Polishing composition, method for producing same, and polishing method

The polishing composition, featuring abrasive grains with specific characteristics and a hydrophobic dispersion medium, addresses the trade-off between polishing time and surface quality, achieving efficient scratch removal and a superior finish by optimizing particle size distribution and surface area.

WO2024203251A1PCT designated stage expired Publication Date: 2024-10-03FUJIMI INCORPORATED

Patent Information

Application Number
PCT/JP2024/009426
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing polishing compositions for buffing resin coatings face a trade-off between polishing time and surface quality, where increasing processing power shortens polishing time but compromises surface finish, and reducing power lengthens time while improving finish, necessitating a high-performance composition that efficiently removes scratches with a good finished surface.

Method used

A polishing composition comprising abrasive grains with specific particle size distribution and specific surface area, combined with a hydrophobic dispersion medium and surfactant, optimized to enhance polishing rate and surface quality, including the use of aluminum oxide and other metal oxides, and a hydrophobic dispersion medium to improve processing efficiency.

Benefits of technology

The composition achieves a high polishing rate while minimizing scratches, resulting in a good finished surface with reduced color difference, effectively balancing efficiency and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009426_03102024_PF_FP_ABST
    Figure JP2024009426_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a high-performance polishing composition, a method for producing same, and a polishing method. The polishing composition contains abrasive particles, water, and a hydrophobic dispersion medium. In the particle size distribution of the abrasive particles, when the cumulative volume of the abrasive particles from the large particle size side in the cumulative particle size distribution on a volume basis becomes 10%, 50%, and 90%, respectively, are defined as D10, D50, and D90, respectively, the particle size distribution width (D10-D90) / D50 of the abrasive particles is 0.4 to 2.0, and the specific surface area (m2 / g) of the abrasive particles is 12 to 20.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing composition, its manufacturing method, and polishing method

[0001] The present invention relates to a polishing composition, a method for producing the same, and a polishing method.

[0002] Buffing is known as a processing method for smoothing and glossing the surface of a resin coating film coated on the surface of an automobile body, etc. Buffing is a processing method in which, for example, a cloth buff is pressed against an object to be polished (e.g., a resin coating film) with an abrasive composition interposed between the buff and the object to be polished, thereby polishing the surface.

[0003] The polishing composition used in buffing contains abrasive grains (abrasive material) and a surfactant, and the abrasive grains used are, for example, aluminum oxide (alumina) particles (see, for example, Patent Documents 1 to 3). Such a polishing composition makes it possible to remove scratches that have occurred on the surface of the object to be polished.

[0004] Japanese Patent Application Laid-Open No. 2008-255232 Japanese Patent Application Laid-Open No. 2008-127456 Japanese Patent Application Laid-Open No. 2007-277379

[0005] However, when the processing power of the polishing composition is increased in order to shorten the time required for removing scratches, the polishing time is shortened but the finished surface after polishing tends to be poor, and when the processing power is decreased, the finished surface is improved but the polishing time is lengthened, which is a contradictory problem. Therefore, there is a demand for a high-performance polishing composition that can efficiently remove scratches on the object to be polished while improving the finished surface after polishing.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-performance polishing composition, a method for producing the same, and a polishing method.

[0007] In order to solve the above problems, a polishing composition according to one aspect of the present invention comprises abrasive grains, water, and a hydrophobic dispersion medium. Regarding the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis is 10%, 50%, and 90%, respectively, are defined as D10, D50, and D90, the particle size distribution width of the abrasive grains (D10-D90) / D50 is 0.4 or more and 2.0 or less, and the specific surface area (m 2 / g) is 12 or more and 20 or less.

[0008] According to one aspect of the present invention, a high-performance polishing composition, a method for producing the same, and a polishing method can be provided.

[0009] FIG. 1 is a diagram showing an example of a polishing apparatus used in an embodiment of the present invention.

[0010] An embodiment of the present invention will be described in detail. Note that the following embodiment shows an example of the present invention, and the present invention is not limited to the embodiment. Furthermore, various modifications and improvements can be made to the following embodiment, and such modifications and improvements can also be included in the present invention.

[0011] <Polishing Composition> The polishing composition according to an embodiment of the present invention (hereinafter referred to as this embodiment) contains abrasive grains, water, and a hydrophobic dispersion medium. Regarding the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis is 10%, 50%, and 90%, respectively, are defined as D10, D50, and D90, the particle size distribution width of the abrasive grains (D10-D90) / D50 is 0.4 or more and 2.0 or less, and the specific surface area (m 2 / g) is 12 or more and 20 or less.

[0012] A polishing composition having such a configuration can achieve a high polishing rate and efficiently remove scratches on the object to be polished. It can also improve the finished surface of the object to be polished after polishing. For example, the polishing composition can reduce the number of processing scratches on the object to be polished or reduce the depth of processing scratches, thereby bringing the color difference ΔE of the finished surface closer to 0 (zero). Therefore, a high-performance polishing composition can be provided. The color difference ΔE will be explained in the examples below.

[0013] Hereinafter, each component contained in the polishing composition according to this embodiment will be described with examples. (1) Abrasive grains The polishing composition according to this embodiment contains abrasive grains. The abrasive grains come into contact with the surface of the object to be polished and have the effect of mechanically polishing the object to be polished. The polishing rate and the surface condition of the object to be polished after polishing (the condition of the finished surface) vary depending on the width of the particle size distribution of the abrasive grains and the degree of surface unevenness. Therefore, it is important to understand the particle size distribution of the abrasive grains and the degree of surface unevenness. Here, the specific surface area (m 2 The greater the degree of surface roughness, the larger the specific surface area tends to be.

[0014] Therefore, the present inventors have conducted extensive research and discovered that there are suitable numerical ranges in which the specific surface area of ​​the abrasive grains and the particle size distribution width (D10-D90) / D50 of the abrasive grains are both within specific ranges, making it possible to achieve a high polishing rate and a good finished surface after polishing.

[0015] In this embodiment, based on this discovery, the particle size distribution width (D10-D90) / D50 value of the abrasive grains and the value of the specific surface area are specified. In this embodiment, the particle size distribution width (D10-D90) / D50 of the abrasive grains is 0.4 or more and 2.0 or less, preferably 0.4 or more and 1.8 or less, and more preferably 0.4 or more and 1.6 or less. In addition, the specific surface area (m 2 / g) is 12 or more and 20 or less, preferably 12 or more and 18 or less, and more preferably 12 or more and 15 or less. If the particle size distribution width of the abrasive grains is smaller than the lower limit of the particle size distribution width, it is difficult to increase the polishing rate, and if it is larger than the upper limit, scratches are likely to occur on the object to be polished after polishing. In addition, the specific surface area (m 2 If the specific surface area (ratio of the surface area to the polishing composition) is less than the lower limit, scratches are likely to occur on the polished object, and if it is greater than the upper limit, the polishing rate is unlikely to be high. By setting both of these within the above ranges, the polishing composition can be polished at a high polishing rate and can provide a good polished surface finish. In other words, the polishing composition can have high performance.

[0016] Specific examples of abrasive grains used in this embodiment include metal oxides such as aluminum oxide (alumina), silicon oxide (silica), cerium oxide (ceria), zirconium oxide, titanium oxide (titania), tin oxide, manganese oxide, and iron oxide; metal carbides such as silicon carbide and titanium carbide; metal nitrides such as silicon nitride and titanium nitride; metal borides such as titanium boride and tungsten boride; zircon (ZrSiO 4 Examples of the abrasive grains include silicate compounds such as quartz, diamond, etc. These abrasive grains may be used alone or in combination of two or more. The abrasive grains may be commercially available or synthetic products.

[0017] Among these abrasive grains, at least one selected from the group consisting of metal oxides and metal carbides is preferred, from the viewpoint that grains with various particle sizes are readily available and an excellent polishing rate can be obtained, with silicon carbide, silicon dioxide, or a metal oxide being more preferred, and at least one of aluminum oxide (alumina), cerium oxide, and zirconium oxide being even more preferred, with aluminum oxide being particularly preferred. Also, a mixture of alumina and zirconium can be preferably used. In this specification, the term "polishing rate" may be rephrased as "polishing removal rate."

[0018] Furthermore, among aluminum oxides, the preferred crystalline structure for polishing grains is one containing an α-phase or a transitional crystalline phase, such as a θ-phase, δ-phase, or γ-phase, which is in the process of becoming the α-phase. Preferably, the α-phase or θ-phase is contained, and more preferably, the α-phase is contained. It is believed that there is an optimal range for the α-phase depending on the degree of α-phase formation.

[0019] Generally, the α-phase crystal structure is considered to be the hardest, but if sintered sufficiently at high temperatures to convert to the α-phase, it is estimated that the particle shape will change to a round shape and the polishing performance will decrease. The α-phase ratio serves as a reference value for expressing the degree of α-phase contained in aluminum oxide. A preferred lower limit of the α-phase ratio is 50% or more. A lower limit of the α-phase ratio is more preferably 60% or more, even more preferably 70% or more, particularly preferably 80% or more, and even more preferably 90% or more. Furthermore, a preferred upper limit of the α-phase ratio is 100% or less. A more preferred upper limit of the α-phase ratio is 98% or less. That is, the α-phase ratio of aluminum oxide is preferably 50% or more and 100% or less, and more preferably 60% or more and 98% or less.

[0020] By setting the α-conversion rate within the above preferred range, it is expected that the polishing power, i.e., the scratch removal speed will be increased and the polishing rate will be improved. The α-conversion rate of the aluminum oxide particles can be calculated from the integrated intensity ratio of the (113) plane diffraction line by X-ray diffraction measurement using an X-ray diffractometer (Ultima-IV, manufactured by Rigaku Corporation).

[0021] The lower limit of the volume average particle diameter (average secondary particle diameter) of the abrasive grains is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. By making the volume average particle diameter (average secondary particle diameter) of the abrasive grains 0.05 μm or more, the polishing rate can be improved and the object to be polished can be polished well in both rough polishing and finish polishing.

[0022] The upper limit of the volume average particle size (average secondary particle size) of the abrasive grains is preferably 15 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less, particularly preferably 4 μm or less, and most preferably 3 μm or less. As the volume average particle size (average secondary particle size) of the abrasive grains becomes smaller, it becomes easier to obtain a good finished surface after polishing.

[0023] Therefore, by setting the volume average particle diameter (average secondary particle diameter) of the abrasive grains to 0.05 μm or more and 15 μm or less (or 0.05 μm or more and 10 μm or less), the polishing rate can be improved while providing a good finished surface after polishing.

[0024] It is also possible to use abrasive grains that have a large particle size before polishing but that become smaller at the interface between the buff and the object to be polished during polishing (abrasive grains in which secondary particles break down to primary particles during polishing). Based on the above, the volume average particle size (average secondary particle size) of the abrasive grains is preferably 0.05 μm to 15 μm (or 0.05 μm to 10 μm), more preferably 0.1 μm to 10 μm, even more preferably 0.2 μm to 5 μm, particularly preferably 0.2 μm to 4 μm, and most preferably 0.2 μm to 3 μm. In one embodiment, the volume average particle size (average secondary particle size) of the abrasive grains is 0.05 μm to 10 μm, 0.2 μm to 4 μm, or 0.2 μm to 3 μm.

[0025] In this specification, the volume average particle size of abrasive grains is defined as the cumulative 50% particle size (D50) based on a volume-based particle size distribution. The D50 of abrasive grains can be measured using a commercially available particle size measuring device. Such particle size measuring devices may be based on any of methods such as dynamic light scattering, laser diffraction, laser scattering, or pore electrical resistance. Examples of methods and devices for measuring D50 include the measuring methods and measuring devices described in the Examples.

[0026] The lower limit of the content of abrasive grains in the polishing composition is preferably 0.1 mass % or more, more preferably 1 mass % or more, even more preferably 5 mass % or more, particularly preferably 7 mass % or more, and most preferably 10 mass % or more, based on the total mass of the polishing composition. By having the content of abrasive grains be 0.1 mass % or more, the polishing rate is improved, and the object to be polished can be polished well in both rough polishing and finish polishing.

[0027] The upper limit of the content of abrasive grains in the polishing composition is preferably 50% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, particularly preferably 20% by mass or less, and most preferably 15% by mass or less, based on the total mass of the polishing composition. By making the content of abrasive grains 50% by mass or less, the production cost of the polishing composition can be reduced, and the finished surface after polishing can be made good.

[0028] In a preferred embodiment, the abrasive grains are contained in an amount of 5 mass % or more and 30 mass % or less based on the total mass of the polishing composition.

[0029] (2) Other Examples of Abrasive Grains In addition to the above-described configuration, the abrasive grains of this embodiment may have a specific surface area (m 2 Alternatively, abrasive grains may be used in which the value of the shape parameter K, calculated by dividing the particle diameter D50 (μm) by the square of the particle diameter D50 (μm), is 0.6 or more and 69 or less. D50 is the particle diameter at which the cumulative volume from the large particle diameter side of the cumulative particle diameter distribution on a volume basis is 50%. D50 can be measured using a commercially available particle size measuring device.

[0030] In these examples, the abrasive grains may also contain, for example, aluminum oxide. As the alumina oxide, it is preferable to use sintered alumina, which has a more uneven surface than fused alumina.

[0031] By polishing the surface of an object to be polished using a polishing composition containing such abrasive grains, the object can be polished at a high polishing rate and the finished surface after polishing can be made good.

[0032] (3) Hydrophobic Dispersion Medium The polishing composition according to this embodiment contains a hydrophobic dispersion medium. The hydrophobic dispersion medium contains, for example, at least one selected from the group consisting of normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons. The hydrophobic dispersion medium preferably has a vapor pressure of 0.004 kPa or more and 2 kPa or less at 20°C. The hydrophobic dispersion medium preferably has a flash point of 30°C or more and 100°C or less. Use of such a hydrophobic dispersion medium improves the processing efficiency (polishing removal rate) when buffing a resin coating film. Hereinafter, the normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons that may be contained in the hydrophobic dispersion medium may be referred to as "organic solvents."

[0033] The hydrophobic dispersion medium and organic solvent in this embodiment are preferably those that are not easily soluble in water. Note that the hydrophobic dispersion medium and organic solvent that can be used may be commercially available products or synthetic products.

[0034] The normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons are preferably derived from mineral oil, and may be obtained by extracting and refining components derived from mineral oil, or may be synthesized using components derived from mineral oil as raw materials (synthetic hydrocarbons derived from mineral oil). The normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons are more preferably synthetic hydrocarbons derived from mineral oil. These hydrophobic organic solvents are generally known to be less toxic than other halogen-based or benzene-based organic solvents, and more volatile than other polyethylene glycols, etc.

[0035] Examples of normal paraffin hydrocarbons include linear hydrocarbons having from 5 to 30 carbon atoms, liquid paraffin, kerosene, and diesel.

[0036] Examples of isoparaffin hydrocarbons include branched hydrocarbons having 5 to 40 carbon atoms, and liquid isoparaffin.

[0037] Examples of naphthenic hydrocarbons include cyclic hydrocarbons having from 5 to about 40 carbon atoms, such as monocyclic cycloparaffins such as cyclohexane, cyclopentane, and cyclononane; polycyclic cycloparaffins such as decalin; and alkylcycloparaffins such as methylcyclopentane, methylcyclohexane, 1-methyl-4-isopropylcyclohexane, butylcyclohexane, and methyldecalin.

[0038] Examples of terpene hydrocarbons include chain terpene hydrocarbons such as myrcene, farnesene, and citral; and cyclic terpene hydrocarbons such as menthol, cineole, pinene, limonene, α-terpinene, γ-terpinene, camphene, phellandrene, terpinene, terpinolene, p-cymene, and cedrene.

[0039] The hydrophobic dispersion medium may further contain an organic solvent other than the above hydrocarbons. Hereinafter, organic solvents other than normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons are referred to as "other organic solvents." Examples of such other organic solvents include methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, diethyl ether, ethyl acetate, butyl acetate, triethyl citrate, acetyltributyl citrate, and acetyltriethyl citrate.

[0040] Hydrophobic dispersion media (organic solvents) generally have a flash point. The flash point is the lowest temperature at which a liquid generates a sufficient concentration of vapor to instantly ignite when heated at a constant temperature and brought close to a flame. The flash point can also be said to be the lowest temperature at which the hydrophobic dispersion medium volatilizes and forms a flammable mixture with air. There are various methods for measuring flash point, depending on the purpose of the measurement and the properties of the sample. Flash point measurement methods include the closed-cell method and the open-cell method. Examples of closed-cell methods include the Tag closed-cell method (JIS K 2265-1:2007), the Seta closed-cell method (JIS K 2265-2:2007), and the Pensky-Martens closed-cell method (JIS K 2265-3:2007). Examples of open-cell methods include the Cleveland open-cell method (JIS K 2265-4:2007).

[0041] (4) Water The polishing composition according to this embodiment contains water. From the viewpoint of preventing the action of other components from being inhibited, the water preferably contains as few impurities as possible. Specifically, pure water or ultrapure water obtained by removing impurity ions with an ion exchange resin and then passing the water through a filter to remove foreign matter, or distilled water is preferred.

[0042] The lower limit of the water content in the polishing composition is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, particularly preferably 15% by mass or more, and most preferably 20% by mass or more, based on the total mass of the polishing composition. The upper limit of the water content in the polishing composition is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, particularly preferably 75% by mass or less, and most preferably 70% by mass or less, based on the total mass of the polishing composition.

[0043] That is, the water content in the polishing composition is preferably 1% by mass or more and 90% by mass or less, more preferably 5% by mass or more and 85% by mass or less, even more preferably 10% by mass or more and 80% by mass or less, particularly preferably 15% by mass or more and 75% by mass or less, and most preferably 20% by mass or more and 70% by mass or less. By having the water content in the above range, the polishing rate can be improved, and the object to be polished can be polished well in both rough polishing and finish polishing.

[0044] (5) Surfactant The polishing composition according to this embodiment contains a surfactant. The surfactant disperses or emulsifies a hydrophobic dispersion medium or water. The surfactant also imparts hydrophilicity to the polished surface after polishing, thereby improving the cleaning efficiency of the polished surface after polishing and preventing the adhesion of dirt to the polished surface.

[0045] The surfactant contained in the polishing composition of the present invention is one or more selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Of these, nonionic surfactants are preferred as the surfactant contained in the polishing composition. These surfactants may be used alone or in combination of two or more. Examples of anionic surfactants include polyoxyethylene alkyl ether acetic acid, polyoxyethylene alkyl sulfate, alkyl sulfate, polyoxyethylene alkyl ether sulfate, alkyl ether sulfate, alkyl benzene sulfonic acid, alkyl phosphate, polyoxyethylene alkyl phosphate, polyoxyethylene sulfosuccinic acid, alkyl sulfosuccinic acid, alkyl naphthalene sulfonic acid, alkyl diphenyl ether disulfonic acid, and salts thereof.

[0046] Examples of cationic surfactants include alkyltrimethylammonium salts, alkyldimethylammonium salts, alkylbenzyldimethylammonium salts, and alkylamine salts.

[0047] Examples of amphoteric surfactants include alkyl betaines and alkyl amine oxides.

[0048] Examples of nonionic surfactants include polyoxyalkylene alkyl ethers such as polyoxyethylene alkyl ethers, sorbitan fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, and alkylalkanolamides.

[0049] When the hydrophobic dispersion medium in the polishing composition of the present invention contains an isoparaffinic hydrocarbon, the surfactant is preferably a polyoxyalkylene alkyl ether (HLB=10-14) from the viewpoint of emulsion stability. Here, the HLB (Hydrophilic-Lipophilic Balance) value represents the degree of affinity of the surfactant for water and oil (a water-insoluble organic compound). Examples of polyoxyalkylene alkyl ethers include alkyl ethers having 10 to 20 carbon atoms to which polyoxyethylene is added, such as polyoxyethylene lauryl ether, polyoxyethylene myristyl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, and polyoxyethylene octyldodecyl ether. The number of moles of polyoxyethylene added to the polyoxyalkylene alkyl ether may be such that the HLB is 10 to 14.

[0050] The content of surfactant in the polishing composition is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, based on the total mass of the polishing composition.The content of surfactant in the polishing composition is preferably 3.0 mass% or less, more preferably 2.0 mass% or less, based on the total mass of the polishing composition.When the content of surfactant is within the above range, the stability of emulsion in the polishing composition is improved.

[0051] For example, the HLB value, which indicates the affinity of a surfactant for water and oil, is 10 or more and 16 or less, and preferably 10 or more and 14 or less.

[0052] (6) Other Examples of Surfactants The surfactant of this embodiment is a compound represented by the formula (i) RO-(AO) n The compound may contain a polyoxyethylene alkyl ether represented by -H. In formula (i), R is a branched alkyl group having from 12 to 20 carbon atoms. n represents the average number of moles of AO added, and is from 3 to 50. The average number of moles of AO added, n, is more preferably from 5 to 20, and even more preferably from 5 to 15. AO refers to alkylene oxide.

[0053] A surfactant containing a polyoxyethylene alkyl ether represented by formula (i) disperses or emulsifies a hydrophobic dispersion medium or water. Furthermore, this surfactant imparts hydrophilicity to the polished surface after polishing, thereby improving the cleaning efficiency of the polished surface after polishing and preventing the adhesion of dirt to the polished surface. Furthermore, this surfactant contributes to the stability of the emulsion after emulsification.

[0054] The surfactant of this embodiment contains, as the polyoxyethylene alkyl ether represented by formula (i), at least one selected from the group consisting of polyoxyethylene alkyl ethers (C12-14 secondary alcohols), polyoxyethylene octyldodecyl ether, and polyoxyethylene 2-hexyldecyl ether. C12-14 indicates that in the polyoxyethylene alkyl ether represented by formula (i), R has 12, 13, or 14 carbon atoms, or a mixture of two or more of these (the same applies hereinafter).

[0055] The polyoxyethylene alkyl ether represented by formula (i) may also be called a polyoxyethylene secondary alcohol ether, a secondary alcohol ethoxylate (secondary alcohol ethoxylate), a polyoxyethylene alkyl ether (secondary alcohol), or a polyoxyethylene secondary alkyl ether. Regardless of the name, it has the same structure as the polyoxyethylene alkyl ether represented by formula (i).

[0056] (7) Various Additives The polishing composition of this embodiment may contain various additives, such as a pH adjuster, a polishing accelerator, an oxidizing agent, a dispersant, a viscosity adjuster, a complexing agent, an anticorrosive agent, and an antifungal agent, in order to improve its performance. Examples of additives that can be blended into the polishing composition of this embodiment are described below.

[0057] (7.1) pH adjuster The polishing composition according to this embodiment may contain a pH adjuster. The pH value of the polishing composition can be adjusted by adding a pH adjuster. The pH adjuster used as needed to adjust the pH value of the polishing composition to a desired value may be either an acid or an alkali, and may be either an inorganic compound or an organic compound.

[0058] Specific examples of acids that can be used as pH adjusters include inorganic acids and organic acids such as carboxylic acids and organic sulfuric acids. Specific examples of inorganic acids include sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Specific examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid. Specific examples of organic sulfuric acids include methanesulfonic acid, ethanesulfonic acid, and isethionic acid. These acids may be used alone or in combination of two or more.

[0059] Specific examples of bases as pH adjusters include alkali metal hydroxides or salts thereof, alkaline earth metal hydroxides or salts thereof, quaternary ammonium hydroxides or salts thereof, ammonia, amines, and the like.

[0060] Specific examples of alkali metals include potassium and sodium. Specific examples of alkaline earth metals include calcium and strontium. Specific examples of salts include carbonates, bicarbonates, sulfates, acetates, etc. Specific examples of quaternary ammonium include tetramethylammonium, tetraethylammonium, and tetrabutylammonium.

[0061] The quaternary ammonium hydroxide compound includes quaternary ammonium hydroxide or a salt thereof, and specific examples thereof include tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrabutylammonium hydroxide.

[0062] Further, specific examples of the amine include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, guanidine, etc. These bases may be used alone or in combination of two or more.

[0063] Among these bases, ammonia, ammonium salts, alkali metal hydroxides, alkali metal salts, quaternary ammonium hydroxide compounds, and amines are preferred, and ammonia, potassium compounds, sodium hydroxide, quaternary ammonium hydroxide compounds, ammonium hydrogen carbonate, ammonium carbonate, sodium hydrogen carbonate, and sodium carbonate are more preferred.

[0064] From the viewpoint of preventing metal contamination, the polishing composition preferably contains a potassium compound as a base. Examples of the potassium compound include potassium hydroxides and potassium salts, such as potassium hydroxide, potassium carbonate, potassium bicarbonate, potassium sulfate, potassium acetate, and potassium chloride.

[0065] Alternatively, instead of or in combination with the above-mentioned acids, salts such as ammonium salts or alkali metal salts of the above-mentioned acids may be used as pH adjusters that function as buffers. In particular, when the acid and buffer are combined as a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base, a pH buffering effect can be expected.

[0066] (7.2) Polishing Accelerator (Oxidizing Agent) The polishing composition according to this embodiment may contain a polishing accelerator. The polishing accelerator serves to chemically polish the object to be polished, and by acting on the outer surface of the resin coating film, can significantly increase the polishing rate.

[0067] Specific examples of the polishing accelerator include at least one salt selected from the group consisting of metal salts of inorganic acids, metal salts of organic acids, ammonium salts of inorganic acids, and ammonium salts of organic acids.

[0068] The inorganic acid may be any of nitric acid, sulfuric acid, and hydrochloric acid. The organic acid may be any of oxalic acid, lactic acid, acetic acid, formic acid, citric acid, tartaric acid, malic acid, gluconic acid, glycolic acid, and malonic acid. The metal salt may be any of aluminum salt, nickel salt, lithium salt, magnesium salt, sodium salt, and potassium salt. These polishing accelerators may be used alone or in combination of two or more.

[0069] An oxidizing agent may also be added as a polishing accelerator. Specific examples of the oxidizing agent include hydrogen peroxide, peroxide, nitrate, iodate, periodate, hypochlorite, chlorite, chlorate, perchlorate, persulfate, dichromate, permanganate, ozone water, silver(II) salt, and iron(III) salt.

[0070] (7.3) Dispersant / Viscosity Adjuster (Thickener) The polishing composition according to this embodiment may contain a dispersant or a thickener. The dispersant or the thickener uniformly disperses the abrasive grains (abrasive) in the liquid, thereby allowing the abrasive grains to act efficiently on the object to be polished, thereby contributing to an improvement in the polishing rate. Furthermore, the presence of the dispersant or the thickener between the abrasive grains can be expected to suppress caking of the abrasive grains. This suppresses the occurrence of scratches (processing flaws) caused by agglomerated abrasive grains.

[0071] Specific examples of dispersants include colloidal substances containing fine particles, such as colloidal alumina, colloidal silica, colloidal zirconia, colloidal titania, alumina sol, silica sol, zirconia sol, titania sol, fumed alumina, fumed silica, fumed zirconia, fumed titania, etc. Commonly used dispersants such as sodium phosphate, sodium hexametaphosphate, and sodium pyrophosphate may also be used.

[0072] Specific examples of thickeners include glycols such as propylene glycol polymers and ethylene glycol polymers, and polymeric compounds. More specifically, glycols include propylene glycol, ethylene glycol, dipropylene glycol, polypropylene glycol, diethylene glycol, polyethylene glycol, etc. Polymeric compounds include sodium polyacrylate, polyvinyl alcohol, hydroxyethyl cellulose, etc.

[0073] (7.4) Complexing Agent The polishing composition according to this embodiment may contain a complexing agent having a chelating effect. The complexing agent traps metal ions and the like derived from the polishing apparatus, the object to be polished, etc., and is therefore expected to suppress metal contamination of the polished surface by metal ions and to provide a good polished surface finish.

[0074] Examples of the complexing agent include organic acids, amino acids, nitrile compounds, and other chelating agents. Specific examples of the organic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, and citric acid. A salt such as an alkali metal salt of an organic acid may be used instead of or in combination with the organic acid.

[0075] Specific examples of amino acids include glycine, α-alanine, β-alanine, N-methylglycine, N,N-dimethylglycine, 2-aminobutyric acid, norvaline, valine, leucine, norleucine, isoleucine, phenylalanine, proline, sarcosine, ornithine, lysine, taurine, serine, threonine, homoserine, tyrosine, bicine, tricine, 3,5-diiodo-tyrosine, β-(3,4-dihydroxyphenyl)-alanine, thyroxine, Examples include 4-hydroxy-proline, cysteine, methionine, ethionine, lanthionine, cystathionine, cystine, cysteic acid, aspartic acid, glutamic acid, S-(carboxymethyl)-cysteine, 4-aminobutyric acid, asparagine, glutamine, azaserine, arginine, canavanine, citrulline, δ-hydroxy-lysine, creatine, histidine, 1-methyl-histidine, 3-methyl-histidine, and tryptophan.

[0076] Specific examples of the nitrile compound include acetonitrile, aminoacetonitrile, propionitrile, butyronitrile, isobutyronitrile, benzonitrile, glutarodinitrile, and methoxyacetonitrile.

[0077] Specific examples of chelating agents other than these include iminodiacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetraacetic acid, N,N,N-trimethylenephosphonic acid, ethylenediamine-N,N,N',N'-tetramethylenesulfonic acid, transcyclohexanediaminetetraacetic acid, 1,2-diaminopropanetetraacetic acid, glycol ether diaminetetraacetic acid, ethylenediamine orthohydroxyphenylacetic acid, ethylenediamine disuccinic acid (SS form), N-(2-carboxylate ethyl)-L-aspartic acid, β-alaninediacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, N,N'-bis(2-hydroxybenzyl)ethylenediamine-N,N'-diacetic acid, 1,2-dihydroxybenzene-4,6-disulfonic acid, etc. These complexing agents may be used alone or in combination of two or more.

[0078] (7.5) Regarding Anticorrosive Agents The polishing composition according to this embodiment may contain an anticorrosive agent. The anticorrosive agent forms a protective film on the metal surface, and is therefore expected to prevent corrosion of the polishing apparatus, the object to be polished, the fixture, etc.

[0079] Usable anticorrosive agents are not particularly limited, and include, for example, heterocyclic compounds or surfactants. The number of members of the heterocyclic ring in the heterocyclic compound is not particularly limited. The heterocyclic compound may be a monocyclic compound or a polycyclic compound having condensed rings. The anticorrosive agents may be used alone or in combination of two or more.

[0080] Specific examples of heterocyclic compounds that can be used as anticorrosive agents include nitrogen-containing heterocyclic compounds such as pyrrole compounds, pyrazole compounds, imidazole compounds, triazole compounds, tetrazole compounds, pyridine compounds, pyrazine compounds, pyridazine compounds, pyrindine compounds, indolizine compounds, indole compounds, isoindole compounds, indazole compounds, purine compounds, quinolizine compounds, quinoline compounds, isoquinoline compounds, naphthyridine compounds, phthalazine compounds, quinoxaline compounds, quinazoline compounds, cinnoline compounds, buteridine compounds, thiazole compounds, isothiazole compounds, oxazole compounds, isoxazole compounds, and furazan compounds.

[0081] (7.6) Antifungal Agent, Preservative The polishing composition according to this embodiment may contain an antifungal agent or a preservative. Specific examples of the antifungal agent or preservative include isothiazolin-based preservatives (e.g., 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one), paraoxybenzoic acid esters, and phenoxyethanol. These antifungal agents and preservatives may be used alone or in combination of two or more.

[0082] <Method for producing polishing composition> The method for producing a polishing composition according to this embodiment includes a step of producing a polishing composition by mixing abrasive grains, a hydrophobic dispersion medium, and water. Regarding the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis is 10% and 90% are respectively defined as D10 and D90, the particle size distribution width (D10-D90) / D50 of the abrasive grains is 0.4 or more and 2.0 or less, and the specific surface area (m 2 / g) is 12 or more and 20 or less.

[0083] This makes it possible to produce a high-performance polishing composition that can polish an object to be polished at a high polishing rate and also can produce a good finished surface after polishing.

[0084] In this manufacturing method, it is preferable to mix a hydrophobic dispersion medium and a surfactant in advance, and then mix them with water and abrasive grains. Also, when the polishing composition of the present invention contains a hydrophilic component such as a thickener or an emulsion stabilizer, it is preferable to mix a hydrophobic dispersion medium and a surfactant in advance to prepare a hydrophobic mixture, and mix water and a hydrophilic component to prepare a hydrophilic mixture, and then mix the hydrophobic mixture, the hydrophilic mixture, and the abrasive grains.

[0085] Furthermore, when the polishing composition of the present invention contains other components such as a pH adjuster, after mixing the hydrophobic dispersion medium, surfactant, water, and abrasive grains, other components such as the pH adjuster may be stirred and mixed, if necessary.

[0086] The temperature at which the components are mixed is not particularly limited, but is preferably, for example, 10° C. or higher and 40° C. or lower. The mixing time is not particularly limited.

[0087] (1) Specific Examples of Methods for Producing Abrasive Grains Specific examples of methods for producing abrasive grains (secondary particles) will be further described. As described above, in this embodiment, the abrasive grains may be aluminum oxide (alumina). While the method for producing alumina is not particularly limited, one example involves appropriately pulverizing and / or classifying powder obtained by firing a starting material such as an aluminum oxide precursor powder. The shape of the abrasive grains, including the degree of surface irregularities, can be controlled by the type of aluminum oxide starting material and the firing conditions.

[0088] The aluminum oxide precursor powder can be aluminum hydroxide powder or aluminum oxide powder containing a transitional aluminum oxide phase. The aluminum hydroxide powder can be gibbsite, boehmite, pseudoboehmite, diaspore, or any combination thereof. The aluminum oxide precursor powder can include gamma (γ), eta (η), theta (θ), chi (χ), (kappa), κ, and / or delta (δ) phase aluminum oxide.

[0089] Aluminum oxide (alumina) can be formed by calcining the aluminum oxide precursor powder. The calcination method is not particularly limited, but examples include a rotary kiln, tunnel kiln, electric furnace, muffle furnace, elevator kiln, and pusher kiln. The calcination conditions include a calcination temperature of approximately 700 to 1600°C and a calcination time of approximately 1 to 48 hours. This allows for the production of α-alumina with a suitable α-conversion rate. The higher the calcination temperature and the longer the calcination time, the smaller the surface roughness, i.e., the smaller the specific surface area.

[0090] The calcined alumina powder can be crushed and classified to obtain alumina having a desired particle size distribution. Crushing and classification can be carried out by wet or dry processes.

[0091] As examples of the pulverization method, various devices can be used, including a roller mill, a jet mill, a high-speed rotary pulverizer, and a container-driven mill. By changing the pulverization conditions, such as the pulverization time, in each device, alumina having a desired particle size distribution can be obtained.

[0092] Examples of classification methods that can be used include filtering, sieving, air classification, elutriation classification, weight classification, inertial classification, and centrifugal classification. Examples of filtering methods that can be used include coarse filtration, microfiltration, ultrafiltration, and reverse osmosis. Examples of filters used for filtering include mesh filters, depth filters, and membrane filters. In filtering, the particle size distribution of the powder can be controlled by the filtration time, filtration rate, and filtration accuracy. For example, the filtration accuracy can be 0.1 to 300 μm.

[0093] By appropriately selecting and / or combining one or more of the above-mentioned firing method, pulverization method, and classification / filtering method and controlling the respective conditions, it is possible to obtain alumina having a desired particle size distribution and specific surface area. This allows the particle size distribution width (D10-D90) / D50 of the abrasive grains to be 0.4 or more and 2.0 or less, and the specific surface area (m 2 It is possible to obtain alumina having a molecular weight of 12 or more and 20 or less.

[0094] <Object to be polished> The object to be polished according to this embodiment is not particularly limited, but preferably includes at least one selected from the group consisting of alloy materials, resin materials, metals, semi-metals, metal oxides, metal carbides, metal nitrides, semi-metal oxides, semi-metal carbides, semi-metal nitrides, and glass materials, and may also be a composite material of these materials. In particular, resin materials (resin coatings) used on painted surfaces such as automobile bodies are preferred. In other words, the polishing composition of this embodiment is preferably used for polishing resins.

[0095] The type of resin coating film is not particularly limited, but the resin constituting the resin coating film is preferably, for example, a urethane resin or an acrylic resin, and the type of resin may be a urethane resin, an acrylic resin, or a mixture thereof. Furthermore, the resin coating film may be a transparent clear coating film. Furthermore, the thickness of the resin coating film is not particularly limited, but may be 100 μm or less, or may be 10 μm or more and 40 μm or less. The hardness of the resin can be adjusted by the drying temperature, and generally, it can be soft at a drying temperature of around 60 ° C and hard at a drying temperature of around 140 ° C. If the polishing composition according to this embodiment is applied to the buffing process of such a resin coating film, the resin coating film can be polished at a high polishing rate, and the finished surface of the resin coating film after polishing can be made good.

[0096] The polishing composition of this embodiment can be used to produce a coated member in which a resin coating film is coated on the surface of a substrate. By using the polishing composition of this embodiment to polish the outer surface of the resin coating film of a coated member, it is possible to produce a coated member having a resin coating film with a beautiful luster and in which cloudiness is unlikely to remain on the surface of the object to be polished, even if a long time is allowed to pass before wiping.

[0097] The type of painted member (i.e., the application of the resin coating film) is not limited to the body of an automobile. The type of painted member is not particularly limited, and examples thereof include railway vehicles, aircraft, and resin members.

[0098] <Polishing Method> The polishing method according to this embodiment includes a step of polishing an object to be polished with the polishing composition or the polishing composition obtained by the production method described above.

[0099] In the step of polishing an object to be polished, for example, a polishing composition is supplied to the surface of the resin coating film of the object to be polished, and the surface to which the polishing composition has been supplied is polished by contacting a polishing buff with the polishing composition. As the polishing buff, for example, a wool buff, a sponge buff, or both are used.

[0100] The configuration of the polishing device is not particularly limited, and may be a general polishing device such as a polisher that can be held by the operator (hereinafter also referred to as a hand polisher), a single-sided polishing machine, a double-sided polishing machine, a lens polishing machine, a vertical electric polishing machine, or a grinder, or an automatic polishing device.

[0101] When using a hand polisher, an operator manually operates the hand polisher to polish the surface of an object to be polished (e.g., a resin coating). The driving means of the hand polisher is not particularly limited, but generally, single action, double action, gear action, etc. are used, and double action is preferred for polishing resin coatings.

[0102] When an automatic polishing device is used, the automatic polishing device moves a robot arm under the control of a controller to polish the surface of an object to be polished (for example, a resin coating).

[0103] <Polishing Apparatus> Fig. 1 is a diagram showing an example of a polishing apparatus used in an embodiment of the present invention. The automatic polishing apparatus 1 in Fig. 1 includes a robot arm 2, a polishing buff 10, a polishing tool 4, a pressing force detection unit 5, and a controller 7. The robot arm 2 has multiple joints 20, 21, and 22, and therefore can move a tip 23 to which the polishing buff 10, the polishing tool 4, and the pressing force detection unit 5 are attached in multiple directions. The object 90 to be polished is, for example, a vehicle body such as an automobile, the surface of which is coated with a resin coating.

[0104] The polishing tool 4 is attached to the tip 23 via a pressing force detection unit 5, and a built-in driving means rotates the polishing buff 10 around a rotation axis perpendicular to the polishing surface 10a of the polishing buff 10. A controller 7 controls the behavior of the robot arm 2 and the rotation of the polishing buff 10 by the polishing tool 4. A polishing composition supply mechanism (not shown) supplies a polishing composition between the polishing surface 10a of the polishing buff 10 and the resin-coated surface of the object 90 to be polished.

[0105] The controller 7 polishes the resin-coated surface by pressing the polishing surface 10 a of the polishing buff 10 against the resin-coated surface of the object 90 to be polished using the robot arm 2 and rotating the polishing buff 10. The pressing force detection unit 5 detects the pressing force of the polishing surface 10 a of the polishing buff 10 against the resin-coated surface. The controller 7 may adjust the force pressing the polishing surface 10 a against the resin-coated surface based on the pressing force detection result by the pressing force detection unit 5. Furthermore, the controller 7 may control the robot arm 2 based on the pressing force detection result by the pressing force detection unit 5 so that the polishing buff 10 moves over the resin-coated surface while maintaining a constant pressing force of the polishing surface 10 a against the resin-coated surface.

[0106] There are no particular limitations on the material of the polishing buff 10, and general nonwoven fabric, suede, wool buff, woven fabric, polyurethane foam, polyethylene foam, porous fluororesin, etc. can be used without particular limitations. The polishing buff 10 that can be used has grooves on the polishing surface 10a for collecting the liquid polishing composition.

[0107] <Examples> The present invention will be described in more detail below with reference to examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. The steps of polishing an object to be polished using the polishing compositions of the following examples and comparative examples were carried out under conditions of room temperature (20°C or higher and 25°C or lower) and relative humidity of 30% RH or higher and 50% RH or lower.

[0108] Table 1 shows the constitution (type, particle size distribution width (D10-D90) / D50, specific surface area SA, secondary particle diameter (D10, D50, D90)) of the polishing compositions according to the examples of the present invention and comparative examples, the polishing rate and color difference ΔE when polishing with a double action using a wool buff, and the polishing rate and color difference ΔE when polishing with a double action using a sponge buff.

[0109] (Preparation of Polishing Compositions of Examples 1 to 3 and Comparative Examples 1 to 4) A hydrophobic dispersion medium solution was prepared by adding 1.6 wt % of a surfactant to 16% by mass (hereinafter, wt %) of a hydrophobic dispersion medium. Next, 1.0 wt % of a polyacrylic acid-based polymer (thickener) and 2.0 wt % of glycerin (emulsion stabilizer) were mixed with water, and the resulting solution was added to the hydrophobic dispersion medium solution and stirred at room temperature (25°C). Thereafter, 12 wt % of abrasive grains shown in Table 1 was added. A preservative was added to the resulting dispersion, and sodium hydroxide was added as an alkali to adjust the pH to 9.0, to prepare the polishing compositions of Examples 1 to 3 and Comparative Examples 1 to 4 as O / W emulsions. In Table 1, columns marked with - indicate that no data is available.

[0110]

[0111] In Examples 1 to 3 and Comparative Examples 1 to 4, the following abrasive grains, hydrophobic dispersion medium, and surfactants were used.

[0112] (Abrasive grains) Abrasive grains having a composition of aluminum oxide (alumina) and an alpha conversion rate of 95% were used in each of Examples 1 to 3 and Comparative Examples 1 to 4. The particle size distribution width (D10-D90) / D50, specific surface area SA, and secondary particle diameter (D10, D50, D90) of the abrasive grains are as shown in Table 1.

[0113] The alpha phase rate of the aluminum oxide particles was measured using an X-ray analyzer (Ultima-IV, manufactured by Rigaku Corporation), and commercially available alpha alumina single crystal particles (alpha phase rate: 100%) that had been fired at a sufficiently high temperature and had undergone sufficient alpha phase change were used as the reference material. The reference material and the target abrasive grains (aluminum oxide particles) were subjected to X-ray diffraction measurement to measure the integrated intensity of the (113) plane diffraction line, and the alpha phase rate of the target abrasive grains (aluminum oxide particles) was calculated from the ratio of the integrated intensity of the (113) plane diffraction line of the target abrasive grains to that of the reference material.

[0114] The secondary particle diameters (D10, D50, D90) of each abrasive grain were measured by a capillary electrical resistance method using a Multisizer 3 (manufactured by Beckman Coulter, Inc.). Note that the abrasive grains of Comparative Examples 2 to 4 had small particle diameters and could not be measured for their secondary particle diameters (D10, D50, D90) using the Multisizer 3. Therefore, 100 particles were randomly selected from images taken with a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8000), and the particle diameters of each were measured to calculate the secondary particle diameters (D10, D50, D90).

[0115] (Hydrophobic Dispersion Medium) The following hydrophobic dispersion medium was used: a synthetic hydrocarbon (isoparaffinic hydrocarbon) derived from mineral oil, with a flash point of 63°C (closed-cell method), a total content of benzene-based organic solvents and halogen-based organic solvents of 0.5% by mass or less, and a vapor pressure of 0.05 kPa (molecular weight 170). Note that the vapor pressure is the value at 20°C.

[0116] (Surfactant) A polyoxyalkylene alkyl ether having an HLB of 13.3 was used as the surfactant.

[0117] (Object to be polished) The object to be polished was a composite material having a clear coating film formed by painting a synthetic resin paint on the surface of a steel plate, which was baked at 60° C. The pencil hardness of the clear coating film after baking was F.

[0118] (Polishing Machine) A double action polisher LHR12E (manufactured by Rupes Co., Ltd.) was used as the polishing machine.

[0119] (Polishing conditions) The polishing conditions are as follows: (1) Polishing test using a sponge buff Buff: sponge buff Pressing load: 4 kg Polisher rotation speed: 5300 rpm Polishing line speed: 200 m / min Flow rate of polishing composition: 0.4 g / 15 seconds Polishing time: 180 seconds Polishing area: 300 x 400 mm (2) Polishing test using a wool buff Buff: wool buff (hair length: about 15 mm) Pressing load: 4 kg Polisher rotation speed: 5300 rpm Polishing line speed: 200 m / min Flow rate of polishing composition: 0.8 g / 20 seconds Polishing time: the time when the clear coating film was dry-sanded with #3000 paper and removal was confirmed visually Polishing area: 400 x 600 mm

[0120] (Evaluation of Polishing Rate) The inventors performed a polishing test using a sponge buff (hereinafter referred to as a sponge buff test) on the polishing compositions of Examples 1 to 3 and Comparative Examples 1 to 4 to measure the polishing rate [μm / min]. Furthermore, for the polishing compositions of Examples 1 and 2 and Comparative Examples 1 and 2, not only the sponge buff test but also a polishing test using a wool buff (hereinafter referred to as a wool buff test) was performed to measure the polishing rate [μm / min]. Specifically, an electromagnetic induction film thickness measuring device was used to measure the film thickness of each film before and after polishing. Then, the removal amount (removal amount) was calculated from the difference in film thickness before and after polishing, and the polishing rate was calculated from the removal amount.

[0121] As a result, as shown in Table 1, Examples 1 and 2 had high polishing rates in both tests, with the polishing rates being 1.31 [μm / min] or more in the wool buff test and 0.82 [μm / min] or more in the sponge buff test. Example 3 had high polishing rates in the wool buff test of 0.92 [μm / min] or more and 0.60 [μm / min] in the sponge buff test.

[0122] On the other hand, in Comparative Example 2, the polishing rate in the wool buff test was 0.73 [μm / min] and the polishing rate in the sponge buff test was 0.45 [μm / min], and the polishing rates were low in both tests. In Comparative Examples 3 and 4, there is no data for the wool buff test, but the polishing rates in the sponge buff test were low, being 0.29 [μm / min] or less.

[0123] (Evaluation of Color Difference ΔE) The state of the finished surface of the object to be polished can be evaluated by measuring the color difference ΔE. It can be said that the smaller the color difference ΔE, that is, the closer it is to 0 (zero), the better the state of the finished surface. Here, the color difference ΔE is a numerical value of the difference in color (difference in surface roughness) between the two measured coating surfaces, and is calculated by the following formula (ii): Color difference ΔE = √(L2 - L1) 2 + (a2-a1) 2 + (b2-b1) 2 ...Formula (ii) In formula (ii), L represents lightness, and a and b represent hue and saturation.

[0124] Using formula (ii), the color difference ΔE of the polished coating surface is calculated based on the coating surface after painting (i.e., a new coating surface). The closer the value of the color difference ΔE is to 0, the fewer or shallower the processing scratches are, and the coating surface after painting and the coating surface after polishing have the same appearance. On the other hand, when the value of the color difference ΔE is large, the processing scratches are many or deep, and there is a difference in appearance between the coating surface after painting and the coating surface after polishing.

[0125] The evaluation device and measurement conditions for the color difference ΔE are as follows: Evaluation device: Multi-angle type spectrophotometer CM-512m3A (manufactured by Konica Minolta, Inc.) Measurement conditions: Field of view is 2°, and the light source is standard illuminant D65 (daylight, correlated color temperature 6504K), and the light source is 25°

[0126] As shown in Table 1, in Examples 1 and 2, the color difference ΔE after degreasing in the wool buff test was 5 or less, and the color difference ΔE after degreasing in the sponge buff test was 1.5 or less, and the color difference ΔE was low in both tests. In Example 3, the color difference ΔE after degreasing in the wool buff test was 0.7, and the color difference ΔE after degreasing in the sponge buff test was 0.3, which were particularly low values. Note that degreasing refers to the process of removing oil from the coating surface after polishing by spraying isopropyl alcohol.

[0127] On the other hand, in Comparative Example 1, the color difference ΔE in the wool buff test was 10 or more, and the color difference ΔE in the sponge buff test was 4 or more, and the color difference ΔE was a high value in both tests.

[0128] (Assessment) Examples 1 to 3 had high polishing rates and low color differences ΔE. A low color difference ΔE means that the scratch removal performance by polishing is high and the finished surface after polishing can be made good. Examples 1 to 3 had high polishing rates and low color differences ΔE, so the performance was judged to be good (◯).

[0129] On the other hand, Comparative Example 1 had a high color difference ΔE and was therefore judged to have poor performance (×).Comparative Examples 2 to 4 had low polishing rates and were therefore judged to have poor performance (×).

[0130] <Other Embodiments> As described above, the present technology has been described using embodiments and examples. However, the descriptions and drawings that form part of this disclosure should not be understood to limit the present technology. Various alternative embodiments, examples, and operational techniques will become apparent to those skilled in the art from this disclosure. It goes without saying that the present technology includes various embodiments not described herein. At least one of various omissions, substitutions, and modifications of components can be made without departing from the spirit of the above-described embodiments and examples. Furthermore, the effects described in this specification are merely examples and are not limiting, and other effects may also be present.

[0131] The present invention can also be configured as follows: (1) A method for producing abrasive particles, comprising: abrasive grains, water, and a hydrophobic dispersion medium, wherein, in the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis are 10%, 50%, and 90%, respectively, are defined as D10, D50, and D90, the particle size distribution width of the abrasive grains (D10-D90) / D50 is 0.4 or more and 2.0 or less, and the specific surface area (m 2 (2) The polishing composition according to (1), wherein the particle size distribution width is 0.4 or more and 1.6 or less. (3) The specific surface area (m 2 / g) is 12 or more and 15 or less. (4) The polishing composition according to any one of (1) to (3) above, wherein the average secondary particle diameter of the abrasive grains is 0.05 μm or more and 10 μm or less. (5) The polishing composition according to any one of (1) to (4) above, wherein the abrasive grains are contained in an amount of 5 mass % or more and 30 mass % or less with respect to the total mass of the polishing composition. (6) The polishing composition according to any one of (1) to (5) above, wherein the abrasive grains contain aluminum oxide. (7) The polishing composition according to (6) above, wherein the alpha conversion rate of the aluminum oxide is 50% or more and 100% or less. (8) The polishing composition according to any one of (1) to (7), wherein the hydrophobic dispersion medium contains at least one selected from the group consisting of normal paraffin hydrocarbons, isoparaffin hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons, and has a flash point of 30° C. or higher and 100° C. or lower. (9) The polishing composition according to (8), wherein the hydrophobic dispersion medium has a vapor pressure of 0.004 kPa or higher and 2 kPa or lower at 20° C. (10) The polishing composition according to any one of (1) to (9), further containing a surfactant. (11) The polishing composition according to any one of (1) to (12), wherein the polishing composition is for polishing resins. (12) A method for producing a polishing composition, comprising the step of mixing abrasive grains, a hydrophobic dispersion medium, and water to produce a polishing composition, wherein, in the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle diameter side of the cumulative particle size distribution on a volume basis is 10%, 50%, and 90%, respectively, are D10, D50, and D90, the particle size distribution width (D10-D90) / D50 of the abrasive grains is 0.4 or more and 2.0 or less, and the specific surface area (m 2 / g) is 12 or more and 20 or less. (13) A polishing method comprising a step of polishing an object to be polished with the polishing composition according to any one of (1) to (11) above. (14) The polishing method according to (13) above, wherein the object to be polished comprises at least one material selected from the group consisting of a resin material, an alloy material, and a glass material. (15) The polishing method according to (13) or (14) above, wherein in the step of polishing the object to be polished, the polishing composition is supplied to a surface of the object to be polished, and a polishing buff is brought into contact with the surface to which the polishing composition has been supplied to polish the object.

[0132] REFERENCE SIGNS LIST 1 Automatic polishing device 2 Robot arm 4 Polishing tool 5 Pressing force detection unit 7 Controller 10 Polishing buff 10a Polishing surface 20, 21, 22 Joint 23 Tip 90 Polishing object

Claims

1. A method for producing a toner comprising the steps of: (1) comprising: abrasive grains; water; and a hydrophobic dispersion medium; and (2) a particle size distribution width (D10-D90) / D50 of the abrasive grains is 0.4 or more and 2.0 or less; and (3) a specific surface area (m 2 / g) is 12 or more and 20 or less.

2. The polishing composition according to claim 1, wherein the particle size distribution width is 0.4 or more and 1.6 or less.

3. The specific surface area (m 2 3. The polishing composition according to claim 1, wherein the polishing composition has a molecular weight of 12 or more and a molecular weight of 15 or less.

4. The polishing composition according to claim 1 or 2, wherein the average secondary particle diameter of the abrasive grains is 0.05 μm or more and 10 μm or less.

5. A polishing composition according to claim 1 or 2, wherein the abrasive grains are contained in an amount of 5 mass % or more and 30 mass % or less relative to the total mass of the polishing composition.

6. The polishing composition according to claim 1 or 2, wherein the abrasive grains contain aluminum oxide.

7. The polishing composition according to claim 6, wherein the alpha conversion rate of the aluminum oxide is 50% or more and 100% or less.

8. The polishing composition according to claim 1 or 2, wherein the hydrophobic dispersion medium contains at least one selected from the group consisting of normal paraffinic hydrocarbons, isoparaffinic hydrocarbons, naphthenic hydrocarbons, and terpene hydrocarbons, and has a flash point of 30°C or higher and 100°C or lower.

9. The polishing composition according to claim 8, wherein the hydrophobic dispersion medium has a vapor pressure at 20° C. of 0.004 kPa or more and 2 kPa or less.

10. The polishing composition according to claim 1 or 2, further comprising a surfactant.

11. The polishing composition according to claim 1 or 2, which is for polishing resin.

12. A method for producing a polishing composition comprising the step of mixing an abrasive grain, a hydrophobic dispersion medium, and water to produce a polishing composition, wherein, with respect to the particle size distribution of the abrasive grains, when the particle sizes at which the cumulative volume from the large particle side of the cumulative particle size distribution on a volume basis is 10%, 50%, and 90%, respectively, are D10, D50, and D90, the particle size distribution width of the abrasive grains (D10-D90) / D50 is 0.4 or more and 2.0 or less, and the specific surface area (m 2 / g) is 12 or more and 20 or less.

13. A polishing method comprising a step of polishing an object to be polished with the polishing composition according to claim 1 or 2.

14. The polishing method according to claim 13, wherein the object to be polished includes at least one material selected from the group consisting of a resin material, an alloy material, and a glass material.

15. The polishing method according to claim 13, wherein in the step of polishing the object to be polished, the polishing composition is supplied to the surface of the object to be polished, and the surface to which the polishing composition has been supplied is polished by contacting the surface with a polishing buff.

Citation Information

Patent Citations

  • Surface treating agent

    JP2007277379A

  • Polishing composition and application thereof

    JP2008127456A

  • Abrasive composition

    JP2008255232A

  • Abrasive composition

    JP2001081443A

  • Polishing material, polishing composition, and polishing method

    JP2017197707A

Cited By

  • Nano aluminum oxide polishing solution for silicon carbide substrate slice as well as preparation method and application of nano aluminum oxide polishing solution

    CN119350975A