymer was measured by GPC (gel permeation chromatography). The Mw / Mn of the (meth)acrylic polymer was also measured in the same manner. Analytical device: HLC-8120GPC, manufactured by Tosoh Corporation Column: G7000H, manufactured by Tosoh Corporation XL +GMH XL +GMH XL Column size: 7.8 mm diameter x 30 cm, total 90 cm Column temperature: 40°C Flow rate: 0.8 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene

[0182] [Preparation of (meth)acrylic polymer A1] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with a monomer mixture containing 78.95 parts by weight of n-butyl acrylate (BA), 16 parts by weight of phenoxyethyl acrylate (PEA), 0.05 parts by weight of 4-hydroxybutyl acrylate (HBA), and 5 parts by weight of acrylic acid (AA). Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN; manufactured by Kishida Chemical Co., Ltd.) as a polymerization initiator was charged together with 100 parts by weight of ethyl acetate per 100 parts by weight of the monomer mixture. While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at around 55°C, and the polymerization reaction was carried out for 8 hours, thereby preparing a solution of (meth)acrylic polymer A1 with a weight average molecular weight (Mw) of 2.5 million. The glass transition temperature of (meth)acrylic polymer A1 calculated from the FOX formula was −43.5° C.

[0183] [Preparation of (meth)acrylic polymer A2] A solution of (meth)acrylic polymer A2 having a weight average molecular weight (Mw) of 1,900,000 was prepared in the same manner as in the preparation of (meth)acrylic polymer A1, except that the monomer mixture charged into the flask was 60 parts by weight of 2-methoxyethyl acrylate (MEA), 39 parts by weight of BA, and 1 part by weight of HBA. The glass transition temperature of (meth)acrylic polymer A2 calculated from the FOX equation was −52.0° C.

[0184] [Preparation of (meth)acrylic polymer A3] A solution of (meth)acrylic polymer A3 having a weight average molecular weight (Mw) of 2,000,000 was prepared in the same manner as in the preparation of (meth)acrylic polymer A1, except that the monomer mixture charged into the flask was 67 parts by weight of MEA, 22 parts by weight of BA, 10 parts by weight of PEA, and 1 part by weight of HBA. The glass transition temperature of (meth)acrylic polymer A3 calculated from the FOX formula was −45.0° C.

[0185] [Preparation of (meth)acrylic polymer A4] A solution of (meth)acrylic polymer A4 having a weight average molecular weight (Mw) of 1,800,000 was prepared in the same manner as in the preparation of (meth)acrylic polymer A1, except that the monomer mixture charged into the flask was 99 parts by weight of BA and 1 part by weight of HBA. The glass transition temperature of (meth)acrylic polymer A4 calculated from the FOX equation was -55.0°C.

[0186] The monomers and the amounts used in synthesizing each (meth)acrylic polymer are summarized in Table 1. In the table, the symbol "-" means that the component in question is not included.

[0187]

[0188] Example 1 [TAC Film with Hard Coat Layer] First, a resin solution (manufactured by DIC Corporation, product name: Unidic 17-806, solids concentration: 80%) in which a UV-curable resin monomer or oligomer containing urethane acrylate as the main component was dissolved in butyl acetate was prepared. For 100 parts by weight of the solids content of this resin solution, 5 parts by weight of a photopolymerization initiator (manufactured by BASF Corporation, product name: IRGACURE 907) and 0.1 parts by weight of a leveling agent (manufactured by DIC Corporation, product name: GRANDIC PC4100) were added to the resin solution. Next, cyclopentanone and propylene glycol monomethyl ether were added to the resin solution in a weight ratio of 45:55 so that the solids concentration in the resin solution was adjusted to 36%. This produced a hard coat layer-forming material. The resulting coating material was applied to a 40 μm-thick transparent protective film containing triacetyl cellulose (TAC film manufactured by Konica Minolta, product name "KC4UY") to form a coating film. The thickness of the coating film was adjusted so that the thickness of the hard coat layer obtained by curing the coating material was adjusted to 7 μm. Next, the coating film was dried at 90° C. for 1 minute and further irradiated with a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm. 2 The coating film was irradiated with ultraviolet light of 1000 kJ / cm 2 , thereby curing the coating film and obtaining a TAC film with a hard coating layer (HC).

[0189] [Polarizing Plate] First, an 80 μm-thick polyvinyl alcohol film was stretched to a stretch ratio of 3x while dyeing it in a 0.3% iodine solution (temperature: 30°C) for 1 minute between multiple rolls with different speed ratios. The resulting stretched film was then immersed in an aqueous solution (temperature: 60°C) containing 4% boric acid and 10% potassium iodide for 0.5 minutes, while being stretched to a total stretch ratio of 6x. The stretched film was then washed by immersing it in an aqueous solution (temperature: 30°C) containing 1.5% potassium iodide for 10 seconds. The stretched film was then dried at 50°C for 4 minutes to obtain a 30 μm-thick polarizer. A transparent protective film (thickness: 30 μm) made of a modified acrylic polymer having a lactone ring structure was bonded to one main surface of the resulting polarizer via a polyvinyl alcohol adhesive. The above-described TAC film (thickness: 47 μm) with a hard coat layer was bonded to the other main surface of the polarizer via a polyvinyl alcohol-based adhesive. At this time, the other main surface of the polarizer was bonded to a transparent protective film. Bonding of the polarizer and the transparent protective film was performed using a roll laminator. After bonding the polarizer and the transparent protective film, the resulting laminate was heated and dried at 70° C. for 5 minutes in an oven to obtain a polarizing plate consisting of the hard coat layer and the polarizing film.

[0190] [Antistatic Layer] First, a coating solution with a solids concentration of 0.5 wt % was prepared by mixing 50 parts of a solution containing PEDOT / PSS (manufactured by Nagase ChemteX Corporation, product numbers N006-45-2A and N006-45-2B) and 50 parts of water. Next, the coating solution was applied to the surface of the polarizing plate facing the polarizing film. The resulting coating film was dried at 80°C for 2 minutes to prepare an antistatic layer. This resulted in a laminate L1 consisting of a polarizing plate and an antistatic layer. The thickness of the antistatic layer was 60 nm.

[0191] [Adhesive Sheet] A solution of the (meth)acrylic adhesive composition of Example 1 was prepared by further blending, per 100 parts by weight of the solids content of the solution of (meth)acrylic polymer A1, 0.3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name: Coronate 2770), 20 parts by weight of 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (EMI-FSI) (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., product name: Elexel AS110) as an antistatic agent, 0.5 parts by weight of an antioxidant (manufactured by BASF, product name: Irganox 1010), and 0.4 parts by weight of a silane coupling agent (manufactured by Kaneka Corporation, product name: Silyl SAT010).

[0192] The resulting solution was then applied to one side of a release liner (Mitsubishi Chemical Polyester Film Corporation's MRF38). The release liner was a polyethylene terephthalate film treated with a silicone-based release agent. The resulting coating was dried at 155°C for 1 minute to obtain a laminate L2 in which a pressure-sensitive adhesive sheet was formed on the surface of the release liner. The pressure-sensitive adhesive sheet had a thickness of 20 µm.

[0193] [Optical laminate] Next, the pressure-sensitive adhesive sheet of the laminate L2 obtained above was transferred onto the antistatic layer of the laminate L1 to produce a laminate L3 in which a polarizing plate, an antistatic layer, a pressure-sensitive adhesive sheet, and a release liner were laminated in this order. The release liner was peeled off from the laminate L3 to obtain the optical laminate of Example 1.

[0194] Example 2 An optical laminate according to Example 2 was obtained by the same method as Example 1, except that in producing the pressure-sensitive adhesive sheet, a solution of (meth)acrylic polymer A2 was used, and 6 parts by weight of EMI-FSI was used as an antistatic agent relative to 100 parts by weight of the solid content of the solution of (meth)acrylic polymer A2.

[0195] Example 3 An optical laminate according to Example 3 was obtained in the same manner as in Example 2, except that the PEDOT / PSS coating solution was applied to the polarizing film so that the antistatic layer had a thickness of 130 nm.

[0196] Example 4 An optical laminate according to Example 4 was obtained in the same manner as Example 1, except that a pressure-sensitive adhesive sheet and an antistatic layer were prepared by the following method. First, a solution of (meth)acrylic polymer A3 was used to prepare the pressure-sensitive adhesive sheet. 8 parts by weight of EMI-FSI was used as an antistatic agent per 100 parts by weight of the solid content of the (meth)acrylic polymer A3 solution. A coating solution of PEDOT / PSS was applied to a polarized film so that the thickness of the antistatic layer would be 30 nm.

[0197] Example 5 An optical laminate according to Example 5 was obtained in the same manner as in Example 4, except that the PEDOT / PSS coating solution was applied to the polarizing film so that the antistatic layer had a thickness of 60 nm.

[0198] Example 6 An optical laminate according to Example 6 was obtained in the same manner as in Example 4, except that the PEDOT / PSS coating solution was applied to the polarizing film so that the antistatic layer had a thickness of 130 nm.

[0199] Example 7 An optical laminate according to Example 7 was obtained by the same method as Example 4, except that a laminate L1 consisting of a polarizing plate and an antistatic layer was prepared by the following method. First, a coating solution with a solids concentration of 0.5 wt % was prepared by mixing 14 parts by weight of a solution containing CNT and a urethane binder (manufactured by Nagase ChemteX Corporation, product name: C-100A) and 86 parts by weight of water. Next, the coating solution was applied to the main surface of the polarizing plate on the polarizing film side. The obtained coating film was dried at 90°C for 1 minute to prepare an antistatic layer. This resulted in a laminate L1 consisting of a polarizing plate and an antistatic layer. The thickness of the antistatic layer was 55 nm.

[0200] Example 8 An optical laminate according to Example 8 was obtained by the same method as in Example 7, except that a coating liquid having a solid content concentration of 0.5 wt % was applied to the main surface of the polarizing film side of the polarizing plate described above by mixing 15.1 parts by weight of a solution containing CNTs and a urethane-based binder (manufactured by Nagase ChemteX Corporation, product name: C-100A), 0.7 parts by weight of a binder containing an oxazoline group (manufactured by Nippon Shokubai Co., Ltd., product name: EPOCROS (registered trademark) WS-700), and 84 parts by weight of water.

[0201] Example 10 An optical laminate according to Example 10 was obtained in the same manner as in Example 2, except that in producing the pressure-sensitive adhesive sheet, 15 parts by weight of EMI-FSI was used as an antistatic agent relative to 100 parts by weight of the solid content of the solution of (meth)acrylic polymer A2, and the PEDOT / PSS coating solution was applied to the polarized film so that the thickness of the antistatic layer was 30 nm.

[0202] Comparative Example 1 An optical laminate according to Comparative Example 1 was obtained in the same manner as in Example 1, except that a pressure-sensitive adhesive sheet was produced by the following method and an antistatic layer was not produced. In producing the pressure-sensitive adhesive sheet, a solution of (meth)acrylic polymer A4 was used. 10 parts by weight of EMI-FSI was used as an antistatic agent per 100 parts by weight of the solid content of the solution of (meth)acrylic polymer A4.

[0203] The following evaluations were carried out for Examples 1 to 10 and Comparative Example 1. The evaluation results are shown in Table 2.

[0204] <Measurement of Surface Resistivity of Pressure-Sensitive Adhesive Sheet> In each of the Examples and Comparative Examples, the surface resistivity of the pressure-sensitive adhesive sheet at 25° C. was measured using a laminate L2 in which a pressure-sensitive adhesive sheet was formed on the surface of a release liner. The surface resistivity of the pressure-sensitive adhesive sheet in laminate L2 was measured using a resistivity meter (Hiresta MCP-HT800 manufactured by Mitsubishi Chemical Analytech Co., Ltd.) under conditions of an applied voltage of 250 V and an application time of 10 seconds.

[0205] <Measurement of surface resistivity of antistatic layer> In each example and comparative example, the surface resistivity of the antistatic layer was measured using a laminate L1 consisting of a polarizing plate and an antistatic layer. The surface resistivity of the antistatic layer at 25°C was measured using the resistivity meter described above in accordance with the method specified in JIS K6911:1995 under conditions of an applied voltage of 10 V and an application time of 10 seconds.

[0206] <Measurement of surface resistivity of pressure-sensitive adhesive sheet side of optical laminate> The surface resistivity of the pressure-sensitive adhesive sheet side was measured using the optical laminates according to each Example and Comparative Example. The surface resistivity R1 of the pressure-sensitive adhesive sheet side of the optical laminate at room temperature (25°C) was measured using the resistivity meter described above under the conditions of an applied voltage of 250 V and an application time of 10 seconds.

[0207] The surface resistivity R of the pressure-sensitive adhesive sheet side of the optical laminate at -15°C was measured before and after the weather resistance test as follows. The polarizing plate side (hard coat layer side) of laminate L3 was placed on a cold plate set at -15°C. After approximately 30 seconds had elapsed, the release liner was immediately peeled off from laminate L3 and the surface resistivity of the pressure-sensitive adhesive sheet side was measured. The surface resistivity R of the pressure-sensitive adhesive sheet side of the optical laminate at -15°C was measured using the resistivity meter described above under conditions of an applied voltage of 250 V and an application time of 10 seconds. The weather resistance test was carried out using an ultraviolet fade tester (U48HB, manufactured by Suga Test Instruments Co., Ltd.) according to the method described above.

[0208] <Durability> The durability of the optical laminate was evaluated by the following method. The prepared optical laminate was fixed to the surface of a glass plate (Corning, Eagle XG) via the adhesive sheet to obtain an optical laminate with a glass plate. Fixing was performed in an atmosphere of 24°C and 50% RH. Next, the optical laminate with the glass plate was treated in an autoclave at 50°C and 5 atmospheres (absolute pressure) for 15 minutes, and then left to cool to 24°C to stabilize the bonding of the optical laminate to the glass plate. Next, the optical laminate with the glass plate was left to stand in a heated atmosphere at 105°C for 500 hours. After standing, the atmosphere was returned to 24°C and 50% RH, and peeling of the polarizing plate from the glass plate and the occurrence of bubbles between the glass plate and the polarizing plate were visually confirmed, and durability was evaluated as follows: (Evaluation Criteria) A: No changes in appearance such as bubbles or peeling were observed. B: Slight individual peeling or bubbles were observed at the edge, but within a range that is not problematic in practical use. C: Slight continuous peeling or bubbling is observed at the edge, but within a range that is not problematic for practical use. D: Significant peeling or bubbling is observed at the edge, and is problematic for practical use.

[0209] <Evaluation of White Spots> The white spots of the optical laminate were evaluated by the following method before and after the weather resistance test. A glass plate simulating a front transparent member was attached to the optical film side of the prepared optical laminate via OCA (LUCIACS CS9821; acrylic acid monomer-free adhesive, thickness 200 μm, manufactured by Nitto Denko Corporation) to prepare an evaluation laminate simulating an image display device. Next, the evaluation laminate was attached to the viewing side of an in-cell liquid crystal cell via the adhesive sheet to prepare an in-cell liquid crystal cell with the laminate. Next, a polarizing plate was attached to the side opposite the viewing side of the in-cell liquid crystal cell with the laminate in a crossed Nicol relationship to prepare a liquid crystal display panel. This liquid crystal display panel was cooled on a cold plate set to −15° C. and then immediately placed on a backlight device. Static electricity was generated by rubbing the polarizing plate surface on the viewing side several times with nitrile gloves. The time until the white spots generated by static electricity disappeared was measured and evaluated according to the following criteria. The weather resistance test was carried out using an ultraviolet fade tester (U48HB, manufactured by Suga Test Instruments Co., Ltd.) according to the method described above. Note that a practically problematic evaluation result is "D". (Evaluation Criteria) A: No white spots occur. B: White spots occur after rubbing several times, but disappear within 1 second. C: White spots occur after rubbing several times, but disappear in more than 1 second but less than 5 seconds. D: White spots occur after rubbing only once, and it takes 5 seconds or more for them to disappear.

[0210]

[0211] As shown in Table 2, in the examples, the surface resistivity of the pressure-sensitive adhesive sheet side of the optical laminate at −15° C. was 1.0×10 10 The optical laminates according to the examples are more suitable for suppressing display defects, typically white spots due to charging, in low-temperature environments.

[0212] The optical laminate of the present invention can be particularly suitably used in image display devices used in environments such as the inside of a vehicle where other electronic devices are present nearby and static electricity is likely to occur, and where the temperature is likely to drop to low temperatures due to the influence of outside air temperature.

Claims

1. An optical laminate comprising an adhesive sheet, an antistatic layer, and an optical film, wherein the adhesive sheet is formed from an adhesive composition containing a polymer (A) and an antistatic agent, and the surface resistivity of the adhesive sheet side of the optical laminate at −15° C. is 1.0×10 10 An optical laminate having a resistivity of Ω / □ or less.

2. The surface resistivity of the antistatic layer at 25° C. is 3.0×10 8 The optical laminate according to claim 1, having a resistance to vibration of Ω / □ or less.

3. The surface resistivity of the antistatic layer at 25° C. is 1.0×10 7 Ω / □ or more 1.0×10 8 The optical laminate according to claim 2, having a resistance of less than Ω / □.

4. The optical laminate according to claim 1, wherein the polymer (A) is a (meth)acrylic polymer.

5. The optical laminate according to claim 1, wherein the polymer (A) has a polyether structure.

6. The optical laminate according to claim 1, wherein the polymer (A) has a structural unit derived from a monomer represented by the following formula (1). In the formula (1), R 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group which may be linear or branched, and n is an integer of 1 to 15.

7. The optical laminate according to claim 5, wherein the polymer (A) has a structural unit derived from an aromatic ring-containing monomer.

8. The optical laminate according to claim 1, wherein in the pressure-sensitive adhesive composition, the blending amount of the antistatic agent is less than 10 parts by weight per 100 parts by weight of the polymer (A).

9. The optical laminate according to claim 1, wherein the glass transition temperature of the polymer (A) calculated from the FOX formula is −40° C. or lower.

10. The optical laminate according to claim 9, wherein the glass transition temperature is −45° C. or lower.

11. An image display panel comprising the optical laminate according to any one of claims 1 to 10.

12. An image display device comprising the image display panel according to claim 11.

Citation Information

Patent Citations

  • Optical film with adhesive layer and liquid crystal panel

    JP2021096308A

  • Polarizer and image display device

    JP2022074622A

  • Polarizing plate and picture display unit using the same

    JP2022129959A

  • Metal connecting apparatus of lead tab of secondary battery

    KR102472380B1

Cited By

  • Polarizing film equipped with adhesive sheet, image display panel, and image display device

    WO2026230301A1

  • Optical laminate and image display device

    WO2026230318A1