Solid electrolyte and lithium-ion battery
The solid electrolyte composition with specific cation and anion combinations improves stability and reduction resistance, addressing the challenges of ionic conductivity and moisture resistance in lithium ion batteries, leading to enhanced safety and energy density in all-solid-state batteries.
Patent Information
- Application Number
- PCT/JP2023/012624
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Solid electrolytes used in lithium ion batteries face challenges with stability and reduction resistance, particularly in maintaining ionic conductivity and moisture resistance at room temperature, which affects the reliability and safety of all-solid-state batteries.
A solid electrolyte composition containing Li, Mα, Mβ, Mγ, Cl, and F, where Mα is Zr or Hf, Mβ is Ta, and Mγ is Gd, Yb, Dy, Er, or Sc, with specific molar ratios and electronegativity differences, enhancing ionic conductivity and stability while improving reduction resistance through the inclusion of fluorine.
The proposed electrolyte achieves high ionic conductivity and stability, suppressing reductive decomposition, thereby enhancing the safety and energy density of all-solid-state lithium ion batteries by improving reduction resistance and maintaining performance at room temperature.
Smart Images

Figure JP2023012624_03102024_PF_FP_ABST
Abstract
Description
Solid Electrolyte and Lithium-Ion Batteries
[0001] The present invention relates to a solid electrolyte and a lithium-ion battery.
[0002] In recent years, there has been a strong demand for smaller size and improved reliability (safety) of batteries that serve as power sources for electronic devices. Therefore, all-solid-state batteries using solid electrolytes have attracted attention. Halides are known as sulfur-free solid electrolytes, and Li 3 YCl 6 exhibits high Li ion conductivity at room temperature (see, for example, Japanese Patent No. 6934626 (Reference 1)). In addition, in International Publication No. 2020 / 070956 (Reference 2), Li 6-4b+ab (Zr 1-a M a ) b X 6 Here, M is at least one element selected from the group consisting of Al, Ga, Bi, Sc, Sm, and Sb, X is a halogen element, and 0<a<1 and 0<b<1.5 are satisfied.
[0003] As mentioned above, Li 3 YCl 6 Chloride electrolytes such as Li2O4 and Li2O5 exhibit high ionic conductivity at room temperature, but no information is disclosed regarding their stability. The present inventors prepared the solid electrolytes disclosed in the above-mentioned documents 1 and 2 and left them in a dry room with a controlled dew point of -40°C. However, they found that the electrolyte decomposed and could not maintain its initial ionic conductivity, i.e., its stability (or moisture resistance) was low. Therefore, in order to improve the stability of chloride electrolytes, the present inventors have investigated the use of Li2O4 and Li2O5 as the solid electrolytes. x MCl 6 In this study, materials were prepared by combining various cations (M) to search for combinations of cations with high stability. As a result, as described below in the related art, a combination of cations exhibiting high ionic conductivity and high stability was identified. Meanwhile, in all-solid-state batteries, it is also necessary to improve the reduction resistance of the solid electrolyte in order to increase the energy density.
[0004] The present invention is directed to a solid electrolyte, and has an object to provide a solid electrolyte having excellent reduction resistance.
[0005] A first aspect of the invention is a solid electrolyte comprising Li, Mα, Mβ, Mγ, Cl, and F, wherein Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, and Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc.
[0006] According to the present invention, a solid electrolyte having excellent reduction resistance can be provided.
[0007] A second aspect of the present invention is the solid electrolyte of the first aspect, in which Mα includes Zr.
[0008] A third aspect of the present invention is the solid electrolyte of the first or second aspect, in which Mβ contains Ta.
[0009] A fourth aspect of the present invention is the solid electrolyte according to any one of the first to third aspects, in which Mγ includes Gd, Yb, or Er.
[0010] A fifth aspect of the present invention is the solid electrolyte of any one of the first to fourth aspects, which is represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6-d F d ...(1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<6 are satisfied.
[0011] A sixth aspect of the invention is the solid electrolyte of any one of the first to fifth aspects, wherein the value obtained by dividing the average ionic radius of Li, Mα, Mβ, and Mγ by the average ionic radius of Cl and F is greater than 0.31 and less than 0.43, and Δχ, which is the difference between the average electronegativity of Cl and F and the average electronegativity of Mα, Mβ, and Mγ, is greater than 1.842.
[0012] A seventh aspect of the invention is a lithium ion battery including the solid electrolyte of any one of the first to sixth aspects.
[0013] The above and other objects, features, aspects and advantages will become more apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings.
[0014] FIG. 1 is a longitudinal sectional view showing an all-solid-state lithium ion secondary battery.
[0015] First, a solid electrolyte according to a related art of the present invention will be described. The solid electrolyte according to the related art is a lithium (Li) ion conductive material that contains lithium (Li), three other metal elements (Mα, Mβ, Mγ) that become cations, and chlorine (Cl).
[0016] Mα is an element that becomes a tetravalent cation and is at least one element selected from the group consisting of zirconium (Zr) and hafnium (Hf). Mβ is an element that becomes a pentavalent cation and is at least one element selected from the group consisting of tantalum (Ta) and niobium (Nb). Mγ is an element that becomes a trivalent cation and is at least one element selected from the group consisting of gadolinium (Gd), ytterbium (Yb), dysprosium (Dy), erbium (Er), holmium (Ho), europium (Eu), and scandium (Sc). The solid electrolyte containing at least one trivalent, tetravalent, and pentavalent element in addition to Li as a cation achieves high ionic conductivity and high stability.
[0017] A preferred example of the solid electrolyte according to the related art is a compound represented by the following composition formula: Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 The conditions 0<a, 0<b, a+b<1, and −0.2≦c≦0.2 are satisfied.
[0018] Next, a solid electrolyte according to one embodiment of the present invention will be described. The solid electrolyte is a Li-ion conductive material, and is obtained by adding fluorine (F) to the solid electrolyte according to the related art. The solid electrolyte is used, for example, in the manufacture of an all-solid-state secondary battery. The solid electrolyte contains Li, three other metal elements (Mα, Mβ, Mγ) that become cations, Cl, and F. The solid electrolyte may be composed only of Li, Mα, Mβ, Mγ, Cl, and F.
[0019] As with the solid electrolytes according to the related art, Mα is an element that forms a tetravalent cation and is at least one element selected from the group consisting of Zr and Hf. Mβ is an element that forms a pentavalent cation and is at least one element selected from the group consisting of Ta and Nb. Mγ is an element that forms a trivalent cation and is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc. Since the solid electrolyte according to the present embodiment contains at least one trivalent, one tetravalent, and one pentavalent element in addition to Li as cations, high ionic conductivity and high stability are also achieved. Since the solid electrolyte further contains F, it has high reduction resistance, as described below. Since the solid electrolyte does not generate hydrogen sulfide gas, a highly safe all-solid-state secondary battery can be provided.
[0020] In the solid electrolyte according to the present embodiment, in order to more reliably achieve high reduction resistance, Mα preferably contains Zr, and Mα may consist of only Zr. Furthermore, Mβ preferably contains Ta, and Mβ may consist of only Ta. Furthermore, Mγ preferably contains Gd, Yb, or Er, and Mγ may consist of only Gd, Yb, or Er. Mγ may contain two or more elements of Gd, Yb, and Er. The amount of substance of Li is, for example, larger than the amount of substance of any of Mα, Mβ, and Mγ, and preferably larger than the sum of the amounts of substance of Mα, Mβ, and Mγ. The amount of substance of Cl is, for example, larger than the sum of the amounts of substance of Li, Mα, Mβ, and Mγ. The amount of substance of F is, for example, smaller than 1 / 2 of the amount of substance of Cl, and preferably smaller than 1 / 4 of the amount of substance of Cl.
[0021] A preferred solid electrolyte is a compound represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6-d F d ... (1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<6 are satisfied. Regarding a and b, 0.1≦a≦0.5 and 0.1≦b≦0.4 may be satisfied. Furthermore, 0.2≦a+b≦0.8 may be satisfied. Regarding the relationship between a and b, a≧b is, for example, a<b, but a<b may also be satisfied. Regarding c, -0.1≦c≦0.1 may be satisfied, or c may be 0. Regarding d, 0<d<3 may be satisfied. Preferably, 0<d≦2 is satisfied, and more preferably, 0<d≦1 is satisfied. The lower limit of d may be 0.1. The solid electrolyte may be crystalline or amorphous.
[0022] When determining whether an unknown solid electrolyte is the solid electrolyte according to the present embodiment, chemical analysis is performed on the unknown solid electrolyte to determine whether the constituent elements are Li, Mα, Mβ, Mγ, Cl, and F. When determining whether the unknown solid electrolyte is of the composition formula (1), Li, Mα, Mβ, and Mγ can be quantified by, for example, ICP-emission spectroscopy. Cl and F can be quantified by, for example, ion chromatography.
[0023] The molar ratio of Li, Mα, Mβ, Mγ, Cl, and F in the composition formula (1) is Li:Mα:Mβ:Mγ:Cl:F=6-(4+a-b)(1+c):(1-a-b)(1+c):a(1+c):b(1+c):6-d:d. In the molar ratio determined by analysis of an unknown solid electrolyte, if the value of Li is 0.90 × {6-(4+a-b)(1+c)} or more and 1.10 × {6-(4+a-b)(1+c)} or less, it is considered that the composition formula (1) is satisfied for Li. It is more preferable that the value of Li is 0.95 × {6-(4+a-b)(1+c)} or more and 1.05 × {6-(4+a-b)(1+c)} or less. The same applies to Mα, Mβ, Mγ, Cl, and F.
[0024] In a preferred solid electrolyte, the value obtained by dividing the average ionic radius of Li, Mα, Mβ, and Mγ by the average ionic radius of Cl and F (hereinafter referred to as the "average ionic radius ratio") is greater than 0.31 and less than 0.43, and the difference Δχ between the average electronegativity of Cl and F and the average electronegativity of Mα, Mβ, and Mγ is greater than 1.842. The average ionic radius ratio is more preferably less than 0.426, and even more preferably less than 0.424. Δχ is more preferably greater than 1.846, and even more preferably greater than 1.850. With such a solid electrolyte, as described below, stability can be more reliably improved. The upper limit of Δχ is not particularly limited, but is, for example, 2.735. The average ionic radius ratio is calculated based on Equation 1 and Equation 2, and the difference Δχ in average electronegativity is calculated using Equation 3.
[0025] (Equation 1) rc = Σ(rC·RC) / ΣRC (Equation 2) ra = Σ(rA·RA) / ΣRA In Equation 1, rC represents the ionic radius of the elements (i.e., cations) contained in Li, Mα, Mβ, and Mγ. RC represents the amount of substance of each element. In Equation 2, rA represents the ionic radius of Cl and F (i.e., anions), and RA represents the amount of substance of each element. The average ionic radius ratio (rc / ra) is obtained by dividing the average ionic radius (rc) of Li, Mα, Mβ, and Mγ by the average ionic radius (ra) of Cl and F. In solid electrolytes with an average ionic radius ratio greater than 0.31 and less than 0.43, the bond distance between cations and anions is thought to be appropriately short, resulting in a strong bond between the cations and anions. It is presumed that this high bond strength improves the stability of the material.
[0026] (Equation 3) Δχ = Σ(XA·RA) / ΣRA - Σ(XC·RC) / ΣRC In Equation 3, XA represents the electronegativity of Cl and F (i.e., anions), and XC represents the electronegativity of Mα, Mβ, and Mγ (i.e., cations excluding Li). In an electrolyte with Δχ exceeding 1.842, the ionic bond between cations excluding Li and anions is thought to be stronger, resulting in a stronger bond. This stronger bond is presumed to improve the stability of the material.
[0027] The solid electrolyte according to this embodiment is manufactured, for example, by the following method. First, a powder of a compound containing Li, a powder of a compound containing Mα, a powder of a compound containing Mβ, and a powder of a compound containing Mγ are prepared. Of these compounds, some compounds are chlorides, and the remaining compounds are fluorides. Fluorides and chlorides containing the same metal element may also be prepared. The chloride containing Li is, for example, LiCl, and the fluoride containing Li is, for example, LiF. The chloride containing Mα is, for example, MαCl. 4 and the fluoride containing Mα is, for example, MαF 4 The chloride containing Mβ is, for example, MβCl 5 and the fluoride containing Mβ is, for example, MβF 5 The chloride containing Mγ is, for example, MγCl3 and the fluoride containing Mγ is, for example, MγF 3 These powders are weighed and mixed to obtain a predetermined molar ratio.
[0028] Next, the mixture is milled (mechanochemical milling). Here, a planetary ball mill is used as an example of the milling process. In a planetary ball mill, the pot rotates on its axis while the stage carrying the pot revolves, making it possible to generate very high impact energy. The milling process may also be performed using other types of grinders. The solid electrolyte according to this embodiment is obtained by the milling process. This solid electrolyte is used to manufacture the positive electrode layer 112, the negative electrode layer 122, or the electrolyte layer 13 in the all-solid-state secondary battery 1 (see FIG. 1 ), which will be described later. In this example, the milling process is performed at room temperature, but the temperature and other conditions may be changed as appropriate. The solid electrolyte according to this embodiment may also be manufactured by a process other than milling, such as firing.
[0029] FIG. 1 is a longitudinal cross-sectional view showing an all-solid-state lithium-ion secondary battery 1 (hereinafter simply referred to as "all-solid-state secondary battery 1"). The all-solid-state secondary battery 1 uses a solid electrolyte according to the present embodiment. The all-solid-state secondary battery 1 includes, from top to bottom in FIG. 1 , a positive electrode 11, an electrolyte layer 13, and a negative electrode 12. That is, the electrolyte layer 13 is provided between the positive electrode 11 and the negative electrode 12. The electrolyte layer 13 is a solid electrolyte layer and also serves as a separator layer. The electrolyte layer 13 is made of or includes the solid electrolyte according to the present embodiment. The positive electrode 11 includes a current collector 111 and a positive electrode layer 112. The positive electrode layer 112 includes a positive electrode active material. The negative electrode 12 includes a current collector 121 and a negative electrode layer 122. The negative electrode layer 122 includes a negative electrode active material.
[0030] The positive electrode active material of the positive electrode layer 112 preferably contains a lithium composite oxide. A preferred positive electrode active material is a lithium composite oxide having a layered rock salt structure, such as NCM (Li(Ni, Co, Mn)O 2 The positive electrode active material may be other lithium composite oxides, for example, NCA (Li(Ni, Co, Al)O) having a layered rock salt structure. 2 ), LCO (LiCoO2 ), LNMO (LiNi) having a spinel structure 0.5 Mn 1.5 O 4 ), LFP (LiFePO) having an olivine structure 4 ) or the like. The positive electrode layer 112 includes the solid electrolyte according to the present embodiment in addition to the positive electrode active material. The positive electrode layer 112 may further include an electron conduction assistant (carbon black, etc.). An example of the positive electrode layer 112 is one in which these materials are integrated by applying pressure or heat.
[0031] The negative electrode active material of the negative electrode layer 122 is, for example, LTO (Li 4 Ti 5 O 12 ), NTO(Nb 2 TiO 7 ), TiO 2 Examples of the materials include compounds such as titanium oxide (TiO 2 ), graphite, and SiO 2 (silicon monoxide). The anode layer 122 includes the solid electrolyte according to this embodiment in addition to the anode active material. The anode layer 122 may further include an electron conduction aid (carbon black, etc.). An example of the anode layer 122 is one in which these materials are integrated by applying pressure or heat. The configurations and materials of the positive electrode 11 and the negative electrode 12 of the all-solid-state secondary battery 1 are not limited to those described above, and various other configurations and materials can be used.
[0032] Next, examples and comparative examples of solid electrolytes will be described. Tables 1 to 4 show the compositions and evaluation results of the solid electrolytes of Examples 1 to 5 and Comparative Examples 1 to 4. The solid electrolytes of Comparative Examples 1 to 4 are solid electrolytes according to the related art described above.
[0033]
[0034]
[0035]
[0036]
[0037] Example 1 [Preparation of Electrolyte] In an argon atmosphere having a dew point of −60° C. or less, LiCl, ZrCl 4 , TaCl 5, YbCl 3 and LiF is LiCl:ZrCl 4 : TaCl 5 : YbCl 3 The raw material powders were weighed to have a molar ratio of 1.85:0.6:0.2:0.2:0.15, and then pulverized and mixed in a mortar. The resulting mixed powder was placed in a zirconia pot and milled at 300 rpm for 20 hours using a planetary ball mill to obtain a solid electrolyte powder.
[0038] [Evaluation of Reduction Stability] A solid electrolyte powder was placed in a mold consisting of a resin sleeve and upper and lower punches made of SUS (stainless steel), and uniaxial press molding was performed under a pressure of 150 MPa. The lower punch was then removed, and Li metal foil was attached to the surface of the powder compact. The lower punch was then reinserted and pressurized at 50 MPa. Lead wires were connected to the upper and lower punches, and cyclic voltammetry measurements were performed at room temperature.
[0039] In the cyclic voltammetry measurement, the scan rate was set to 1 mV / sec, and the working electrode was scanned from the OCV (open circuit voltage) at the time of cell construction to −1.0 V (vs. Li) in the reduction direction. To quantify the stability against the reduction potential, when scanning from the OCV in the reduction direction, the reduction current per unit area of the working electrode was measured to be −20 μV / cm. 2 The potential at which the potential exceeded this value was taken as the reduction onset potential. In Table 1, the obtained values are shown in the "reduction onset potential" column (the same applies to Tables 2 to 4).
[0040] In addition, in the evaluation of reduction stability, the amount of electricity generated by reductive decomposition was calculated. The operating potential (0.1 V vs. Li) of graphite, which is a common negative electrode active material for lithium-ion batteries, was used as a reference, and the amount of electricity (unit: coulomb [C]) was calculated by integrating the reduction current flowing from the reduction onset potential to 0.1 V, to quantitatively evaluate the stability of the negative electrode relative to the potential. In Table 1, the obtained values are shown in the column "Amount of electricity for decomposition up to 0.1 V" (similarly in Tables 2 to 4).
[0041] [Calculation of Average Ionic Radius Ratio] The average ionic radius ratio of the solid electrolyte of Example 1 was calculated using the above-mentioned Equations 1 and 2. Here, the solid electrolyte of Example 1 contains Li, Zr, Ta, and Yb as cations and Cl and F as anions. The ionic radii (coordination number 6) of Li, Zr, Ta, Yb, Cl, and F are 0.76 Å, 0.72 Å, 0.64 Å, 0.868 Å, 1.81 Å, and 1.33 Å, respectively. The molar ratio of Li, Zr, Ta, and Yb is 2.000:0.600:0.200:0.200. Therefore, the average ionic radius rc of the cation was calculated to be 0.7512 Å by calculating (2.000 × 0.76 + 0.600 × 0.72 + 0.200 × 0.64 + 0.200 × 0.868) / (2.000 + 0.600 + 0.200 + 0.200). The average ionic radius ra of the anion was calculated to be 1.798 Å by calculating (5.850 × 1.81 + 0.150 × 1.33) / (5.850 + 0.150). Therefore, the average ionic radius ratio rc / ra was calculated to be 0.418.
[0042] [Calculation of Δχ] The Δχ of the solid electrolyte of Example 1 was calculated using the above-mentioned Equation 3. Here, the solid electrolyte of Example 1 contains Zr, Ta, and Yb as cations other than Li, and Cl and F as anions. The electronegativities of Zr, Ta, Yb, Cl, and F are 1.33, 1.5, 1.1, 3.16, and 3.98, respectively. The molar ratio of Zr, Ta, Yb, Cl, and F is 0.600:0.200:0.200:5.850:0.150. Therefore, Δχ was calculated to be 1.863 by calculating (5.850×3.16+0.150×3.98) / (5.850+0.150)−(0.600×1.33+0.200×1.5+0.200×1.1) / (0.600+0.200+0.200).
[0043] In the column of Table 1 entitled "Meets the conditions of rc / ra and Δχ," if 0.31<(rc / ra)<0.43 and Δχ>1.842 are simultaneously satisfied, the evaluation is "Good," and if neither of these conditions are simultaneously satisfied, the evaluation is "Poor" (similar to Tables 2 to 4).
[0044] Example 2 In the electrolyte preparation of Example 1, LiCl, ZrCl were used as raw material powders. 4 , TaCl 5 , YbCl 3 and LiF is LiCl:ZrCl 4 : TaCl 5 : YbCl 3 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to have a molar ratio of 1.7:0.6:0.2:0.2:0.3, and tests and evaluations were carried out.
[0045] Example 3 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 , DyCl 3 and ZrF 4 LiCl:ZrCl 4 : TaCl 5 : DyCl 3 : ZrF 4 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.9:0.55:0.2:0.1:0.15, and then tested and evaluated.
[0046] Example 4 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , NbCl 5 , YbCl 3 and ZrF 4 LiCl:ZrCl 4 : NbCl 5 : YbCl 3 : ZrF 4 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.9:0.35:0.3:0.2:0.15, and then tested and evaluated.
[0047] Example 5 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 , ErCl 3 and ZrF 4 LiCl:ZrCl 4 : TaCl 5 : ErCl 3 : ZrF 4An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.75:0.1:0.5:0.25:0.15, and then tested and evaluated.
[0048] Comparative Example 1 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and YbCl 3 LiCl:ZrCl 4 : TaCl 5 : YbCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 2.0:0.6:0.2:0.2, and then tested and evaluated.
[0049] Comparative Example 2 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 and DyCl 3 LiCl:ZrCl 4 : TaCl 5 : DyCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.9:0.7:0.2:0.1, and then tested and evaluated.
[0050] Comparative Example 3 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , NbCl 5 and YbCl 3 LiCl:ZrCl 4 : NbCl 5 : YbCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.9:0.5:0.3:0.2, and then tested and evaluated.
[0051] Comparative Example 4 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and ErCl 3 LiCl:ZrCl 4 : TaCl 5 : ErCl 3An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.75:0.25:0.5:0.25, and then tested and evaluated.
[0052] Table 1 compares Examples 1 and 2 with Comparative Example 1, which have the same composition ratio of Li, Zr, Ta, and Yb. In Examples 1 and 2, which contain F, a decrease in the reduction onset potential was observed compared to Comparative Example 1, which does not contain F. The decomposition charge up to 0.1 V was also reduced. Tables 2 to 4 also compare Examples and Comparative Examples, which have the same composition ratio of Li, Mα, Mβ, and Mγ. The solid electrolyte of the Example containing F exhibited a lower reduction onset potential and a lower decomposition charge up to 0.1 V than the solid electrolyte of the Comparative Example, which does not contain F. As described above, the presence or absence of F caused changes in the above characteristics at the same cation ratio. These results confirmed that introducing F into a solid electrolyte containing Li, Mα, Mβ, Mγ, and Cl suppressed the reductive decomposition reaction of the solid electrolyte and improved its reduction resistance. Furthermore, Examples 1 and 2 confirmed a tendency for the reduction resistance to increase as the ratio of the amount of F to the amount of Cl increased.
[0053] The reason why solid electrolytes containing F have improved reduction resistance is not entirely clear, but when focusing on Pauling's electronegativity, F is 3.98, while Cl is 3.16. Therefore, F is thought to bond more strongly with cations than Cl, and it is presumed that this improved bonding strength contributes to the improved reduction resistance.
[0054] The mechanism by which reduction resistance is improved is believed to be the same even when the cation species is changed. Specifically, when Hf, which becomes a tetravalent cation like Zr, is used instead of Zr or together with Zr, the presence of F is believed to improve reduction resistance. The same is true when both Ta and Nb are used as Mβ. Furthermore, the same is true when Gd, Ho, Eu, and Sc, which become trivalent cations like Yb, Dy, and Er and have ionic radii similar to those of Yb, Dy, and Er, are used instead of Yb, Dy, or Er, or together with Yb, Dy, or Er.
[0055] As described above, the solid electrolyte according to this embodiment contains Li, Mα, Mβ, Mγ, Cl, and F. Mα is at least one element selected from the group consisting of Zr and Hf. Mβ is at least one element selected from the group consisting of Ta and Nb. Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc. This makes it possible to realize a solid electrolyte with excellent reduction resistance. Since the potential window of this solid electrolyte is wide, when this solid electrolyte is applied to an all-solid-state secondary battery 1, the limitations on the operating voltage are alleviated, and the energy density of the all-solid-state secondary battery 1 can be improved.
[0056] A preferred solid electrolyte is represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6-d F d ...(1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<6 are satisfied. x MCl 6―d F d By optimizing the fluorine content d and the type and combination of cations M in the chloride electrolyte represented by the formula (1), a solid electrolyte having excellent reduction resistance can be more reliably realized.
[0057] The solid electrolyte and all-solid-state secondary battery 1 can be modified in various ways.
[0058] The solid electrolyte containing Li, Mα, Mβ, Mγ, Cl, and F may not satisfy the above composition formula (1).
[0059] The solid electrolyte may be mixed with other substances (which may include Li) and used as an electrolyte material. In this case, the solid electrolyte is preferably the component with the largest mass ratio among the components contained in the electrolyte material, i.e., the main component. The mass ratio of the main component in the electrolyte material is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more.
[0060] The solid electrolyte used in the all solid state secondary battery 1 does not necessarily need to be contained in all of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13, but may be contained in at least one of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13. Furthermore, the solid electrolyte may be used in batteries other than all solid state secondary batteries, and may be used for purposes other than batteries.
[0061] The configurations in the above-described embodiment and each modification may be combined as appropriate as long as they are not mutually contradictory.
[0062] While the invention has been particularly illustrated and described, it should be understood that the foregoing description is illustrative and not restrictive, and that numerous modifications and variations are possible without departing from the scope of the invention.
[0063] 1 All-solid-state lithium-ion secondary battery 11 Positive electrode 12 Negative electrode 13 Electrolyte layer
Claims
1. A solid electrolyte comprising Li, Mα, Mβ, Mγ, Cl and F, wherein Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, and Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu and Sc.
2. The solid electrolyte according to claim 1, wherein Mα contains Zr.
3. The solid electrolyte according to claim 1, wherein Mβ contains Ta.
4. The solid electrolyte according to claim 1, wherein Mγ contains Gd, Yb or Er.
5. The solid electrolyte according to claim 1, which is represented by the following compositional formula (1): Li6-(4 + a - b)(1 + c)(Mα (1-a-b) Mβ a Mγ b )( 1+c Cl 6-d F d ...(1) A solid electrolyte satisfying 0 < a, 0 < b, a + b < 1, -0.2 ≤ c ≤ 0.2, and 0 < d < 6.
6. The solid electrolyte according to claim 1, wherein the value obtained by dividing the average ionic radius of Li, Mα, Mβ and Mγ by the average ionic radius of Cl and F is greater than 0.31 and less than 0.43, and the difference Δχ between the average electronegativity of Cl and F and the average electronegativity of Mα, Mβ and Mγ is greater than 1.
842.
7. A lithium ion battery comprising the solid electrolyte according to any one of claims 1 to 6.
Citation Information
Patent Citations
Solid electrolyte material and battery
JP6934626B2
Halide solid electrolyte material and battery using this
WO2020070956A1
Oxide, method of preparing the same, solid electrolyte including the oxide, and electrochemical device including the oxide
US20210043966A1
Solid electrolyte, preparation method thereof, metal air battery including the same, and electrochemical device including the same
US20210167419A1
Solid electrolyte material and battery using same
WO2020188914A1