Film-provided copper terminal material and method for producing same
The coated copper terminal material addresses adhesion and friction issues by optimizing the tin layer thickness and curvature, and incorporating a copper-tin alloy and nickel layer, resulting in reduced friction and improved reliability for connector applications.
Patent Information
- Application Number
- PCT/JP2024/006760
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-20
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-03
AI Technical Summary
Existing copper terminal materials face issues with adhesion and excessive insertion/extraction force due to the softness of the tin layer, leading to increased frictional forces, especially in multi-pin connectors, and the formation of copper oxide at high temperatures, which affects contact resistance.
A coated copper terminal material with a base material of copper or copper alloy, featuring a tin layer with a specific thickness and curvature, and a copper-tin alloy layer, along with a nickel layer to prevent copper diffusion, is developed. The manufacturing process involves sequential plating and reflow treatment to achieve a stable and low-friction surface.
The solution effectively reduces the dynamic friction coefficient, prevents adhesion, and stabilizes the insertion/extraction force, while maintaining good electrical properties and heat resistance, thus enhancing the reliability and performance of the terminal material.
Smart Images

Figure JP2024006760_03102024_PF_FP_ABST
Abstract
Description
Coated copper terminal material and its manufacturing method
[0001] The present invention relates to a coated copper terminal material useful as a terminal for connectors used to connect electrical wiring in automobiles, consumer devices, etc., particularly as a terminal for multi-pin connectors, and a method for manufacturing the same. This application claims priority based on Japanese Patent Application No. 2023-049742 filed in Japan on March 27, 2023, and Japanese Patent Application No. 2024-23852 filed in Japan on February 20, 2024, the contents of which are incorporated herein by reference.
[0002] As a coated copper terminal material, there is a type in which a copper (Cu) plating layer and a tin (Sn) plating layer are formed on a substrate made of a copper alloy, and then a reflow treatment is performed to suppress the generation of whiskers, thereby forming a copper-tin (CuSn) alloy layer below the surface tin layer. This coated copper terminal material has high connection reliability and can be produced inexpensively, so it is widely used as a terminal material.
[0003] For example, in Patent Document 1, a Cu alloy plate is formed on the surface of a base material. 6 Sn 5 The document discloses a conductive material having a Cu—Sn alloy coating layer mainly composed of a Cu—Sn alloy phase and a Sn coating layer formed in this order. This conductive material is produced by roughening the surface of a base material to a surface roughness of 0.15 μm or more in at least one direction and 4.0 μm or less in all directions, forming a Cu plating layer and a Sn plating layer in this order on the surface of the base material, and then performing a reflow treatment.
[0004] Patent Document 2 discloses a Sn-plated product in which a Cu—Sn-based alloy layer consisting of numerous Cu—Sn-based alloy crystal grains and a Sn layer in recesses between adjacent Cu—Sn-based alloy crystal grains are formed on the surface of an underlayer on a substrate made of copper or a copper alloy. It is described that in this Sn-plated product, the area ratio of the Sn layer 16 on the outermost surface is 20 to 80%, and the maximum thickness of the Sn layer 16 is smaller than the average grain size of the Cu—Sn-based alloy crystal grains.
[0005] However, because the tin layer (Sn layer) is soft, adhesion between the contacts is likely to occur, and the increased contact area between the contacts results in excessive friction when inserting the connector, making insertion particularly difficult in multi-pin terminals.
[0006] Patent Document 3 discloses a plating material in which a base layer of Ni or the like is provided on a conductive substrate, an intermediate layer of copper or a copper alloy is provided on the base layer, and an outermost layer made of a Cu-Sn intermetallic compound is provided on the intermediate layer.It is described that this plating material is less likely to cause fretting even if the contact pressure between terminals is reduced, because the outermost layer is made of a hard Cu-Sn intermetallic compound layer.
[0007] However, if the outermost layer is a Cu--Sn intermetallic compound layer, copper (Cu) diffuses at high temperatures, and copper oxides are likely to form on the surface.
[0008] JP 2006-077307 A JP 2015-180770 A JP 2007-247060 A
[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a coated copper terminal material that prevents adhesion when used as a connector and stably reduces insertion and removal force.
[0010] The coated copper terminal material of the present invention has a substrate made of copper or a copper alloy and a coating formed on the substrate, the coating having a tin layer made of tin or a tin alloy with an average thickness of 0.2 μm or more and 2.0 μm or less on the surface thereof, and the arithmetic mean curvature Spc of the peaks on the surface of the coating is 10 mm -1 Over 70mm -1 or less, and the standard deviation / average value (CV value) of the arithmetic mean curvature Spc of the peak apex when measuring 10 visual fields is 30% or less.
[0011] This coated copper terminal material has a tin layer on the surface, which allows it to maintain the excellent electrical properties inherent to the tin layer. If the average thickness of this tin layer is less than 0.2 μm, Cu will diffuse at high temperatures, easily forming Cu oxides on the surface, which may increase contact resistance. If the average thickness of the tin layer is more than 2.0 μm, the soft tin layer increases the insertion and extraction force during use as a connector, making it difficult to reduce the insertion and extraction force associated with increased pin counts. The average thickness of the tin layer is preferably 0.3 μm or more and 1.8 μm or less.
[0012] The arithmetic mean curvature Spc of the peaks on the coating surface is 10 mm -1 Over 70mm -1 By setting the standard deviation / average value of Spc at 10 visual fields to 30% or less, the dynamic friction coefficient can be reduced, and by setting the standard deviation / average value of Spc at 10 visual fields to 30% or less, the dynamic friction coefficient is stabilized and local fluctuations are suppressed.
[0013] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point that contacts the mating terminal. -1 If the Spc is less than 70 mm, the connector will be nearly flat, resulting in a large contact area when it comes into contact with a mating terminal, and an increased coefficient of dynamic friction. -1 If the standard deviation / average value of Spc exceeds 30%, the coefficient of dynamic friction will fluctuate locally and become unstable.
[0014] Spc is 20mm -1 60mm or more -1 It is more preferable that the standard deviation / average value of Spc is 25% or less.
[0015] In the film-coated copper terminal material of the present invention, the film preferably has a copper-tin alloy layer made of an alloy of copper and tin under the tin layer. The copper-tin alloy layer preferably has an average thickness of 0.2 μm to 2.5 μm.
[0016] In the film-coated copper terminal material of the present invention, the film may have a nickel layer made of nickel or a nickel alloy in contact with the substrate.
[0017] The nickel layer can prevent copper from diffusing from the substrate and improve heat resistance. The average thickness of this nickel layer is preferably 0.05 μm or more and 1.0 μm or less.
[0018] The method for producing a film-coated copper terminal material of the present invention includes a plating step of forming a plated material on the substrate, the plated material having a tin plating layer made of tin or a tin alloy on the surface, and a reflow step of heating the plated material to perform a reflow treatment. The thickness of the tin plating layer in the plating step is 0.2 μm or more and 3.0 μm or less. The reflow treatment includes a heating step of heating the plated material to a peak temperature of 240°C or more and 300°C or less, a primary cooling step after the heating step in which the plated material is passed through a cooling furnace with an internal temperature of 20°C or more and 70°C or less to reduce the material temperature to 150°C or more and 220°C or less, and a secondary cooling step of cooling the plated material at a cooling rate of 100°C / sec or more and 300°C / sec or less after the primary cooling. In the primary cooling step, cooling air is blown onto the surface of the plated material at a rate of 10 m / s. 3 / min or more 300m 3 Spray at a rate of less than 1 / min.
[0019] If the thickness of the tin plating layer made of tin or a tin alloy is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer after reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer cannot be obtained.
[0020] If the peak temperature of the heating step is less than 240°C, the tin will not melt uniformly, and if the peak temperature exceeds 300°C, copper from the substrate will diffuse into the tin plating layer, forming voids at the interface between the substrate and the tin layer, which may cause the tin layer to peel off, which is undesirable.
[0021] In the cooling process of the reflow treatment, a primary cooling process is provided in which the plated material is passed through a cooling furnace with an internal temperature of 20°C to 70°C so that the material reaches a temperature of 150°C to 220°C, and is cooled to a temperature below the melting point of tin, and then the plated material is rapidly cooled at a high cooling rate in a secondary cooling process.
[0022] In the primary cooling process, a predetermined cooling air is blown onto the surface of the plated material in a cooling furnace at a predetermined furnace temperature, thereby appropriately controlling the surface shape at a temperature below the melting point of tin, and the arithmetic mean curvature Spc of the peaks on the plated film surface is set to 10 mm. -1 Over 70mm -1 With the above, the standard deviation / average value (CV value: coefficient of variation) of Spc when measuring 10 visual fields can be reduced to 30% or less.
[0023] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate will be too fast and the CV value (standard deviation / average value) of Spc and Spc will be too large. -1 Hereinafter, the CV value (standard deviation / average value) of Spc cannot be set to 30% or less. If the temperature inside the furnace exceeds 70°C, the cooling time to a temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0024] Regarding the material temperature of the plated material, if it is less than 150°C, the cooling time will be too long, resulting in an excessively large CV value (standard deviation / average value) of Spc. If the material temperature exceeds 220°C, the tin will be secondary cooled while still in a semi-molten state, resulting in an excessively large CV value (standard deviation / average value) of Spc. The material temperature is preferably 160°C or higher and 210°C or lower, and more preferably 170°C or higher and 200°C or lower.
[0025] Cooling air volume: 10m 3 If the cooling rate is less than 10 mm / min, the Spc will be too small due to insufficient cooling. -1 On the other hand, the cooling air volume cannot be increased to 300 m 3 If the cooling air temperature exceeds 100°C / min, the molten tin will flow due to the large amount of air blown, and the Spc and CV value (standard deviation / average value) of Spc will become excessively large. The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0026] The material is then rapidly cooled in a secondary cooling step to achieve the desired surface shape. If the cooling rate in this secondary cooling step is less than 100°C / sec, the desired surface shape cannot be obtained. It is difficult to achieve a cooling rate exceeding 300°C / sec.
[0027] In the method for producing a film-coated copper terminal material of the present invention, in the plating step, the tin plating layer may be formed after a copper plating layer made of copper or a copper alloy is formed on the substrate.
[0028] When a copper plating layer is formed, the heating rate of the plated material in the heating step is preferably 20°C / s or more and 75°C / s or less. If the heating rate is less than 20°C / s, copper atoms preferentially diffuse into the grain boundaries of the tin before the tin melts, causing abnormal growth of copper-tin intermetallic compounds near the grain boundaries, making it impossible to obtain a desired copper-tin alloy layer. On the other hand, if the heating rate exceeds 75°C / s, the growth of the copper-tin intermetallic compounds is insufficient, making it impossible to obtain a desired copper-tin alloy layer.
[0029] When a copper plating layer is formed, if the peak temperature in the heating step is less than 240° C., the tin does not melt uniformly, and if the peak temperature exceeds 300° C., copper-tin intermetallic compounds grow rapidly, resulting in large irregularities in the copper-tin alloy layer, which is undesirable. Furthermore, if the cooling rate in the secondary cooling step is less than 100° C. / sec, copper-tin intermetallic compounds grow, making it impossible to obtain the desired copper-tin alloy layer.
[0030] In the method for producing a film-coated copper terminal material of the present invention, the plating step may include forming a nickel plating layer made of nickel or a nickel alloy on the surface of the substrate.
[0031] According to the present invention, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer forming the surface of the terminal material is set to 10 mm. -1 Over 70mm -1 By setting the standard deviation / average value of Spc to 30% or less when measuring 10 visual fields, it is possible to prevent adhesion when used as a connector, reduce the dynamic friction coefficient, and stabilize the dynamic friction coefficient, thereby providing a coated copper terminal material with a stably reduced insertion / extraction force.
[0032] FIG. 1 is a cross-sectional view schematically showing a first embodiment of the film-coated copper terminal material of the present invention. FIG. 2 is a cross-sectional view showing a plated material in the middle of manufacturing the film-coated copper terminal material of FIG. 1. FIG. 3 is a cross-sectional view schematically showing a second embodiment of the film-coated copper terminal material of the present invention. FIG. 4 is a cross-sectional view showing a plated material in the middle of manufacturing the film-coated copper terminal material of FIG. 3. FIG. 5 is a cross-sectional view schematically showing a third embodiment of the film-coated copper terminal material of the present invention. FIG. 6 is a cross-sectional view showing a plated material in the middle of manufacturing the film-coated copper terminal material of FIG. 7.
[0033] An embodiment of the film-coated copper terminal material of the present invention will be described.
[0034] (First embodiment) As shown in FIG. 1, the film-coated copper terminal material 1 of the first embodiment has a film 5 formed on a substrate 2 made of copper or a copper alloy, and a tin layer 3 made of tin or a tin alloy laminated thereon.
[0035] The substrate 2 is a strip material formed in a strip shape, and its composition is not particularly limited as long as the surface is made of copper or a copper alloy.
[0036] The tin layer 3 is formed by forming a plating layer made of tin or a tin alloy on the substrate 2 and then performing a reflow treatment.
[0037] The average thickness of the tin layer 3 is 0.2 μm or more and 2.0 μm or less. The tin layer 3 has lubricity that reduces the insertion and extraction force of the connector and reduces contact resistance, resulting in excellent electrical properties. However, if the average thickness is less than 0.2 μm, it becomes difficult to obtain the excellent properties of tin. In addition, solderability and corrosion resistance may also be reduced.
[0038] On the other hand, if the average thickness of the tin layer 3 exceeds 2.0 μm, adhesion is likely to occur due to the softness, and the insertion / extraction force during use as a connector increases, making it difficult to reduce the insertion / extraction force as the number of pins in the connector increases. The average thickness of this tin layer 3 is preferably 0.3 μm or more and 1.8 μm or less.
[0039] On the surface of the tin layer 3, the arithmetic mean curvature Spc of the peaks (hereinafter sometimes simply referred to as Spc) is 10 mm -1 Over 70mm -1or less, and the standard deviation / average value (coefficient of variation) of Spc when measuring 10 visual fields is 30% or less.
[0040] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point that comes into contact with other objects. -1 If the thickness is less than 1 / 2 mm, the surface becomes nearly flat, so that the contact area when the connector comes into contact with a mating terminal becomes large, and the coefficient of dynamic friction increases.
[0041] Spc is 70mm -1 If the standard deviation / average value of Spc exceeds 30%, the coefficient of dynamic friction will fluctuate locally and become unstable. -1 60mm or more -1 It is more preferable that the standard deviation / average value of Spc is 25% or less.
[0042] The following describes a method for manufacturing the film-coated copper terminal material 1 configured as described above. The film-coated copper terminal material 1 is formed by applying tin plating made of tin or a tin alloy to the substrate 2 to form a plated material 7 in which a tin plating layer 4 is laminated on the substrate 2 as shown in Fig. 2, and then performing a reflow treatment.
[0043] As the substrate 2, a plate made of copper or a copper alloy is prepared, and the surface of this plate is cleaned by degreasing, pickling, or other treatments.
[0044] As a plating bath for tin plating, a general tin plating bath may be used, for example, sulfuric acid (H 2 SO 4 ) and stannous sulfate (SnSO 4 The plating bath temperature is 15 to 35°C, and the current density is 1 to 30 A / dm 2 The thickness of the tin plating layer 4 is set to be 0.2 μm or more and 3.0 μm or less.
[0045] If the thickness of the tin plating layer 4 is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer 3 after reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer 3 will not be obtained.
[0046] The reflow treatment involves heating the plated material 7 to melt the tin plating layer 4, followed by rapid cooling. Specifically, the treatment includes a heating step in which the plated material 7 is heated in a heating furnace in a CO reducing atmosphere to a temperature of 240°C to 300°C, which is higher than the melting point of tin, a primary cooling step in which the plated material 7 is passed through a cooling furnace with an internal temperature of 20°C to 70°C to reach a material temperature of 150°C to 220°C, and a secondary cooling step in which the plated material 7 is cooled at a cooling rate of 100°C / sec to 300°C / sec after the primary cooling.
[0047] In this case, in the primary cooling step, cooling air is blown onto the surface of the plated material 7 at a speed of 10 m 3 / min or more 300m 3 The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0048] By carrying out the heating step in a reducing atmosphere, it is possible to prevent the formation of a tin oxide film with a high melting temperature on the surface of the tin plating layer 4, and to carry out the reflow treatment at a lower temperature in a shorter time.
[0049] If the peak temperature of the heating step is less than 240°C, the tin will not melt uniformly, which is undesirable. If the peak temperature exceeds 300°C, copper from the substrate 2 will diffuse into the tin plating layer 4, forming voids at the interface between the substrate 2 and the tin layer 3, which may cause the tin layer to peel off, which is also undesirable.
[0050] The cooling process after heating is carried out in two stages. In the primary cooling process, the plated material 7 is passed through a cooling furnace with an internal temperature of 20°C to 70°C, and the material reaches a temperature of 150°C to 220°C. The material is cooled to below the melting point of tin, and then rapidly cooled at a faster cooling rate in the secondary cooling process.
[0051] In the primary cooling step, a predetermined cooling air is blown onto the surface of the plated material 7 in a cooling furnace at a predetermined furnace temperature, thereby appropriately controlling the surface shape at a temperature below the melting point of tin. As a result, the arithmetic mean curvature Spc of the peaks on the surface of the coating 5 (tin layer 3) is reduced to 10 mm. -1 Over 70mm -1 Hereinafter, the standard deviation / average value (CV value) of Spc when measuring 10 visual fields can be made 30% or less.
[0052] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate is too fast, and the Spc and CV values (standard deviation / average value) of Spc become excessively large. -1 Hereinafter, the CV value (standard deviation / average value) of Spc cannot be set to 30% or less. If the temperature inside the furnace exceeds 70°C, the cooling time required to reach a temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0053] If the material temperature of the plated material 7 in the primary cooling step is less than 150°C, the cooling time is too long, resulting in an excessively large CV value (standard deviation / average value) of Spc. If the temperature of the plated material 7 does not drop to 220°C or less in the primary cooling step, the tin will remain in a semi-molten state during secondary cooling, resulting in an excessively large CV value (standard deviation / average value) of Spc. The material temperature of the plated material 7 in the primary cooling step is preferably 160°C or higher and 210°C or lower, and more preferably 170°C or higher and 200°C or lower.
[0054] The volume of cooling air in the primary cooling process is 10 m 3 If the cooling rate is less than 10 mm / min, the Spc will be too small due to insufficient cooling. -1 On the other hand, the cooling air volume cannot be increased to 300 m 3 If the time exceeds 1 / min, the molten tin will flow due to the large amount of air blown, and the Spc and CV values (standard deviation / average value) of Spc will become excessively large.
[0055] The cooling air is blown perpendicularly onto the plated material 7 from a height of about 10 cm above the surface of the plated material 7 .
[0056] Next, in the secondary cooling step, the plated material 7 is rapidly cooled to obtain the desired surface shape. If the cooling rate in this secondary cooling step is less than 100°C / sec, the desired surface shape cannot be obtained. It is difficult to achieve a cooling rate exceeding 300°C / sec.
[0057] The coating 5 of the thus-produced coated copper terminal material 1 has the excellent electrical properties inherent to tin, since the surface is made of the tin layer 3. In addition, the arithmetic mean curvature Spc of the peaks on the surface of the coating 5 (tin layer 3) is 10 mm -1 Over 70mm -1 Since the coefficient of dynamic friction is less than or equal to 100 kJ / s, the coefficient of dynamic friction can be reduced.
[0058] Furthermore, by setting the standard deviation / average value of Spc when measuring in 10 visual fields to 30% or less, the dynamic friction coefficient is stabilized and local fluctuations are suppressed.
[0059] Therefore, by using the coated copper terminal material 1 as a terminal material for a connector, the insertion / withdrawal force can be stably reduced, and adhesion with the mating terminal can be prevented.
[0060] 3, the film-coated copper terminal material 11 of the second embodiment is formed by laminating a copper-tin alloy layer 13 made of an alloy of copper and tin and a tin layer 14 in this order on a film 12 provided on a substrate 2. In other words, the film 12 has the copper-tin alloy layer 13 below the tin layer 14.
[0061] As will be described later, the copper-tin alloy layer 13 and the tin layer 14 are formed by sequentially plating the substrate 2 with copper or a copper alloy and tin or a tin alloy, followed by a reflow treatment.
[0062] The copper-tin alloy layer 13 is formed to an average thickness of 0.2 μm or more and 2.5 μm or less. If the thickness is less than 0.2 μm, contact resistance may increase in a high-temperature environment. If the thickness exceeds 2.5 μm, the copper-tin alloy layer 13 is hard and may cause cracks during bending. The copper-tin alloy layer 13 preferably has an average crystal grain size of 0.2 μm or more and 1.5 μm or less.
[0063] This copper-tin alloy layer 13 is made of the Cu3 Sn layer 15 and Cu 3 Cu disposed on the Sn layer 15 6 Sn 5 layer 16. 3 The Sn layer 15 is formed partially on the surface of the substrate 2. 6 Sn 5 The alloy layer 16 is formed by the Cu on the substrate 2. 3 On the Sn alloy layer 15, and on the Cu 3 The Sn alloy layer 15 is formed on both the substrate 2 and the substrate 2 where the Sn alloy layer 15 is not present.
[0064] As in the first embodiment, the average thickness of the tin layer 14 is 0.2 μm or more and 2.0 μm or less. If the thickness of the tin layer 14 is less than 0.2 μm, copper diffuses at high temperatures and copper oxide is likely to form on the surface, which may increase contact resistance and reduce connection reliability. Furthermore, solderability and corrosion resistance may also be reduced.
[0065] On the other hand, if the average thickness of the tin layer 14 exceeds 2.0 μm, the effect of hardening the surface base by the copper-tin alloy layer 13 present below the soft tin layer 14 is weakened, the insertion and extraction force when used as a connector increases, and it becomes difficult to reduce the insertion and extraction force as the number of pins in the connector increases. The average thickness of this tin layer 14 is preferably 0.3 μm or more and 1.8 μm or less.
[0066] As in the first embodiment, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer 14 is 10 mm -1 Over 70mm -1 or less, and the standard deviation / average value of Spc when measuring 10 visual fields is 30% or less.
[0067] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point that comes into contact with other objects. -1 If the Spc is less than 70 mm, the connector will be nearly flat, resulting in a large contact area when it comes into contact with a mating terminal, and an increased coefficient of dynamic friction. -1 If the surface roughness exceeds this value, the surface roughness becomes too steep, causing the mating terminal to be dug up.
[0068] If the standard deviation / average value of Spc exceeds 30%, the dynamic friction coefficient will fluctuate locally and become unstable. -1 60mm or more -1 It is more preferable that the standard deviation / average value of Spc is 25% or less.
[0069] The following describes a method for manufacturing the film-coated copper terminal material 11 configured as described above. The film-coated copper terminal material 11 is formed by sequentially plating the substrate 2 with copper or copper alloy and tin or tin alloy, thereby forming a plated material 19 in which a copper plating layer 17 and a tin plating layer 18 are laminated on the substrate 2 as shown in Fig. 4, and then performing a reflow treatment.
[0070] As the substrate 2, a plate made of copper or a copper alloy is prepared, and the surface of this plate is cleaned by degreasing, pickling, or other treatments.
[0071] Copper plating can be performed using a general copper plating bath, for example, copper sulfate (CuSO 4 ) and sulfuric acid (H 2 SO 4 The plating bath temperature is 20 to 50°C, and the current density is 1 to 50 A / dm 2 The thickness of the copper plating layer 17 formed by this Cu plating is set to 0.05 μm or more and 0.50 μm or less.
[0072] As a plating bath for tin plating, a general tin plating bath may be used, for example, sulfuric acid (H 2 SO 4 ) and stannous sulfate (SnSO 4 The plating bath temperature is 15 to 35°C, and the current density is 1 to 30 A / dm 2 The thickness of the tin plating layer 18 is set to be 0.2 μm or more and 3.0 μm or less.
[0073] If the thickness of the tin plating layer 18 is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer 14 after reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer 14 will not be obtained.
[0074] By carrying out these plating processes, a plated material 19 is formed in which a copper plating layer 17 and a tin plating layer 18 are sequentially laminated on the base material 2 .
[0075] The reflow treatment involves heating the plated material 19 to melt the copper plating layer 17 and the tin plating layer 18, followed by rapid cooling. Specifically, the treatment includes a heating step in which the plated material 19 is heated to a temperature of 240°C or higher and 300°C or lower at a temperature increase rate of 20°C / sec or higher and 75°C / sec or lower in a heating furnace in a CO reducing atmosphere, a primary cooling step in which the plated material is passed through a cooling furnace with an internal temperature of 20°C or higher and 70°C or lower to a material temperature of 150°C or higher and 220°C or lower, and a secondary cooling step in which the plated material is cooled at a cooling rate of 100°C / sec or higher and 300°C / sec or lower after the primary cooling.
[0076] In this case, in the primary cooling step, cooling air is blown onto the surface of the plated material 19 at a speed of 10 m 3 / min or more 300m 3 The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0077] By carrying out the heating process in a reducing atmosphere, it is possible to prevent the formation of a tin oxide film with a high melting temperature on the surface of the tin plating layer 18, and it is possible to carry out the reflow treatment at a lower temperature in a shorter time, making it easier to produce the desired copper-tin alloy structure.
[0078] If the heating rate in the heating step is less than 20°C / sec, copper atoms will preferentially diffuse through the grain boundaries of the tin before the tin melts, causing abnormal growth of copper-tin intermetallic compounds near the grain boundaries, making it impossible to obtain the desired copper-tin alloy layer 13. On the other hand, if the heating rate exceeds 75°C / sec, growth of the copper-tin intermetallic compounds will be insufficient, making it impossible to obtain the desired copper-tin alloy layer.
[0079] If the peak temperature in the heating step is less than 240° C., the tin will not melt uniformly, and if the peak temperature exceeds 300° C., the copper-tin intermetallic compound will grow rapidly, causing the copper-tin alloy layer 13 to become uneven.
[0080] In the primary cooling step, a predetermined cooling air is blown onto the surface of the plated material 19 in a cooling furnace at a predetermined furnace temperature, thereby appropriately controlling the surface shape at a temperature below the melting point of tin. As a result, the arithmetic mean curvature Spc of the peaks on the surface of the coating 12 is reduced to 10 mm. -1 Over 70mm -1 Hereinafter, the standard deviation / average value of Spc when measuring 10 visual fields can be made 30% or less.
[0081] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate is too fast, and the Spc and CV values (standard deviation / average value) of Spc become excessively large. -1 Hereinafter, the CV value (standard deviation / average value) of Spc cannot be set to 30% or less. If the temperature inside the furnace exceeds 70°C, the cooling time required to reach a temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0082] If the material temperature of the plated material 19 in the primary cooling process is less than 150°C, the cooling time is too long, resulting in an excessively large CV value (standard deviation / average value) of Spc. If the temperature of the plated material 19 in the primary cooling process does not drop to 220°C or less, the tin will remain in a semi-molten state during secondary cooling, resulting in an excessively large CV value (standard deviation / average value) of Spc. The material temperature of the plated material 19 in the primary cooling process is preferably 160°C or higher and 210°C or lower, and more preferably 170°C or higher and 200°C or lower.
[0083] The volume of cooling air in the primary cooling process is 10 m 3 If the cooling rate is less than 10 mm / min, the Spc will be too small due to insufficient cooling. -1 On the other hand, the cooling air volume cannot be increased to 300 m 3 If the time exceeds 1 / min, the molten tin will flow due to the large amount of air blown, and the Spc and CV values (standard deviation / average value) of Spc will become excessively large.
[0084] The cooling air is blown perpendicularly onto the plated material 19 from a height of about 10 cm above the surface of the plated material 19 .
[0085] Next, in the secondary cooling step, the plated material 19 is rapidly cooled to obtain the desired surface shape. If the cooling rate in this secondary cooling step is less than 100°C / sec, the copper-tin intermetallic compound grows excessively, making it impossible to obtain the desired copper-tin alloy layer. It is difficult to achieve a cooling rate exceeding 300°C / sec.
[0086] The coating 12 of the coated copper terminal material 11 manufactured in this manner has a composite structure in which the copper-tin alloy layer 13 and the tin layer 14 form an uneven interface, and the relatively soft tin layer 14 is supported by the hard copper-tin alloy layer 13. The arithmetic mean curvature Spc of the peaks on the surface of the coating 12 is 10 mm. -1 Over 70mm -1 Since the coefficient of dynamic friction is less than or equal to 100 kJ / s, the coefficient of dynamic friction can be reduced.
[0087] Furthermore, by setting the standard deviation / average value of Spc when measuring in 10 visual fields to 30% or less, the dynamic friction coefficient is stabilized and local fluctuations are suppressed.
[0088] Therefore, by using the film-coated copper terminal material 11 as the terminal material of a connector, the insertion / withdrawal force can be stably reduced, and adhesion with the mating terminal can be prevented.
[0089] 5, in a film-coated copper terminal material 21 of the third embodiment, the film 22 has a nickel layer 23 made of nickel or a nickel alloy in contact with the substrate 2, and a tin layer 24 made of tin or a tin alloy laminated on the nickel layer 23. In other words, the film 22 has the nickel layer 23 below the tin layer 24.
[0090] By providing the nickel layer 23, it is possible to prevent copper from diffusing from the substrate 2 into the coating 22, thereby improving heat resistance.
[0091] The average thickness of the nickel layer 23 is set to 0.05 μm or more and 1.0 μm or less. If it is less than 0.05 μm, the effect of preventing copper diffusion from the base material 2 is reduced, and if it exceeds 1.0 μm, bending and other processes may become difficult.
[0092] On the surface of the tin layer 24, the arithmetic mean curvature Spc of the peak is 10 mm -1 Over 70mm-1 The standard deviation / average value of Spc when measuring 10 visual fields is 30% or less, which is the same as in the first embodiment.
[0093] The Spc on the surface of the tin layer 24 is 20 mm -1 60mm or more -1 The standard deviation / average value of Spc is more preferably 25% or less.
[0094] The film-coated copper terminal material 21 thus constructed is formed by sequentially applying nickel plating made of nickel or a nickel alloy and tin plating made of tin or a tin alloy to the substrate 2, thereby forming a plated material 27 in which a nickel plating layer 25 and a tin plating layer 26 are laminated on the substrate 2 as shown in FIG. 6, and then performing a reflow treatment.
[0095] The nickel plating for forming the nickel plating layer 25 may be carried out using a general nickel plating bath, for example, sulfuric acid (H 2 SO 4 ) and nickel sulfate (NiSO 4 The temperature of the plating bath is 20°C or higher and 60°C or lower, and the current density is 5 to 60 A / dm 2 The thickness of the nickel plating layer 25 is set to 0.05 μm or more and 1.0 μm or less.
[0096] The conditions for tin plating and the conditions for reflow treatment are the same as those described in the first embodiment.
[0097] The film-coated copper terminal material 21 thus manufactured has the nickel layer 23, which prevents copper from diffusing and improves heat resistance.
[0098] 7 , in a film-coated copper terminal material 31 of the fourth embodiment, the film 32 has a nickel layer 33 made of nickel or a nickel alloy in contact with the substrate 2, a copper-tin alloy layer 34 made of an alloy of copper and tin laminated on the nickel layer 33, and a tin layer 35 made of tin or a tin alloy laminated on the copper-tin alloy layer 34. In other words, the film 32 has the tin layer 35 on the surface, the copper-tin alloy layer 34 below the tin layer 35, and the nickel layer 33 in contact with the substrate 2 below the copper-tin alloy layer 34.
[0099] By providing the nickel layer 33, copper of the substrate 2 can be prevented from diffusing into the coating 32, thereby improving heat resistance.
[0100] The average thickness of the nickel layer 33 is set to 0.05 μm or more and 1.0 μm or less. If it is less than 0.05 μm, the effect of preventing copper diffusion from the base material 2 is reduced, and if it exceeds 1.0 μm, bending and other processes may become difficult.
[0101] The copper-tin alloy layer 34 is a Cu layer formed partially on the substrate 2 side. 3 The Sn alloy layer 36 and the Cu layer formed to cover the Sn alloy layer 36 6 Sn 5 The alloy layer 37 is composed of Cu. 6 Sn 5 The alloy layer 37 is a Cu layer on the nickel layer 33. 3 On the Sn alloy layer 36, and on the Cu 3 The Sn alloy layer 36 is formed so as to cover both the top and bottom of the nickel layer 33 where no Sn alloy layer 36 is present.
[0102] The copper-tin alloy layer 34 preferably has an average thickness of 0.2 μm to 2.5 μm and an average crystal grain size of 0.2 μm to 1.5 μm, and the tin layer 35 has an average thickness of 0.2 μm to 2.0 μm.
[0103] As in the first embodiment, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer 35 is 10 mm -1 Over 70mm -1 The standard deviation / average value of Spc when measuring 10 visual fields is 30% or less. -1 60mm or more -1The standard deviation / average value of Spc is more preferably 25% or less.
[0104] The film-coated copper terminal material 31 thus constructed is formed by sequentially plating the substrate 2 with nickel or a nickel alloy, copper or a copper alloy, and tin or a tin alloy, to form a plated material 44 having a nickel plating layer 41, a copper plating layer 42, and a tin plating layer 43 stacked on the substrate 2, as shown in FIG. 8, and then performing a reflow treatment.
[0105] The conditions for nickel plating, copper plating, and tin plating are the same as those described in the first to third embodiments.
[0106] The plated material 44 having the nickel plating layer 41, copper plating layer 42, and tin plating layer 43 formed thereon is subjected to a reflow treatment to form the film-coated copper terminal material 31. This reflow treatment is the same as that in the second embodiment, and therefore a description thereof will be omitted.
[0107] The thus-manufactured coated copper terminal material 31 has a nickel layer 33 below the coating 32, which prevents copper diffusion and improves heat resistance. In addition, the copper-tin alloy layer 34 and the tin layer 35 have an uneven interface, the copper-tin alloy layer 34 supports the tin layer 35, and the arithmetic mean curvature of the peaks on the surface and the CV value when measured from 10 fields of view are within predetermined ranges, so the dynamic friction coefficient is uniformly and stably low.
[0108] A copper alloy plate having a thickness of 0.25 mm was used as a substrate, and various plating processes were carried out under the following plating bath conditions.
[0109] (Nickel plating) Nickel sulfate: 300 g / L Sulfuric acid: 2 g / L Solution temperature: 45°C Current density: 20 ASD (A / dm 2 )
[0110] (Copper plating) Copper sulfate: 250g / L Sulfuric acid: 50g / L Liquid temperature: 25℃ Current density: 5ASD
[0111] (Tin plating) Tin sulfate: 75 g / L Sulfuric acid: 85 g / L Additive: 10 g / L Solution temperature: 25°C Current density: 2ASD
[0112] Plated materials were prepared in which a tin plating layer was formed on a substrate (Examples 1, 5, 9, Comparative Examples 1, 5), in which a copper plating layer and a tin plating layer were formed in that order on a substrate (Examples 2, 6, 10, Comparative Examples 2, 6), in which a nickel plating layer and a tin plating layer were formed in that order on a substrate (Examples 3, 7, 11, Comparative Example 3), and in which a nickel plating layer, a copper plating layer, and a tin plating layer were formed in that order on a substrate (Examples 4, 8, 12, Comparative Examples 4, 7), and these were subjected to reflow treatment under the conditions shown in Tables 1 and 2.
[0113]
[0114]
[0115] The average thickness of the tin layer on the surface, the arithmetic mean curvature of the peaks Spc, and the dynamic friction coefficient μ of the obtained samples were measured to evaluate the stability.
[0116] [Average Thickness of Tin Layer] The average thickness of the tin layer was measured using a fluorescent X-ray film thickness meter (SEA5120A) manufactured by SII NanoTechnology Inc.
[0117] For samples having a copper-tin alloy layer, the thickness of the entire tin-containing layer of the sample after reflow was first measured, and then the tin layer was removed to expose the underlying copper-tin alloy layer, and the thickness of the copper-tin alloy layer was measured. The thickness of the tin layer was then defined as (thickness of the entire tin-containing layer - thickness of the copper-tin alloy layer). The thickness of the entire tin-containing layer includes the copper-tin alloy layer portion and the tin layer portion, but since the tin solidified material is uneven, it is calculated as an average thickness. The tin layer was removed by immersing the sample for 5 minutes in an etching solution for stripping the plating film, which contains ingredients that do not corrode the copper-tin alloy layer.
[0118] [Arithmetic Mean Curvature of Peaks Spc] Ten fields of view were observed using a laser microscope (Keyence Corporation VKX-1100, objective lens × 10), and Spc was measured over the entire field of view in accordance with ISO 25178, and the CV value (standard deviation / average value) of Spc was calculated.
[0119] [Dynamic Friction Coefficient and Stability] A hemispherical female test piece and a plate-shaped male test piece with an inner diameter of 1.5 mm were prepared for each sample to simulate the contact area between the male and female terminals of a mating connector. Using a friction measuring machine (horizontal load tester, model M-2152ENR) manufactured by Aiko Engineering Co., Ltd., a load of 100 gf or more and 500 gf or less was applied between the female test piece and the male test piece, and the friction force was measured when the male test piece was pulled 10 mm horizontally at a sliding speed of 80 mm / min to determine the dynamic friction coefficient μ.
[0120] The dynamic friction coefficient increases as the tin layer becomes thicker because the tin layer is less affected by the hard substrate, nickel layer, and copper-tin alloy layer underneath and more affected by the soft tin layer. Test pieces with a dynamic friction coefficient μ of 0.3 or less when the average tin layer thickness was less than 1.0 μm, a dynamic friction coefficient μ of 0.4 or less when the average tin layer thickness was 1.0 μm or more but less than 1.5 μm, and a dynamic friction coefficient μ of 0.45 or less when the average tin layer thickness was 1.5 μm or more were classified as pass (A), and test pieces with exceeding these values were classified as fail (B).
[0121] The average value of 30 measurements was calculated using the above method, and test pieces with 30 measured values within the range of the average value ±25% were rated as stability "A," and test pieces with measured values of ±25% or more were rated as stability "B."
[0122] [Contact Resistance Value] To evaluate electrical reliability, the contact resistance of each sample was measured after heating in air at 150°C for 500 hours. The measurement method conformed to JIS-C-5402, and a four-terminal contact resistance tester (Yamazaki Seiki Kenkyusho: CRS-113-AU) was used to measure the contact resistance as a function of load (1 mm) from 0 to 50 g, and the contact resistance was evaluated as the contact resistance value when the load was 50 g.
[0123] These results are shown in Tables 3 and 4.
[0124]
[0125]
[0126] As is clear from Tables 1 to 4, in all of the Examples, the dynamic friction coefficient μ was small depending on the average thickness of the tin layer, and the dynamic friction coefficient μ showed good stability. For example, in Example 8, the tin layer was somewhat thick at 1.2 μm, and was less affected by the hard underlying substrate, nickel layer, and copper-tin alloy layer but more affected by the soft tin layer, but the dynamic friction coefficient μ was 0.37, showing good stability.
[0127] In contrast, the following problems were observed in each comparative example. In comparative example 1, the temperature inside the cooling furnace exceeded 70°C, so the CV value of Spc was excessively large, resulting in poor stability of the dynamic friction coefficient μ. In comparative example 2, the cooling air volume for primary cooling was too weak, so Spc was too small, increasing the real contact area between the platings and resulting in a poor dynamic friction coefficient μ and poor stability. In comparative example 3, the cooling air volume for primary cooling was too strong, so Spc was excessively large, resulting in puncture due to surface irregularities during insertion / extraction tests, resulting in an excessively large dynamic friction coefficient μ, and the CV value of Spc was excessively large, resulting in poor stability of the dynamic friction coefficient μ.
[0128] In Comparative Example 4, the temperature inside the cooling furnace was less than 20°C, so the Spc and Spc CV values were excessively large, and the dynamic friction coefficient μ was excessively large, resulting in poor stability. In Comparative Example 5, the material temperature reached was less than 150°C, so the Spc CV value was excessively large, resulting in poor stability of the dynamic friction coefficient μ. In Comparative Example 6, the material temperature reached was more than 220°C, so the Spc CV value was excessively large, resulting in poor stability of the dynamic friction coefficient μ. In Comparative Example 7, the cooling air volume for primary cooling was too strong, so the Spc and Spc CV values were excessively large, resulting in the dynamic friction coefficient μ being excessively large, resulting in poor stability.
[0129] In Comparative Example 8, the tin layer was too thin, resulting in a thin tin layer and a poor contact resistance.In Comparative Example 9, the tin layer was too thick, resulting in a thick tin layer and a poor dynamic friction coefficient.
[0130] It is possible to provide a coated copper terminal material that prevents adhesion when used as a connector, reduces the dynamic friction coefficient, stabilizes the dynamic friction coefficient, and stably reduces insertion and extraction force.
[0131] REFERENCE SIGNS LIST 1 Copper terminal material with coating 2 Substrate 3 Tin layer 4 Tin plating layer 7 Plated material 11 Copper terminal material with coating 12 Coating 13 Copper-tin alloy layer 14 Tin layer 15 Cu3 Sn alloy layer 16 Cu 6 Sn 5 Alloy layer 17 Copper plating layer 18 Tin plating layer 19 Plated material 21 Coated copper terminal material 22 Coating 23 Nickel layer 24 Tin layer 25 Nickel plating layer 26 Tin plating layer 27 Plated material 31 Coated copper terminal material 32 Coating 33 Nickel layer 34 Copper-tin alloy layer 35 Tin layer 36 Cu 3 Sn alloy layer 37 Cu 6 Sn 5 Alloy layer 41 Nickel plating layer 42 Copper plating layer 43 Tin plating layer 44 Plating material
Claims
1. A coated copper terminal material having a substrate made of copper or a copper alloy and a coating formed on the substrate, the coating having a tin layer made of tin or a tin alloy with an average thickness of 0.2 μm or more and 2.0 μm or less on the surface, and the arithmetic mean curvature Spc of the peaks on the surface of the coating is 10 mm -1 More than 70 mm -1 and the standard deviation / average value of the arithmetic mean curvature Spc of the peaks when measured in 10 visual fields is 30% or less.
2. A film-coated copper terminal material according to claim 1, characterized in that the film has a copper-tin alloy layer made of an alloy of copper and tin under the tin layer.
3. A coated copper terminal material according to claim 1 or 2, characterized in that the coating has a nickel layer made of nickel or a nickel alloy in contact with the base material.
4. A method for producing a film-coated copper terminal material in which a film is formed on a substrate made of copper or a copper alloy, comprising: a plating step for forming a plated material having a plating layer made of tin or a tin alloy on the substrate; and a reflow step for heating and reflowing the plated material, wherein the film thickness of the tin plating layer in the plating step is 0.2 μm or more and 3.0 μm or less, and the reflow treatment comprises: a heating step for heating the plated material to a peak temperature of 240°C or more and 300°C or less; a primary cooling step for passing the plated material through a cooling furnace having an internal temperature of 20°C or more and 70°C or less after the heating step so that the material reaches a temperature of 150°C or more and 220°C or less; and a secondary cooling step for cooling the plated material at a cooling rate of 100°C / s or more and 300°C / s or less after the primary cooling, wherein in the primary cooling step, cooling air is blown at a rate of 10 m to the surface of the plated material. 3 / min or more 300m 3 3. A method for producing a coated copper terminal material, comprising: blowing the copper on the surface of the substrate at a rate of 1 / min or less.
5. A method for producing a film-coated copper terminal material according to claim 4, characterized in that in the plating step, a copper plating layer made of copper or a copper alloy is formed under the tin plating layer.
6. A method for producing a film-coated copper terminal material according to claim 5, characterized in that the heating rate of the plated material in the heating step is 20°C / sec or more and 75°C / sec or less.
7. A method for producing a coated copper terminal material as described in claim 4, characterized in that in the plating step, a nickel plating layer made of nickel or a nickel alloy is formed by contacting the surface of the base material.
8. A method for producing a coated copper terminal material according to claim 6, characterized in that in the plating step, a nickel plating layer made of nickel or a nickel alloy is formed by contacting the surface of the base material.
9. A film-coated copper terminal material according to claim 2, characterized in that the average thickness of the copper-tin alloy layer is 0.2 μm or more and 2.5 μm or less.
10. A film-coated copper terminal material according to claim 3, characterized in that the average thickness of the nickel layer is 0.05 μm or more and 1.0 μm or less.
11. A coated copper terminal material according to claim 1, characterized in that the coating has a copper-tin alloy layer made of an alloy of copper and tin and having an average thickness of 0.2 μm or more and 2.5 μm or less under the tin layer, and a nickel layer made of nickel or a nickel alloy and having an average thickness of 0.05 μm or more and 1.0 μm or less in contact with the base material.
12. A method for producing a film-coated copper terminal material according to claim 6, characterized in that the thickness of the copper plating layer is 0.05 μm or more and 0.50 μm or less.
13. A method for producing a film-coated copper terminal material as described in claim 8, characterized in that the thickness of the copper plating layer is 0.05 μm or more and 0.50 μm or less, and the thickness of the nickel plating layer is 0.05 μm or more and 1.0 μm or less.
14. A method for producing a film-coated copper terminal material according to claim 7, characterized in that the thickness of the nickel plating layer is 0.05 μm or more and 1.0 μm or less.
Citation Information
Patent Citations
Conductive member and method for manufacturing the same
JP2010168598A
Sn-PLATED MATERIAL
JP2013213249A
Tin plated copper alloy terminal material, manufacturing method therefor and wire terminal part structure
JP2016166397A
Tin-plated copper terminal material and method of manufacturing the same
JP2019178365A
Surface-treated copper foil, carrier-attached copper foil, copper-clad laminate, and printed wiring board
WO2020105289A1
Cited By
Connector terminal material, production method thereof, and connector
JP2025114450A
Terminal material for connector, manufacturing method thereof, and connector
JP7670224B1