Dispersion and use thereof
By controlling the electron spin resonance signal peak position and X-ray diffraction angle of cerium oxide particles, combined with pH adjustment, a nanoscale cerium oxide dispersion is prepared, which solves the problem of low grinding removal rate of cerium oxide abrasives and many surface scratch defects. problem, achieving a more efficient planarization process effect.
Patent Information
- Application Number
- PCT/CN2024/084409
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Due to the particle size limitation of existing cerium oxide abrasives in the planarization process, the grinding removal rate is low and the surface has many scratch defects, making it difficult to improve the grinding effect without increasing the particle size.
By controlling the electron spin resonance signal peak position of the cerium oxide particles to be 2.05 or less, the X-ray diffraction angle 2θ is less than or equal to 28.6°, and adjusting the pH value in the range of 2.0-4.0, a nanoscale cerium oxide dispersion is prepared. Improve its dispersion and grinding effect in the planarization process.
Without increasing the particle size of cerium oxide particles, the grinding removal rate is significantly increased and the occurrence of surface scratch defects is reduced, improving the efficiency and effect of the planarization process.
Smart Images

Figure CN2024084409_03102024_PF_FP_ABST
Abstract
Description
Dispersions and their applications
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 31, 2023, with application number 202310366812.7 and application name “Dispersion and Its Application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The embodiments of the present application relate to the field of planarization technology, and in particular to a dispersion liquid and its application. Background Art
[0003] Ceria has been widely reported as an abrasive for planarization processes in semiconductor manufacturing. This widespread interest stems primarily from its high abrasive removal activity against silicon dioxide, achieved at relatively low solids content. Therefore, planarization compositions using ceria as an abrasive offer greater application prospects and market advantages compared to traditional silicon oxide or aluminum oxide materials in terms of performance and cost.
[0004] In the grinding liquid with cerium oxide as the abrasive, the particle characteristics of cerium oxide have a crucial influence on the grinding effect. For example, in the application of dielectric layer planarization, the particle size and morphological characteristics of cerium oxide have an important influence on the generation of defects and the grinding removal rate selectivity during the planarization process. In the application of the planarization process, surface scratch defects are mainly caused by large particles in the grinding liquid. However, if abrasives with small particle size are used, it will lead to a loss of grinding removal rate. In advanced processes, surface scratches and grinding removal rate are very important indicators for measuring grinding effects. Therefore, how to increase the grinding removal rate without increasing the particle size is a difficult problem in the preparation and synthesis of cerium oxide abrasives.
[0005] Summary of the Invention
[0006] In view of this, an embodiment of the present application provides a dispersion and its application. The dispersion is a colloidal cerium oxide material. The dispersion can be used as an abrasive in the planarization process to increase the grinding removal rate without increasing the particle size of the cerium oxide particles, thereby solving the problem of low grinding removal rate caused by the existing cerium oxide abrasive in order to reduce surface scratches.
[0007] Specifically, the first aspect of the embodiment of the present application provides a dispersion, which includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the cerium oxide particles have an electron spin resonance signal peak, and the peak position of the electron spin resonance signal peak is less than or equal to 2.05. The embodiment of the present application controls the signal peak position of the electron spin resonance of the cerium oxide particles in the dispersion to a value of 2.05 or less, thereby improving the grinding removal rate without increasing the particle size of the cerium oxide particles. Among them, electron spin resonance (ESR) is a detection method for studying paramagnetic substances containing unpaired electrons, and the detection objects include free radicals, transition metal ions, multistate molecules and crystal defects. Electron spin resonance can identify information such as the valence state of single-electron substances in the catalyst, the properties of neighboring atoms, the symmetry of surface sites, and the total number of unpaired spin electrons in a unit catalyst. The electron spin resonance signal peak is the g factor, which can represent information about the unpaired electron environment and is an important indicator for characterizing crystal defects. The signal peak of the electron spin resonance can be obtained by electron spin resonance spectrometer testing.
[0008] In the embodiment of the present application, the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles is less than or equal to 28.6°. In the embodiment of the present application, by controlling the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the dispersion to a value of 28.6° or less, the grinding removal rate can be increased without increasing the particle size of the cerium oxide particles. This is mainly because controlling the diffraction angle 2θ to a smaller value can allow the cerium oxide particles to obtain more lattice defects, and the lattice defects include oxygen vacancy defects. The presence of oxygen vacancy defects in cerium oxide will cause the overall potential oxygen deficiency imbalance, and part of the tetravalent cerium will become trivalent cerium, and the presence of trivalent cerium will increase the grinding removal rate. The angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles can be obtained by X-ray diffractometer testing.
[0009] In an embodiment of the present application, the pH value of the dispersion is in the range of 2.0-4.0. Controlling the pH value of the dispersion within the range of 2.0-4.0 is advantageous for obtaining cerium oxide particles having an electron spin resonance signal peak position of less than or equal to 2.05, and for obtaining cerium oxide particles having an X-ray diffraction angle 2θ corresponding to the (111) crystal plane of less than or equal to 28.6°. It is also advantageous for reducing the hydrated particle size of the cerium oxide particles, thereby improving the dispersibility of the cerium oxide particles in the dispersion, facilitating the flattening operation, and facilitating storage.
[0010] In an embodiment of the present application, the pH value of the dispersion is in the range of 2.0-3.0. Controlling the pH value of the dispersion within the range of 2.0-3.0 is advantageous for obtaining cerium oxide particles having an electron spin resonance signal peak position of less than or equal to 2.05, and for obtaining cerium oxide particles having an X-ray diffraction angle 2θ corresponding to the (111) crystal plane of less than or equal to 28.6°. It is also advantageous for reducing the hydrated particle size of the cerium oxide particles, thereby improving the dispersibility of the cerium oxide particles in the dispersion, facilitating the leveling operation, and facilitating storage.
[0011] In the embodiment of the present application, the hydrated particle size of the cerium oxide particles is at the nanometer level, that is, cerium oxide nanoparticles. The hydrated particle size of the cerium oxide particles is the particle size of the composite particles in the solution state, which is the hydrodynamic diameter. The hydrated particle size of the cerium oxide particles includes the core of the cerium oxide particles and the expanded micelles. The cerium oxide particles have a hydrated particle size at the nanometer level, that is, they have a small size, which is beneficial to reduce the generation of scratch defects on the surface of the flattened object during the flattening process, thereby improving the grinding effect. The hydrated particle size of the cerium oxide particles can be measured by dynamic light scattering (DLS). Specifically, after obtaining the diffusion coefficient D of the cerium oxide particles, the hydrated diameter of the cerium oxide particles can be obtained according to the Stokes-Einstein equation:
[0012] Stokes-Einstein equations:
[0013] Where D is the diffusion coefficient, k B is the Boltzmann constant; T is the absolute temperature; η0 is the viscosity of the system; d is the fluid dynamics diameter, i.e. the hydration diameter.
[0014] In the embodiment of the present application, the hydrated particle size of the cerium oxide particles is less than or equal to 50 nm. The hydrated particle size of the cerium oxide particles is smaller than or equal to 50 nm, which can better reduce the generation of scratch defects on the surface of the planarized object during the planarization process, thereby improving the polishing effect.
[0015] In an embodiment of the present application, when the solid content of the dispersion is adjusted to 0.3 wt%, the average transmittance of the dispersion for light with a wavelength of 190 nm to 370 nm is less than 5%. When the solid content of the dispersion is adjusted to 0.3 wt%, the average transmittance of the dispersion for light with a wavelength of 190 nm to 370 nm is less than 5%, which can improve the grinding effect when used as an abrasive in a planarization process.
[0016] In an embodiment of the present application, when the solid content of the dispersion is adjusted to 0.3% by weight, the average transmittance of light with a wavelength of 190 nm to 370 nm is less than or equal to 2.5%. The lower average transmittance indicates that the solid particles in the dispersion are small and well dispersed, thereby improving the grinding effect when used as an abrasive in a planarization process.
[0017] In an embodiment of the present application, when the solid content of the dispersion is adjusted to 0.3 wt%, the average transmittance of the dispersion for light with a wavelength of 190 nm to 320 nm is less than 0.01%. When the solid content of the dispersion is adjusted to 0.3 wt%, the average transmittance of the dispersion for light with a wavelength of 190 nm to 320 nm is less than 0.01%, which can improve the grinding effect when used as an abrasive in a planarization process.
[0018] In an embodiment of the present application, when the solid content of the dispersion is adjusted to 0.3% by weight, the average transmittance of light with a wavelength of 190 nm to 320 nm is less than or equal to 0.005%. The lower average transmittance indicates that the solid particles in the dispersion are small and well dispersed, thereby improving the grinding effect when used as an abrasive in a planarization process.
[0019] In the embodiment of the present application, the solid content of the dispersion is 1 wt% to 5 wt%. Appropriate control of the solid content is not only beneficial for the storage of the dispersion, but also facilitates the subsequent addition to the grinding liquid system.
[0020] The dispersion provided in the embodiments of the present application can be used as an abrasive to prepare a grinding liquid. The abrasive is a small-sized, defect-rich, and highly active colloidal nano-cerium oxide abrasive. The grinding liquid prepared using the abrasive is used in the planarization process of the dielectric layer to obtain a higher grinding removal rate and lower surface scratches, thereby improving the grinding effect.
[0021] A second aspect of the present invention provides a method for preparing a dispersion, comprising:
[0022] A soluble cerium salt is added to an organic alcohol or a mixture of an organic alcohol and water to obtain a mixed solution, an organic base is added to the mixed solution to form a precipitate in the mixed solution to obtain a precipitate mixture, and a supernatant in the precipitate mixture is removed and a first solvent is added to obtain a dispersion. During the above preparation process, a pH regulator is used to adjust the pH of the system so that the pH of the dispersion is 2.0-4.0. The dispersion includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the electron spin resonance signal peak position of the cerium oxide particles is less than or equal to 2.05.
[0023] The method for preparing the dispersion liquid of the embodiment of the present application can achieve the preparation of colloidal cerium oxide in which the electron spin resonance signal peak position of the cerium oxide particles is less than or equal to 2.05 by selecting specific reaction raw materials and reaction solvents and specifically regulating the pH of the system. The prepared colloidal cerium oxide can be used as an abrasive in the planarization process to increase the grinding removal rate without increasing the particle size of the cerium oxide particles. The method for preparing the dispersion liquid of the embodiment of the present application is simple in process and easy to realize industrial production.
[0024] In the embodiment of the present application, the soluble cerium salt includes one or more of cerium nitrate, cerium sulfate, ammonium cerium nitrate, cerium chloride, cerium acetate, cerium oxalate, and cerium acetylacetonate. The soluble cerium salt can provide a cerium source for the reaction system.
[0025] In the embodiment of the present application, the organic alcohol includes a monohydric alcohol having 1 to 10 carbon atoms, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, n-pentanol, and isopentanol.
[0026] In an embodiment of the present application, the organic base includes one or more of ammonia, ethanolamine, diethanolamine, triethanolamine, imidazole, pyridine, pyrazole, diethylamine, and triethylamine.
[0027] In the embodiment of the present application, the pH adjuster includes nitric acid. Using nitric acid as a pH adjuster is beneficial for its adaptability to the application scenario of dielectric layer planarization.
[0028] A third aspect of the embodiments of the present application provides a planarization composition, which includes the dispersion described in the first aspect of the embodiments of the present application and a second solvent.
[0029] In the embodiment of the present application, the planarization composition further includes additives. The additives can be added according to actual needs.
[0030] In an embodiment of the present application, the pH of the planarization composition is 4.0-7.0.
[0031] The fourth aspect of the embodiments of the present application provides the use of the dispersion described in the first aspect of the embodiments of the present application, or the planarization composition described in the third aspect of the embodiments of the present application in planarization of a dielectric layer.
[0032] In the embodiment of the present application, the dielectric layer may be a dielectric material layer commonly used in the field of electronic manufacturing, for example, it may include a silicon dioxide layer, a silicon nitride layer, or a polysilicon layer.
[0033] The present embodiments also provide use of the dispersion described in the first aspect of the present embodiments, or the planarization composition described in the third aspect of the present embodiments, for glass planarization. Examples of the glass include colorless optical glass, colored optical glass, laser glass, quartz optical glass, radiation-resistant glass, ultraviolet and infrared (high transmittance and absorption) optical glass, fiber optic glass, acousto-optic glass, magneto-optical glass, photochromic glass, and photomask glass.
[0034] The embodiment of the present application further provides a planarization method, which comprises bringing the planarization composition described in the third aspect of the embodiment of the present application into contact with the surface of an object to be planarized and moving the object to be planarized relative to the surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] FIG1 is a schematic diagram of the operation of the planarization process. DETAILED DESCRIPTION
[0036] The embodiments of the present application will be described below with reference to the accompanying drawings.
[0037] Cerium oxide has high grinding and removal activity for silicon dioxide, and can achieve better grinding effects at lower solid content. Therefore, grinding fluids with cerium oxide as abrasive have greater application prospects and market advantages in terms of performance and cost compared to traditional silicon oxide or aluminum oxide materials. In grinding fluids with cerium oxide as abrasive, the particle size and morphological characteristics of cerium oxide have an important influence on the generation of defects and the grinding removal rate during the planarization process. In the application of the planarization process, surface scratch defects are mainly caused by large particles in the grinding fluid, but the use of abrasives with small particle size will lead to a loss of grinding removal rate. In advanced processes, surface scratches and grinding removal rates are very important indicators for measuring grinding effects. Therefore, how to increase the grinding removal rate without increasing the particle size is a difficult problem in the preparation and synthesis of cerium oxide abrasives. To solve the above problems, an embodiment of the present application provides a dispersion and its application. The dispersion is a colloidal cerium oxide material. The dispersion can be used as an abrasive in the planarization process to improve the grinding removal rate without increasing the particle size of the cerium oxide particles, thereby solving the problem of the existing cerium oxide abrasive that continuously reduces the particle size of the cerium oxide particles to reduce surface scratches, resulting in a low grinding removal rate.
[0038] The embodiment of the present application provides a dispersion, namely a cerium oxide dispersion, which includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the cerium oxide particles have an electron spin resonance signal peak, and the peak position of the electron spin resonance signal peak is less than or equal to 2.05. The embodiment of the present application controls the peak position of the electron spin resonance signal peak of the cerium oxide particles in the cerium oxide dispersion to a value of 2.05 or less, thereby improving the grinding removal rate without increasing the particle size of the cerium oxide particles. Among them, electron spin resonance (ESR) is a detection method for studying paramagnetic substances containing unpaired electrons, and the detection objects include free radicals, transition metal ions, multistate molecules and crystal defects. Electron spin resonance can identify information such as the valence state of single-electron substances in the catalyst, the properties of neighboring atoms, the symmetry of the surface site, and the total number of unpaired spin electrons in the unit catalyst. The electron spin resonance signal peak is the g factor, which can represent information about the unpaired electron environment and is an important indicator for characterizing crystal defects. The signal peak of the electron spin resonance can be obtained by electron spin resonance spectrometer testing. In the embodiments of the present application, in the cerium oxide dispersion, the peak position of the electron spin resonance signal peak of the cerium oxide particles can be, for example, 2.05, 2.02, 2.00, 1.99, 1.98, 1.97, 1.96, etc. In some embodiments of the present application, in the cerium oxide dispersion, the peak position of the electron spin resonance signal peak of the cerium oxide particles is within the range of 1.0-2.05.
[0039] The cerium oxide dispersion in the embodiment of the present application is a colloidal cerium oxide material. In the colloidal cerium oxide material, the dispersoid is cerium oxide particles, and the dispersant is a first solvent, which can specifically be water.
[0040] In the embodiment of the present application, the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles is less than or equal to 28.6°. In the embodiment of the present application, by controlling the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the cerium oxide dispersion to a value of 28.6° or less, the grinding removal rate can be increased without increasing the particle size of the cerium oxide particles. This is mainly because controlling the diffraction angle 2θ to a smaller value can allow the cerium oxide particles to obtain more lattice defects, and the lattice defects include oxygen vacancy defects, and the presence of oxygen vacancy defects in cerium oxide will cause the overall potential oxygen deficiency imbalance, and part of the tetravalent cerium will become trivalent cerium, and the presence of trivalent cerium can increase the grinding removal rate. The angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles can be obtained by X-ray diffractometer testing. In the embodiment of the present application, the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles can be, for example, 28.6°, 28.5°, 28.4°, 28.3°, 28.2°, etc.
[0041] In an embodiment of the present application, the pH value of the cerium oxide dispersion may be in the range of 2.0-4.0. Controlling the pH value of the cerium oxide dispersion within the range of 2.0-4.0 is advantageous for obtaining cerium oxide particles having an electron spin resonance signal peak position of less than or equal to 2.05, and for obtaining cerium oxide particles having an X-ray diffraction angle 2θ corresponding to the (111) crystal plane of less than or equal to 28.6°. It is also advantageous for reducing the hydrated particle size of the cerium oxide particles, thereby improving the dispersibility of the cerium oxide particles in the cerium oxide dispersion, facilitating the planarization operation, and facilitating storage.
[0042] In some embodiments of the present application, the pH value of the cerium oxide dispersion is in the range of 2.0-3.0. Controlling the pH value of the cerium oxide dispersion within the range of 2.0-3.0 is advantageous for obtaining cerium oxide particles having an electron spin resonance signal peak position of less than or equal to 2.05, and for obtaining cerium oxide particles having an X-ray diffraction angle 2θ corresponding to the (111) crystal plane of less than or equal to 28.6°. It is also advantageous for reducing the hydrated particle size of the cerium oxide particles, thereby improving the dispersibility of the cerium oxide particles in the cerium oxide dispersion and facilitating their preservation.
[0043] In some embodiments of the present application, the pH value of the cerium oxide dispersion can be, for example, 2.0, 2.2, 2.5, 2.8, 3.0, 3.5, or 4.0.
[0044] In the embodiment of the present application, the hydrated particle size of the cerium oxide particles is nanometer-level, that is, cerium oxide nanoparticles. The hydrated particle size of the cerium oxide particles is the particle size of the composite particles in the solution state, which is the hydrodynamic diameter. The hydrated particle size of the cerium oxide particles includes the core of the cerium oxide particles and the expanded micelles. The cerium oxide particles have a hydrated particle size at the nanometer level, that is, they have a small size, which is beneficial to reduce the generation of surface scratch defects during the smoothing process, thereby improving the grinding effect. The hydrated particle size of the cerium oxide particles can be measured by dynamic light scattering (DLS). Specifically, after obtaining the diffusion coefficient D of the cerium oxide particles, the hydrated particle size of the cerium oxide particles can be obtained according to the Stokes-Einstein equation:
[0045] Stokes-Einstein equations:
[0046] Where D is the diffusion coefficient, k B is the Boltzmann constant; T is the absolute temperature; η0 is the viscosity of the system; d is the hydrodynamic diameter, i.e. the hydrated particle size.
[0047] In some embodiments of the present application, the hydrated particle size of the cerium oxide particles is less than or equal to 50 nm. The cerium oxide particles have a smaller hydrated particle size of less than or equal to 50 nm, which can better reduce the generation of scratch defects on the surface of the flattened object (i.e., the object being ground) during the flattening process, thereby improving the grinding effect. In some embodiments of the present application, the hydrated particle size of the cerium oxide particles can be, for example, 50 nm, 47 nm, 45 nm, 40 nm, 36 nm, 35 nm, 30 nm, 27 nm, 25 nm, 20 nm, 16 nm, 15 nm, 10 nm, etc.
[0048] In an embodiment of the present application, when the solid content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm is less than 5%. In some embodiments, when the solid content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm is 4.5%, 4.0%, 3.5%, 3.0%, or 2.5%. The solid content refers to the percentage of the weight of the cerium oxide particles in a dry state relative to the total weight of the cerium oxide dispersion. When the solid content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm is less than 5%, which can improve the grinding effect when used as an abrasive in a planarization process.
[0049] In some embodiments of the present application, when the solid content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of light with a wavelength of 190 nm to 370 nm is less than or equal to 2.5%. In some embodiments, when the solid content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of light with a wavelength of 190 nm to 370 nm is 2.5%, 2.0%, 1.5%, 1.0%, 0.5%, 0.2%, or 0.1%. The lower average transmittance indicates that the cerium oxide solid particles in the cerium oxide dispersion are small in size and well-dispersed, which is more conducive to improving the grinding effect when used as an abrasive in a planarization process.
[0050] In an embodiment of the present application, when the solids content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 320 nm is less than 0.01%. In some embodiments, when the solids content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 320 nm is 0.0095%, 0.009%, 0.0085%, 0.008%, 0.007%, 0.006%, or 0.0055%. When the solids content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 320 nm is less than 0.01%, which can improve the grinding effect when used as an abrasive in a planarization process.
[0051] In embodiments of the present application, when the solids content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 320 nm is less than or equal to 0.005%. In some embodiments, when the solids content of the cerium oxide dispersion is adjusted to 0.3% by weight, the average transmittance of the cerium oxide dispersion for light with a wavelength of 190 nm to 320 nm is 0.005%, 0.004%, 0.003%, 0.002%, or 0.001%. The lower average transmittance indicates that the solid particles in the cerium oxide dispersion are small in size and well-dispersed, thereby enhancing the grinding effect when used as an abrasive in a planarization process.
[0052] In an embodiment of the present application, the solid content of the cerium oxide dispersion is 1% to 5% by weight. In some embodiments, the solid content of the cerium oxide dispersion is 1% by weight. In some embodiments, the solid content of the cerium oxide dispersion is 2% by weight. In some embodiments, the solid content of the cerium oxide dispersion is 3% by weight. In some embodiments, the solid content of the cerium oxide dispersion is 4% by weight. In some embodiments, the solid content of the cerium oxide dispersion is 5% by weight. Appropriate control of the solid content, i.e., appropriate control of the content of cerium oxide particles, is not only beneficial for the storage of the cerium oxide dispersion, but also facilitates its subsequent addition to the polishing liquid system.
[0053] The cerium oxide dispersion provided in the embodiments of the present application can be used as an abrasive to prepare a grinding liquid (i.e., a polishing liquid). The abrasive is a small-sized, defect-rich, and highly active colloidal nano-cerium oxide abrasive. The grinding liquid prepared using the abrasive is used in the planarization process of the dielectric layer (i.e., the chemical-mechanical-polishing process), which can obtain a higher grinding removal rate and lower surface scratches, thereby improving the grinding effect.
[0054] In the prior art, the preparation methods of cerium oxide abrasives mainly include calcination, hydrothermal method, spray pyrolysis method, and sand milling method; wherein, the calcination method has a simple preparation process, low cost, and is suitable for expanding production, but the product particles are uneven and the particles are large; the hydrothermal method has controllable product morphology and particle size, and good crystallinity, but the existing preparation process is complicated and carried out under high temperature and high pressure, which is not conducive to expanding production, and the by-products have environmental hazards; the spray pyrolysis method has uniform and controllable product particles, which is suitable for expanding production, and the product purity is high, but the preparation process has high energy consumption and high cost, the product morphology is complex, and the particles are large; the sand milling method has a simple preparation process and is suitable for expanding production, but it uses large-particle solids as raw materials for physical cutting, the morphology is uncontrollable, and the product particle size is large. To this end, the present application embodiment provides a preparation method for a cerium oxide dispersion, which can achieve cerium oxide preparation with smaller particle size and better grinding effect, and the process is simpler and suitable for expanding production.
[0055] Specifically, the present invention provides a method for preparing a cerium oxide dispersion, comprising:
[0056] A soluble cerium salt is added to an organic alcohol or a mixture of an organic alcohol and water to obtain a mixed solution, an organic base is added to the mixed solution to form a precipitate in the mixed solution to obtain a precipitate mixture, and a supernatant in the precipitate mixture is removed and then a first solvent is added to obtain a cerium oxide dispersion. In the above preparation process, a pH regulator is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0. The cerium oxide dispersion includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the electron spin resonance signal peak position of the cerium oxide particles is less than or equal to 2.05.
[0057] The method for preparing the cerium oxide dispersion in the embodiment of the present application can achieve the preparation of colloidal cerium oxide with a smaller particle size and an electron spin resonance signal peak position of cerium oxide particles less than or equal to 2.05 by selecting specific reaction raw materials and specifically regulating the pH of the system. The prepared colloidal cerium oxide can be used as an abrasive in the planarization process to increase the grinding removal rate without increasing the particle size of the cerium oxide particles. The method for preparing the cerium oxide dispersion in the embodiment of the present application has a simple process and is easy to implement in industrial production.
[0058] In the embodiments of the present application, the above preparation process is carried out at a temperature of 25° C. to 60° C. In some embodiments, the temperature is 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., or 60° C. Controlling the temperature during the preparation process within a suitable range is beneficial for preparing cerium oxide particles with improved grinding performance.
[0059] In an embodiment of the present application, the organic base is added dropwise at a rate of 10 mL / min-40 mL / min. In some embodiments, the organic base is added dropwise at a rate of 10 mL / min, 15 mL / min, 20 mL / min, 25 mL / min, 30 mL / min, 35 mL / min, or 40 mL / min. The organic base is added dropwise at a suitable rate so that the nucleation rate of cerium oxide is greater than the growth rate, thereby facilitating better control of the formation of cerium oxide particles with a smaller particle size.
[0060] In the embodiment of the present application, the soluble cerium salt can be one or more of cerium nitrate, cerium sulfate, ammonium cerium nitrate, cerium chloride, cerium acetate, cerium oxalate, and cerium acetylacetonate. The soluble cerium salt can provide a cerium source for the reaction system.
[0061] In the embodiment of the present application, the organic alcohol includes a monohydric alcohol having a carbon number of 1 to 10. Specific examples of the organic alcohol include methanol, ethanol, n-propanol, isopropanol, n-butanol, n-pentanol, isopentanol, and the like.
[0062] In the embodiment of the present application, the above-mentioned organic base can be one or more of ammonia, ethanolamine, diethanolamine, triethanolamine, imidazole, pyridine, pyrazole, diethylamine, and triethylamine.
[0063] In the embodiment of the present application, the pH adjuster includes nitric acid. Using nitric acid as a pH adjuster is beneficial for its adaptability to the application scenario of dielectric layer planarization.
[0064] The present invention also provides a planarization composition comprising the cerium oxide dispersion described above and a second solvent. The second solvent may be water. The planarization composition can achieve a planarization treatment of the dielectric layer through both chemical and mechanical action. The planarization composition is a grinding liquid (i.e., a polishing liquid).
[0065] In embodiments of the present application, the planarization composition may further include additives. The additives may primarily include betaine, glycine, proline, polyethyleneimine, histidine, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, lauryl betaine, betaine citrate, hexadecyl sulfobetaine, tetradecyl sulfobetaine, sulfobetaine 8, and sulfobetaine 10. The additives may be added in appropriate amounts as needed.
[0066] In embodiments of the present application, the pH of the planarization composition is 4.0-7.0. In some embodiments of the present application, the pH of the planarization composition can be, for example, 4.0, 5.0, 6.0, or 7.0. Controlling the pH of the planarization composition within the range of 4.0-7.0 can promote adsorption of cerium oxide to the dielectric layer, thereby improving the polishing effect.
[0067] The present application also provides an application of the cerium oxide dispersion described above in the present application or the planarization composition described above in the present application in planarizing a dielectric layer.
[0068] In the embodiment of the present application, the dielectric layer may be a dielectric material layer commonly used in the field of electronic manufacturing, for example, it may include a silicon dioxide layer, a silicon nitride layer, a polysilicon layer, etc.
[0069] The present invention also provides the use of the cerium oxide dispersion or the planarization composition described in the embodiments of the present invention for glass planarization. Examples of the glass include colorless optical glass, colored optical glass, laser glass, quartz optical glass, radiation-resistant glass, ultraviolet and infrared (high transmittance and absorption) optical glass, fiber optic glass, acousto-optic glass, magneto-optical glass, photochromic glass, and photomask glass.
[0070] The embodiment of the present application also provides a planarization method, using the above-mentioned planarization composition of the embodiment of the present application as a polishing liquid, so that the above-mentioned planarization composition of the embodiment of the present application is in contact with the surface of the object to be planarized and the object to be planarized is moved relatively. Taking the object to be planarized as a semiconductor structure having a silicon dioxide dielectric layer (hereinafter referred to as a substrate) as an example, the planarization method specifically includes: bringing the planarization composition of the embodiment of the present application into contact with the silicon dioxide dielectric layer on the surface of the substrate, and moving the silicon dioxide dielectric layer on the surface of the substrate relative to the substrate to polish the substrate. This planarization method can not only effectively reduce the occurrence of surface scratch defects by using the planarization composition of the embodiment of the present application for planarization treatment, but also obtain a higher polishing removal rate, thereby improving the polishing effect.
[0071] As shown in Figure 1, during the process of the flattening method of the embodiment of the present application, the grinding pad 102 is flat on the grinding table 101, and the object to be flattened 103 is hung upside down on the grinding head 104 (the surface to be ground of the object to be flattened 103 is in contact with the grinding head 104), and then pressed on the grinding pad 102 rotating on the grinding table 101 with a certain pressure. When the flattening process is carried out, the grinding head 104 starts to rotate with the object to be flattened 103, and the grinding table 101 also rotates at a certain speed. At the same time, the grinding liquid 105, i.e., the flattening composition, is added to the grinding pad 102 at a certain rate and spreads out with the centrifugal force. The object to be flattened 103 is removed from the silicon dioxide dielectric layer under the dual action of chemistry and mechanics. After the flattening process is completed, the abrasive and organic matter remaining on the surface of the substrate are removed by a post-cleaning process.
[0072] The embodiments of the present application are further described below with reference to a number of embodiments.
[0073] Example 1
[0074] At 25°C, about 1 kg of cerium nitrate is added to a sufficient amount of anhydrous ethanol and stirred to obtain a mixed solution; an ammonia solution is added dropwise to the mixed solution at a rate of 40 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0075] The hydrated particle size d of the cerium oxide particles in the cerium oxide dispersion obtained in Example 1 was measured using a dynamic light scattering (DLS) method; the signal peak position of the electron spin resonance (ESR) of the cerium oxide particles in the cerium oxide dispersion obtained in Example 1 was measured using an electron spin resonance (ESR) spectrometer; and the angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the cerium oxide dispersion obtained in Example 1 was measured using an X-ray diffractometer. The solid content of the cerium oxide dispersion obtained in Example 1 was adjusted to 0.3%, and the average transmittance of the cerium oxide dispersion at a solid content of 0.3% by weight for light with a wavelength of 190 nm to 370 nm and the average transmittance for light with a wavelength of 190 nm to 320 nm were measured using a spectrophotometer. The above test results are shown in Table 1.
[0076] Table 1
[0077] Example 2
[0078] About 1 kg of cerium nitrate is added to a sufficient amount of isopropanol at 25° C. and stirred to obtain a mixed solution; a triethanolamine solution is added dropwise to the mixed solution at a rate of 30 mL / min until a precipitate is formed in the mixed solution to obtain a precipitate mixture; after removing the supernatant of the precipitation mixture except the precipitate, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion includes water and cerium oxide particles dispersed in the water.
[0079] The hydrated particle size d, the electron spin resonance (ESR) signal peak position, and the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the resulting cerium oxide dispersion were measured using the same methods as in Example 1. The average transmittance of the resulting cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm and the average transmittance for light with a wavelength of 190 nm to 320 nm at a solids content of 0.3 wt% were also measured. The test results are shown in Table 2.
[0080] Table 2
[0081] Example 3
[0082] At 40°C, about 1 kg of cerium nitrate is added to a sufficient amount of n-butanol and stirred to obtain a mixed solution; an ethanolamine solution is added dropwise to the mixed solution at a rate of 20 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0083] The hydrated particle size d, the electron spin resonance (ESR) signal peak position, and the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the resulting cerium oxide dispersion were measured using the same methods as in Example 1. The average transmittance of the resulting cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm and the average transmittance for light with a wavelength of 190 nm to 320 nm at a solids content of 0.3 wt% were also measured. The test results are shown in Table 3.
[0084] Table 3
[0085] Example 4
[0086] At 60° C., about 1 kg of cerium nitrate is added to a sufficient amount of an ethanol-water mixture and stirred to obtain a mixed solution; an ammonia solution is added dropwise to the mixed solution at a rate of 10 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0087] The hydrated particle size d, the electron spin resonance (ESR) signal peak position, and the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the resulting cerium oxide dispersion were measured using the same methods as in Example 1. The average transmittance of the resulting cerium oxide dispersion for light with a wavelength of 190 nm to 370 nm and the average transmittance for light with a wavelength of 190 nm to 320 nm at a solids content of 0.3 wt% were also measured. The test results are shown in Table 4.
[0088] Table 4
[0089] Example 5
[0090] At 25°C, about 1 kg of cerium nitrate is added to a sufficient amount of n-pentanol and stirred to obtain a mixed solution; an ammonia aqueous solution is added dropwise to the mixed solution at a rate of 20 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion includes water and cerium oxide particles dispersed in the water.
[0091] Example 6
[0092] At 25° C., about 1 kg of cerium nitrate is added to a sufficient amount of isoamyl alcohol and stirred to obtain a mixed solution; a triethanolamine solution is added dropwise to the mixed solution at a rate of 25 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0093] Example 7
[0094] At 25°C, about 1 kg of cerium nitrate is added to a sufficient amount of n-propanol and stirred to obtain a mixed solution; an ammonia aqueous solution is added dropwise to the mixed solution at a rate of 20 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0095] Example 8
[0096] At 25°C, about 1 kg of cerium nitrate is added to sufficient amounts of n-butanol and water, and stirred to obtain a mixed solution; an imidazole solution is added dropwise to the mixed solution at a rate of 25 mL / min until a precipitate is formed in the mixed solution, thereby obtaining a precipitate mixture; after removing the supernatant other than the precipitate from the precipitate mixture, a certain amount of ultrapure water is added to form a cerium oxide colloid, thereby obtaining a cerium oxide dispersion; in the above preparation process, a pH adjuster is used to adjust the pH of the system so that the pH of the cerium oxide dispersion is 2.0-4.0; the obtained cerium oxide dispersion comprises water and cerium oxide particles dispersed in the water.
[0097] The hydrated particle size d of the cerium oxide particles in the cerium oxide dispersions obtained in Examples 5 to 8 was measured using a dynamic light scattering (DLS) method. The electron spin resonance (ESR) signal peak position of the cerium oxide particles in the cerium oxide dispersions obtained in Examples 5 to 8 was measured using an electron spin resonance (ESR) spectrometer. The angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles in the cerium oxide dispersions obtained in Examples 5 to 8 was measured using an X-ray diffractometer. The solid content of the cerium oxide dispersions obtained in Examples 5 to 8 was adjusted to 0.3% respectively. The average transmittance of the cerium oxide dispersions for light with a wavelength of 190 nm to 370 nm and the average transmittance for light with a wavelength of 190 nm to 320 nm at a solid content of 0.3 wt% were measured using a spectrophotometer. The above test results are shown in Table 5.
[0098] Table 5
[0099] The cerium oxide dispersions of Examples 1 to 8 of the present application were prepared into a flattening composition with a solid content of 0.3% using solvent water, and the pH was adjusted to 5.0. At the same time, two commercially available cerium oxide particle dispersions were used as Comparative Examples 1 and 2, and were prepared into a flattening composition with a solid content of 0.3% using solvent water according to the same method as in Examples 1 to 8, and the pH was adjusted to 5.0. In Comparative Example 1, the hydrated particle size of the cerium oxide particles was 50 nm, there was no electron spin resonance signal peak, and the angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane was 28.5. In Comparative Example 2, the hydrated particle size of the cerium oxide particles was 10 nm, there was no electron spin resonance signal peak, and the angle value of the X-ray diffraction angle 2θ corresponding to the (111) crystal plane was 28.6.
[0100] The planarization compositions obtained in Examples 1 to 8, and Comparative Examples 1 and 2 were used for planarization of a silicon dioxide dielectric layer, and the silicon dioxide removal rate results are shown in Table 6.
[0101] Table 6
[0102] The results in Table 6 indicate that the planarization compositions prepared using the cerium oxide dispersions of Examples 1 to 8 of the present application exhibit significantly improved silicon dioxide removal rates compared to the planarization compositions prepared using commercially available cerium oxide particle dispersions in Comparative Examples 1 and 2. The cerium oxide dispersions of the present examples are capable of increasing the silicon dioxide removal rate when the cerium oxide particles have a relatively small particle size, thereby reducing the occurrence of surface scratches while increasing the planarization rate, ultimately enhancing the dielectric planarization effect.
[0103] It should be understood that the first, second and various numerical numbers involved in this document are only distinguished for the convenience of description and are not intended to limit the scope of this application.
[0104] In this application, "and / or" describes the relationship between related objects, indicating that three possible relationships exist. For example, "A and / or B" can mean: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the related objects are in an "or" relationship.
[0105] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0106] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
Claims
1. A dispersion, It is characterized in that The dispersion includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the cerium oxide particles have an electron spin resonance signal peak, and the peak position of the electron spin resonance signal peak is less than or equal to 2.
05.
2. The dispersion according to claim 1, It is characterized in that The X-ray diffraction angle 2θ corresponding to the (111) crystal plane of the cerium oxide particles is less than or equal to 28.6°.
3. The dispersion according to claim 1 or 2, It is characterized in that The pH value of the dispersion is in the range of 2.0-4.
0.
4. The dispersion according to claim 3, It is characterized in that The pH value of the dispersion is in the range of 2.0-3.
0.
5. The dispersion according to any one of claims 1 to 4, It is characterized in that The hydrated particle size of the cerium oxide particles is at nanometer level.
6. The dispersion according to claim 5, It is characterized in that The hydrated particle size of the cerium oxide particles is less than or equal to 50 nm.
7. The dispersion according to any one of claims 1 to 6, It is characterized in that When the solid content of the dispersion is adjusted to 0.3 wt %, the average transmittance of the dispersion to light with a wavelength of 190 nm to 370 nm is less than 5%.
8. The dispersion according to claim 7, It is characterized in that When the solid content of the dispersion is adjusted to 0.3 wt %, the average transmittance of the dispersion to light with a wavelength of 190 nm to 370 nm is less than or equal to 2.5%.
9. The dispersion according to any one of claims 1 to 8, It is characterized in that When the solid content of the dispersion is adjusted to 0.3 wt %, the average light transmittance of the dispersion to light with a wavelength of 190 nm to 320 nm is less than 0.01%.
10. The dispersion according to claim 9, It is characterized in that When the solid content of the dispersion is adjusted to 0.3 wt %, the average transmittance of the dispersion to light with a wavelength of 190 nm to 320 nm is less than or equal to 0.005%.
11. The dispersion according to any one of claims 1 to 10, It is characterized in that The solid content of the dispersion is 1 wt % to 5 wt %.
12. A method for preparing a dispersion, It is characterized in that include: A soluble cerium salt is added to an organic alcohol or a mixture of an organic alcohol and water to obtain a mixed solution, an organic base is added to the mixed solution to form a precipitate in the mixed solution to obtain a precipitate mixture, and a first solvent is added after removing the supernatant in the precipitate mixture to obtain a dispersion; in the above preparation process, a pH regulator is used to adjust the pH of the system so that the pH of the dispersion is 2.0-4.0; the dispersion includes a first solvent and cerium oxide particles dispersed in the first solvent, wherein the signal peak position of the electron spin resonance of the cerium oxide particles is less than or equal to 2.
05.
13. The preparation method according to claim 12, It is characterized in that The soluble cerium salt includes one or more of cerium nitrate, cerium sulfate, cerium ammonium nitrate, cerium chloride, cerium acetate, cerium oxalate, and cerium acetylacetonate.
14. The preparation method according to claim 12 or 13, It is characterized in that The organic alcohol includes a monohydric alcohol having 1 to 10 carbon atoms.
15. The preparation method according to any one of claims 12 to 14, It is characterized in that The organic base includes one or more of ammonia water, ethanolamine, diethanolamine, triethanolamine, imidazole, pyridine, pyrazole, diethylamine, and triethylamine.
16. The preparation method according to any one of claims 12 to 15, It is characterized in that The pH adjuster includes nitric acid.
17. A planarization composition, It is characterized in that The planarization composition comprises the dispersion according to any one of claims 1 to 11 and a second solvent.
18. The planarization composition according to claim 17, It is characterized in that The planarization composition further includes an additive.
19. The planarization composition according to claim 17 or 18, It is characterized in that The pH of the planarizing composition is 4.0-7.
0.
20. Use of the dispersion according to any one of claims 1 to 11, or the planarization composition according to any one of claims 17 to 19 in planarization of a dielectric layer.
21. The use according to claim 20, It is characterized in that The dielectric layer includes a silicon dioxide layer, a silicon nitride layer, and a polysilicon layer.
22. Use of the dispersion according to any one of claims 1 to 11, or the planarization composition according to any one of claims 17 to 19 in glass planarization.
23. A planarization method, It is characterized in that The planarizing composition according to any one of claims 17 to 19 is brought into contact with a surface of an object to be planarized and the object to be planarized is relatively moved.
Citation Information
Patent Citations
Liquid suspension and powder of cerium oxide particles, methods for making the same and uses thereof in polishing
CN102627310A
Method for efficiently manufacturing oxygen vacancies on surface of metal oxide catalyst
CN113492004A
Preparation of vacancy cerium oxide loaded bimetallic nanoparticles and application of vacancy cerium oxide loaded bimetallic nanoparticles in electrocatalytic reduction of nitrate
CN115287693A
Polishing composition suitable for silicon wafer regeneration, preparation method and application thereof
CN115386300A
Cerium dioxide particle and preparation method and application thereof
CN115403063A