Capacitor

The capacitor design with a needle-like inorganic conductive layer addresses peeling issues by enhancing electrode contact, reducing ESR, and achieving high heat resistance and conductivity.

WO2024202699A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/005841
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing capacitors face issues with peeling between the inorganic layer and the electrode, leading to increased equivalent series resistance (ESR) due to insufficient contact.

Method used

A capacitor design featuring a conductive layer with a needle-like structure made of inorganic material on the surface layer, which suppresses peeling and enhances anchoring, thereby reducing ESR. The conductive layer is formed using a method like liquid phase growth, and materials such as zinc oxide or other metal oxides with oxygen vacancies can be used to improve conductivity and heat resistance.

Benefits of technology

The capacitor design effectively prevents peeling between the inorganic layer and the electrode, thereby reducing ESR and achieving high heat resistance and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024005841_03102024_PF_FP_ABST
    Figure JP2024005841_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The capacitor includes a first electrode, a dielectric layer formed on the surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer. The conductive layer has a needle-like structure made of an inorganic material on a surface layer on the second electrode side.
Need to check novelty before this filing date? Find Prior Art

Description

capacitor

[0001] The present disclosure relates to capacitors.

[0002] Various capacitors have been proposed in the past. Claim 1 of Patent Document 1 (JP 2018-182106 A) describes a multilayer ceramic capacitor comprising: "a laminated chip having a substantially rectangular parallelepiped shape, in which dielectric layers and internal electrode layers, each of which is primarily made of ceramic, are alternately laminated, with the plurality of laminated internal electrode layers exposed at two end faces that alternately face each other; and external electrodes formed on the two end faces, the external electrodes having a structure in which a plating layer is formed on a base layer, and at least a portion of the surface of the base layer includes a region in which the bottom-to-peak height is 0.4 μm or more and the average spacing between local peaks is 0.5 μm or less."

[0003] Claim 1 of Patent Document 2 (JP 2020-35890 A) describes "a solid electrolytic capacitor comprising an anode body made of a valve metal, a dielectric layer formed on the surface of the anode body, a semiconductor layer formed on the dielectric layer, and a cathode layer formed on the semiconductor layer, wherein the semiconductor layer is formed using a p-type inorganic semiconductor."

[0004] JP 2018-182106 A JP 2020-35890 A

[0005] One aspect of the present disclosure relates to a capacitor including a first electrode, a dielectric layer formed on a surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer, the conductive layer having needle-like structures made of an inorganic material on a surface layer facing the second electrode.

[0006] According to the present disclosure, a capacitor can be obtained in which peeling is less likely to occur between the inorganic layer (conductive layer) and the electrode.

[0007] FIG. 1 is a cross-sectional view schematically showing the structure of an example capacitor according to this embodiment. FIG. 2 is a cross-sectional view schematically showing a portion of the capacitor shown in FIG. 1. FIG. 3 is a cross-sectional view schematically showing the structure of another example capacitor according to this embodiment. FIG. 4A is a cross-sectional image of the surface layer of the zinc oxide layer of an example capacitor produced in Experiment 1. FIG. 4B is a cross-sectional image of the surface layer of the zinc oxide layer of another example capacitor produced in Experiment 1. FIG. 4C is a cross-sectional image of the surface layer of the zinc oxide layer of another example capacitor produced in Experiment 1. FIG. 4D is a cross-sectional image of the surface layer of the zinc oxide layer of another example capacitor produced in Experiment 1. FIG. 5 is a cross-sectional image showing an example of the measurement results of the aspect ratio of the needle-shaped portion.

[0008] As described in Patent Document 2, a capacitor having an inorganic layer disposed between two electrodes is known. However, if the inorganic layer and the electrode have insufficient contact, peeling occurs between the inorganic layer and the electrode layer, resulting in problems such as an increase in equivalent series resistance (ESR). In this situation, the present disclosure provides a capacitor in which peeling is less likely to occur between the inorganic layer (conductive layer) and the electrode.

[0009] Below, embodiments according to the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and other materials may be applied as long as the invention according to the present disclosure can be implemented. In this specification, the expression "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits of numerical values ​​related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.

[0010] (Capacitor) Hereinafter, the capacitor according to this embodiment may be referred to as a "capacitor (C)." The capacitor (C) includes a first electrode, a dielectric layer formed on the surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer. The conductive layer has needle-like structures made of an inorganic material on the surface layer facing the second electrode.

[0011] As a result of their investigations, the present inventors have discovered a new method for forming a conductive layer having a needle-like structure made of an inorganic material on the surface. By using a conductive layer having a needle-like structure on the surface, it is possible to prevent peeling between the surface layer (inorganic layer) having the needle-like structure and the second electrode. Therefore, it is possible to prevent an increase in ESR due to peeling.

[0012] The conductive layer can be formed of an inorganic material. Therefore, the conductive layer can be interpreted as an inorganic layer. A preferred example of the conductive layer of the capacitor (C) does not contain an organic material (e.g., a conductive polymer). By forming the conductive layer from an inorganic material, a capacitor (C) with high heat resistance can be obtained.

[0013] The needle-like structures may be partially embedded in the second electrode, and this configuration allows the inorganic layer and the second electrode to be firmly fixed together by an anchor effect.

[0014] The average aspect ratio As in a cross-sectional image of the needle-like portion at the end of the needle-like structure may be in the range of 4.6 to 17.2 (for example, in the range of 5 to 16). The cross-sectional image is an image of a cross section parallel to the thickness direction Dt of the conductive layer. The average aspect ratio As is determined by a method described in the examples. The diameter of the needle-like portion in the cross-sectional image of the needle-like portion at the end of the needle-like structure may be 0.2 μm or less.

[0015] At least a part of the needle-like portion at the end of the needle-like structure may be curved. This configuration particularly enhances the anchoring effect of the needle-like structure. At least a part of the needle-like portion may be a needle-like crystal. That is, the needle-like structure may include a needle-like crystal.

[0016] The conductive layer may be made of an inorganic material containing a metal oxide. In this case, the needle-like structures may be made of the metal oxide. By using a conductive layer made of an inorganic material, a capacitor with high heat resistance can be obtained.

[0017] Metal oxides include ZnO and TiO 2 , indium tin oxide, In 2 O 3 , SnO 2 , Ga 2O 3 , MnO 2 , NiO 2 , CuInO 2 , CuCrO 2 , CuAlO 2 , and CuScO 2 The metal oxide may be a conductive metal oxide mainly composed of at least one selected from the group consisting of (a) and (b), or may be a conductive metal oxide consisting of at least one of the metal oxides. The metal oxide may be a conductive metal oxide mainly composed of any one selected from the above group, or may be a conductive metal oxide consisting of the one selected from the above group. For example, the metal oxide may be a conductive metal oxide mainly composed of ZnO, or may be ZnO. Although ZnO is sometimes classified as a semiconductor, it is conductive and is therefore treated as a conductive metal oxide in this specification. With respect to metal oxides, "main component" means that the content is 50% by mass or more. The content of the main component in the metal oxide may be in the range of 80 to 100% by mass, 90 to 100% by mass, or 95 to 100% by mass.

[0018] The conductive metal oxide may contain oxygen vacancies. By containing oxygen vacancies, the conductivity of the conductive metal oxide can be increased. When the conductive metal oxide is mainly composed of zinc oxide (ZnO), ZnO 1-x The main component may be zinc oxide represented by the formula (0≦x≦0.25), where x may be greater than 0.

[0019] The conductive metal oxide may contain an additive element for improving conductivity. When the conductive metal oxide is mainly composed of ZnO, at least one element selected from the group consisting of Al, Ga, B, and In may be added to ZnO so that the content of the element is 10 atomic % or less.

[0020] The conductive metal oxide is Ga 2 O 3 When the main component is Ga, at least one element selected from the group consisting of Ta and Hf is added to Ga so that the content of the element is 0.1 atomic % or less. 2 O 3 The conductive metal oxide may be TiO 2When the main component is TiO , at least one element selected from the group consisting of Nb and Ta is added to the TiO 4 so that the content of the element is 10 atomic % or less. 2 The conductive metal oxide may be SnO 2 When SnO is used as the main component, Sb is added so that the content is 12.5 atomic % or less. 2 The conductive metal oxide may be CuCrO 2 When the main component is CuCrO, Mg is added so that its content is 5 atomic % or less. 2 The conductive metal oxide may be CuInO 2 When the main component is CuInO, the Ca content is 3 atomic % or less. 2 It may also be added to.

[0021] In the capacitor (C), the first electrode may be an anode and the second electrode may be a cathode. In the capacitor (C), the first electrode may be an aluminum foil or a tantalum sintered body.

[0022] In the capacitor (C), the first electrode may have a porous portion on its surface. In this case, the dielectric layer is formed on the surface of the porous portion, and a portion of the conductive layer is disposed in the voids of the porous portion. The first electrode having a porous portion on its surface may be an etched aluminum foil or a sintered body of a valve metal (e.g., a tantalum sintered body).

[0023] The conductive layer may include a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode. The conductive layer may be composed of the first conductive layer and the second conductive layer. The second conductive layer has the above-mentioned needle-like structure on its surface. The first conductive layer and the second conductive layer may have different compositions or the same composition. The first conductive layer and the second conductive layer may be composed of the above-mentioned conductive metal oxide. When a porous portion is present on the surface layer of the first electrode, at least a portion of the first conductive layer may be formed in the recesses of the porous portion.

[0024] The conductivity of the conductive layer may be 1 S / cm or more, or 10 S / cm or more. The conductivity of the conductive layer may be 10,000 S / cm or less, or 1,000 S / cm or less. The conductive layer may be an inorganic layer having a conductivity of 1 S / cm or more.

[0025] The thickness of the conductive layer is not particularly limited and may be in the range of 0.1 μm to 100 μm (for example, in the range of 1 μm to 10 μm).

[0026] (Method for manufacturing a capacitor) Hereinafter, the manufacturing method according to this embodiment may be referred to as manufacturing method (M). According to manufacturing method (M), a capacitor (C) can be manufactured. However, the capacitor (C) may be manufactured by a method other than manufacturing method (M). The matters described for the capacitor (C) can be applied to manufacturing method (M), so redundant explanations will be omitted. The matters described for manufacturing method (M) can also be applied to the capacitor (C).

[0027] The manufacturing method (M) is a method for manufacturing a capacitor including a first electrode and a dielectric layer formed on the surface of the first electrode. The manufacturing method (M) includes steps (i) and (ii) in this order. These steps are described below.

[0028] Step (i) is a step of forming a conductive layer on the dielectric layer formed on the surface of the first electrode. The conductive layer is the conductive layer described for the capacitor (C). In step (i), the conductive layer is formed so that the surface layer of the conductive layer has a needle-like structure made of an inorganic material. At least the surface layer of the conductive layer can be formed by liquid phase growth. According to the liquid phase growth method, a conductive layer (a crystalline layer having conductivity) can be formed by crystal growth. At this time, by selecting the conditions for the liquid phase growth method, a surface layer having a needle-like structure can be formed.

[0029] When the surface layer is made of zinc oxide, a zinc oxide layer having a needle-like structure can be formed under the following conditions. First, a solution for liquid phase growth (solution growth) is prepared. Examples of the solution include an aqueous solution in which zinc nitrate and other additives are dissolved. Examples of the additives include hexamethylenetetramine, ammonia, citric acid, ammonium nitrate, aluminum nitrate, gallium nitrate, and indium nitrate. When adding the additive elements described above to ZnO, a compound containing the additive elements can be dissolved. The pH of the solution is, for example, in the range of 6 to 11. The concentration of zinc nitrate in the solution is, for example, in the range of 0.01 mol / L to 2 mol / L. Furthermore, when forming a surface layer having a needle-like structure, the temperature of the first electrode is, for example, in the range of 65°C to 75°C. The temperature of the solution is, for example, 75°C or less. The temperature of the solution may be in the range of 0 to 75°C (for example, in the range of 10 to 50°C or 10 to 40°C).

[0030] If the temperature of the first electrode is high (e.g., 85°C or higher), a columnar structure is formed instead of a needle-like structure. Conventionally, when forming a zinc oxide layer, conditions that result in the formation of a dense columnar structure have been selected. However, the inventors of the present application have discovered that a needle-like structure can be formed at a relatively low temperature. At least the surface layer of the above-mentioned conductive layer is formed under conditions that result in the formation of a needle-like structure. The average aspect ratio As of the needle-like portion at the end of the needle-like structure can be changed by changing the temperature of the first electrode, the pH of the solution, the concentration of the solution, etc.

[0031] Before forming the zinc oxide layer, a base layer made of zinc oxide may be formed in advance. For example, the base layer made of zinc oxide may be formed by a vapor phase method. Examples of the vapor phase method include atomic layer deposition (ALD), sputtering, and chemical vapor deposition (CVD). The use of the base layer makes it easier to form the zinc oxide layer by a liquid phase deposition method. The ALD method is preferred because it is easy to form a layer in the recesses of the porous portion.

[0032] The conductive layer made of the conductive metal oxide described above can also be formed by liquid phase deposition, similar to the zinc oxide layer, by selecting a solution appropriate for the conductive metal oxide to be formed.

[0033] The method for forming the conductive layer other than the surface layer having the needle-like structure is not limited. The conductive layer other than the surface layer may be formed by a vapor phase method or a liquid phase method. Examples of vapor phase methods include the vapor phase method described above. The entire conductive layer may be formed by a liquid phase deposition method, or the entire conductive layer may be formed under the same conditions as those for forming the surface layer described above. When the entire conductive layer is formed by a liquid phase deposition method, as described above, a base layer may be formed in advance on the dielectric layer. Alternatively, a first conductive layer having a certain thickness may be formed on the dielectric layer by an ALD method, and then a second conductive layer may be formed by a liquid phase deposition method. In either case, the surface layer of the conductive layer is formed under conditions that form a needle-like structure. Note that even when the entire conductive layer is formed under conditions that form a needle-like structure, the conductive layer close to the dielectric layer may grow so far that it does not have a needle-like structure.

[0034] When the conductive layer includes a first conductive layer and a second conductive layer, the first conductive layer and the second conductive layer may be formed by the same formation method or by different formation methods. For example, the first conductive layer and the second conductive layer may have different compositions and be formed by the same formation method. Alternatively, the first conductive layer and the second conductive layer may have the same composition and be formed by different formation methods.

[0035] Step (ii) is a step of forming a second electrode on the conductive layer. At this time, the second electrode is formed on the needle-like structures on the surface of the conductive layer. As a result, the conductive layer and the second electrode are firmly fixed together.

[0036] The second electrode is formed using a conductive material. The material of the second electrode is not particularly limited, as long as it is a material that can be used as an electrode of a capacitor. The method for forming the second electrode is not particularly limited, but it is preferable to use a formation method that firmly connects the conductive layer and the second electrode. For example, the second electrode may be formed by applying a conductive paste containing conductive particles. Alternatively, the second electrode may be formed by a vapor phase method, a plating method, or the like.

[0037] The second electrode may include a carbon layer and a silver particle layer stacked in this order from the conductive layer side. In this case, first, a carbon paste containing conductive carbon particles is applied. Next, a silver paste containing silver particles is applied. Then, a heat treatment is performed to form the carbon layer and the silver particle layer. In this manner, the second electrode is formed. Note that, if necessary, heat treatment may be performed not only after application of the silver paste but also before application of the silver paste. The carbon paste and silver paste are not limited, and known carbon pastes and silver pastes may be used.

[0038] Through the above steps, a capacitor element including a first electrode, a dielectric layer, a conductive layer, and a second electrode is formed. After step (ii), if necessary, lead connections and housing of the capacitor element in an outer casing are performed. In this way, a capacitor (C) is obtained.

[0039] Examples of the configuration and components of the capacitor (C) are described below. Known components may be used for components other than those characteristic of the present disclosure.

[0040] (First Electrode) The first electrode can be formed using a valve metal, an alloy containing a valve metal, a compound containing a valve metal, or the like. These materials may be used alone or in combination of two or more. Examples of valve metals that are preferably used include aluminum, tantalum, niobium, and titanium. The first electrode may be formed using a foil of the above material (e.g., a metal foil such as aluminum foil).

[0041] The first electrode having a porous portion on its surface can be obtained by roughening the surface of a metal foil containing a valve metal, for example. The roughening may be performed by electrolytic etching or the like.

[0042] The first electrode may be formed by sintering particles of the above material. For example, the first electrode may be a sintered body of tantalum. When the first electrode is a sintered body, a porous portion exists on the surface of the sintered body. When the first electrode is a sintered body, the capacitor (C) may include an anode wire partially embedded in the sintered body.

[0043] (Dielectric Layer) The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer may be formed by anodizing a valve metal on the surface of the first electrode (e.g., a metal foil). The dielectric layer may be formed so as to cover at least a portion of the first electrode. The dielectric layer is usually formed on the surface of the first electrode. When a porous portion exists on the surface of the first electrode, the dielectric layer is formed on the surface of the porous portion of the first electrode.

[0044] A typical dielectric layer includes an oxide of a valve metal. The first electrode may be formed of a valve metal, and the dielectric layer may be formed of an oxide of the valve metal. For example, if tantalum is used as the material of the first electrode, the dielectric layer may be a tantalum oxide layer. If aluminum is used as the material of the first electrode, the dielectric layer may be an aluminum oxide layer. However, the dielectric layer is not limited to these, and any material may be used as long as it functions as a dielectric layer.

[0045] (Second Electrode) The second electrode is a conductive layer. The second electrode may be formed using conductive carbon or metal. Specifically, the second electrode may be formed using a carbon paste containing conductive carbon particles or a metal paste containing metal particles. Alternatively, the second electrode may include a layer consisting of only metal (a vapor deposition layer or a metal foil). Examples of conductive carbon include graphite, carbon black, graphene flakes, and carbon nanotubes. Examples of metal paste include a silver paste containing silver particles.

[0046] The second electrode may include a first layer formed on the conductive layer and a second layer formed on the first layer, in which case the first layer may be a carbon layer containing conductive carbon, and the second layer may be a layer formed of a metal paste.

[0047] (Leads and exterior body) The capacitor (C) may include other components as necessary, for example, leads and exterior body. The leads and exterior body are not particularly limited, and known leads and exterior bodies may be used.

[0048] (Structure of Capacitor (C)) The capacitor (C) may include only one capacitor element. Alternatively, the capacitor (C) may include multiple capacitor elements. For example, the capacitor element (C) may include multiple capacitor elements connected in parallel. The multiple capacitor elements (C) are usually connected in parallel in a stacked state and covered with an exterior body.

[0049] Examples of embodiments according to the present disclosure will be described in detail below with reference to the drawings. The components described above can be applied to the components of the examples described below. The examples described below can be modified based on the above description. The matters described below may also be applied to the above embodiments. In the embodiments described below, components that are not essential to the capacitor of the present disclosure may be omitted. Note that the following drawings are schematic and may differ from the actual configuration.

[0050] 1 is a cross-sectional view schematically illustrating a capacitor according to embodiment 1. A capacitor 10 shown in Fig. 1 includes a capacitor element 100, a first lead terminal 21, a second lead terminal 22, a metal paste layer 23, and an outer casing 30.

[0051] The capacitor element 100 includes a first electrode 111, a dielectric layer 112, a conductive layer 120, and a second electrode 131. The dielectric layer 112 is formed so as to cover at least a portion of the surface of the first electrode 111. The conductive layer 120 is formed so as to cover at least a portion of the dielectric layer 112. The second electrode 131 is formed so as to cover at least a portion of the conductive layer 120. The conductive layer 120 is the conductive layer described above.

[0052] The first lead terminal 21 is connected to the first electrode 111. The second lead terminal 22 is connected to the second electrode 131 via a metal paste layer 23. The metal paste layer 23 is formed of a metal paste (silver paste) or the like. The exterior body 30 is formed so as to cover a portion of the first lead terminal 21, a portion of the second lead terminal 22, and the capacitor element 100. A portion of the first lead terminal 21 and a portion of the second lead terminal 22 are exposed from the exterior body 30 and function as terminals.

[0053] FIG. 2 is a schematic cross-sectional view of an example of a portion where the conductive layer 120 is present. FIG. 2 shows the thickness direction Dt of the conductive layer 120. The cross-sectional view of FIG. 2 is a cross-sectional view parallel to the thickness direction Dt of the conductive layer 120. The example first electrode 111 in FIG. 2 has a porous portion 111a on its surface. The actual porous portion 111a may have a more complex shape, but FIG. 2 shows a simplified depiction of the porous portion 111a. The surface layer 120a of the conductive layer 120 has a needle-like structure. However, the needle-like structure is not shown in FIG. 2.

[0054] 1 shows a case where the capacitor 10 includes only one capacitor element 100. However, the capacitor 10 may include a plurality of capacitor elements 100. A cross-sectional view of an example of a capacitor 10 including a plurality of capacitor elements 100 is shown in FIG. 3. Note that, to make the drawing easier to understand, some components are omitted from FIG. 3.

[0055] 3 includes a plurality of stacked capacitor elements 100. The plurality of capacitor elements 100 are connected in parallel.

[0056] (Additional Note) The above description discloses the following techniques.

[0057] (Technology 1) A capacitor comprising: a first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; and a second electrode disposed on the conductive layer, wherein the conductive layer has needle-like structures made of an inorganic material on a surface layer facing the second electrode.

[0058] (Technology 2) The capacitor according to Technology 1, wherein a part of the needle-like structure is buried in the second electrode.

[0059] (Technology 3) The capacitor according to Technology 1 or 2, wherein the average aspect ratio in a cross-sectional image of the needle-like portion at the end of the needle-like structure is in the range of 4.6 to 17.2.

[0060] (Technology 4) The capacitor according to any one of Technologies 1 to 3, wherein the diameter of the needle-like portion at the end of the needle-like structure in a cross-sectional image is 0.2 μm or less.

[0061] (Technology 5) The capacitor according to any one of Technologies 1 to 4, wherein at least a part of the needle-like portion at the end of the needle-like structure is curved.

[0062] (Technology 6) The capacitor according to any one of Technologies 1 to 5, wherein the conductive layer contains an inorganic material containing a metal oxide, and the needle-like structures are made of the metal oxide.

[0063] (Technology 7) The metal oxide is ZnO, TiO 2 , indium tin oxide, In 2 O 3 , SnO 2 , Ga 2 O 3 , MnO 2 , NiO 2 , CuInO 2 , CuCrO 2 , CuAlO 2 , and CuScO 2 The capacitor according to claim 6, wherein the conductive metal oxide is mainly composed of at least one selected from the group consisting of:

[0064] (Technology 8) The capacitor according to technology 7, wherein the conductive metal oxide contains oxygen vacancies.

[0065] (Technology 9) The capacitor according to Technology 7, wherein the conductive metal oxide contains an additive element for improving conductivity.

[0066] (Technology 10) The capacitor according to any one of Technologies 1 to 9, wherein the first electrode is an anode and the second electrode is a cathode.

[0067] (Technology 11) The capacitor according to any one of Technologies 1 to 10, wherein the first electrode is an aluminum foil or a tantalum sintered body.

[0068] (Technology 12) The capacitor according to any one of Technologies 1 to 11, wherein the first electrode has a porous portion on a surface thereof, the dielectric layer is formed on the surface of the porous portion, and a portion of the conductive layer is disposed within the voids of the porous portion.

[0069] (Technology 13) The capacitor according to any one of Technologies 1 to 12, wherein the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode, and the second conductive layer has the needle-like structure and a composition different from a composition of the first conductive layer.

[0070] The capacitor (C) according to the present disclosure will be described in more detail by way of examples.

[0071] (Experiment 1) In Experiment 1, conductive layers (ZnO layers) were formed under different conditions and evaluated. First, aluminum foil was prepared with a dielectric layer (aluminum oxide layer) formed on its surface. The aluminum foil used had porous portions formed on its surface by etching. The aluminum oxide layer was formed by chemical conversion treatment of the aluminum foil.

[0072] Next, a base layer made of zinc oxide was formed on the dielectric layer by ALD. Next, a conductive layer made of zinc oxide (ZnO) was formed on the base layer. Specifically, the aluminum foil on which the base layer was formed was immersed in a predetermined solution and held for 6 hours to form the zinc oxide layer on the base layer.

[0073] The solution used was an aqueous solution containing zinc nitrate hexahydrate and hexamethylenetetramine dissolved in a 1:1 molar ratio. The concentration of zinc nitrate hexahydrate in the solution was 0.05 mol / L. The pH of the solution was 6.5 to 7.5. The solution temperature was room temperature (approximately 24°C). During zinc oxide growth, a heater was placed in contact with the backside of the aluminum foil (the side opposite the zinc oxide growth surface) to heat the aluminum foil to a constant temperature. In Experiment 1, four types of zinc oxide layers were formed by varying the temperature of the aluminum foil. Figure 4A shows a cross-sectional image of the surface of the zinc oxide layer formed when the aluminum foil temperature was 65°C. Figures 4B to 4D show cross-sectional images of the surface of the zinc oxide layer formed when the aluminum foil temperature was 75°C, 85°C, and 95°C. Note that the cross-sectional images in Figures 4A to 4D are images of a cross section parallel to the thickness direction Dt of the conductive layer. In other words, the cross-sectional images of FIGS. 4A to 4D are images of a cross section perpendicular to the surface of the aluminum foil.

[0074] As shown in Figures 4A to 4D, when the temperature of the aluminum foil was in the range of 65 to 75°C, a needle-like structure was formed. On the other hand, when the temperature of the aluminum foil was in the range of 85 or 95°C, a needle-like structure was not formed, but a columnar structure was formed. As shown in Figures 4A and 4B, the needle-like portions at the ends of the formed needle-like structures were not oriented in a fixed direction, but extended in various directions. In addition, at least a portion of the needle-like portions at the ends of the needle-like structures was curved. Note that when the temperature of the aluminum foil was 50°C or lower, zinc oxide growth was difficult to proceed, and a needle-like structure was not formed.

[0075] The average value As of the aspect ratios of the needle-like portions at the ends of the needle-like structures shown in FIG. 4A was calculated. The average value As was determined by the following procedure. First, 22 needle-like portions at the ends of the needle-like structures were randomly selected in the cross-sectional image. The unbranched portions at the ends of the needle-like structures were defined as the needle-like portions. Next, the diameter D and length L of each selected needle-like portion were determined from the cross-sectional image. The diameter D was determined by measuring the diameter at an arbitrary point on the needle-like portion. When the needle-like portion was curved, the length L of the needle-like portion was determined from the entire length along the curved portion. Next, the aspect ratio of each needle-like portion was determined using the formula aspect ratio = length L / diameter D. The average value As was then obtained by arithmetically averaging the 22 aspect ratios obtained. Figure 5 shows the aspect ratios of each needle-like portion. In Figure 5, the needle-like portions for which the aspect ratios were determined are shown as rod-shaped figures. As described above, the average aspect ratio As can be determined by arbitrarily selecting and measuring 20 or more (for example, 20) needle-like portions.

[0076] The average aspect ratio As of the needle-like portions at the ends of the needle-like structures shown in Figure 4A was 4.6. The average aspect ratio As of the needle-like portions at the ends of the needle-like structures shown in Figure 4B was 17.2. The diameter of the needle-like portions in each of Figures 4A and 4B was 0.2 μm or less.

[0077] (Experiment 2) In Experiment 2, a second electrode was formed on a conductive layer (ZnO layer) formed under different conditions, and the peel resistance between the conductive layer and the second electrode was evaluated.

[0078] First, an aluminum foil having a dielectric layer formed on its surface was prepared. The aluminum foil having a dielectric layer formed on its surface was the same as that used in Experiment 1. Next, a zinc oxide layer (conductive layer) was formed on the dielectric layer using the same method and conditions as those described in Experiment 1. At this time, multiple types of zinc oxide layers were formed by changing the temperature of the aluminum foil, as described in Experiment 1. Next, a second electrode was formed on the zinc oxide layer. Two types of electrodes were used as the second electrode. One second electrode was formed by laminating a carbon layer and a silver particle layer in this order on a conductive layer. The other second electrode was formed only with a silver particle layer. In this manner, four types of samples A1 to A4 were prepared. Furthermore, comparative samples R1 to R4 were prepared using the same method and conditions as those used for samples A1 to A4, except that the substrate was changed from aluminum foil to a glass substrate.

[0079] The surface structure of the zinc oxide layer of the prepared samples was observed. Furthermore, a peeling test of the second electrode was performed on the prepared samples. The peeling test was performed using a method called a tape peeling test. Specifically, tape was adhered to the surface of the second electrode, and then the tape was peeled off, and the presence or absence of peeling of the second electrode was observed. The sample preparation conditions and the evaluation results of the peeling test are shown in Table 1.

[0080] Samples A1 to A4 have the structure of the capacitor (C) according to the present disclosure. In comparative samples R1 to R4, no needle-like structures were observed on the surface of the zinc oxide layer. As shown in Table 1, in samples A1 to A4, no peeling of the second electrode occurred, regardless of the configuration of the second electrode.

[0081] The present disclosure can be used for capacitors.

[0082] 10: Capacitor 21: First lead terminal 22: Second lead terminal 30: Exterior body 100: Capacitor element 111: First electrode 111a: Porous portion 112: Dielectric layer 120: Conductive layer 120a: Surface layer 131: Second electrode

Claims

1. A capacitor comprising: a first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; and a second electrode disposed on the conductive layer, the conductive layer having needle-shaped structures made of an inorganic material on its surface layer facing the second electrode.

2. The capacitor of claim 1, wherein a portion of said needle-like structure is embedded in said second electrode.

3. A capacitor according to claim 1 or 2, wherein the average aspect ratio in a cross-sectional image of the needle-like portion at the end of the needle-like structure is in the range of 4.6 to 17.

2.

4. The capacitor according to claim 1 or 2, wherein the diameter of the needle-shaped portion at the end of the needle-like structure in a cross-sectional image is 0.2 μm or less.

5. The capacitor according to claim 1 or 2, wherein at least a portion of the needle-like portion at the end of the needle-like structure is curved.

6. The capacitor according to claim 1 or 2, wherein the conductive layer includes an inorganic material containing a metal oxide, and the needle-like structure is made of the metal oxide.

7. The metal oxide is ZnO, TiO 2 , indium tin oxide, In 2 O 3 , SnO 2 , Ga 2 O 3 , MnO 2 , NiO 2 , CuInO 2 , CuCrO 2 , CuAlO 2 , and CuScO 2 7. The capacitor according to claim 6, wherein the conductive metal oxide is composed mainly of at least one selected from the group consisting of:

8. The capacitor of claim 7, wherein the conductive metal oxide contains oxygen vacancies.

9. The capacitor of claim 7, wherein the conductive metal oxide includes an additive element for improving electrical conductivity.

10. The capacitor of claim 1 or 2, wherein the first electrode is an anode and the second electrode is a cathode.

11. The capacitor according to claim 1 or 2, wherein the first electrode is an aluminum foil or a tantalum sintered body.

12. A capacitor as described in claim 1 or 2, wherein the first electrode has a porous portion on its surface, the dielectric layer is formed on the surface of the porous portion, and a portion of the conductive layer is disposed within the voids of the porous portion.

13. The capacitor of claim 1 or 2, wherein the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode, the second conductive layer having the needle-like structure and a composition different from the composition of the first conductive layer.

Citation Information

Patent Citations

  • Metal oxide structural form and its production

    JP2000159599A

  • Conductive composition, conductive coating, capacitor and method for manufacturing the same

    JP2005298563A

  • Solid electrolytic capacitor

    JP2017103412A

  • Element for electronic component

    WO2009099127A1