Road repairing material
The road repair material, comprising asphalt, aggregate, and a fatty acid-based softening agent, addresses VOC emission and usability issues by hardening under pressure, allowing for room-temperature application and extended usability, improving workability and physical properties without high-temperature mixing.
Patent Information
- Application Number
- PCT/JP2023/046427
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional road repair materials face issues such as VOC emission, requirement of water for application, and limited usability after package opening due to moisture absorption and hardening, necessitating immediate use and high-temperature mixing processes.
A road repair material composed of asphalt, aggregate, and a fatty acid-based softening agent, which can be applied at room temperature, reduces VOC emission and remains usable after package opening, utilizing a polymer-modified asphalt emulsion with a specific fatty acid compound and minimal cement content, allowing for mixing at lower temperatures.
The material hardens under pressure, reducing VOC concentration and maintaining usability over time, improving workability and physical properties while eliminating the need for immediate use and high-temperature mixing, thus enhancing construction flexibility and reducing environmental impact.
Smart Images

Figure JP2023046427_03102024_PF_FP_ABST
Abstract
Description
Road repair materials
[0001] The present invention relates to a road repair material for application at room temperature.
[0002] Asphalt mixtures containing cutback materials such as mineral oil are known as road repair materials for repairing potholes and other defects in asphalt roads. It is known that the strength of these asphalt mixtures increases as the cutback materials volatilize.
[0003] Furthermore, asphalt mixtures containing cement as described in Patent Documents 1 and 2 are also known as road repair materials, and these asphalt mixtures can be hardened by adding water.
[0004] These road repair materials can be applied at room temperature, but are heated to high temperatures and mixed during production. Patent Document 3 discloses an asphalt pavement regeneration device, and while this regeneration device does not require heating and mixing the asphalt mixture, Patent Document 3 does not relate to road repair materials for repairing potholes, etc.
[0005] JP 2010-248472 A JP 2020-66980 A JP 2000-317434 A
[0006] Asphalt mixtures containing cutback materials such as mineral oil have the problem of generating volatile organic compounds (VOCs). Furthermore, once a bagged asphalt mixture is opened, it must be used up, and if it is not used up, it must be discarded.
[0007] The road repair materials described in Patent Documents 1 and 2 have the problem that they require water when used. While water is not required for normal road repair work, water must be prepared separately in order to use these road repair materials, which can be problematic in construction. Furthermore, these road repair materials also absorb moisture and begin to harden after opening, so they must be used within the same day after opening.
[0008] The present invention aims to provide a new road repair material that can be applied at room temperature, generates substantially no VOCs, and can be used even after a long time has passed since it was opened, and a method for producing the same.
[0009] The present inventors have found that the above-mentioned problems can be solved by the present invention having the following aspects. Aspect 1: A road repair material comprising asphalt, aggregate, and a softening agent, wherein the softening agent comprises a fatty acid-based compound. Aspect 2: The road repair material according to Aspect 1, wherein the asphalt is a polymer-modified asphalt. Aspect 3: The road repair material according to Aspect 1, wherein the asphalt is contained as an asphalt emulsion. Aspect 4: The road repair material according to Aspect 3, wherein the asphalt emulsion comprises polymer-modified asphalt. Aspect 5: The road repair material according to Aspect 1, wherein the content of recycled asphalt concrete aggregate is less than 20% by mass. Aspect 6: The road repair material according to Aspect 1, wherein the content of cement is less than 20% by mass. Aspect 7: The road repair material according to Aspect 1, wherein the softening agent comprises a fatty acid-based compound represented by the following general formula (1). R 1 -CO-(AO)m-OR 2 ...General formula (1) (wherein, R 1 represents a linear or branched hydrocarbon group having 15 to 19 carbon atoms, and R 2 represents hydrogen or a linear or branched hydrocarbon group having 1 to 18 carbon atoms. AO represents a linear or branched alkylene oxide unit having 2 to 4 carbon atoms, and m represents the average number of moles added and is a number from 0 to 30.) Aspect 8 The road repair material according to Aspect 1, wherein the iodine value of the fatty acid compound is 50 to 110. Aspect 9 The road repair material according to Aspect 1, wherein the softener is contained in an amount of 10 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the asphalt. Aspect 10 A method for producing the road repair material according to any one of Aspects 1 to 9, comprising mixing the asphalt, the aggregate, and the softener. Aspect 11 A method for producing the road repair material according to Aspect 10, wherein the mixing is performed at a temperature of 100°C or less. Aspect 12 A method for producing the road repair material according to Aspect 10, wherein the asphalt and the softener are mixed together and then aggregate is mixed.
[0010] According to the present invention, it is possible to provide a new road repair material that can be applied at room temperature, generates substantially no VOCs, and can be used even after a long time has passed since opening, and a method for producing the same.
[0011] Fig. 1 is a diagram illustrating a penetration resistance test performed in the examples. Fig. 2 is a diagram illustrating a flow test performed in the examples.
[0012] <Road Repair Material> The road repair material of the present invention is a road repair material containing asphalt, aggregate, and a softening agent, and the softening agent contains a fatty acid-based compound.
[0013] The inventors discovered that this road repair material hardens under pressure. Unlike conventional repair materials, this road repair material does not require waiting for the cutback material to volatilize. Instead, it can be used immediately by spreading it over potholes on asphalt roads, temporarily compacting it with a shovel, and then compacting it with a vehicle or plate. Without being bound by theory, it is believed that applying pressure to a road repair material containing asphalt, aggregate, and softener improves the interlocking of the aggregate, increasing the contact area between the aggregates and separating the softener from the asphalt, allowing it to harden quickly. Furthermore, because the road repair material of the present invention does not harden until a large amount of pressure is applied, it has been found that it can remain usable even after opening.
[0014] The road repair material of the present invention may have a VOC concentration of 100 mg / L or less, 50 mg / L or less, 30 mg / L or less, 20 mg / L or less, 10 mg / L or less, or 5 mg / L or less when measured at 20°C in accordance with JIS K0125.
[0015] <Asphalt> The road repair material of the present invention contains asphalt.
[0016] As the asphalt, various types of asphalt can be used. For example, in addition to straight asphalt, which is petroleum asphalt for paving, modified asphalt can be mentioned. Modified asphalt includes blown asphalt, polymer-modified asphalt modified with polymer materials such as thermoplastic elastomers and thermoplastic resins, and the like. The asphalt is preferably contained as an asphalt emulsion. Furthermore, it is more preferable that the asphalt emulsion contains polymer-modified asphalt.
[0017] The asphalt preferably contains a thermoplastic elastomer. Examples of such asphalt compositions include straight asphalt (modified asphalt) modified with a thermoplastic elastomer.
[0018] The thermoplastic elastomer used in modified asphalt may be any thermoplastic elastomer commonly used in this field, including, for example, one or more of styrene / butadiene block copolymer, styrene / butadiene / styrene block copolymer, styrene / butadiene random copolymer, styrene / isoprene block copolymer, styrene / isoprene / styrene block copolymer, styrene / isoprene random copolymer, ethylene / vinyl acetate copolymer, ethylene / acrylic acid ester copolymer, etc. Among these, it is particularly preferable to use styrene / butadiene random copolymer and styrene / butadiene / styrene block copolymer.
[0019] The content of the thermoplastic elastomer in the modified asphalt may be 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 2% by mass or more, 3% by mass or more, 5% by mass or more, or 10% by mass or more, relative to the total amount of the modified asphalt, and may be 30% by mass or less, 20% by mass or less, 10% by mass or less, 5% by mass or less, 3% by mass or less, or 2% by mass or less.
[0020] The content of asphalt or straight asphalt in the modified asphalt may be 70% by mass or more, 80% by mass or more, 85% by mass or more, 90% by mass or more, 95% by mass or more, or 97% by mass or more, relative to the total amount of the modified asphalt, and may be 99.5% by mass or less, 99% by mass or less, 98% by mass or less, 97% by mass or less, 95% by mass or less, or 90% by mass or less.
[0021] The asphalt content in the road repair material of the present invention may be 2.0% by mass or more, 3.0% by mass or more, 4.0% by mass or more, or 5.0% by mass or more, or may be 20% by mass or less, 15% by mass or less, 10% by mass or less, 8.0% by mass or less, 5.0% by mass or less, or 4.0% by mass or less.
[0022] <Aggregate> The road repair material of the present invention contains aggregate. Aggregates commonly used in this field can be used. For example, recycled aggregate or recycled asphalt concrete aggregate may be used as the aggregate. These recycled aggregates may account for 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, or 40% by mass or more of the total aggregate, and may be 100% by mass or less, 90% by mass or less, 80% by mass or less, 70% by mass or less, or 60% by mass or less. These recycled aggregates may not be used substantially, for example, less than 20% by mass, 10% by mass or less, 5% by mass or less, or none at all in the total road repair material.
[0023] The road repair material of the present invention preferably uses coarse aggregate and / or fine aggregate as aggregate. Coarse aggregate with a particle size of 2.36 mm or more and fine aggregate with a particle size of less than 2.36 mm can be used by selecting the particle size, blending ratio, etc. from the viewpoints of interlocking of the coarse aggregates and fluidity.
[0024] Examples of coarse aggregate include No. 7 crushed stone with a particle size range of 2.36 mm or more and less than 4.75 mm, No. 6 crushed stone with a particle size range of 4.75 mm or more and less than 13.2 mm, No. 5 crushed stone with a particle size range of 13.2 mm or more and less than 19 mm, and No. 4 crushed stone with a particle size range of 19 mm or more and less than 31.5 mm. Of these, it is particularly preferable to use coarse aggregate with a particle size range of 2.36 mm or more and less than 4.75 mm.
[0025] Examples of fine aggregates include fine aggregates of less than 2.36 mm, such as river sand, dune sand, mountain sand, sea sand, crushed sand, fine sand, screenings, crushed stone dust, silica sand, artificial sand, glass cullet, and foundry sand.
[0026] The particle sizes of the coarse aggregate and fine aggregate are the values specified in JIS A5001-2008.
[0027] The aggregate content in the road repair material of the present invention may be 70% by mass or more, 75% by mass or more, 80% by mass or more, 85% by mass or more, or 90% by mass or more, or may be 97% by mass or less, 95% by mass or less, 93% by mass or less, 90% by mass or less, or 85% by mass or less.
[0028] <Softener> The road repair material of the present invention may contain a fatty acid compound as a softener, which makes the road repair material of the present invention substantially free from VOC emissions and allows it to be used even after a long time has passed since it was opened.
[0029] As the fatty acid compound, for example, a fatty acid compound having an iodine value of 50 to 110 can be used. The softener may be a combination of multiple fatty acid compounds, in which case the iodine value refers to the value of the fatty acid compound in which multiple compounds are combined. The iodine value of the fatty acid compound is the iodine value measured in accordance with JIS K0070-1992.
[0030] The fatty acid compound is preferably a compound represented by the following general formula (1): 1 -CO-(AO)m-OR 2 ...General formula (1) (wherein, R 1 represents a linear or branched hydrocarbon group having 15 to 19 carbon atoms, and R 2 represents hydrogen or a linear or branched hydrocarbon group having 1 to 18 carbon atoms; AO represents a linear or branched alkylene oxide unit having 2 to 4 carbon atoms; and m represents the average number of moles added and is a number from 0 to 30.
[0031] The fatty acid compound represented by general formula (1) is preferably a fatty acid, a fatty acid alkyl ester, a fatty acid polyoxyalkylene alkyl ester, or a polyoxyalkylene fatty acid ester, and these can be used alone or in combination of two or more selected from these.
[0032] The molecular weight (g / mol) of the fatty acid compound may be, for example, 100 or more, 150 or more, 200 or more, 250 or more, 270 or more, or 280 or more, or 500 or less, 450 or less, 400 or less, 350 or less, 330 or less, or 320 or less. When a fatty acid compound is used in combination with a plurality of compounds, the molecular weights thereof may be weight-average molecular weights.
[0033] Here, R 1 is preferably a linear or branched alkyl group having 15 to 17 carbon atoms and a linear or branched alkenyl group having 15 to 17 carbon atoms. 2 is preferably hydrogen or a methyl group. AO is preferably an ethylene oxide unit. m is preferably 0 to 15. This is because the workability of the produced road repair material is improved. In order to improve workability, the iodine value of the fatty acid compound is preferably 60 to 100 (g / 100 mg), and more preferably 70 to 85 (g / 100 mg). In the present invention, the term "alkenyl group" refers to a hydrocarbon group containing 1 to 3 double bonds.
[0034] The fatty acid compound (b) represented by the general formula (1) includes fatty acids: R 1 COOH, fatty acid methyl ester: R 1 COOCH 3 , fatty acid (poly)oxyethylene methyl ester: R 1 COO (CH 2 CH 2 O) m CH 3 , (poly)oxyethylene fatty acid ester: R 1 COO (CH 2 CH 2 O) mSpecific examples include palmitic acid, palmitic acid methyl ester, palmitic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene palmitic acid ester (average number of moles added: 1 to 15), stearic acid, stearic acid methyl ester, stearic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene stearate ester (average number of moles added: 1 to 15), oleic acid, oleic acid methyl ester, oleic acid (poly)oxyethylene methyl oleic acid esters (average number of moles added: 1 to 15), (poly)oxyethylene oleic acid esters (average number of moles added: 1 to 15), linoleic acid, linoleic acid methyl ester, linoleic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene linoleic acid esters (average number of moles added: 1 to 15), linolenic acid, linolenic acid methyl ester, linolenic acid (poly)oxyethylene methyl ester (average number of moles added: 1 to 15), (poly)oxyethylene linolenic acid esters (average number of moles added: 1 to 15).
[0035] Among these, it is preferable to use a fatty acid methyl ester mixture containing 75 to 95 mass% of oleic acid methyl ester and having an iodine value of 50 to 110 (g / 100 mg) or a polyoxyethylene fatty acid ester having 16 to 18 carbon atoms (average number of added moles: 3 to 15), because this improves the workability of the road repair material produced.
[0036] The content of the softener in the road repair material of the present invention may be 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, or 40 parts by mass or more, per 100 parts by mass of asphalt, or may be 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less.
[0037] The content of the softener in the road repair material of the present invention may be 0.1 mass% or more, 0.3 mass% or more, 0.5 mass% or more, 0.8 mass% or more, or 1.0 mass% or more, and may be 10 mass% or less, 5.0 mass% or less, 3.0 mass% or less, 2.0 mass% or less, 1.5 mass% or less, or 1.0 mass% or less.
[0038] <Others> It is preferable that the road repair material of the present invention is substantially free of cement. For example, it is preferable that the cement content of the entire road repair material is less than 20% by mass, 10% by mass or less, 5% by mass or less, or that no cement is contained at all.
[0039] <<Method for Manufacturing Road Repair Material>> The method for manufacturing a road repair material of the present invention includes mixing asphalt, aggregate, and a softener. Here, for each component of the method for manufacturing a road repair material of the present invention, reference can be made to each component described for the road repair material of the present invention. In other words, for the types and blending amounts of asphalt, aggregate, softener, etc., reference can be made to the types and contents described above.
[0040] The method for producing a road repair material of the present invention can include a step of mixing asphalt and aggregate to obtain a first mixture, and a step of adding a softener to the first mixture and mixing it to obtain a road repair material. Here, during each mixing, the mixture can be heated to approximately 150°C to 180°C and mixed, but can be cooled to a certain temperature before packaging the road repair material. Furthermore, it is preferable that the first mixture is in a state in which the aggregate is substantially coated with asphalt.
[0041] The road repair material of the present invention is advantageous because it allows the softener to be mixed into the asphalt mixture while it is still hot after production. That is, with conventional road repair materials that use mineral oil, the mineral oil would ignite if the asphalt mixture was still hot after production, so it was necessary to cool it before mixing the mineral oil, but the road repair material of the present invention does not require such cooling and reheating steps.
[0042] The method for manufacturing road repair material of the present invention can include, depending on the type of softener, a step of heating the softener to about 20°C as necessary before adding the softener in order to prevent the softener from freezing and improve its mixability.
[0043] In the method for producing a road repair material of the present invention, the above-mentioned mixing step can also be carried out at a temperature of 100°C or less. In road repair materials of the prior art, when asphalt and aggregate are mixed at a temperature of 100°C or less, the viscosity of the asphalt becomes too high, making it difficult to achieve a homogeneous mixture. However, in the production method of the present invention, the softener can reduce the viscosity of the asphalt to a level that allows homogeneous mixing of the asphalt and aggregate at a temperature of 100°C or less. Therefore, in the production method of the present invention, there is no need to mix the asphalt and aggregate at a high temperature exceeding 100°C, and carbon dioxide emissions can be reduced.
[0044] The mixing of asphalt, aggregate, and softener may be carried out at 100°C or less, 80°C or less, 60°C or less, or 30°C or less, or at 0°C or more, 10°C or more, 20°C or more, 30°C or more, or 50°C or more.
[0045] When mixing asphalt, aggregate, and softener, it is preferable to first mix the asphalt with the softener to reduce the viscosity of the asphalt, and then mix the aggregate in. This makes it easy to obtain a homogeneous road repair material.
[0046] The present invention will be explained in more detail in the following examples, but the present invention is not limited thereto.
[0047] <Production Example> As aggregates, aggregates 1 and 2 having particle size distributions as shown in the table below were used.
[0048] The following seven types of softeners were used.
[0049] The above aggregate 1 was mixed with asphalt and softener 1 at approximately 160°C so that the content of asphalt and softener 1 in the road repair material was 5.7% by mass, thereby obtaining the road repair material of Example 1. Here, polymer-modified asphalt type II (Nichireki Corporation, Polyphalt SS) was used as the asphalt, and approximately 38 parts by mass of softener 1 was used per 100 parts by mass of asphalt.
[0050] <Test Method> The obtained road repair material and the road repair material of Comparative Example 1 containing a mineral oil-derived product as a softener (NIPPO Corporation, Remiphalt ST) were evaluated for workability by a penetration resistance test and a flow test, and various physical properties were measured by a Marshall density test, a room temperature wheel tracking test, and a Cantablo test. Furthermore, VOC measurements were also performed on the obtained road repair material.
[0051] In the penetration resistance test, the road repair material was filled up to the top surface of the Marshall mold, leveled, and compacted three times. After that, a needle as shown in Figure 1 was inserted into the material at a speed of 1 inch / second using a push-pull gauge, and the resistance value was measured.
[0052] In the flow test, the road repair material was placed in a funnel as shown in Figure 2, and after smoothing it evenly on the top surface of the funnel, the funnel was lifted horizontally and the time until all of the road repair material in the funnel fell out was measured. The flow test also included observations of changes over time immediately after opening the product bag.
[0053] The Marshall density test was carried out by preparing a test specimen according to the method described in B001 (Marshall stability test method) of the "Pavement Survey and Test Method Handbook, Volume 3 (published by the Japan Road Association)" and then measuring the density according to the method described in B008-1 ("Density test method for dense-graded asphalt mixtures, etc."). The Marshall density test was carried out by observing the change over time immediately after opening the product bag.
[0054] Specifically, first, the height (A) of the mold is measured. Next, the mass of the empty mold (B) and two sheets of filter paper (C) is measured, and a predetermined mass of 900 grams of composite material is placed into the mold and tamped 30 times on one side. The weight of the mold, filter paper, and sample (D) is measured, and the drop (E) from the edge of the mold to the surface of the composite material is measured. Here, measurements are taken at four locations, and the average drop is calculated. Next, the thickness (t) of the sample after tamping is measured. Here, thickness (t) = (A) - (E) - 0.5. Then, the thickness (t) is multiplied by the base area of the Marshall mold (81.03 mm 2 ) to find the volume (V). Then, the mass (m) of the sample is found by (m) = (D) - (B) - (C). Finally, the density (ρ) is calculated by (ρ) = (m) / (V).
[0055] The room temperature wheel tracking test was carried out according to the method described in B003 (Wheel Tracking Test Method) of the "Pavement Survey and Test Method Handbook, Volume 3 (published by the Japan Road Association)."
[0056] The Cantablo test was carried out at 5°C according to the method described in B010 (Cantablo test method) of the Pavement Survey and Test Method Handbook, Volume 3 (published by the Japan Road Association).
[0057] The VOC measurement was outsourced to Green Search Co., Ltd., and measurements were carried out at room temperature in accordance with JIS K0125.
[0058] Results The results are summarized in the table below.
[0059] The results of the flow test and Marshall density test over time are summarized in the table below. Note that the density ratio indicates the percentage of the density at that time relative to the density immediately after opening.
[0060] In the flow test, the repair material of Comparative Example 1 was difficult to disintegrate after one day, and measurements were taken after three days after disintegrating the lumps, and after seven and fourteen days after forcibly disintegrating the lumps, whereas the repair material of Example 1 remained within the target range in the flow test even after 28 days. Similarly, in the Marshall density test, the density of the repair material of Comparative Example 1 decreased over time, whereas the density of the repair material of Example 1 remained essentially unchanged even after 28 days.
[0061] Furthermore, when VOCs were measured for the road repair material of the present invention, no VOCs were detected.
[0062] The results of the penetration resistance test and flow test regarding the workability of Example 1 were equivalent to those of the conventional product, Comparative Example 1, and the workability was good. In addition, in other physical property tests, Example 1 obtained better results than the conventional product, Comparative Example 1. Furthermore, the road repair material of Example 1 did not generate VOCs.
[0063] Road repair materials were manufactured by changing Softener 1 to Softeners 2 to 7, and evaluated in the same manner, with results generally equivalent to those in Example 1 or within the target range. Similar good results were obtained with the road repair material in which Aggregate 1 was changed to Aggregate 2, but due to the large particle size of the aggregate, the road repair material had high durability and load-bearing capacity, although the road repair material using Aggregate 1 was better in terms of workability and appearance.
[0064] Furthermore, the mixing temperature, which was about 160°C when producing the road repair material of Example 1, was changed to about 30°C. In this case, softener 1 and asphalt were mixed first, and then aggregate 1 was mixed. The obtained road repair material had the same appearance and physical properties as the road repair material of Example 1, or were within the target range.
[0065] Furthermore, when the road repair material of Example 1 was produced using an asphalt emulsion containing polymer-modified asphalt as the asphalt, not only were the physical properties equivalent to those of Example 1 obtained, but the material was also easier to mix, making production much easier.
Claims
1. A road repair material comprising asphalt, aggregate, and a softening agent, the softening agent comprising a fatty acid-based compound.
2. The road repair material according to claim 1, wherein the asphalt is a polymer-modified asphalt.
3. The road repair material according to claim 1, wherein the asphalt is contained as an asphalt emulsion.
4. The road repair material according to claim 3, wherein the asphalt emulsion comprises a polymer-modified asphalt.
5. A road repair material as described in claim 1, in which the content of recycled asphalt concrete aggregate is less than 20 mass%.
6. The road repair material according to claim 1, wherein the cement content is less than 20% by mass.
7. The road repair material according to claim 1, wherein the softening agent contains a fatty acid compound represented by the following general formula (1). 1 -CO-(AO)m-OR 2 ...General formula (1) (wherein, R 1 represents a linear or branched hydrocarbon group having 15 to 19 carbon atoms; R 2 represents either hydrogen or a linear or branched hydrocarbon group having 1 to 18 carbon atoms; AO represents a linear or branched alkylene oxide unit having 2 to 4 carbon atoms; and m represents the average number of moles added and is a number from 0 to 30.
8. The road repair material according to claim 1, wherein the iodine value of the fatty acid compound is 50 to 110.
9. The road repair material according to claim 1, comprising 10 parts by mass or more and 60 parts by mass or less of the softening agent per 100 parts by mass of the asphalt.
10. A method for producing a road repair material according to any one of claims 1 to 9, comprising mixing the asphalt, the aggregate, and the softening agent.
11. The method for producing a road repair material according to claim 10, wherein the mixing is carried out at a temperature of 100°C or less.
12. The method for producing a road repair material according to claim 10, wherein aggregate is mixed after the asphalt and the softening agent are mixed.
Citation Information
Patent Citations
Additive for asphalt emulsion and asphalt composition
JP1997059354A
Asphalt composition, its production and use
JP2001072860A
Modified asphalt composition and mineral oil-based softener
JP2003160732A
Asphalt composition
JP2009221436A
Workability improver for asphalt
JP2018080212A
Cited By
Pothole primer composition
JP7938885B1