Method for producing plated steel sheet
A controlled heat treatment process for plated steel sheets with high Si and Mn content addresses the challenge of achieving both excellent plating properties and hydrogen embrittlement resistance, resulting in high-strength, high-performance steel for car body applications.
Patent Information
- Application Number
- PCT/JP2023/013698
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for manufacturing plated steel sheets with high Si and Mn content fail to achieve both excellent plating properties and hydrogen embrittlement resistance, leading to suboptimal performance in car body applications.
A controlled heat treatment process involving oxidation, reduction, soaking, rapid heating, and cooling steps in specific atmospheric conditions is applied to the steel sheets, ensuring effective reduction of Fe oxides and hydrogen management to enhance plating properties and hydrogen embrittlement resistance.
The method produces plated steel sheets with improved strength, excellent plating properties, and enhanced hydrogen embrittlement resistance, meeting the requirements for high-strength car body components.
Smart Images

Figure JPOXMLDOC01-APPB-I000003 
Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Manufacturing method of plated steel sheet
[0001] The present invention relates to a method for producing a plated steel sheet.
[0002] In recent years, from the perspective of global environmental conservation, 2 There is a strong demand for improved fuel efficiency to reduce emissions. Accordingly, there has been a growing trend to reduce the weight of vehicle bodies by thinning the body parts. This has led to an increasing need for higher strength steel sheets, which are used as materials for vehicle body parts.
[0003] In order to increase the strength of steel sheets, it is effective to add elements having solid solution strengthening ability, such as Si and Mn.
[0004] Furthermore, plated steel sheets are often used as steel sheets for vehicle body parts. Here, plated steel sheets, for example, hot-dip galvanized steel sheets, are generally produced by annealing a base steel sheet in an annealing furnace of a continuous hot-dip galvanizing line (hereinafter also referred to as CGL), and then performing a hot-dip galvanizing treatment.
[0005] For example, Patent Document 1 describes a method for producing such a plated steel sheet as follows: "A steel sheet containing, by mass%, C: 0.3% or less, Si: 0.1 to 2.5%, Mn: 0.5 to 3.0%, with the balance being Fe and unavoidable impurities is subjected to oxidation treatment, then reduction annealing, and then hot-dip plating treatment. In the oxidation treatment, in the first stage, O 2 Concentration 1000 ppm by volume or more, H 2 The mixture is heated at a temperature of 400 to 750°C in an atmosphere with an O concentration of 1000 ppm by volume or more, and then 2 Concentration less than 1000 ppm by volume, H 2 The steel sheet is heated at a temperature of 600 to 850°C in an atmosphere having an O concentration of 1000 ppm by volume or more, and in the reduction annealing, H 2 Concentration 5 to 30% by volume, H 2 O concentration 500 to 5000 volume ppm, balance N 2 and unavoidable impurities in an atmosphere at a temperature of 650 to 900°C."
[0006] Patent Document 2 states that "in the production of galvanized steel sheets, hot-rolled steel sheets are pickled and cleaned, and then the steel sheet surface is reduced and immersed in molten zinc for plating, H is added between the reduction treatment and the plating process. 2 : 8-20%, N 2 : A method for manufacturing a galvanized steel sheet, characterized by inserting a step of promoting dehydrogenation by setting the steel sheet temperature at 450 to 550°C in an atmosphere of 92 to 80% humidity."
[0007] Patent Document 3 discloses the following: "A method for producing a hot-dip galvanized steel sheet in which a hot-rolled steel sheet having a thickness of 1.5 mm or more is pickled, annealed in a continuous hot-dip galvanizing line, and then plated in a molten zinc bath without alloying treatment, characterized in that, when the hydrogen concentration (%) of the atmosphere in the annealing furnace is H and the annealing temperature (°C) is RT, these are controlled so as to satisfy the following formulas (1) and (2): 650≦RT≦950 ... (1) 1≦H≦-0.05×RT+57.5 ... (2)."
[0008] Patent Document 4 describes a method for producing a hot-dip galvanized steel sheet, which comprises continuously hot-dip galvanizing a steel sheet having a chemical composition containing, in mass %, at least 0.2 to 2.0% Si, 0.2 to 3.0% Mn, and 0.001 to 1.5% Al, with the ratios of Si, Mn, and Al satisfying the following formulas (1), (2), and (3), in a hot-dip galvanizing line having a radiant tube type reducing furnace, wherein the temperature of the steel sheet during heating in the reducing furnace is such that: the logarithmic ratio of the hydrogen partial pressure to the water vapor partial pressure of the atmospheric gas in a temperature range of 650°C or higher and lower than 750°C satisfies the following formula (4), and the logarithmic ratio of the hydrogen partial pressure to the water vapor partial pressure of the atmospheric gas in a temperature range of 750°C or higher and 950°C or lower satisfies the following formula (5). 5≦(Si / (Si+Mn+Al))×100≦54 ... (1) 30≦(Mn / (Si+Mn+Al))×100≦95...(2) 0≦(Al / (Si+Mn+Al))×100≦30...(3) log(PH 2 O / PH 2)≦-1.55...(4) -0.91≦log(PH 2 O / PH 2 )≦−0.635 (5)" is disclosed.
[0009] Furthermore, Patent Document 5 states that "a cold-rolled steel sheet having a predetermined composition is annealed in an annealing furnace atmosphere having a hydrogen concentration of 1 vol% or more and 13 vol% or less at an annealing furnace temperature T1: (A c3 The method for manufacturing a high-strength galvanized steel sheet comprises: an annealing step of heating the steel sheet in a temperature range of 400°C or higher (temperature point -10°C) or higher and 900°C or lower for 5 seconds or longer, cooling the steel sheet, and allowing it to remain in a temperature range of 400°C or higher and 550°C or lower for 20 seconds or longer and 1500 seconds or shorter; a plating step of plating the steel sheet after the annealing step and cooling it to 100°C or lower at an average cooling rate of 3°C / s or higher; and a post-heat treatment step of allowing the plated steel sheet after the plating step to remain at a temperature T2 (°C) of 70°C or higher and 450°C or lower in a furnace atmosphere having a hydrogen concentration of 10 vol% or lower and a dew point of 50°C or lower for a time t (hr) or longer that satisfies the following formula (2):
[0010] Japanese Patent Application Laid-Open No. 2016-53211 Japanese Patent Application Laid-Open No. 54-130443 Japanese Patent No. 3266008 Japanese Patent No. 5811841 Japanese Patent Application Laid-Open No. 2020-45568
[0011] Incidentally, Si and Mn are easily oxidizable elements that are more easily oxidized than Fe. When a plated steel sheet, for example, a hot-dip galvanized steel sheet, is manufactured using a steel sheet having a chemical composition containing a large amount of such easily oxidizable elements as a base steel sheet, the easily oxidizable elements contained in the base steel sheet are oxidized during annealing and concentrate on the surface of the base steel sheet, forming oxides on the surface of the base steel sheet. These oxides can reduce the wettability of the base steel sheet with molten zinc, resulting in poor appearance, such as bare spots, and poor coating adhesion. Hereinafter, the term "coatability" will be used to refer to both coating appearance and coating adhesion.
[0012] Furthermore, steel sheets used as materials for vehicle body parts are also required to have excellent resistance to hydrogen embrittlement.
[0013] However, in the methods for manufacturing plated steel sheets disclosed in Patent Documents 1 to 5, when a steel sheet having a chemical composition containing large amounts of easily oxidizable elements Si and Mn is used as a base steel sheet, it cannot be said that both excellent plateability and excellent hydrogen embrittlement resistance can be achieved, and this point remains a problem.
[0014] That is, when a steel sheet having a chemical composition containing a large amount of Si and Mn is used as a base steel sheet, it cannot be said that a method for producing a plated steel sheet that has both excellent plateability and excellent hydrogen embrittlement resistance has been developed, and the development of such a method is currently desired.
[0015] The present invention has been developed in view of the above-described current situation, and has an object to provide a method for manufacturing a plated steel sheet that enables the manufacture of a plated steel sheet that has both excellent plateability and excellent hydrogen embrittlement resistance, even when a steel sheet having a chemical composition containing large amounts of Si and Mn is used as a base steel sheet.
[0016] The inventors have conducted extensive research to achieve the above object. As a result, they have found that the above object can be achieved by subjecting a base steel sheet to a heat treatment in which the atmosphere and heat pattern are appropriately controlled in a step prior to the plating treatment step. The present invention has been completed based on the above finding and through further research.
[0017] That is, the gist and configuration of the present invention are as follows: 1. The present invention relates to an oxidation process in which a base steel sheet having a chemical composition containing, by mass, Si: 0.10% to 2.00% and Mn: 1.00% to 5.00% is heated under the following conditions: an atmosphere: oxygen concentration of 1000 volume ppm to 30000 volume ppm, and a heating temperature of 600°C or higher; a reduction process in which the base steel sheet is held under the following conditions: an atmosphere: hydrogen concentration of 8 volume % to 30 volume %, a holding temperature of 700°C or higher, and a holding time of 20 seconds or longer; a soaking process in which the base steel sheet is held under the following conditions: an atmosphere: hydrogen concentration of 0.2 volume % to less than 8 volume %, a soaking temperature of 700°C to less than 900°C, and a soaking time of 20 seconds to 300 seconds; and a reduction process in which the base steel sheet is held under the following conditions: an atmosphere: hydrogen concentration of 0.2 volume % to less than 30 volume %, a soaking temperature of 700°C to less than 900°C, and a soaking time of 20 seconds to 300 seconds. a rapid heating step of heating the base steel sheet under the conditions of an average heating rate from the soaking temperature of 10°C / s or more, and a maximum temperature reached of 10°C or more above the soaking temperature; a cooling step of cooling the base steel sheet under the conditions of an atmosphere having a hydrogen concentration of 0.2% by volume or more and 30% by volume or less, a residence time in a temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature of 20 seconds or less, and a cooling stop temperature of 500°C or less; and a plating step of plating one or both sides of the base steel sheet to obtain a plated steel sheet.
[0018] 2. The method for producing a plated steel sheet according to item 1, which satisfies at least one of the following (1) to (3): (1) an atmosphere in the soaking step: a hydrogen concentration of 0.2 vol% or more and 5 vol% or less; (2) an atmosphere in the rapid heating step: a hydrogen concentration of 0.2 vol% or more and less than 8 vol%; and (3) an atmosphere in the cooling step: a hydrogen concentration of 0.5 vol% or more and 20 vol% or less.
[0019] 3. The method for producing a plated steel sheet according to 1 or 2 above, wherein the chemical composition further contains, in mass%, C: 0.05% or more and 0.40% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% or more and 2.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.
[0020] 4. The chemical composition further includes, in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, 4. The method for producing a plated steel sheet according to 3 above, containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less.
[0021] 5. The method for producing a plated steel sheet according to any one of 1 to 4 above, wherein the plating treatment is a hot-dip galvanizing treatment or a hot-dip galvannealing treatment.
[0022] 6. The method for producing a plated steel sheet according to any one of 1 to 4 above, wherein the plating treatment is a galvannealed hot-dip plating treatment, and further comprising, after the plating treatment step, a cooling-reheating step of cooling the plated steel sheet under the conditions of a cooling stop temperature of Ms point or lower, and then reheating the plated steel sheet under the conditions of an atmosphere having a hydrogen concentration of 0.2 volume % or lower, a reheating temperature of 100°C or higher and 450°C or lower, and a reheating time of 5 seconds or longer.
[0023] 7. The method for producing a plated steel sheet according to 6 above, wherein the cooling stop temperature in the cooling-reheating step is (Ms point - 50°C) or lower.
[0024] According to the present invention, it is possible to manufacture a plated steel sheet that has both excellent galvanization ability and excellent hydrogen embrittlement resistance, even when a steel sheet having a chemical composition containing large amounts of Si and Mn is used as a base steel sheet. That is, according to the present invention, it is possible to manufacture a plated steel sheet that has high strength and also has both excellent galvanization ability and excellent hydrogen embrittlement resistance.
[0025] The present invention will be described based on the following embodiments: First, the gist of a method for producing a plated steel sheet according to one embodiment of the present invention will be described.
[0026] When a steel sheet having a chemical composition containing large amounts of the easily oxidizable elements Si and Mn is used as a base steel sheet, the following points are important for obtaining excellent galvanizability. Specifically, in a step prior to the galvanizing process, the base steel sheet is oxidized. In other words, oxides mainly composed of Fe (hereinafter also referred to as Fe oxides) are formed on the surface of the base steel sheet, and then these Fe oxides are reduced. However, the reduction of Fe oxides requires heat treatment in a high-hydrogen-concentration atmosphere, which inevitably results in the penetration of a large amount of hydrogen into the base steel sheet. Furthermore, if the hydrogen concentration of the heat treatment atmosphere is low, the reduction of Fe oxides is insufficient, and the Fe oxides remaining on the surface of the base steel sheet result in deterioration of galvanizability.
[0027] Therefore, in a method for producing a plated steel sheet according to one embodiment of the present invention, the heat treatment is divided into a reduction step and a soaking step. In the reduction step, Fe oxides are reduced in a high-hydrogen-concentration atmosphere. Next, in the soaking step, the hydrogen concentration in the atmosphere is reduced to a level at which Fe is not reoxidized, thereby reducing the hydrogen that has penetrated into the base steel sheet during the reduction step. However, holding the base steel sheet at a high temperature for a long period of time in the soaking step may increase the amount of austenite, which has a high hydrogen solid solubility, and may result in an increase in the amount of hydrogen dissolved in the base steel sheet (hereinafter also referred to as the in-steel hydrogen amount). Therefore, in a method for producing a plated steel sheet according to one embodiment of the present invention, the soaking step is performed at a relatively low temperature at which recrystallization proceeds. Then, after recrystallization is completed, the base steel sheet is rapidly heated, thereby securing the necessary amount of austenite. As a result, it is possible to produce a plated steel sheet that has high strength, excellent coatability, and excellent hydrogen embrittlement resistance.
[0028] Hereinafter, each step of the method for producing a plated steel sheet according to one embodiment of the present invention will be described.
[0029] [Preparation Step] First, a base steel sheet is prepared having a chemical composition containing, by mass%, Si: 0.10% to 2.00% and Mn: 1.00% to 5.00%. Such a base steel sheet can be prepared, for example, by manufacturing according to a conventional method. In one example, a steel slab having the above chemical composition is hot-rolled and cold-rolled to produce a cold-rolled steel sheet. The conditions for hot rolling and cold rolling are not particularly limited, and conventional methods may be followed. The base steel sheet corresponds to the base steel sheet of the plated steel sheet after plating. The plated steel sheet has a plating layer on one or both sides of the base steel sheet.
[0030] Next, the chemical composition of the base steel sheet will be described. Note that the unit of chemical composition is always "mass %", but hereinafter, unless otherwise specified, it will be simply expressed as "%".
[0031] Si: 0.10% or more and 2.00% or less Si is a solid-solution strengthening element and contributes to increasing the strength of steel sheets. Si also has the effect of suppressing carbide formation and facilitating the formation of retained austenite. In other words, Si is an element that is effective in achieving both strength and ductility in steel sheets. To achieve these effects, the Si content is set to 0.10% or more. On the other hand, if the Si content exceeds 2.00%, hot rolling and cold rolling properties are significantly reduced. This may adversely affect productivity or even reduce the ductility of the base steel sheet itself. Furthermore, a large amount of Si oxide may be formed on the surface of the base steel sheet, potentially hindering good galvanizability. Therefore, the Si content is set to 0.10% or more and 2.00% or less. The Si content is preferably 0.25% or more. Furthermore, the Si content is preferably 1.70% or less.
[0032] Mn: 1.00% or more and 5.00% or less Like Si, Mn is a solid-solution strengthening element and contributes to increasing the strength of steel sheets. Furthermore, Mn also has the effect of improving hardenability and promoting the formation of retained austenite, bainite, and martensite. To achieve these effects, the Mn content is set to 1.00% or more. On the other hand, if the Mn content exceeds 5.00%, costs increase. Furthermore, the formation of Mn oxides on the surface of the base steel sheet during plating may not be sufficiently suppressed, which may result in poor plating performance. Therefore, the Mn content is set to 1.00% or more and 5.00% or less. The Mn content is preferably 1.50% or more, more preferably 2.00% or more. The Mn content is preferably 4.00% or less, more preferably 3.50% or less.
[0033] The chemical composition of the base steel sheet is not particularly limited as long as the Si and Mn contents are within the above ranges. For example, to achieve a tensile strength of 340 MPa or more, the following chemical composition is preferred: C: 0.05% to 0.40%, Si: 0.10% to 2.00%, Mn: 1.00% to 5.00%, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% to 2.000%, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.
[0034] C: 0.05% or more and 0.40% or less C is an element effective in increasing the strength of steel sheets. C also contributes to increasing strength by forming martensite, which is one of the hard phases in steel structures. Therefore, the C content is preferably 0.05% or more. The C content is more preferably 0.07% or more. In order to obtain good weldability, the C content is preferably 0.40% or less. The C content is more preferably 0.35% or less.
[0035] P: 0.100% or less (excluding 0%) The P content is preferably 0.100% or less, and more preferably 0.050% or less. By suppressing the P content in this manner, better weldability can be obtained. In addition, P is prevented from segregating at grain boundaries, which can particularly improve ductility, bendability, and toughness. Furthermore, ferrite transformation can be suppressed, which can prevent coarsening of crystal grains. The lower limit of the P content is not particularly limited. However, due to constraints on production technology, the P content may be more than 0% and may be 0.001% or more.
[0036] S: 0.0200% or less (excluding 0%) The S content is preferably 0.0200% or less, more preferably 0.0150% or less, and even more preferably 0.0100% or less. By suppressing the S content in this way, it is possible to prevent a decrease in weldability. In addition, it is possible to prevent a decrease in ductility during hot rolling, suppress hot cracking, and improve surface properties. Furthermore, it is possible to prevent the formation of coarse sulfides, thereby achieving better ductility, bendability, and stretch flangeability. The lower limit of the S content is not particularly limited. However, due to constraints in production technology, the S content may be more than 0% and may be 0.0001% or more.
[0037] Al: 0.003% or more and 2.000% or less Al is an element that is thermodynamically easily oxidized. Therefore, Al oxidizes before Si and Mn. That is, Al has the effect of suppressing the oxidation of Si and Mn in the surface layer portion of the base steel sheet and promoting the oxidation of Si and Mn inside the base steel sheet. Such an effect can be obtained when the Al content is 0.003% or more. On the other hand, from the viewpoint of cost, the Al content is preferably 2.000% or less. Therefore, the Al content is preferably 0.003% or more and 2.000% or less. The Al content is more preferably 0.010% or more.
[0038] N: 0.0100% or less (excluding 0%) The N content is preferably 0.0100% or less. By setting the N content to 0.0100% or less, it is possible to more effectively prevent N from forming coarse nitrides with Ti, Nb, and V at high temperatures. As a result, it is possible to prevent the effect of increasing the strength of the steel sheet by adding Ti, Nb, and V from being impaired. In addition, it is possible to obtain better toughness. Furthermore, it is possible to prevent the occurrence of slab cracks and surface defects during hot rolling. Therefore, the N content is preferably 0.0100% or less, and more preferably 0.0050% or less. The lower limit of the N content is not particularly limited. However, due to constraints on production technology, the N content may be more than 0% and may be 0.0005% or more.
[0039] As described above, the base steel sheet has a composition that contains, for example, the basic components, with the balance other than the basic components including Fe (iron) and unavoidable impurities. Furthermore, the base steel sheet preferably has a composition that contains the basic components, with the balance consisting of Fe and unavoidable impurities. Furthermore, in addition to the basic components, the base steel sheet may contain, as an optional additional element, at least one element selected from the following, either alone or in combination: B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less. Note that the above-mentioned optional additional elements have no particular lower limit because the desired effects can be obtained as long as they are contained in amounts not exceeding the above-mentioned upper limits. Furthermore, when the above-mentioned optional additional elements are contained in amounts less than the preferred lower limit described below, the elements are considered to be contained as inevitable impurities.
[0040] B: 0.0100% or less B is an element effective in improving the hardenability of steel. To improve hardenability, the B content is preferably 0.0001% or more, and more preferably 0.0005% or more. Furthermore, when B is contained to obtain better formability, the B content is preferably 0.0100% or less, and more preferably 0.0050% or less.
[0041] Ti: 0.200% or less Ti is an element effective for precipitation strengthening of steel. The lower limit of Ti is not particularly limited. However, in order to obtain the effect of adjusting strength, the Ti content is preferably 0.001% or more. Furthermore, when Ti is contained in order to obtain better formability, the Ti content is preferably 0.200% or less, and more preferably 0.060% or less.
[0042] Nb: 0.200% or less Nb is an element effective in improving the strength of steel. To obtain this effect, the Nb content is preferably 0.001% or more, more preferably 0.005% or more. Furthermore, by setting the Nb content to 0.200% or less, an increase in cost can be prevented. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less, more preferably 0.060% or less.
[0043] Sb: 0.200% or less Sb is an element that suppresses excessive decarburization in the surface layer of the base steel sheet and prevents a decrease in the amount of martensite formed. That is, Sb can be added for the purpose of improving the fatigue properties and surface quality of the steel sheet. To achieve this effect, the Sb content is preferably 0.001% or more. Furthermore, when Sb is added, in order to obtain better toughness, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.060% or less.
[0044] Sn: 0.200% or less Sn is an element that is effective in suppressing decarburization, denitrification, etc., and suppressing a decrease in the strength of steel. To achieve this effect, the Sn content is preferably 0.002% or more. On the other hand, when Sn is contained to obtain better impact resistance, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.060% or less.
[0045] V: 0.100% or less V is an element effective in improving the strength of steel. To obtain this effect, the V content is preferably 0.001% or more, more preferably 0.005% or more. Furthermore, by setting the V content to 0.100% or less, an increase in cost can be prevented. Therefore, when V is contained, the V content is preferably 0.100% or less, more preferably 0.060% or less.
[0046] Cu: 1.00% or less Cu is an element effective in improving the hardenability of steel. Cu is also an element effective in keeping the area ratio of the hard phase within a more preferable range and thereby keeping the tensile strength within a more preferable range. To achieve this effect, the Cu content is preferably 0.005% or more, and more preferably 0.020% or more. When Cu is contained, from the viewpoint of preventing an increase in cost, the Cu content is preferably 1.00% or less, and more preferably 0.20% or less.
[0047] Cr: 1.00% or less Cr is an element that improves hardenability and improves the balance between strength and ductility. To achieve this effect, the Cr content is preferably 0.001% or more. When Cr is contained, from the viewpoint of preventing an increase in cost, the Cr content is preferably 1.00% or less, and more preferably 0.80% or less.
[0048] Ni: 1.00% or less Ni is an element that improves hardenability and improves the balance between strength and ductility. To achieve these effects, the Ni content is preferably 0.005% or more. When Ni is contained, from the viewpoint of preventing an increase in cost, the Ni content is preferably 1.00% or less, and more preferably 0.80% or less.
[0049] Mo: 1.00% or less Mo is an element that has the effect of adjusting strength. To obtain this effect, the Mo content is preferably 0.005% or more, more preferably 0.01% or more. When Mo is contained, from the viewpoint of preventing an increase in cost, the Mo content is preferably 0.80% or less, more preferably 0.60% or less.
[0050] Ta: 0.100% or less Ta is an element that has the effect of improving strength. To obtain such an effect, the Ta content is preferably 0.001% or more. Furthermore, when Ta is contained, from the viewpoint of preventing an increase in cost, the Ta content is preferably 0.100% or less, and more preferably 0.050% or less.
[0051] W: 0.500% or less W is an element that has the effect of improving strength. To obtain such an effect, the W content is preferably 0.001% or more, more preferably 0.003% or more. Furthermore, when W is contained, from the viewpoint of preventing an increase in cost, the W content is preferably 0.500% or less, more preferably 0.450% or less.
[0052] Zr: 0.020% or less Zr is an element that has the effect of improving the ultimate deformability and stretch flangeability of a steel sheet. To obtain such effects, the Zr content is preferably 0.0005% or more, more preferably 0.0010% or more. Furthermore, when Zr is contained, from the viewpoint of preventing an increase in cost, the Zr content is preferably 0.020% or less, more preferably 0.010% or less.
[0053] Ca: 0.0200% or less Ca is an element that has the effect of controlling the morphology of sulfides and further improving ductility and toughness. To obtain such effects, the Ca content is preferably 0.0005% or more. Furthermore, when Ca is contained, from the viewpoint of obtaining better ductility, the Ca content is preferably 0.0200% or less, and more preferably 0.0100% or less.
[0054] Mg: 0.0200% or less Mg is an element that has the effect of controlling the morphology of sulfides and further improving ductility and toughness. To obtain such effects, the Mg content is preferably 0.0005% or more. Furthermore, when Mg is contained, from the viewpoint of obtaining better ductility, the Mg content is preferably 0.0200% or less, and more preferably 0.0100% or less.
[0055] Zn: 0.020% or less Zn is an element that has the effect of improving the ultimate deformability and stretch flangeability of the steel sheet. To obtain such effects, the Zn content is preferably 0.001% or more. Furthermore, when Zn is contained, from the viewpoint of preventing an increase in cost, the Zn content is preferably 0.020% or less, and more preferably 0.010% or less.
[0056] Co: 0.020% or less Co is an element that has the effect of improving the ultimate deformability and stretch flangeability of a steel sheet. To achieve this effect, the Co content is preferably 0.001% or more. When Co is contained, from the viewpoint of preventing an increase in cost, the Co content is preferably 0.020% or less, and more preferably 0.010% or less.
[0057] Ce, Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, REM: 0.0200% or less. All of the above elements have the effect of improving the ultimate deformability and stretch flangeability of the steel sheet. To achieve such effects, it is preferable to contain at least one of the above elements in an amount of 0.0001% or more. Furthermore, when the above elements are contained, the content of each of the above elements is preferably 0.0200% or less from the viewpoint of preventing an increase in costs.
[0058] The elements other than those mentioned above are Fe and unavoidable impurities.
[0059] The thickness of the base steel plate is not particularly limited, and may be, for example, 0.5 mm or more and 3.2 mm or less.
[0060] Then, before subjecting the base steel sheet to a galvanizing treatment, the base steel sheet is subjected to a heat treatment in which the atmosphere and heat pattern are appropriately controlled. Specifically, the following conditions are met for the oxidation step, reduction step, soaking step, rapid heating step, and cooling step. In one example, these steps are performed in a CGL. The configuration of the CGL is not particularly limited. For example, the CGL may include a continuous annealing furnace having a heating zone, a soaking zone, and a cooling zone arranged in this order, a hot-dip galvanizing facility provided downstream of the cooling zone, and an alloying furnace provided downstream of the hot-dip galvanizing facility. In one example, the base steel sheet is transported through the heating zone, the soaking zone, and the cooling zone in this order and subjected to the above heat treatment. Next, the base steel sheet discharged from the cooling zone is hot-dip galvanized using the hot-dip galvanizing facility to produce a hot-dip galvanized steel sheet, and then the hot-dip galvanized steel sheet is alloyed using an alloying furnace to produce a hot-dip galvanized steel sheet.
[0061] [Oxidation Process] In the oxidation process, the base steel sheet is heated under the following conditions: atmosphere: oxygen concentration of 1,000 volume ppm or more and 30,000 volume ppm or less; heating temperature: 600°C or higher. This oxidizes the base steel sheet, forming Fe oxides on the surface of the base steel sheet. As an example, the oxidation process is carried out in the heating zone of a CGL. Note that the temperature is the surface temperature of the base steel sheet. The same applies to the following processes. Furthermore, unless otherwise specified, the average heating rate in each of the following processes is also based on the surface temperature of the base steel sheet.
[0062] Atmosphere: Oxidizing atmosphere with oxygen concentration of 1000 volume ppm or more and 30000 volume ppm or less By setting the oxygen concentration of the atmosphere in the oxidation step (hereinafter simply referred to as oxygen concentration) to 1000 volume ppm or more, an oxidizing atmosphere is created, which promotes oxidation of the base steel sheet. If the oxygen concentration is less than 1000 volume ppm, the base steel sheet is not oxidized sufficiently, and excellent galvanization properties cannot be obtained. On the other hand, if the oxygen concentration exceeds 30000 volume ppm, the base steel sheet is oxidized excessively. As a result, unreduced Fe oxides remain in the reduction step described below, which causes deterioration of galvanization properties. Therefore, the oxygen concentration is set to 1000 volume ppm or more and 30000 volume ppm or less. The oxygen concentration is preferably 1500 volume ppm or more, more preferably 2000 volume ppm or more. Furthermore, the oxygen concentration is preferably 29500 volume ppm or less, more preferably 29000 volume ppm or less. The oxygen (O 2 The remaining gas other than the above is not particularly limited. For example, the remaining gas is N 2 , CO, CO 2 , H 2 O and unavoidable impurities, and combinations thereof. The ratio of these components is not particularly limited.
[0063] Heating temperature: 600°C or higher To promote the oxidation of the base steel sheet in the oxidation process, it is necessary to heat the base steel sheet to 600°C or higher. If the heating temperature of the base steel sheet is less than 600°C, the oxidation of the base steel sheet will be insufficient, and excellent galvanization will not be achieved. Therefore, the heating temperature of the base steel sheet is 600°C or higher. The heating temperature of the base steel sheet is preferably 620°C or higher. There is no particular upper limit to the heating temperature of the base steel sheet. As an example, the heating temperature of the base steel sheet is preferably 900°C or lower. By setting the heating temperature of the base steel sheet to 900°C or lower, excessive oxidation of the base steel sheet can be suitably prevented. As a result, unreduced Fe oxides are prevented from remaining in the reduction process described below, and galvanization is further improved. Note that the heating temperature here refers to the maximum temperature reached in the oxidation process.
[0064] Furthermore, there is no particular limitation on the residence time in the temperature range of 600° C. or higher in the oxidation step. For example, the residence time in the temperature range is preferably 1 second or more and 60 seconds or less.
[0065] [Reduction step] Next, the base steel sheet is held under the following conditions: atmosphere: hydrogen concentration of 8% by volume or more and 30% by volume or less, holding temperature: 700°C or more, holding time: 20 seconds or more. This reduces the Fe oxide formed on the surface of the base steel sheet in the oxidation step.
[0066] Atmosphere: Hydrogen concentration of 8% by volume or more and 30% by volume or less The atmosphere in the reduction step is a reducing atmosphere, and in particular, the higher the hydrogen concentration of the atmosphere (hereinafter simply referred to as hydrogen concentration in this paragraph), the more the reduction of Fe oxides formed on the surface of the base steel sheet is promoted. However, the higher the hydrogen concentration, the greater the amount of hydrogen in the steel, leading to deterioration of hydrogen embrittlement resistance. Here, if the hydrogen concentration is 8% by volume or less, unreduced Fe oxides remain, causing deterioration of platability. On the other hand, if the hydrogen concentration exceeds 30% by volume, the reduction effect of Fe oxides becomes saturated. Furthermore, it becomes difficult to sufficiently reduce the amount of hydrogen in the steel in the soaking step described below. Therefore, the hydrogen concentration is set to 8% by volume or more and 30% by volume or less. The hydrogen concentration is preferably 20% by volume or less, more preferably 18% by volume or less. Furthermore, the hydrogen concentration is preferably 12% by volume or more. The hydrogen (H 2The remaining gas other than the above is not particularly limited. For example, the remaining gas is N 2 , H 2 O, CO 2 , CO and unavoidable impurities, and combinations thereof. The ratios of these impurities are also not particularly limited. In addition, the hydrogen (H 2 The same applies to the remaining gases other than the above.
[0067] Holding temperature: 700°C or higher If the temperature at which the base steel sheet is held in the reduction process (hereinafter also referred to as the holding temperature) is lower than 700°C, unreduced Fe oxides will remain, causing deterioration of platability. Therefore, the holding temperature is set to 700°C or higher. The holding temperature is preferably 750°C or higher. There is no particular upper limit to the holding temperature. However, from the viewpoint of more effectively preventing deterioration of the furnace body, the holding temperature is preferably 950°C or lower. The holding temperature is the maximum temperature in the reduction process. Furthermore, the holding temperature in the reduction process may be constant or may vary as long as it is within the range of 700°C or higher.
[0068] Holding time: 20 seconds or more A longer holding time in the reduction step (hereinafter also simply referred to as holding time) is more advantageous in completing the reduction of Fe oxides. Here, if the holding time is less than 20 seconds, the reduction of Fe oxides may not be completed. Therefore, the holding time is set to 20 seconds or more. The holding time is preferably 25 seconds or more. There is no particular upper limit to the holding time. However, from the viewpoint of productivity, the holding time is preferably 150 seconds or less. The holding time is the residence time in a temperature range of 700°C or higher in the reduction step.
[0069] [Soaking step] Next, the base steel sheet is held under the following conditions: atmosphere: hydrogen concentration of 0.2 vol% or more and less than 8 vol%, soaking temperature: 700°C or more and less than 900°C, soaking time: 20 s or more and 300 s or less. This reduces the amount of hydrogen that has penetrated into the base steel sheet during the reduction step, and also recrystallizes the steel structure.
[0070] Atmosphere: Hydrogen concentration of 0.2 vol% or more and less than 8 vol% In the soaking process, the hydrogen concentration is kept lower than that in the reduction process, thereby reducing the amount of hydrogen that has penetrated into the base steel sheet. Therefore, the hydrogen concentration of the atmosphere in the soaking process (hereinafter simply referred to as hydrogen concentration) is less than 8 vol%. Furthermore, the hydrogen concentration is preferably 5 vol% or less. On the other hand, if the hydrogen concentration is less than 0.2 vol%, it becomes difficult to control the uniformity inside the furnace. Furthermore, there is a risk of reoxidation of reduced Fe. Therefore, the hydrogen concentration is set to 0.2 vol% or more. The hydrogen concentration is preferably 0.5 vol% or more.
[0071] Soaking temperature: 700°C or higher but lower than 900°C. If the soaking temperature is lower than 700°C, there is a risk of reoxidation of reduced Fe. Furthermore, the recrystallization of the steel structure may be insufficient, or the volume fraction of ferrite may become excessive, making it difficult to obtain the required properties. Therefore, the soaking temperature is set to 700°C or higher. The soaking temperature is preferably set to 750°C or higher. In the method for producing a plated steel sheet according to one embodiment of the present invention, a rapid heating step (described later) is performed to obtain the desired steel structure, so the soaking temperature only needs to promote recrystallization. Furthermore, excessively increasing the soaking temperature increases the amount of austenite, which increases the amount of hydrogen in the steel. Therefore, the soaking temperature is set to lower than 900°C. The soaking temperature is preferably set to lower than 880°C. The soaking temperature is set to the maximum temperature in the soaking step. The soaking temperature may be constant or variable as long as it is within the range of 700°C or higher but lower than 900°C.
[0072] Soaking time: 20 seconds or more and 300 seconds or less If the holding time in the soaking step (hereinafter also referred to as soaking time) is less than 20 seconds, the amount of hydrogen in the steel may not be sufficiently reduced. On the other hand, if the soaking time exceeds 300 seconds, large amounts of Si oxides and Mn oxides may be formed in the surface layer of the base steel sheet, which may lead to deterioration of platability. Therefore, the soaking time is set to 20 seconds or more and 300 seconds or less. The soaking time is preferably 50 seconds or more. Furthermore, the soaking time is preferably 200 seconds or less. The soaking time is the residence time in the temperature range of 700°C or more and less than 900°C in the soaking step.
[0073] [Rapid Heating Step] Next, the base steel sheet is heated under the following conditions: atmosphere: hydrogen concentration of 0.2% by volume or more and 30% by volume or less, average heating rate from the soaking temperature: 10°C / s or more, maximum temperature: soaking temperature + 10°C or more. In this way, the base steel sheet is heated in a short time to a temperature required to obtain the desired steel sheet texture and, ultimately, the desired mechanical properties such as strength.
[0074] Atmosphere: Hydrogen concentration of 0.2 vol% or more and 30 vol% or less To prevent reoxidation of the surface of the base steel sheet, the hydrogen concentration in the atmosphere during the rapid heating process (hereinafter simply referred to as hydrogen concentration) is 0.2 vol% or more. The hydrogen concentration is preferably 0.5 vol% or more. As will be described later, in the rapid heating process, the temperature rise rate is increased to suppress hydrogen penetration into the steel. However, it is difficult to completely prevent hydrogen penetration into the steel. Therefore, the hydrogen concentration is set to 30 vol% or less. The hydrogen concentration is preferably less than 8 vol%, more preferably less than 5 vol%.
[0075] Average heating rate from the soaking temperature: 10°C / s or more. The amount of hydrogen in the steel increases with an increase in the temperature of the base steel sheet and an increase in the amount of austenite in the steel structure of the base steel sheet. In order to suppress this increase in the amount of hydrogen in the steel, it is preferable to heat the steel to a temperature necessary to obtain the desired steel structure in as short a time as possible. Therefore, the average heating rate from the soaking temperature in the rapid heating step (hereinafter also referred to as the average heating rate) is set to 10°C / s or more. The average heating rate is preferably 20°C / s or more, more preferably 30°C / s or more. The upper limit of the average heating rate is not particularly limited. However, from the viewpoint of ease of industrial implementation, the average heating rate is preferably 300°C / s or less, and more preferably 150°C / s or less.
[0076] Maximum temperature reached: soaking temperature + 10°C or more As described above, in the method for producing a plated steel sheet according to one embodiment of the present invention, the soaking temperature is set low in the soaking step to reduce hydrogen inside the base steel sheet, while the desired steel structure is obtained in the rapid heating step. Therefore, the maximum temperature reached in the rapid heating step is set to be the soaking temperature + 10°C or more. The maximum temperature reached in the rapid heating step is preferably the soaking temperature + 15°C or more, more preferably the soaking temperature + 20°C or more. There is no particular upper limit to the maximum temperature reached in the rapid heating step. However, in order to more effectively prevent deterioration of the furnace body, the maximum temperature reached in the rapid heating step is preferably 950°C or less.
[0077] After the maximum temperature is reached, it is preferable to start cooling immediately, for example, within 20 seconds.
[0078] The dew points in the reduction step, soaking step, and rapid heating step described above are not particularly limited. However, from the viewpoint of industrial ease of handling, it is preferable to set the dew point at −50° C. or higher in all steps. By setting the dew point at −50° C. or higher, the equipment costs for maintaining the atmosphere can be further reduced. Furthermore, it is preferable to set the dew point at +20° C. or lower in all steps. By setting the dew point at +20° C. or lower, it becomes easier to control the dew point inside the furnace. Furthermore, adverse effects on the furnace body can be suitably avoided.
[0079] The atmosphere (hydrogen concentration and dew point) and temperature may be different in the reduction step, the soaking step, and the rapid heating step. The control method is not particularly limited. For example, a furnace for performing each step may be divided into separate furnaces, which are connected via a seal roll. By controlling the atmosphere in each of the divided regions, the atmosphere and temperature in the reduction step, the soaking step, and the rapid heating step can be controlled within a predetermined range.
[0080] Furthermore, the method for monitoring the hydrogen concentration and dew point of the atmosphere is not particularly limited. For example, an atmosphere measurement port capable of guiding gas inside the furnace to the outside of the furnace is provided at a necessary position in each furnace. Then, the hydrogen concentration and dew point of the atmosphere are measured by connecting the atmosphere measurement port to a hydrogen concentration meter and a dew point meter. Furthermore, for example, when the reduction step, the soaking step, and the rapid heating step are each performed in separate regions of the furnace, independent atmosphere measurement ports are provided at three locations: the top, middle, and bottom of each region. Then, it is preferable to use the average values of the hydrogen concentration and dew point measured by the hydrogen concentration meter and dew point meter connected to each atmosphere measurement port as the hydrogen concentration and dew point of each step.
[0081] [Cooling step] Next, the base steel sheet is cooled under the following conditions: atmosphere: hydrogen concentration of 0.2 volume % or more and 30 volume % or less, residence time in the temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature: 20 seconds or less, cooling stop temperature: 500°C or less.
[0082] Atmosphere: Hydrogen concentration of 0.2% by volume or more and 30% by volume or less To prevent reoxidation of the surface of the base steel sheet, the hydrogen concentration in the atmosphere during the cooling process (hereinafter simply referred to as hydrogen concentration in this paragraph) is set to 0.2% by volume or more. The hydrogen concentration is preferably 0.5% by volume or more. Furthermore, the lower the hydrogen concentration, the more advantageous it is for reducing the amount of hydrogen in the steel when cooling is stopped. Therefore, the hydrogen concentration is set to 30% by volume or less. The hydrogen concentration is preferably 20% by volume or less, and more preferably less than 15% by volume.
[0083] Residence time in the temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature: 20 seconds or less As described above, in the method for producing a plated steel sheet according to one embodiment of the present invention, the soaking temperature is set low in the soaking step to reduce hydrogen inside the base steel sheet, while the desired steel structure is obtained in the rapid heating step. However, if the residence time in the temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature (hereinafter also referred to as the residence time in the high temperature region) in the cooling step exceeds 20 seconds, the above-mentioned effect may be negated. Therefore, the residence time in the high temperature region is set to 20 seconds or less. The residence time in the high temperature region is preferably 15 seconds or less, more preferably 10 seconds or less. There is no particular limitation on the lower limit of the residence time in the high temperature region. The residence time in the high temperature region may be, for example, 0.1 seconds or more.
[0084] Cooling stop temperature: 500°C or less When a coating layer is formed on the surface of the base steel sheet in the plating process described below, it becomes difficult to desorb hydrogen from the steel. Therefore, it is preferable to lower the temperature of the base steel sheet as much as possible before the plating process to reduce the hydrogen solid solubility and minimize the amount of hydrogen in the steel. Therefore, the cooling stop temperature is set to 500°C or less. There is no particular restriction on the lower limit of the cooling stop temperature, and it is sufficient as long as it is industrially feasible. For example, the cooling stop temperature may be lower than room temperature (25°C).
[0085] [Plating Step] Next, one or both sides of the base steel sheet are plated to obtain a plated steel sheet having a plating layer on one or both sides.
[0086] The type of plating layer is not particularly limited, and examples thereof include zinc-based plating (plating with a Zn content of 50% by mass or more), nickel-based plating (plating with a Ni content of 50% by mass or more), and aluminum-based plating (plating with an Al content of 50% by mass or more). The treatment method is also not particularly limited, and examples thereof include hot-dip plating, electroplating, and vapor deposition plating such as PVD and CVD. Hereinafter, as an example, a case where a hot-dip galvanizing treatment and a hot-dip galvannealing treatment are performed using CGL will be described.
[0087] In the hot-dip galvanizing process, the conditions for immersion in the hot-dip galvanizing bath are not particularly limited, and a general method may be used. The composition of the hot-dip galvanizing bath (hereinafter also referred to as the galvanizing bath composition) is not particularly limited, but generally consists of Al, Zn, and the remainder being unavoidable impurities. In one example, the Al concentration may be 0.05 mass% or more and 0.190 mass% or less. An Al concentration of 0.05 mass% or more can more effectively prevent the occurrence of bottom-dross. Furthermore, an Al concentration of 0.190 mass% or less can more effectively prevent the occurrence of top-dross. From a cost perspective, it is preferable that the Al concentration be 0.190 mass% or less. The temperature of the hot-dip galvanizing bath (hereinafter also referred to as the galvanizing bath temperature) is also not particularly limited. The galvanizing bath temperature may be 420°C or more. Alternatively, the galvanizing bath temperature may be 500°C or less.
[0088] In addition, the plating weight per side of the plating layer (hereinafter simply referred to as plating weight) is, in one example, 25 g / m 2 The plating coating weight is 25 g / m 2 If the coating weight is 80 g / m or more, the corrosion resistance is particularly good and the coating weight is particularly easy to control. 2 The plating weight is 80 g / m or less. 2 The coating adhesion is particularly good if the coating weight is below 1000 kJ / s. The method for adjusting the coating weight is not particularly limited. For example, gas wiping can be used, and the coating weight can be adjusted by adjusting the gas pressure and the distance between the wiping nozzle and the steel sheet.
[0089] In the galvannealing treatment, the above-mentioned hot dip galvanizing treatment is performed, followed by an alloying treatment. The conditions for the alloying treatment are not particularly limited. For example, the alloying treatment temperature may be 440°C or higher. The alloying treatment temperature may be 600°C or lower. The alloying treatment time may be 5 seconds or more and 60 seconds or less. The alloying treatment time is the holding time at the alloying treatment temperature.
[0090] In the galvannealed layer obtained by alloying treatment, the degree of alloying (i.e., the Fe content of the galvannealed layer, hereinafter also simply referred to as the degree of alloying) is preferably 7% by mass or more. By setting the degree of alloying to 7% by mass or more, it is possible to prevent the η phase from remaining in the galvannealed layer. Therefore, when performing the cooling-reheating treatment step described below, it is possible to more suitably reduce the amount of hydrogen in the steel. Furthermore, the degree of alloying is preferably 15% by mass or less. By setting the degree of alloying to 15% by mass or less, it is possible to more suitably prevent the formation of the Γ phase at the interface between the galvannealed layer and the base steel sheet, and to obtain more suitable coating adhesion.
[0091] [Cooling-Reheating Step] When alloyed hot-dip galvanizing treatment is carried out, it is preferable to carry out cooling-reheating according to the following conditions after the plating step, particularly after the alloying treatment.
[0092] Cooling Stop Temperature: Ms Point or Less Austenite dissolves more hydrogen than ferrite. Meanwhile, the diffusion rate of hydrogen is faster in BCC-structured ferrite and BCT-structured martensite than in FCC-structured austenite. Therefore, by transforming austenite to martensite and then performing the reheating described below, the amount of hydrogen in the steel can be more efficiently reduced. Therefore, the cooling stop temperature (after alloying treatment) is preferably Ms point or less. Furthermore, the greater the degree of undercooling relative to the Ms point, the more accelerated the martensitic transformation. This allows the reheating described below to be performed with less untransformed austenite, which is advantageous for reducing the amount of hydrogen in the steel. Therefore, the cooling stop temperature is preferably (Ms point - 50°C) or less, and even more preferably (Ms point - 100°C) or less. The lower limit of the cooling stop temperature is not particularly limited. However, a cooling stop temperature below 20°C requires a high heat removal capacity in the cooling zone, resulting in increased costs. Therefore, the cooling stop temperature is preferably 20°C or higher.
[0093] Here, the Ms point is calculated as follows: Ms (°C) = 539 - 423 x {[C%] x 100 / (100 - [α area %])} - 30 x [Mn%] - 12 x [Cr%] - 18 x [Ni%] - 8 x [Mo%], where [C%], [Mn%], [Cr%], [Ni%], and [Mo%] are the C content, Mn content, Cr content, Ni content, and Mo content (all in mass%) in the chemical composition of the substrate steel sheet (base steel sheet) of the plated steel sheet, respectively. Furthermore, [α area %] is the area fraction (%) of ferrite in the steel structure of the substrate steel sheet of the plated steel sheet. The area fraction of ferrite in the steel structure of the substrate steel sheet of the plated steel sheet is measured, for example, as follows. That is, the plating layer on the surface of the plated steel sheet is removed. Next, a sample is cut out from the substrate steel sheet of the plated steel sheet so that the observation surface is a thickness cross section (L cross section) parallel to the rolling direction of the substrate steel sheet (base steel sheet). The observation surface of the sample is then polished. The observation surface of the sample is then corroded with 1 vol. % nital to reveal the steel structure. Ten fields of view are then observed at a 1 / 4 thickness position of the substrate steel sheet of the plated steel sheet (a position corresponding to 1 / 4 of the thickness in the depth direction from the surface of the base steel sheet) at a magnification of 3000x using an SEM. In the observed images, ferrite is a structure in which the interior is flat and does not contain carbides. The area of the region occupied by ferrite is then determined for each field of view. The total area of the regions occupied by ferrite is then divided by the total area of the observation fields, and the result multiplied by 100 is used as the area ratio of ferrite in the steel structure of the substrate steel sheet of the plated steel sheet. The measurement may be carried out immediately before the cooling-reheating step, that is, after the alloying treatment in the plating treatment step, on a plated steel sheet that has been rapidly cooled to a temperature of 200°C or less by water quenching or the like at an average cooling rate of 50°C / s or more in the temperature range of 200 to 600°C. In addition, the measurement is preferably carried out in advance, for example, separately from the series of steps.
[0094] Next, the plated steel sheet (galvannealed steel sheet) is preferably reheated under the following conditions: atmosphere: hydrogen concentration 0.2% by volume or less; reheating temperature: 100°C or higher and 450°C or lower; and reheating time: 5 seconds or longer.
[0095] Atmosphere: Hydrogen concentration of 0.2% by volume or less From the viewpoint of promoting the release of diffusible hydrogen in steel during reheating, it is advantageous to lower the hydrogen concentration of the atmosphere (hereinafter simply referred to as hydrogen concentration in this paragraph). Therefore, the hydrogen concentration is preferably 0.2% by volume or less, and more preferably 0.1% by volume or less. The lower limit of the hydrogen concentration is not particularly limited. However, hydrogen is unavoidably contained in the atmosphere. Therefore, the hydrogen concentration can be, for example, 0.00001% by volume or more. The hydrogen (H 2 The remaining gas other than the above is not particularly limited. For example, the remaining gas is N 2 , O 2 , H 2 O, CO 2、 Ar and unavoidable impurities, and combinations thereof. The ratio of these is not particularly limited.
[0096] Reheating temperature: 100°C or higher and 450°C or lower In order to fully achieve the effect of reducing the amount of hydrogen in the steel, the reheating temperature is preferably 100°C or higher. On the other hand, if the reheating temperature exceeds 450°C, there is a risk of deterioration in the coating appearance. Therefore, the reheating temperature is preferably 100°C or higher and 450°C or lower. However, the reheating temperature is preferably equal to or higher than the cooling stop temperature after the alloying treatment. Furthermore, the reheating temperature is more preferably 120°C or higher. The reheating temperature is more preferably 430°C or lower. Here, the reheating temperature is the maximum temperature reached during reheating. Furthermore, the temperature during reheating may be constant or may vary as long as it is within the range of 100°C or higher and 450°C or lower.
[0097] Reheating time: 5 seconds or more If the reheating time is less than 5 seconds, the effect of reducing the hydrogen concentration in the steel may not be sufficiently obtained. Therefore, the reheating time is preferably 5 seconds or more. The reheating time is more preferably 10 seconds or more, and even more preferably 30 seconds or more. The upper limit of the reheating time is not particularly limited. However, from the viewpoint of productivity, the reheating time is preferably 300 seconds or less. The reheating time is the holding time at a temperature equal to or higher than the cooling stop temperature after the alloying treatment and in a temperature range of 100°C to 450°C.
[0098] Conditions other than those mentioned above are not particularly limited, and may be carried out in accordance with conventional methods.
[0099] According to the method for producing a plated steel sheet according to one embodiment of the present invention, a plated steel sheet having a tensile strength of preferably 340 MPa or more, more preferably 500 MPa or more, and even more preferably 980 MPa or more can be obtained. Here, the tensile strength is measured in accordance with JIS Z 2241. For example, a JIS No. 5 test piece is taken from the plated steel sheet so that the longitudinal direction is perpendicular to the rolling direction of the plated steel sheet (base steel sheet). Next, using the test piece, a crosshead displacement speed Vc of 1.67 × 10 -1 A tensile test is carried out under the condition of 1 / 2 mm / s to measure the tensile strength.
[0100] Furthermore, according to the method for producing a plated steel sheet according to one embodiment of the present invention, a plated steel sheet having a reduced amount of diffusible hydrogen can be obtained. In particular, a plated steel sheet having a diffusible hydrogen amount of preferably 0.30 ppm by mass (wt. ppm) or less, more preferably 0.20 ppm by weight or less can be obtained. There is no particular lower limit for the amount of diffusible hydrogen. The amount of diffusible hydrogen can be, for example, 0.01 ppm by weight or more.
[0101] Here, the amount of diffusible hydrogen is measured as follows: A 5 mm x 30 mm test piece is cut out from a plated steel sheet, and the plating layer on the surface of the test piece is removed using a router (precision grinder). Next, using a thermal desorption analyzer, hydrogen analysis is performed under the following conditions: analysis start temperature: 25°C, analysis end temperature: 300°C, and temperature rise rate: 200°C / hr, and the amount of hydrogen released from the test piece is measured. The cumulative value of the amount of hydrogen released from the test piece in the temperature range from the analysis start temperature to 210°C is then taken as the amount of diffusible hydrogen.
[0102] Furthermore, according to the method for producing a plated steel sheet according to one embodiment of the present invention, a plated steel sheet that combines excellent plateability and excellent hydrogen embrittlement resistance can be obtained. Here, excellent plateability means that the appearance and adhesion evaluations are both ranked 1 or 2 in the plateability evaluations in the Examples described below. Furthermore, excellent hydrogen embrittlement resistance means that the hydrogen embrittlement resistance is ranked 1 or 2 in the hydrogen embrittlement resistance evaluations in the Examples described below.
[0103] A cold-rolled steel sheet having a thickness of 1.4 mm and the chemical composition shown in Table 1 (the balance being Fe and unavoidable impurities) was prepared as a base steel sheet. Next, using the prepared base steel sheet, a plated steel sheet was manufactured under the conditions shown in Tables 2 and 3 and below. Note that the cooling stop temperature in the column for the cooling-reheating step in Tables 2 and 3 when no alloying treatment was performed is the cooling stop temperature after the hot-dip galvanizing treatment. - Plating bath composition: 0.13 mass% Al, balance being Zn and unavoidable impurities - Plating bath temperature: 460°C - Coating weight: 40 to 60 g / m 2 - Alloying degree: 8.0 to 14.0 mass% - Hydrogen concentration in the reheating atmosphere in the cooling-reheating process: 0.1 vol% In the production of the plated steel sheets, a CGL was used in which the upstream and downstream uniforming zones were connected by seal rolls. Conditions other than those mentioned above were in accordance with the general description section of the specification or conventional methods.
[0104] The tensile strength (TS) and diffusible hydrogen content of the plated steel sheets thus obtained were measured in the same manner as described above. The diffusible hydrogen content was evaluated according to the following criteria. The evaluation results are shown in Tables 2 and 3. Rank 1 (pass, particularly excellent): Diffusible hydrogen content of 0.10 wt. ppm or less Rank 2 (pass, excellent): Diffusible hydrogen content of more than 0.10 wt. ppm and less than 0.20 wt. ppm Rank 3 (pass): Diffusible hydrogen content of more than 0.20 wt. ppm and less than 0.30 wt. ppm Rank 4 (fail): Diffusible hydrogen content of more than 0.30 wt. ppm
[0105] The plateability and hydrogen embrittlement resistance of the plated steel sheets were evaluated in the same manner as described above. The evaluation results are shown in Tables 2 and 3.
[0106] <Platability> The "appearance evaluation" and "adhesion" of plated steel sheets were evaluated by the following methods, and the platability was evaluated as follows based on each evaluation result. Ranks 1 and 2 were considered to be acceptable. Rank 1 (pass, excellent): "Appearance evaluation" and "adhesion" were both ranked 1 Rank 2 (pass): "Either appearance evaluation" or "adhesion", or both, were ranked 1 or 2 (excluding cases where both "appearance evaluation" and "adhesion" were ranked 1) Rank 3 (fail): "Either appearance evaluation" or "adhesion", or both, were ranked 3
[0107] Appearance evaluation The surface of the plated steel sheet (plating layer) was visually observed and evaluated according to the following criteria. Ranks 1 and 2 were considered acceptable. Rank 1: No bare spots or uneven appearance Rank 2: No bare spots but uneven appearance Rank 3: Bare spots present
[0108] Adhesion Evaluation [Ball Impact Test] When the plated steel sheet was a hot-dip galvanized steel sheet (GI, a steel sheet manufactured using hot-dip galvanizing as the plating treatment), the plating adhesion was evaluated by a ball impact test. Note that, when the plated steel sheet was a type other than a galvannealed steel sheet (described later), such as an electrogalvanized steel sheet (EG, a steel sheet manufactured using electrogalvanizing as the plating treatment), the plating adhesion may also be evaluated by the ball impact test. Specifically, a ball was dropped under the following conditions: ball mass: 1.8 kg, drop height: 100 cm, and the ball was allowed to collide with the plated steel sheet. The ball impacted portion of the plated steel sheet was then peeled off with Cellophane Tape (registered trademark; the same applies hereinafter). The presence or absence of peeling of the plating layer was visually confirmed and evaluated according to the following criteria. Ranks 1 and 2 were considered acceptable. Rank 1: No peeling of the plating layer Rank 2: Minor peeling of the plating layer Rank 3: Not minor peeling of the plating layer Note that when the ratio of the area of the peeled portion of the plating layer to the total area of the steel sheet deformed by the impact of the ball (hereinafter also referred to as the peeling area ratio) was less than 20%, it was rated as "minor peeling," and when the peeling area ratio was 20% or more, it was rated as "not minor peeling."
[0109] [Powdering Test] When the plated steel sheet was a galvannealed steel sheet (GA, a steel sheet manufactured by galvannealing), the coating adhesion was evaluated by a powdering test. Specifically, a plated steel sheet (length (rolling direction): 80 mm, width: 40 mm) was bent and unbent at 90 degrees so that the bending ridgeline was perpendicular to the rolling direction. Next, a 24 mm-wide cellophane tape was attached to the inside of the bent portion (compression side) of the plated steel sheet parallel to the bending ridgeline (aligning the bending ridgeline with the width center of the cellophane tape). The tape was pressed against the steel sheet surface so that the adhesive surface was in close contact with the steel sheet surface, and then removed. The amount of zinc adhering to a 40 mm-long portion of the peeled cellophane tape was measured as a Zn count using fluorescent X-rays. The measurement conditions were a measurement diameter of 30 mm, a fluorescent X-ray acceleration voltage of 50 kV, an acceleration current of 50 mA, and a measurement time of 20 seconds. Next, the measured Zn count was converted to a value per unit length (1 m), and the converted value (hereinafter also referred to as the fluorescent X-ray count) was evaluated according to the following criteria. Ranks 1 and 2 were deemed acceptable. Rank 1: Fluorescent X-ray count of 0 or more to less than 8,000 Rank 2: Fluorescent X-ray count of 8,000 or more to less than 15,000 Rank 3: Fluorescent X-ray count of 15,000 or more
[0110] <Hydrogen Embrittlement Resistance> Hydrogen embrittlement resistance was evaluated based on the occurrence of cracks during resistance spot welding. Specifically, two 30 mm × 100 mm test pieces were cut from the resulting plated steel sheet. Next, a 2 mm-thick spacer (30 mm × 30 mm) was placed on one of the test pieces so that the spacer spacing was 40 mm (the end of the spacer was aligned with the end of the test piece), and the test piece and the spacer were fixed by welding. Then, another test piece was placed on top of the first test piece, and the test piece and the spacer were fixed by welding. In this way, the spacer was sandwiched between the two test pieces. The centers of the test pieces were then spot-welded to prepare welded test pieces. Here, welded test pieces were prepared so that the nugget diameter was 3.8 mm when the tensile strength of the plated steel sheet was less than 1250 MPa, and 4.8 mm when the tensile strength of the plated steel sheet was 1250 MPa or greater. For the spot welding, an inverter DC resistance spot welding machine was used, and a dome-shaped electrode made of chromium copper and with a tip diameter of 6 mm was used. The pressure was 380 kgf, the current application time was 16 cycles / 50 Hz, and the holding time (the time during which the pressure was applied without current application after the end of current application) was 5 cycles / 50 Hz. The welding current value was set to the condition required to form the above-mentioned nugget diameter. After welding, the welded test piece was left in an atmospheric environment for 24 hours, and then the spacer portion was cut off from the welded test piece. Next, the cross section of the nugget was observed using an optical microscope (magnification: 100x), and the hydrogen embrittlement resistance was evaluated according to the following criteria. Rank 1 (pass, excellent): No cracks occurred. Rank 2 (pass): Only microcracks with a length of 100 μm or less occurred. Rank 3 (fail): Cracks with a length of more than 100 μm occurred.
[0111]
[0112]
[0113]
[0114] As shown in Table 3, in all of the inventive examples, plated steel sheets that achieved both excellent galvanizability and excellent hydrogen embrittlement resistance were produced, even when steel sheets having chemical compositions containing large amounts of easily oxidizable elements Si and Mn in order to increase strength were used as base steel sheets. On the other hand, in the comparative examples, at least one of the galvanizability and hydrogen embrittlement resistance was unacceptable.
Claims
1. A base steel sheet having a composition containing, by mass, Si: 0.10% to 2.00% and Mn: 1.00% to 5.00% is heated under the following conditions: an oxidation process, in which an oxygen concentration of 1000 ppm by volume to 30000 ppm by volume is heated at a heating temperature of 600°C or higher; and then a reduction process, in which the base steel sheet is held under the following conditions: an atmosphere with a hydrogen concentration of 8% by volume to 30% by volume, a holding temperature of 700°C or higher, and a holding time of 20 seconds or longer; and then a soaking process, in which the base steel sheet is held under the following conditions: an atmosphere with a hydrogen concentration of 0.2% by volume to less than 8% by volume, a soaking temperature of 700°C to less than 900°C, and a soaking time of 20 seconds to 300 seconds; and then a reduction process, in which the base steel sheet is held under the following conditions: an atmosphere with a hydrogen concentration of 0.2% by volume to less than 8% by volume, a soaking temperature of 700°C to less than 900°C, and a soaking time of 20 seconds to 300 seconds. a rapid heating step of heating the base steel sheet under the following conditions: an atmosphere having a hydrogen concentration of 0.2 volume % or more and 30 volume % or less; an average heating rate from the soaking temperature of 10°C / s or more; and a maximum temperature reached of 10°C or more above the soaking temperature; and a cooling step of cooling the base steel sheet under the following conditions: an atmosphere having a hydrogen concentration of 0.2 volume % or more and 30 volume % or less; a residence time in a temperature range from the maximum temperature reached in the rapid heating step to the soaking temperature of 20 s or less; and a cooling stop temperature of 500°C or less. and a plating step of plating one or both sides of the base steel sheet to obtain a plated steel sheet.
2. The method for producing a plated steel sheet according to claim 1, which satisfies at least one of the following (1) to (3): (1) An atmosphere in the soaking step: a hydrogen concentration of 0.2 volume % or more and 5 volume % or less (2) An atmosphere in the rapid heating step: a hydrogen concentration of 0.2 volume % or more and less than 8 volume % (3) An atmosphere in the cooling step: a hydrogen concentration of 0.5 volume % or more and 20 volume % or less 3. A method for producing plated steel sheet as described in claim 1 or 2, wherein the chemical composition further contains, in mass %, C: 0.05% or more and 0.40% or less, P: 0.100% or less, S: 0.0200% or less, Al: 0.003% or more and 2.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.
4. The composition further includes, in mass%, B: 0.0100% or less, Ti: 0.200% or less, Nb: 0.200% or less, Sb: 0.200% or less, Sn: 0.200% or less, V: 0.100% or less, Cu: 1.00% or less, Cr: 1.00% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ta: 0.100% or less, W: 0.500% or less, Zr: 0.020% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, Zn: 0.020% or less, Co: 0.020% or less, Ce: 0.0200% or less, Se: 0.0200% or less, The method for producing a plated steel sheet according to claim 3, containing at least one selected from the group consisting of Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0200% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less.
5. The method for producing plated steel sheet according to claim 1 or 2, wherein the plating treatment is a hot-dip galvanizing treatment or a hot-dip galvannealing treatment.
6. The method for producing plated steel sheet according to claim 3, wherein the plating treatment is a hot-dip galvanizing treatment or a hot-dip galvannealing treatment.
7. The method for producing plated steel sheet according to claim 4, wherein the plating treatment is a hot-dip galvanizing treatment or a hot-dip galvannealing treatment.
8. A method for producing a plated steel sheet according to claim 1 or 2, wherein the plating treatment is a galvannealed hot-dip plating treatment, and further comprising, after the plating treatment step, a cooling-reheating step of cooling the plated steel sheet under the conditions of a cooling stop temperature of Ms point or lower, and then reheating the plated steel sheet under the conditions of an atmosphere of hydrogen concentration of 0.2 volume % or less, a reheating temperature of 100° C. or higher and 450° C. or lower, and a reheating time of 5 s or longer.
9. A method for producing a plated steel sheet according to claim 3, wherein the plating treatment is a galvannealed hot-dip plating treatment, and further comprising, after the plating treatment step, a cooling-reheating step of cooling the plated steel sheet under the conditions of a cooling stop temperature of Ms point or lower, and then reheating the plated steel sheet under the conditions of an atmosphere of hydrogen concentration of 0.2 volume % or less, a reheating temperature of 100° C. or higher and 450° C. or lower, and a reheating time of 5 s or longer.
10. A method for producing a plated steel sheet according to claim 4, wherein the plating treatment is a galvannealed hot-dip plating treatment, and further comprising, after the plating treatment step, a cooling-reheating step of cooling the plated steel sheet under the conditions of a cooling stop temperature of Ms point or lower, and then reheating the plated steel sheet under the conditions of an atmosphere of hydrogen concentration of 0.2 volume % or less, a reheating temperature of 100° C. or higher and 450° C. or lower, and a reheating time of 5 s or longer.
11. The method for producing a plated steel sheet according to claim 8, wherein the cooling stop temperature in the cooling-reheating step is (Ms point - 50°C) or lower.
12. The method for producing a plated steel sheet according to claim 9, wherein the cooling stop temperature in the cooling-reheating step is (Ms point - 50°C) or lower.
13. The method for producing a plated steel sheet according to claim 10, wherein the cooling stop temperature in the cooling-reheating step is (Ms point - 50°C) or lower.
Citation Information
Patent Citations
Method for producing hot dip galvannealed steel sheet having excellent plating adhesion and sliding property
JP2012149307A
Method for manufacturing steel sheet products with a metal protective layer formed by hot-dip plating.
JP2014525986A
Alloyed hot-dip galvanized steel sheet and method for manufacturing same
WO2014073520A1
Galvanized steel sheet and production method therefor
WO2019212045A1
Method for producing high-strength hot dipped galvanized steel sheet
WO2021166350A1