Method for producing lithium-containing solution

A two-stage elution process with lithium manganate adsorbents and manganese oxidation enhances lithium content and reduces solution usage, addressing cost and efficiency limitations in lithium production.

WO2024203175A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO METAL MINING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009099
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-08
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current methods for producing lithium-containing solutions are limited in reducing manufacturing costs and minimizing the amount of solution used after the elution process, as they require high acid concentrations that increase the amount of eluent solution needed.

Method used

A method involving a two-stage elution process with varying hydrogen ion concentrations, using a lithium adsorbent from lithium manganate to increase lithium content and reduce the amount of eluent solution, along with a manganese oxidation step to suppress manganese concentration, is employed.

Benefits of technology

This approach effectively reduces manufacturing costs by minimizing the amount of acid and eluent solution used, increasing lithium content, and improving elution efficiency while suppressing manganese dissolution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009099_03102024_PF_FP_ABST
    Figure JP2024009099_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing a lithium-containing solution is provided in which a solution resulting from an elution step is made to have an increased lithium content and the amount of the solution in a step succeeding the elution step is reduced, thereby reducing the cost of lithium production. The method for producing a lithium-containing solution includes, in the following order, an adsorption step, an elution step in which lithium manganate resulting from the adsorption is brought into contact with an acid-containing solution to obtain an eluate, and a manganese oxidation step. The elution step comprises a first elution step, in which the acid-containing solution has a high H+ concentration, and a second elution step, in which the acid-containing solution has a lower H+ concentration than in the first elution step. The second elution step is performed after the first elution step. Due to the configuration, elution is efficiently performed in the first elution step and, in the second elution step, there is no need of heightening the hydrogen ion concentration of the acid-containing solution and the amount of an acid to be added to the acid-containing solution can hence be reduced. Thus, the amount of the eluate to be used in the manganese oxidation step can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing lithium-containing solution

[0001] The present invention relates to a method for producing a lithium-containing solution. More specifically, the present invention relates to a method for producing a lithium-containing solution that can reduce the production cost for lithium production by increasing the lithium content in the solution after an elution step and reducing the amount of solution used in steps after the elution step.

[0002] Lithium manganese oxide (LiMn) has a spinel structure. 2 O 4 , Li 1.33 Mn 1.67 O 4 , Li 1.6 Mn 1.6 O 4 λ-MnO obtained by contacting a mineral acid such as hydrochloric acid with 2 (HMn 2 O 4 , H 1.33 Mn 1.67 O 4 , H 1.6 Mn 1.6 O 4 It is known that λ-MnO etc. selectively adsorbs lithium. 2 When used for lithium recovery, λ-MnO 2 Since λ-MnO does not adsorb impurities, it has the advantage of being able to significantly reduce the amount of neutralizing agent used in lithium recovery. For this reason, commercial use of this method is expected. 2 Patent Document 1 discloses a method for producing a lithium-containing solution using the above.

[0003] In the method for producing a lithium-containing solution of Patent Document 1, an acid-containing solution used in the elution step is prepared by adding an acid to the total amount of the elution solution obtained in the elution step, thereby adjusting the hydrogen ion concentration of the acid-containing solution, thereby reducing the amount of the elution solution used in the steps after the elution step.

[0004] International Publication No. 2022 / 210847

[0005] However, acid-containing solutions require the addition of acid to adjust the hydrogen ion concentration to a predetermined value, and if a large amount of acid is added, the effect of reducing the amount of solution used in steps after the elution step is limited.

[0006] In view of the above circumstances, an object of the present invention is to provide a method for producing a lithium-containing solution that can reduce the production cost for lithium production by increasing the lithium content in the solution after the elution step and reducing the amount of solution used in the steps after the elution step.

[0007] A method for producing a lithium-containing solution according to a first aspect of the present invention includes the steps of: an adsorption step of contacting a low-concentration lithium-containing solution with a lithium adsorbent obtained from lithium manganate to obtain an adsorbed lithium manganate; an elution step of contacting the adsorbed lithium manganate with an acid-containing solution to obtain an eluate; and a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the eluate to oxidize manganese and obtain a lithium-containing solution with a reduced manganese concentration, the elution step including a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step.A method for producing a lithium-containing solution according to the first aspect of the present invention is characterized in that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less. A third aspect of the present invention relates to a method for producing a lithium-containing solution, wherein the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution containing lithium at a lower concentration than the high-concentration lithium elution solution in the elution step, the acid-containing solution used in the elution step includes the low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step includes the high-concentration lithium elution solution.A fourth aspect of the present invention relates to a method for producing a lithium-containing solution, wherein the high-concentration lithium elution solution is obtained by extracting a predetermined volume of the elution solution obtained through the elution step, based on the start of the elution solution.A fifth aspect of the present invention relates to a method for producing a lithium-containing solution, wherein the high-concentration lithium elution solution is obtained between a predetermined start time and an end time after the start of the elution step.A sixth invention is a method for producing a lithium-containing solution according to any one of the first to fifth inventions, characterized in that a water-washing step of washing the post-elution lithium adsorbent obtained after the elution step is provided after the elution step, and the post-washing solution obtained in the water-washing step is added to the acid-containing solution.

[0008] According to the first invention, the elution process includes a first elution process and a second elution process in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution process. By performing the second elution process after the first elution process, elution is efficiently performed in the first elution process. Furthermore, since the hydrogen ion concentration of the acid-containing solution does not need to be increased in the second elution process, the amount of acid added to the acid-containing solution can be reduced, thereby reducing the amount of elution solution used in the manganese oxidation process. This reduces the production cost for lithium production. According to the second invention, the hydrogen ion concentrations of the acid-containing solution in the first elution process and the acid-containing solution in the second elution process are set to predetermined values, thereby suppressing dissolution of manganese from the lithium adsorbent and improving elution efficiency. According to the third invention, the elution solution used in the manganese oxidation process contains a high-concentration lithium elution solution, thereby increasing the lithium content of the elution solution used in the manganese oxidation process. Furthermore, because only the low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by simply adding a small amount of acid, thereby further reducing the amount of acid-containing solution and the amount of elution solution used in the manganese oxidation step. According to the fourth invention, the high-concentration lithium elution solution is an elution solution obtained by extracting a predetermined volume based on the start of the elution solution, thereby increasing the lithium content of the high-concentration lithium elution solution. According to the fifth invention, the high-concentration lithium elution solution is an elution solution obtained between a predetermined start time and a predetermined end time after the start of the elution step, thereby making it easy to obtain a high-concentration lithium elution solution. According to the sixth invention, the post-water washing solution obtained in the water washing step is added to the acid-containing solution, thereby recovering lithium that would otherwise be discarded in the water washing step.

[0009] Fig. 1 is a flow chart of a method for producing a lithium-containing solution according to a first embodiment of the present invention. Fig. 2 is a flow chart of a method for producing a lithium-containing solution according to a second embodiment of the present invention. Fig. 3 is a flow chart of a method for producing a lithium-containing solution according to a third embodiment of the present invention. Fig. 4 is a flow chart of a method for producing a lithium-containing solution according to a fourth embodiment of the present invention. Fig. 5 is a graph showing the lithium concentration for each predetermined volume fraction, with the start of obtaining an elution solution as a reference, in the method for producing a lithium-containing solution of Fig. 2. Fig. 6 is a graph showing the lithium concentration for each predetermined volume fraction, with the start of obtaining a post-water-washing solution as a reference, in the method for producing a lithium-containing solution of Fig. 3.

[0010] Next, embodiments of the present invention will be described with reference to the drawings. However, the embodiments shown below are merely examples of methods for producing a lithium-containing solution to embody the technical concept of the present invention, and the present invention does not limit the method for producing a lithium-containing solution to the following.

[0011] The method for producing a lithium-containing solution according to the present invention includes the following steps, carried out in this order: an adsorption step of bringing a low-concentration lithium-containing solution into contact with a lithium adsorbent obtained from lithium manganate to obtain post-adsorption lithium manganate; an elution step of bringing the post-adsorption lithium manganate into contact with an acid-containing solution to obtain an elution solution; and a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the elution solution to oxidize manganese and obtain a lithium-containing solution with a reduced manganese concentration. The elution step includes a first elution step and a second elution step in which the acid-containing solution has a lower hydrogen ion concentration than that of the first elution step, and the second elution step is carried out after the first elution step.

[0012] The elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step. This allows for efficient elution in the first elution step, and eliminates the need to increase the hydrogen ion concentration of the acid-containing solution in the second elution step. This reduces the amount of acid added to the acid-containing solution and the amount of elution solution used in the manganese oxidation step, thereby reducing the production cost for lithium production.

[0013] It is also preferable that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less. This embodiment can suppress dissolution of manganese from the lithium adsorbent and can increase elution efficiency.

[0014] In addition, the elution solution is preferably separated into a high-concentration lithium elution solution containing a high concentration of lithium and a low-concentration lithium elution solution containing a lower concentration of lithium than the high-concentration lithium elution solution in the elution step, and the acid-containing solution used in the elution step contains the low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step contains the high-concentration lithium elution solution. This embodiment allows the lithium content of the elution solution used in the manganese oxidation step to be increased. Furthermore, because only the low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by simply adding a small amount of acid, which results in further reduction in the amount of acid-containing solution and the amount of elution solution used in the manganese oxidation step.

[0015] Furthermore, the high-concentration lithium elution solution is preferably an elution solution obtained by extracting a predetermined volume of the elution solution obtained through the elution step, based on the start of the elution solution being obtained. This embodiment allows the lithium content of the high-concentration lithium elution solution to be increased.

[0016] In addition, the high-concentration lithium elution solution is preferably the elution solution obtained between a predetermined start time and a predetermined end time after the start of the elution step. In this embodiment, the high-concentration lithium elution solution can be easily obtained.

[0017] In addition, it is preferable that a water-washing step for washing the eluted lithium adsorbent obtained after the elution step is provided after the elution step, and the post-washing water obtained in the water-washing step is added to the acid-containing solution. This embodiment makes it possible to recover lithium that would otherwise be discarded in the water-washing step.

[0018] (First embodiment) (Pre-stage of adsorption step) In the adsorption step, a low-concentration lithium-containing solution is brought into contact with a lithium adsorbent to obtain lithium manganese oxide after adsorption. A method for obtaining the lithium adsorbent used in this adsorption step will be described. Note that, while Fig. 1 shows a flow chart of a method for producing a lithium-containing solution according to the first embodiment of the present invention, the explanation of the "pre-stage of the adsorption step" will be given in the H at the top of Fig. 1. 1.6 Mn 1.6 O 4 This is the stage where you can obtain the following.

[0019] Lithium manganate becomes a lithium adsorbent by acid treatment as shown in Equation 1. In Equation 1, lithium manganate is expressed as Li 1.6 Mn 1.6 O 4 However, the lithium manganese oxide is not limited to this. For example, Li 1.33 Mn 1.67 O 4 It is also possible to use lithium manganate. 1.6 Mn 1.6 O 4 When the lithium adsorbent is H 1.6 Mn 1.6 O 4 However, if lithium manganese oxide is used, for example, Li 1.33 Mn 1.67 O 4 When the lithium adsorbent is H 1.33 Mn 1.67 O 4 Although the acid used in the acid treatment is HCl, it is not limited to this. For example, sulfuric acid, nitric acid, etc. can also be used.

[0020] The shape of the lithium manganate is determined in consideration of the adsorption of lithium in the adsorption process. For example, the lithium manganate can be in various shapes such as powder, granulated powder, or sprayed onto column fibers. When the acid treatment is performed, for example, H 1.6 Mn 1.6 O 4The shape of the lithium adsorbent is the same as that of the lithium manganese oxide before the acid treatment.

[0021] [Math 1] Li 1.6 Mn 1.6 O 4 +1.6HCl → H 1.6 Mn 1.6 O 4 +1.6LiCl

[0022] 1 shows a flow diagram of a method for producing a lithium-containing solution according to a first embodiment of the present invention. In the adsorption step, a low-concentration lithium-containing solution is brought into contact with a lithium adsorbent to obtain adsorbed lithium manganate through an ion exchange reaction between H and Li as shown in Equation 2. In this specification, the lithium manganate obtained in the adsorption step may be referred to as adsorbed lithium manganate.

[0023] [Math 2] H 1.6 Mn 1.6 O 4 +1.6LiCl → Li 1.6 Mn 1.6 O 4 +1.6HCl

[0024] Examples of low-concentration lithium-containing solutions include seawater and brine from salt lakes. For example, seawater contains an average of 0.17 ppm of lithium. However, these low-concentration lithium-containing solutions also contain dissolved elements such as sodium, magnesium, and calcium in addition to lithium. According to the method for producing a lithium-containing solution of the present invention, it is possible to selectively recover lithium from a low-concentration lithium-containing solution containing these dissolved elements. Note that a low-concentration lithium-containing solution means that the amount of lithium per unit volume is smaller, i.e., the lithium concentration is lower, compared to the lithium-containing solution described below.

[0025] In the adsorption process, the method of contacting the low-concentration lithium-containing solution with the adsorbent varies depending on the shape of the adsorbent. For example, when the adsorbent is powdery, one method is to add a predetermined amount of the adsorbent to the low-concentration lithium-containing solution and stir it for a predetermined time, thereby bringing the low-concentration lithium-containing solution into contact with the adsorbent and adsorbing lithium onto the adsorbent. When the adsorbent is particulate, one method is to seal the particulate adsorbent in a liquid-passing container and pass the low-concentration lithium-containing solution through the container, thereby bringing the low-concentration lithium-containing solution into contact with the adsorbent and adsorbing lithium onto the adsorbent. When the adsorbent is sprayed onto the fibers of a column, one method is to pass the low-concentration lithium-containing solution through the column, thereby bringing the low-concentration lithium-containing solution into contact with the adsorbent and adsorbing lithium onto the adsorbent. Note that when passing the low-concentration lithium-containing solution through the column, the liquid may be passed repeatedly to ensure the number of times it comes into contact with the adsorbent.

[0026] After the adsorption process, the adsorbent becomes lithium manganese oxide after adsorption. The low-concentration lithium-containing solution becomes a post-adsorption liquid after the lithium is adsorbed by the adsorbent. This post-adsorption liquid is discharged into the sea or lake from which the low-concentration lithium-containing solution was collected. The post-adsorption liquid is then discharged after being treated, for example, by neutralization, to make it suitable for discharge.

[0027] (Elution Step) In the elution step, the post-adsorption lithium manganate is brought into contact with an acid-containing solution to obtain an elution solution by the reaction shown in Equation 3. At this time, the post-adsorption lithium manganate is converted into Li + and H + This exchange reaction between cations causes the lithium adsorbent to be regenerated, and the lithium adsorbent can be reused in the adsorption step.

[0028] [Math 3] Li 1.6 Mn 1.6 O 4 +1.6HCl → H 1.6 Mn 1.6 O 4 +1.6LiCl

[0029] In this embodiment, the acid-containing solution includes a solution of a simple acid such as hydrochloric acid, and an elution solution obtained by adding an acid to the elution solution obtained by a first elution step. For example, in this embodiment, the elution step is divided into multiple steps, such as a first elution step and a second elution step. The first elution step is an elution step in which the hydrogen ion concentration of the acid-containing solution is relatively high, and the second elution step is an elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step. For example, in the initial stage of the first elution step, the acid-containing solution can be a solution of simple acid, and in subsequent steps, the elution solution obtained in the previous step can be adjusted to a predetermined hydrogen ion concentration by adding an acid. In this case, the second elution step can be an elution solution obtained in the previous step to which an acid has been added. Alternatively, the acid-containing solution in the first elution step can be a solution of simple acid alone, and the acid-containing solution in the second elution step can be an elution solution obtained in the previous step to which an acid has been added.

[0030] The reaction shown in Equation 3 proceeds better as the pH value of the acid-containing solution used in the elution step is smaller. However, when the reaction shown in Equation 3 progresses to a certain extent, the pH value of the acid-containing solution increases, and the reaction shown in Equation 3 no longer proceeds. In Patent Document 1, International Publication No. 2022 / 210847, in order to prevent this state from occurring, the elution step is carried out in multiple stages, and in the second stage and subsequent stages of the multiple stages, an elution solution obtained in the previous stage is added with acid and used as the acid-containing solution. However, since the acid was supplied so as to have the same pH as the acid-containing solution supplied initially, the amount of elution solution was limited.

[0031] The elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step. This allows for efficient elution in the first elution step, and eliminates the need to increase the hydrogen ion concentration of the acid-containing solution in the second elution step. This reduces the amount of acid added to the acid-containing solution and the amount of elution solution used in the manganese oxidation step, thereby reducing the production cost for lithium production.

[0032] Increasing the lithium content of the elution solution in this way can reduce the size of the equipment in subsequent processes and the load on the process of obtaining lithium as a solid. In other words, increasing the lithium content allows for a reduction in the amount of lithium-containing solution itself, eliminating the need to increase the size of the equipment in subsequent processes. In addition, when obtaining lithium as a solid, the time required to boil the solution can be shortened, and the amount of pH adjuster in the manganese oxidation process (described below) or the neutralization process performed after the manganese oxidation process can be reduced. This neutralization process is performed, for example, to remove magnesium. Furthermore, the solution containing a high concentration of lithium can be shipped directly to the customer.

[0033] Although the elution step is divided into multiple steps, the elution step is not limited to this. For example, the elution step may include a case in which an acid is continuously added to the elution solution to form an acid-containing solution.

[0034] In the elution step of this embodiment, i.e., the first elution step and the second elution step, the hydrogen ion concentration of the acid-containing solution contacted with the lithium manganate after adsorption is preferably 0.1 mol / L or more and 4.0 mol / L or less. Furthermore, the hydrogen ion concentration is preferably 0.25 mol / L or more and 2.0 mol / L or less. Furthermore, the hydrogen ion concentration is preferably 0.5 mol / L or more and 1.0 mol / L or less.

[0035] In this elution step, the hydrogen ion concentration of the acid-containing solution is 0.1 mol / L or more and 4.0 mol / L or less, so that Li + and H + This makes it possible to suppress the dissolution of the entire lithium manganate while maintaining the efficiency of the exchange reaction between cations. In other words, it becomes possible to reuse the lithium adsorbent repeatedly.

[0036] If the hydrogen ion concentration of the acid-containing solution is lower than 0.1 mol / L, the exchange reaction between cations cannot proceed sufficiently, resulting in a decrease in the efficiency of this exchange reaction. Furthermore, if the acid-containing solution is more concentrated than 4.0 mol / L, the entire lithium manganate dissolves in the acid-containing solution, making it impossible to reuse the lithium manganate as a lithium adsorbent after adsorption. The acid used in the acid-containing solution is preferably, but not limited to, hydrochloric acid. For example, sulfuric acid or acetic acid may also be used.

[0037] It is preferable that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and that the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less.

[0038] When the hydrogen ion concentration of the acid-containing solution in the first elution step and the hydrogen ion concentration of the acid-containing solution in the second elution step are set to predetermined values, dissolution of manganese from the lithium adsorbent can be suppressed and the efficiency of elution can be increased.

[0039] The contact form between the adsorbed lithium manganate and the acid-containing solution in the elution step varies depending on the form of the lithium manganate. For example, if the lithium manganate is in powder form, one method is to add the adsorbed lithium manganate powder to the acid-containing solution and stir it to bring the adsorbed lithium manganate and the acid-containing solution into contact. If the lithium manganate is in particulate form or sprayed onto the fibers of a column, one method is to place the particulate lithium manganate and the column in a liquid-passing container and pass the acid-containing solution through the liquid-passing container to bring the adsorbed lithium manganate and the acid-containing solution into contact.

[0040] (Manganese Oxidation Step) In the manganese oxidation step, an oxidizing agent and a pH adjuster are added to the elution solution obtained in the elution step to oxidize divalent manganese to tetravalent manganese, thereby obtaining a lithium-containing solution with a reduced manganese concentration. Tetravalent manganese is sparingly soluble, so it precipitates in the solution. This allows the manganese concentration in the elution solution to be reduced. Furthermore, the precipitated manganese can be reused as a raw material for a lithium adsorbent.

[0041] To oxidize divalent manganese to tetravalent manganese, an oxidizing agent and a pH adjuster are added to the elution solution. When the oxidizing agent and the pH adjuster are added, it is preferable to adjust the pH to a range of 3 to 7 and the redox potential to 600 mV to 1100 mV using a silver-silver chloride electrode. That is, the pH and the redox potential are measured simultaneously, and the oxidizing agent and the pH adjuster are added simultaneously or alternately so that they fall within the above range. Examples of oxidizing agents that can be used include sodium hypochlorite, sodium chlorite, ozone, and permanganate. However, they are not limited to these, and any agent capable of adjusting the redox potential can be used. Examples of pH adjusters that can be used include alkaline neutralizers such as sodium hydroxide and slaked lime. However, they are not limited to these, and any agent capable of adjusting the pH can be used.

[0042] (Post-Stage of Manganese Oxidation Step) In the lithium-containing solution obtained in the manganese oxidation step, lithium exists in the form of lithium chloride (LiCl) in this embodiment. Therefore, by adding an alkali to this solution or by concentrating it by superheating, lithium can be obtained in the form of, for example, lithium carbonate.

[0043] After the adsorption, the lithium manganate becomes a lithium adsorbent in the presence of an acid-containing solution, and this lithium adsorbent is reused in the adsorption step.

[0044] Second Embodiment Fig. 2 shows a flow diagram of a method for producing a lithium-containing solution according to a second embodiment of the present invention. The method for producing a lithium-containing solution according to the second embodiment differs from the method for producing a lithium-containing solution according to the first embodiment in that, in the elution step, the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution having a lower lithium concentration than the high-concentration lithium elution solution, the acid-containing solution contains a low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step contains a high-concentration lithium elution solution. Other points are the same as those in the first embodiment. Therefore, the following describes these differences.

[0045] (Elution Step in Second Embodiment) In this embodiment, the elution solution is separated into a high-concentration lithium elution solution and a low-concentration lithium elution solution in the elution step. The high-concentration lithium elution solution is an elution solution containing lithium at a high concentration, and the low-concentration lithium elution solution is an elution solution having a lower lithium concentration than the high-concentration lithium elution solution.

[0046] In this embodiment, the acid-containing solution in the elution step includes a solution of a simple acid such as hydrochloric acid, and a solution in which an acid is added to a low-concentration lithium elution solution.

[0047] The high-concentration lithium elution solution is an elution solution containing lithium at a high concentration, and is therefore used in a process carried out after the elution process, such as a manganese oxidation process.

[0048] By including a high-concentration lithium elution solution in the elution solution used in the manganese oxidation step, the lithium content of the elution solution used in the manganese oxidation step can be increased. Also, because only a low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by adding only a small amount of acid, which results in a reduction in the amount of acid-containing solution and therefore the amount of elution solution used in the manganese oxidation step. This reduces the production cost for lithium production.

[0049] For example, when the elution step is performed by batch processing, the separation of the high-concentration lithium elution solution and the low-concentration lithium elution solution can be performed by extracting a predetermined volume of elution solution from the point at which the elution solution begins to be obtained by adding an acid-containing solution, and using the extracted volume as the high-concentration lithium elution solution, and the remaining volume as the low-concentration lithium elution solution. For example, when it is possible to predict the type of low-concentration lithium-containing solution and the amount of lithium eluted from the lithium adsorbent, the elution solution with a volume that is a predetermined multiple of the volume of the lithium adsorbent can be used as the high-concentration lithium elution solution, and the subsequent elution solution can be used as the low-concentration lithium elution solution.

[0050] 5 shows a graph illustrating the lithium concentration for each predetermined volume fraction based on the start of the elution solution in this embodiment. The horizontal axis represents BV (Bed Volume: a unit representing the number of times the volume of the lithium adsorbent in the column), and the vertical axis represents the lithium concentration contained in the elution solution obtained after the elution step. For example, in the case shown in FIG. 5, BV2 and BV3, which exceed the second horizontal line from the top, can be extracted as "predetermined volumes based on the start of the elution solution," and the remaining BV1 and BV4 to BV9 can be separated as low-concentration lithium elution solutions.

[0051] The high-concentration lithium elution solution is the elution solution extracted by a predetermined volume based on the start of the elution solution being obtained, so that the lithium content of the high-concentration lithium elution solution can be increased.

[0052] In this embodiment, BV2 and BV3 are extracted to form the high-concentration lithium elution solution, but this is not limiting. For example, it is also possible to extract a predetermined volume from the beginning of the elution solution production, i.e., BV1 to BV4 can be used as the high-concentration lithium elution solution. It is also possible to use only BV3 as the high-concentration lithium elution solution.

[0053] Furthermore, for example, when the elution step is performed by batch processing and the flow rate of the acid-containing solution used in the elution step is a predetermined rate, the separation of the high-concentration lithium elution solution and the low-concentration lithium elution solution can be performed by using the elution solution obtained between a predetermined start time and end time after the start of the elution step as the high-concentration lithium elution solution, and the elution solution obtained thereafter as the low-concentration lithium elution solution. The flow rate is generally expressed as SV (Space Velocity: the amount of liquid passed per unit time (1 hour) BV). When this SV is constant, the high-concentration lithium elution solution can be used as the elution solution obtained between a predetermined start time and end time after the start of the elution step. The start of the elution step can be predetermined, such as when the acid-containing solution begins to be injected or when the elution solution begins to be recovered.

[0054] The high-concentration lithium elution solution can be easily obtained by being an elution solution obtained within a predetermined time period after the start of the elution step.

[0055] 3 shows a flow diagram of a method for producing a lithium-containing solution according to a third embodiment of the present invention. The method for producing a lithium-containing solution according to the third embodiment differs from the method for producing a lithium-containing solution according to the first embodiment in that a water-washing step for washing the eluted lithium adsorbent obtained through the elution step is provided after the elution step, and that the post-washing water obtained in the water-washing step is added to the acid-containing solution. The other points are the same as those in the first embodiment. Therefore, the above differences will be described below.

[0056] (Water-washing step) In the elution step in the second embodiment, an eluted lithium adsorbent is obtained. This eluted lithium adsorbent is washed in a water-washing step. In the water-washing step, for example, pure water is used, or industrial water is used in consideration of cost. The eluted lithium adsorbent washed in the water-washing step is regenerated as a lithium adsorbent, and this lithium adsorbent is used again in the adsorption step.

[0057] The post-rinsing water obtained after washing the lithium adsorbent after elution in the water washing step may contain lithium. For example, the post-rinsing water obtained immediately after starting washing has a relatively high lithium concentration. In this embodiment, this post-rinsing water is added to the acid-containing solution. It does not matter whether all or a portion of the post-rinsing water is added to the acid-containing solution. However, since the post-rinsing water obtained immediately after starting washing has a high lithium concentration, it is preferable to add a predetermined amount of the post-rinsing water to the acid-containing solution after starting washing.

[0058] 6 is a graph showing the lithium concentration for each predetermined volume fraction in this embodiment, with the start of the post-rinsing solution being used as a reference. The horizontal axis represents the BV of the post-rinsing solution, and the vertical axis represents the lithium concentration contained in the post-rinsing solution obtained after the rinsing step. For example, in this embodiment, it is preferable to use BV1 of the post-rinsing solution, i.e., the start of the post-rinsing solution being used as a reference, and to repeat the post-rinsing solution of only BV1 from the start of its production into the acid-containing solution.

[0059] The post-washing solution obtained in the water-washing step is added to the acid-containing solution, whereby lithium that would otherwise have been discarded in the water-washing step can be recovered.

[0060] (Fourth Embodiment) Fig. 4 shows a flow diagram of a method for producing a lithium-containing solution according to a fourth embodiment of the present invention. The method for producing a lithium-containing solution according to the fourth embodiment differs from the method for producing a lithium-containing solution according to the second embodiment in that a water-washing step for washing the eluted lithium adsorbent obtained through the elution step is provided after the elution step, and that the post-washing water obtained in the water-washing step is added to the acid-containing solution. The remaining points are the same as those of the second embodiment. A detailed description of the water-washing step is included in the description of the third embodiment. Therefore, a detailed description of the water-washing step will be omitted.

[0061] Specific examples of the method for producing a lithium-containing solution according to the present invention will be described below, but the present invention is not limited to these examples.

[0062] Example 1 (Adsorption step) Powdered lithium adsorbent H 1.6 Mn 1.6O 4 A 10 ml portion of the solution was held in a glass column having a diameter of 20 mm. A solution containing dissolved lithium, simulating salt lake brine, which is a low-concentration lithium-containing solution, was passed through the column to adsorb the lithium adsorbent and then the lithium manganate Li 1.6 Mn 1.6 O 4 The lithium concentration of the low-concentration lithium-containing solution was 0.7 g / L. In the adsorption step, the solution was passed through at SV15, and the low-concentration lithium-containing solution was passed through at BV30.

[0063] (Elution Step) The post-adsorption lithium manganate in the glass column was contacted with an acid-containing solution. In the first elution step, an acid-containing solution consisting solely of 1 mol / L hydrochloric acid was passed through the column for BV2. In the subsequent second elution step, the acid-containing solution was prepared by repeating the elution solution from the first elution step and adding hydrochloric acid to it to obtain a 0.5 mol / L solution. The flow rate was BV10 and the flow rate was SV15. That is, the second elution step was performed from BV3 to BV12, and the hydrogen ion concentration of the acid-containing solution was 0.5 mol / L. The solution flowing out of the column was separated into a high-concentration lithium elution solution containing a high concentration of lithium in the initial stage of elution and a low-concentration lithium elution solution in a later stage with a lower lithium concentration than the high-concentration lithium elution solution. In this example, the concentration of the high-concentration lithium elution solution was 6.5 g / L. The volume of the eluent solution was 120 ml because only BV12 was passed through. The manganese concentration in the eluent solution was 0.02 g / L.

[0064] (Manganese oxidation step) The eluate obtained in the elution step was used to carry out the manganese oxidation step. An oxidizing agent and a pH adjuster were used in this step to obtain a lithium-containing solution. The manganese concentration in this step was 0.0 g / L.

[0065] Comparative Example 1 In Comparative Example 1, the hydrogen ion concentration of all the acid-containing solutions in the elution step was set to 0.5 mol / L (initially, 0.5 mol / L using hydrochloric acid alone, and then 0.5 mol / L was obtained by adding hydrochloric acid to the elution solution that had been subjected to the elution step once). The parameters were the same as in Example 1. The concentration of the high-concentration lithium elution solution in Comparative Example 1 was 3.4 g / L. The volume of the elution solution at this time was 120 ml, the same as in Example 1. The manganese concentration of the elution solution at this time was 0.02 g / L.

[0066] Comparative Example 2 In Comparative Example 2, the hydrogen ion concentration of all the acid-containing solutions in the elution step was set to 1.0 mol / L (initially, 1.0 mol / L using hydrochloric acid alone, and then 1.0 mol / L was obtained by adding hydrochloric acid to the elution solution that had been subjected to the elution step once). The parameters were the same as in Example 1. The concentration of the high-concentration lithium elution solution in Comparative Example 2 was 5.2 g / L. The volume of the elution solution at this time was 120 ml, the same as in Example 1. The manganese concentration of the elution solution at this time was 0.06 g / L.

[0067] (Summary) With regard to the high-concentration lithium elution solution, in Example 1, the lithium concentration was 6.5 g / L, or more than 6.0 g / L, maintaining a high lithium concentration. In contrast, in Comparative Example 1, the lithium concentration was 3.4 g / L, and in Comparative Example 2, it was 5.2 g / L, less than 6.0 g / L, indicating a lower lithium concentration in the high-concentration lithium elution solution. Thus, since the lithium concentration of the high-concentration lithium elution solution in Example 1 is higher, it was found that the total amount of elution solution can be reduced when the final amount of lithium obtained is constant. Furthermore, in Example 1, the manganese concentration can also be reduced to a lower level compared to Comparative Example 2, indicating that deterioration of the lithium adsorbent can be suppressed.

[0068] The phrase "based on the start of acquisition" includes "based on the physical quantity at the start of acquisition," and physical quantities include concentration, time, volume, and the like.

Claims

1. A method for producing a lithium-containing solution, comprising the steps of: an adsorption step of contacting a low-concentration lithium-containing solution with a lithium adsorbent obtained from lithium manganate to obtain an adsorbed lithium manganate; an elution step of contacting the adsorbed lithium manganate with an acid-containing solution to obtain an elution solution; and a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the elution solution to oxidize manganese and obtain a lithium-containing solution having a reduced manganese concentration, wherein the elution step includes a first elution step and a second elution step in which the acid-containing solution has a lower hydrogen ion concentration than that of the first elution step, and the second elution step is performed after the first elution step.

2. The method for producing a lithium-containing solution according to claim 1, characterized in that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less.

3. The method for producing a lithium-containing solution according to claim 1 or 2, characterized in that the elution solution is separated in the elution step into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution having a lower lithium concentration than the high-concentration lithium elution solution, the acid-containing solution used in the elution step includes the low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step includes the high-concentration lithium elution solution.

4. The method for producing a lithium-containing solution according to claim 3, characterized in that the high-concentration lithium elution solution is an elution solution obtained by extracting a predetermined volume from the elution solution obtained through the elution process, based on the start of the elution solution being obtained.

5. The method for producing a lithium-containing solution according to claim 3, characterized in that the high-concentration lithium elution solution is the elution solution obtained between a predetermined start time and end time after the start of the elution process.

6. The method for producing a lithium-containing solution according to any one of claims 1 to 5, characterized in that a water-washing process for washing the eluted lithium adsorbent obtained after the elution process is provided after the elution process, and the post-washing liquid obtained in the water-washing process is added to the acid-containing solution.

Citation Information

Patent Citations

  • Recovery method of lithium

    JP2019044246A

  • Method for producing lithium hydroxide

    JP2023051387A

  • Lithium-containing solution production method

    WO2022210847A1