Decorative sheet and decorative member

The decorative sheet addresses the issue of unnatural glossiness by structuring layers with a lower protective layer gloss and increased raised layer area ratio, achieving a strong tactile and realistic feel while maintaining durability.

WO2024203279A1PCT designated stage expired Publication Date: 2024-10-03DAI NIPPON PRINTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009539
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-13
Filing Date
2024-03-12
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Decorative sheets with large particle size beads for a strong tactile sensation often result in an unnatural, glossy appearance that lacks authenticity, making it difficult to replicate natural designs like wood grain patterns.

Method used

A decorative sheet with a base layer, design layer, protective layer, and raised layer in sequence, where the protective layer has a lower 60° gloss value than the raised layer, and the ratio of the raised layer area to the protective layer area is 10% or more, with an average distance between raised portions of 1.6 mm or more, to achieve a strong tactile and realistic feel.

Benefits of technology

The solution provides a decorative sheet with a strong tactile sensation and a realistic, authentic appearance by reducing glossiness and enhancing design realism while maintaining abrasion and scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009539_03102024_PF_FP_ABST
    Figure JP2024009539_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a decorative sheet including, in order, in the thickness direction: a base material layer; a design layer; a protective layer; and a raised layer having raised portions arranged in a pattern. The decorative sheet is configured so that: the 60° gloss value of the protective layer is smaller than the 60° gloss value of the raised layer, and the 60° gloss value of the raised layer is 20 or less; in the thickness direction, the ratio of the area of the raised layer to the area of the protective layer is 10% or more; and an average interval between adjacent raised portions is 1.6 mm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Decorative sheets and decorative materials

[0001] The present disclosure relates to decorative sheets and decorative members.

[0002] For example, decorative members having a substrate and a decorative sheet are used to impart design features to the surfaces of building materials, furniture, and the like.

[0003] A decorative sheet has, for example, a base layer, a design layer, and a surface protection layer on top of it. Furthermore, it has been proposed to provide a raised portion on the surface of the decorative sheet to provide a tactile feel (Patent Document 1).

[0004] JP 2008-87158 A

[0005] In recent years, there has been a demand for decorative sheets with a strong, rough feel. It has been thought that a strong feel can be imparted by incorporating large particle diameter beads into the raised portion. However, incorporating large particle diameter beads into the raised portion can result in a high gloss, which can lead to an unnatural design that lacks a sense of authenticity. Therefore, there is a demand for decorative sheets that enhance the feel of the raised portion while still maintaining a sense of authenticity.

[0006] The present disclosure has been made in view of the above circumstances, and has as its main object to provide a decorative sheet that has a strong feel and a genuine feel.

[0007] The present disclosure provides a decorative sheet having, in this order in the thickness direction, a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, wherein the 60° gloss value of the protective layer is smaller than that of the raised layer, and the 60° gloss value of the raised layer is 20 or less, the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction is 10% or more, and the average spacing between adjacent raised portions is 1.6 mm or more.

[0008] The present disclosure provides a decorative member having a substrate and the decorative sheet described above.

[0009] The present disclosure has the effect of providing a decorative sheet that has a strong feel and a genuine feel.

[0010] Fig. 3 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. Fig. 4 is a schematic top view illustrating a decorative sheet according to the present disclosure. Fig. 5 is a schematic top view illustrating an enlarged raised portion 4a within the dotted line frame P of the decorative sheet shown in Fig. 2. Fig. 6 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. Fig. 7 is a schematic cross-sectional view illustrating a decorative member according to the present disclosure.

[0011] Below, embodiments will be described with reference to the drawings etc. However, the present disclosure can be implemented in many different forms and is not limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may show the width, thickness, and shape of each part schematically compared to the actual form, but this is merely an example and should not be construed as limiting.

[0012] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. Also, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" refers to both a case in which another component is disposed directly above or below the certain component so as to be in contact with the component, and a case in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.

[0013] As mentioned above, by including beads with large particle diameters in the raised portion, a strong tactile feel can be obtained, but the raised portion has a high gloss, making it difficult to reproduce the appearance of a natural material such as natural wood.

[0014] A. Decorative Sheet The decorative sheet of the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view illustrating an example of a decorative sheet of the present disclosure. The decorative sheet 10 shown in Fig. 1 is made up of a base layer 1, a design layer 2, a protective layer 3, and a raised layer 4 having a patterned raised portion 4a, and is arranged in a thickness direction D. TIn the present disclosure, the 60° gloss value of the protective layer 3 is smaller than the 60° gloss value of the protruding layer 4, and the 60° gloss value of the protruding layer 4 is 20 or less, and the thickness direction D T In this case, the ratio of the area of ​​the protruding layer 4 to the area of ​​the protective layer 3 is 10% or more, and the average distance between adjacent protruding portions 4a is 1.6 mm or more.

[0015] According to the present disclosure, a strong uneven feel can be obtained by ensuring that the average spacing between adjacent raised portions 4a is equal to or greater than a predetermined value and that the ratio of the area of ​​the raised layer 4 to the area of ​​the protective layer 3 is equal to or greater than a predetermined value. Furthermore, by ensuring that the 60° gloss value of the protective layer 3 is smaller than that of the raised layer 4 and that the 60° gloss value of the raised layer 4 is equal to or less than a predetermined value, the glossiness of the raised layer can be reduced while maintaining a matte gloss feel, resulting in a natural and authentic design with a reduced layer configuration.

[0016] 1, the raised layer 4 in the present disclosure is disposed on the surface of the protective layer 3 opposite the design layer 2, and has a patterned raised portion 4a. The raised layer 4 is formed from a large number of raised portions 4a provided on the protective layer 3, thereby enhancing the design of the decorative sheet.

[0017] (1) 60° Gloss The 60° gloss value of the raised layer is greater than the 60° gloss value of the protective layer and is 20 or less. The 60° gloss value of the raised layer is preferably 15 or less, and more preferably 10 or less. When the 60° gloss value is within the above range, the glossiness of the raised layer can be reduced, resulting in a natural and authentic design. On the other hand, the 60° gloss value may be, for example, 4 or more, or 6 or more. When the 60° gloss value is within the above range, the raised layer can be prevented from becoming too low in gloss, and an excellent gloss matte appearance can be maintained between the raised layer and the protective layer.

[0018] In the present disclosure, the 60° gloss value of the protruding layer is a value measured by the following method. The decorative sheet is placed with the protruding layer side facing up, and the 60° specular gloss of the protruding layer is measured from the protruding layer side using a gloss meter in accordance with Method 3 of JIS Z 8741:1997. The 60° gloss value of the protruding layer is the average value of measurements taken at 10 arbitrary locations on the protruding layer. At each measurement location, the protruding layer is located at the center of the measurement site of the gloss meter, and the measurement is performed so that 50% or more of the area of ​​the measurement site overlaps with the protruding layer. The center of the measurement site of the gloss meter refers to the center of the incident area into which light from the light source of the gloss meter enters.

[0019] The 60° gloss value of the raised layer can be adjusted by the type, average particle size, content, etc. of the filler, which will be described later. For example, the gloss value tends to decrease when inorganic particles are used as a filler. The gloss value tends to decrease when the average particle size of the inorganic particles is increased. The gloss value tends to decrease when the content of the inorganic particles is increased. Although organic particles have a weaker matting effect than inorganic particles, the gloss value tends to decrease when the content of the organic particles is increased. Furthermore, organic particles generally have a larger average particle size than inorganic particles, but the 60° gloss value tends to decrease when the average particle size is reduced.

[0020] (2) Raised portion The raised layer has a patterned raised portion 4a. The raised portion 4a is preferably arranged to harmonize with the design of the design layer 2. "Harmony" means that the shapes and positions of the two target patterns generally match. Specifically, this means that the shapes and positions of the raised portion 4a and at least a portion of the patterns constituting the design of the design layer 2 match to an extent that does not impair realism or a sense of luxury.

[0021] In FIG. 1 , the design layer 2 has a pattern layer 2y, and the raised portion 4a is in harmony with the pattern layer 2y. By arranging the raised portion 4a so that it is in harmony with the pattern of the design layer, the design of the decorative sheet can be improved by the synergistic effect of the raised portion 4a and the pattern of the design layer. For example, in the case of a wood grain pattern, the texture can be improved by harmonizing the pattern of the raised portion 4a with a dark pattern such as a vessel. For example, when the decorative sheet is viewed in plan, if the total area of ​​the pattern layer is 100, the area of ​​the raised portion 4a in harmony with the pattern layer is preferably 90 or more, more preferably 95 or more, even more preferably 97 or more, and even more preferably 99 or more. On the other hand, the raised portion 4a does not have to be arranged in harmony with the pattern of the design layer.

[0022] In the present disclosure, the average spacing between adjacent raised portions 4a is typically 1.6 mm or more, preferably 2.0 mm or more, and more preferably 2.3 mm or more. If the average spacing between adjacent raised portions 4a is smaller than the above range, a strong tactile sensation cannot be obtained. On the other hand, the average spacing between adjacent raised portions 4a may be, for example, 4.0 mm or less, or 3.0 mm or less.

[0023] In the present disclosure, the average spacing between adjacent raised portions 4a refers to the average of 80 values ​​obtained by measuring the spacing W4 between the upper ends of adjacent raised portions 4a at 100 locations on a cross-sectional image of the decorative sheet, excluding the smallest to tenth smallest values ​​and the largest to tenth largest values. For example, in Figures 1 and 2, the average spacing between adjacent raised portions 4a corresponds to the average spacing between adjacent raised portions 4a in the direction D2 perpendicular to the longitudinal direction D1 of the raised portions 4a. In particular, when the pattern of the decorative layer is a wood grain pattern, the direction in which the vessels of the wood grain extend corresponds to the longitudinal direction of the raised portions 4a. Furthermore, when the pattern of the decorative layer is a stone grain pattern, for example, and the raised portions 4a do not have a specific longitudinal direction, the average spacing corresponds to the average spacing between adjacent raised portions 4a in any multiple directions, not limited to a specific direction.

[0024] The cross-sectional shape of the mound portion in the direction D2 is not particularly limited, and examples thereof include a substantially rectangular shape, a substantially polygonal shape, a substantially circular shape, etc. In Fig. 4, the cross-sectional shape of the mound portion 4a is a substantially rectangular shape (trapezoidal shape).

[0025] FIG. 3 is a schematic top view of an enlarged portion of a raised portion 4a within the dotted-line frame P of the decorative sheet shown in FIG. 2 . As shown in FIG. 3 , one raised portion 4a may include an irregularly textured surface 45. Examples of such textured surfaces include the textured surface of a raised portion described in JP 2022-55319 A. Specifically, the textured surface 45 includes convex portions 46 and concave portions 47. The convex portions 46 and concave portions 47 forming the irregularly textured surface 45 may be irregularly arranged. The convex portions 46 and concave portions 47 may also be irregularly shaped. As shown in FIG. 3 , the textured surface 45 of the raised portion 4a may have a wood surface pattern. As shown in FIG. 3 , at least one of the convex portions 46 and concave portions 47 may be linear portions 49 whose orientation and / or length are not constant. Both the convex portions 46 and concave portions 47 may be linear portions 49 whose orientation and / or length are not constant.

[0026] This raised portion 4a can provide a tactile sensation in its internal region due to the steps between the convex portions 46 and concave portions 47. In other words, the raised layer 4 can provide a tactile sensation not only at the edges of the raised portion 4a, but also inside the raised portion 4a. Therefore, the unevenness of the surface of the decorative sheet 10 can be emphasized with a stronger tactile sensation.

[0027] In addition, by eliminating the regularity of the uneven surface 45, it is possible to suppress the artificial impression that appears when observing the uneven surface 45. Therefore, the raised portion 4a can express a natural texture, and in combination with the design layer, the design can be synergistically improved.

[0028] The size of the linear portion 49 in the direction in which it extends is defined as the total length of the linear portion 49. The size of the linear portion 49 in the direction perpendicular to the direction in which it extends is defined as the width of the linear portion 49. T The size in the direction (depth direction of the paper) is the depth of the linear portion 49 .

[0029] In the decorative sheet 10 shown in Figure 3, the convex portion 46 includes a convex portion D that is surrounded on all sides by a concave portion 47 in a plan view. The convex portions D may be irregularly arranged inside the raised portion 4a in a plan view. The shape of the convex portion D included in one raised portion 4a in a plan view does not have to be a typical geometric shape such as a triangle, rectangle, circle, or ellipse, and may be an irregular shape. The area of ​​the convex portion D in a plan view may vary irregularly among the multiple convex portions D. In other words, the area of ​​the multiple convex portions D in a plan view may differ from one another.

[0030] The dimensions of the projections D in a plan view can be set taking into consideration the tactile feel and realization of a natural texture. The maximum dimension of the projections D along the D2 direction is preferably 30 μm or more and 500 μm or less, and more preferably 100 μm or more and 300 μm or less. The maximum dimension of the projections D along the D1 direction is preferably 40 μm or more and 20,000 μm or less, and more preferably 400 μm or more and 8,000 μm or less.

[0031] As shown in FIG. 3, the decorative sheet 10 may include protrusions 46 that are not partially surrounded by recesses 47 in addition to protrusions D that are completely surrounded by recesses 47 in a plan view.

[0032] The length of the linear portions 49 is not particularly limited. Both ends of at least some of the linear portions 49 may be located on the edge of the raised portion 4a. At least some of the linear portions 49 may include one end or both ends located inside the raised portion 4a. That is, only one end of the linear portion 49 may be located on the edge of the raised portion 4a. Both ends of the linear portion 49 may be located inside the raised portion 4a. The end positions of these linear portions 49 may differ between the linear portions 49 included in one raised portion 4a.

[0033] The width W49 of the linear portion 49 (see FIG. 3) is not particularly limited. The width W49 of the linear portion 49 may be 50 μm or more and 250 μm or less. The width W49 may vary among the plurality of linear portions 49. The height difference of the linear portion 49, i.e., the height difference between the recessed portion 47 and the protruding portion 46, is D TThe height difference is the difference between the smallest (lowest) part of the recess 47 and the largest (highest) part of the protrusion 46 in the direction (depth direction of the paper). The height difference is not particularly limited, but may be 10 μm or more and 200 μm or less. The height differences caused by multiple linear portions 49 may be the same or different from each other. The height difference caused by one linear portion 49 may be constant or may vary along the longitudinal direction of the linear portion 49.

[0034] There are no particular limitations on the cross-sectional shape of the linear portion 49 in a cross section perpendicular to the longitudinal direction, and the cross-sectional shape of the linear portion 49 in a cross section perpendicular to the longitudinal direction may be any shape, such as a semicircle, a semi-ellipse, a triangle, a rectangle, a pentagon, a hexagon, or any other polygon, or an irregular geometric shape.

[0035] (3) Area In the decorative sheet of the present disclosure, the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction is typically 10% or more, preferably 20% or more, more preferably 30% or more, and particularly preferably 40% or more. In the present disclosure, when the average spacing between adjacent raised portions 4a is a predetermined value or more and the ratio of the area of ​​the raised layer 4 to the area of ​​the protective layer 3 is a predetermined value or more, a strong uneven feel is obtained. Furthermore, when the ratio of the area of ​​the raised layer to the area of ​​the protective layer is within the above range, abrasion resistance, scratch resistance, and contamination resistance are improved. Meanwhile, the area ratio of the raised layer is, for example, 55% or less, and preferably 50% or less.

[0036] The ratio of the area of ​​the protruding layer to the area of ​​the protective layer in the thickness direction is the ratio of the area of ​​the protruding region in the measurement region where the protruding layer is provided to the area of ​​the region in the measurement region where the protective layer is provided, as viewed from the thickness direction, and is the average value calculated from the above area ratios at 100 locations within a 10 mm x 10 mm measurement region.

[0037] (4) Thickness In the present disclosure, the average thickness T4 of the protruding layer is, for example, 2.0 times or more, or 2.5 times or more, or even 3.0 times or more, the average thickness T3 of the protective layer. Having the average thickness of the protruding layer within the above range improves abrasion resistance, scratch resistance, and contamination resistance. A specific average thickness of the protruding layer is, for example, 10 μm or more, or 15 μm or more, or even 20 μm or more. Meanwhile, the average thickness of the protruding layer is, for example, 50 μm or less, or 40 μm or less, or even 30 μm or less.

[0038] The average thickness of the raised layer is determined by measuring the thickness T4 of the raised portion 4a at 100 points on an image of the cross section of the decorative sheet taken using a scanning electron microscope (SEM), and excluding the 10 points with the smallest value and the 10 points with the largest value, for a total of 80 points. If the raised portion has an uneven surface, the thickness is measured at the convex portions. The same applies to the average thickness of the protective layer.

[0039] (5) Composition (i) Filler The raised portion preferably contains a filler. That is, the raised layer preferably contains a filler. Examples of fillers include organic particles and inorganic particles. Examples of organic particles include beads made of resins such as acrylic resin, urethane resin, silicone resin, and polyamide resins such as nylon. Examples of inorganic particles include beads made of inorganic materials such as silica, alumina, zirconia, titania (titanium dioxide), kaolinite, calcium carbonate, and barium sulfate. The particles may be used alone or in combination of two or more of the above types.

[0040] The average particle size of the inorganic particles is not particularly limited. The average particle size of the inorganic particles is, for example, 2 μm or more, or may be 3 μm or more, or 5 μm or more. On the other hand, the average particle size of the inorganic particles is, for example, 12 μm or less, or may be 10 μm or less. In this specification, the average particle size is D50 according to the volume-based particle size distribution measured by a laser diffraction scattering method.

[0041] The content of the inorganic particles in the protruding portion may be 2 parts by mass or more, preferably 5 parts by mass or more, or may be 15 parts by mass or more, or may be 18 parts by mass or more, relative to 100 parts by mass of the resin component of the protruding portion. On the other hand, the content of the inorganic particles in the protruding portion may be, for example, 38 parts by mass or less, 28 parts by mass or less, or may be 25 parts by mass or less.

[0042] The average particle size of the organic particles is not particularly limited. The average particle size of the organic particles is, for example, 20 μm or more, and may be 30 μm or more. On the other hand, the average particle size of the organic particles is, for example, 60 μm or less, and may be 50 μm or less.

[0043] The content of the organic particles in the protruding portion is preferably 7 parts by mass or more, and may be 10 parts by mass or more, relative to 100 parts by mass of the resin component of the protruding portion. On the other hand, the content of the organic particles in the protruding layer may be, for example, 38 parts by mass or less, 33 parts by mass or less, or 25 parts by mass or less.

[0044] When the protruding portion contains both organic and inorganic particles as fillers, the content of the organic particles relative to the content of the fillers in the protruding portion is, for example, 20% by mass or more, or alternatively 30% by mass or more, or even 40% by mass or more, while the content of the organic particles is, for example, 80% by mass or less, or alternatively 70% by mass or less, or alternatively 60% by mass or less.

[0045] When the protruding portion contains both organic and inorganic particles as fillers, the content of the inorganic particles relative to the content of the filler in the protruding portion is, for example, 20% by mass or more, or alternatively 30% by mass or more, or even 40% by mass or more, while the content of the inorganic particles is, for example, 80% by mass or less, or alternatively 70% by mass or less, or alternatively 60% by mass or less.

[0046] (ii) Resin Component The material constituting the protruding portion contains a resin component. The resin component is typically a cured product (crosslinked structure) of a curable resin X. On the other hand, the resin component may be a thermoplastic resin. In particular, the protruding portion preferably contains a cured product of a curable resin X. The curable resin X may be, for example, at least one selected from a two-component curable resin, a thermosetting resin, and an ionizing radiation curable resin.

[0047] Examples of two-component curing resins include two-component curing urethane resins, which contain a polyol compound as a base compound and an isocyanate compound as a curing agent, two-component curing epoxy resins, two-component curing urethane-modified acrylic resins, and two-component curing polyester resins.

[0048] Examples of thermosetting resins include acrylic resins, urethane resins, phenolic resins, melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins.

[0049] The ionizing radiation curable resin is a composition containing a compound having an ionizing radiation curable functional group. Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl groups, vinyl groups, and allyl groups, as well as epoxy groups and oxetanyl groups. The ionizing radiation curable resin may be a compound having an ethylenically unsaturated bond group. The ionizing radiation curable resin may be a compound having two or more ethylenically unsaturated bond groups, preferably a polyfunctional (meth)acrylate compound having two or more ethylenically unsaturated bond groups. The polyfunctional (meth)acrylate compound may be a monomer or oligomer. The ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Examples of ionizing radiation include ultraviolet (UV) rays and electron beams (EB). The ionizing radiation may be electromagnetic waves such as X-rays and gamma rays, or charged particle beams such as alpha rays and ion beams.

[0050] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxydiacrylate, bisphenol A tetrapropoxydiacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher functional (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The (meth)acrylate monomers may have a partially modified molecular skeleton. The (meth)acrylate monomers may be modified with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, or the like.

[0051] Examples of polyfunctional (meth)acrylate oligomers include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. Urethane (meth)acrylate can be obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. The epoxy (meth)acrylate may be a (meth)acrylate obtained by reacting a trifunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with (meth)acrylic acid; a (meth)acrylate obtained by reacting a difunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with a polybasic acid and (meth)acrylic acid; or a (meth)acrylate obtained by reacting a difunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with a phenol and (meth)acrylic acid. The ionizing radiation curable resins may be used alone or in combination of two or more.

[0052] When the ionizing radiation curable resin is an ultraviolet curable resin, the composition may contain additives such as a photopolymerization initiator and a photopolymerization accelerator. In the case of a compound having an ethylenically unsaturated group, the photopolymerization initiator may be one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc. The photopolymerization accelerator can reduce polymerization inhibition by air during curing and increase the curing rate. Examples of the photopolymerization accelerator include one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.

[0053] Examples of thermoplastic resins include acrylic resins, cellulose resins, urethane resins, vinyl chloride resins, polyester resins, polyolefin resins, polycarbonate, nylon, polystyrene, and ABS resins.

[0054] The protruding layer may be transparent or colored. The material used for the protruding layer may be colored by adding a colorant (pigment or dye) to the composition. The colorant may be a known or commercially available pigment or dye. One type of colorant may be used alone, or two or more types may be used in combination. The amount of colorant added may be appropriately determined depending on the desired color tone, etc.

[0055] The protruding layer may contain various additives such as a foaming agent, a flame retardant, a lubricant, an antistatic agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a radical scavenger, and a soft component (e.g., rubber).

[0056] The method for forming the raised layer can be, for example, by gravure printing using a plate or a grid, applying a raised layer-forming ink containing the curable resin X to the surface of the protective layer opposite the design layer, and curing it as needed to form the raised portion. When the raised portion has the above-mentioned uneven surface, for example, the plate described in JP 2022-55319 A can be used.

[0057] When the protruding layer-forming ink contains an electron beam-curable resin as the curable resin X, a cured product of the electron beam-curable resin is typically obtained by irradiating it with an electron beam. Examples of electron beam sources include various electron beam accelerators, such as Cockcroft-Waldt type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high-frequency type. The energy of the electron beam is, for example, 100 kV or more and 1000 kV or less, or may be 100 kV or more and 300 kV or less. The irradiation dose of the electron beam is, for example, 2 Mrad or more and 15 Mrad or less.

[0058] When the protruding layer-forming ink contains an ultraviolet-curable resin as the curable resin X, a cured product of the ultraviolet-curable resin is typically obtained by irradiating the ink with ultraviolet light. Examples of ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of the ultraviolet light is, for example, 190 nm or more and 380 nm or less.

[0059] When the protruding layer forming ink contains a thermosetting resin as the curable resin X, it is usually heated to obtain a cured product of the thermosetting resin. The heating temperature is set appropriately depending on the type of thermosetting resin. The protruding layer forming ink may contain a curing agent such as a crosslinking agent or a polymerization initiator, and a polymerization accelerator in addition to the thermosetting resin. Examples of curing agents include isocyanates, organic sulfonates, organic amines, peroxides (e.g., methyl ethyl ketone peroxide), and radical initiators (azoisobutylnitrile).

[0060] The protruding layer-forming ink may contain a solvent, if necessary. Examples of the solvent include water; hydrocarbon compounds such as toluene and xylene; alcohol compounds such as methanol, ethanol, and methyl glycol; ketone compounds such as acetone and methyl ethyl ketone; ester compounds such as methyl formate, ethyl acetate, and butyl acetate; nitrogen-containing compounds such as N-methylpyrrolidone and N,N-dimethylformamide; ether compounds such as tetrahydrofuran and dioxane; halogenated hydrocarbon compounds such as methylene chloride and chloroform; and dimethyl sulfoxide.

[0061] 2. Protective Layer As shown in Figure 1, the protective layer 3 in the present disclosure is disposed between the design layer 2 and the raised layer 4. The protective layer in the present disclosure may be disposed partially or entirely on the substrate layer described below. In particular, it is preferable that the protective layer be disposed entirely on the substrate layer. Also, as shown in Figure 1, it is preferable that the protective layer 3 be in direct contact with the raised layer 4. The decorative sheet of the present disclosure can achieve a natural and authentic design with a minimal layer configuration.

[0062] The 60° gloss value of the protective layer in the present disclosure is not particularly limited as long as it is smaller than the 60° gloss value of the protruding layer, but may be, for example, 3 or less, or 2 or less. On the other hand, the 60° gloss value of the protective layer is, for example, 1 or more.

[0063] The protective layer is not particularly limited as long as it protects the design layer and has a predetermined 60° gloss value. The material constituting the protective layer contains, for example, a resin component. Examples of the resin component include the same types as those exemplified for the raised layer.

[0064] The protective layer contains, for example, a matting agent. Examples of the matting agent include the same types of inorganic particles as those exemplified for the protruding layer. The average particle diameter of the inorganic particles used in the protective layer is, for example, 1 μm or more, or may be 3 μm or more, or may be 5 μm or more. On the other hand, the average particle diameter of the inorganic particles used in the protective layer is, for example, 20 μm or less, or may be 15 μm or less.

[0065] The content of the inorganic particles in the protective layer is preferably 10 parts by mass or more, and may be 20 parts by mass or more, relative to 100 parts by mass of the resin component of the protective layer, while the content of the inorganic particles in the protective layer may be, for example, 40 parts by mass or less, or may be 30 parts by mass or less.

[0066] The average thickness of the protective layer is not particularly limited, but is, for example, 1 μm or more, preferably 5 μm or more. When the average thickness of the protective layer is within the above range, abrasion resistance, scratch resistance, and cellophane tape resistance are improved. On the other hand, the average thickness of the protective layer is, for example, 50 μm or less, or may be 30 μm or less, or may be 20 μm or less. When the protective layer thickness is within the above range, for example, when the protective layer contains silica, an increase in the opacity caused by the silica can be suppressed, improving the visibility of the design layer. Furthermore, the protective layer does not become too hard, and surface cracking when bent can be suppressed.

[0067] 3. Design Layer The design layer in the present disclosure is disposed between the base layer and the protective layer. The design layer preferably has a pattern.

[0068] Examples of patterns for the design layer include organic patterns, inorganic patterns, and abstract patterns. Organic patterns are patterns derived from the life activities of living organisms such as animals and plants. Inorganic patterns are patterns that do not fall under the category of organic patterns. Abstract patterns are patterns that interpret objects (such as images found in nature) abstractly and do not represent a clear shape. Examples of organic patterns include wood grain patterns, leather patterns, floral patterns, and botanical patterns. Examples of inorganic patterns include stone patterns, concrete patterns, sand patterns, fabric patterns, metal patterns, tile patterns, and brickwork patterns. Examples of abstract patterns include flickering patterns (such as ink flickering patterns), smoke patterns, and marble patterns.

[0069] The design layer may have, for example, a picture layer. The design layer may also have a solid layer on the base layer side of the picture layer. In the present disclosure, the picture layer refers to a layer formed partially (particularly in a pattern) on one side of the base layer. The solid layer refers to a layer formed entirely on one side of the base layer.

[0070] The design layer contains, for example, a colorant and a resin component. Examples of the colorant include inorganic pigments such as carbon black, titanium white, zinc white, red iron oxide, Prussian blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. Dyes may also be used as the colorant.

[0071] Examples of the resin component include (meth)acrylic resins, ester urethane resins, acrylamide resins, ethylene oxide resins, N-vinylpyrrolidone resins, ester resins, amide resins, vinyl acetate resins, vinyl chloride resins, urethane (meth)acrylic resins, natural rubber, synthetic rubber, cellulose derivatives, etc. Among these, (meth)acrylic resins and urethane (meth)acrylic resins are preferred.

[0072] The design layer may contain additives such as fillers (e.g., silica), extender pigments (e.g., organic beads), neutralizers, surfactants, etc. The thickness of the design layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less.

[0073] The design layer can be formed, for example, by coating an ink containing a colorant, a binder resin, and a solvent (or a dispersion medium) onto one side of the substrate layer, followed by drying to obtain the design layer.

[0074] Examples of the solvent (or dispersion medium) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water.

[0075] Examples of the coating method include printing. Examples of printing methods include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. Examples of coating methods for forming a solid layer include various coating methods such as roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating.

[0076] 4. Substrate Layer The decorative sheet of the present disclosure has a substrate layer. The substrate layer is a member that supports the design layer, protective layer, and raised layer. By having the substrate layer in the decorative sheet, various performance properties such as mechanical strength, post-processing suitability, and design are improved, thereby improving usability as a sheet.

[0077] The substrate layer is not particularly limited, and examples thereof include a resin substrate, a glass substrate, a metal substrate, and a fiber substrate. The type of substrate layer is appropriately selected depending on the application of the decorative sheet.

[0078] Resins used for the resin substrate include, for example, various synthetic resins and various natural resins. Examples of synthetic resins include thermoplastic resins and curable resins. Considering the manufacturing suitability, handling suitability, and post-processing suitability of the decorative sheet, thermoplastic resins are preferred.

[0079] Examples of thermoplastic resins include olefin resins such as polyethylene, polypropylene, polymethylpentene, ionomers, and various olefin-based thermoplastic elastomers; vinyl chloride resins such as polyvinyl chloride, polyvinylidene chloride, and vinyl chloride-vinyl acetate copolymers; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, ethylene glycol-terephthalic acid-isophthalic acid copolymers, and polyester-based thermoplastic elastomers; acrylic resins such as polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, and methyl (meth)acrylate-butyl (meth)acrylate copolymers; polyamide resins typified by nylon 6 and nylon 66; cellulose resins such as cellulose triacetate, cellophane, and celluloid; styrene resins such as polystyrene, acrylonitrile-styrene copolymers, and acrylonitrile-butadiene-styrene copolymers (ABS resins); polyvinyl alcohol, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, polycarbonate resins, polyarylate resins, and polyimide resins.

[0080] Examples of the curable resin include ionizing radiation curable resin and thermosetting resin.

[0081] Examples of natural resins include natural rubber, pine resin, and amber.

[0082] Examples of metals used for the metal substrate include aluminum or aluminum alloys such as duralumin, iron or iron alloys such as carbon steel and stainless steel, copper or copper alloys such as brass and bronze, gold, silver, chromium, nickel, cobalt, tin, and titanium. The metal substrate may have a plated film or an anodized film on its surface.

[0083] Examples of fibrous materials used for the fiber substrate include paper such as tissue paper, kraft paper, fine paper, Japanese paper, titanium paper, linter paper, parchment paper, parchment paper, glassine paper, wallpaper backing paper, paperboard, and plasterboard base paper; and woven or nonwoven fabrics made from fibers such as polyester resin fiber, acrylic resin fiber, protein or cellulose-based natural fibers such as silk, cotton, and hemp, glass fiber, and carbon fiber. Various resins such as acrylic resin, styrene-butadiene rubber, melamine resin, and urethane resin may be added to the fiber substrate. When the fiber substrate is a paper substrate, the strength between the fibers of the paper substrate or the interlayer strength between the paper substrate and other substrates can be improved. Furthermore, fluffing can be suppressed. Resin addition methods include impregnation with the resin after papermaking, or filling the resin during papermaking. Examples of paper substrates to which resin has been added include inter-paper reinforced paper and resin-impregnated paper.

[0084] The substrate layer may contain additives as needed. In the case of a resin substrate, examples of additives include inorganic fillers, flame retardants, lubricants, foaming agents, antioxidants, ultraviolet absorbers, light stabilizers, and colorants. Various additives can be used alone or in combination. The content of the additives is not particularly limited as long as it does not impair surface properties and processing properties, and can be appropriately set depending on the required properties.

[0085] The substrate layer may be a single layer or a laminate of two or more layers. In the case of a laminate, the substrate layer may have two or more layers of the same type of substrate, or two or more layers of different types of substrate.

[0086] The substrate layer may be transparent or opaque.

[0087] The substrate layer may be colored. The coloring mode is not particularly limited, and may be transparent or opaque (hiding), which can be selected arbitrarily.

[0088] When the base layer is colored, it may contain a colorant. Examples of colorants include inorganic pigments such as white pigments such as titanium white, iron black, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, phthalocyanine blue, nickel-azo complexes, azomethine azo-based black pigments, and perylene-based black pigments; metal pigments consisting of scaly foil flakes such as aluminum and brass; and pearlescent (pearl) pigments consisting of scaly foil flakes such as titanium dioxide-coated mica and basic lead carbonate. For example, when the surface hue of the adherend on which the decorative sheet is laminated varies, and it is desired to conceal the surface hue and improve the color stability of the decorative layer, an inorganic pigment such as a white pigment may be used.

[0089] The substrate layer may be subjected to a surface treatment to enhance adhesion with layers in contact with the substrate layer, such as adhesion with a decorative layer or an adhesive layer. Examples of surface treatments include physical surface treatments such as oxidation and roughening, and chemical surface treatments. Examples of oxidation methods include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, and ozone-ultraviolet treatment. Examples of roughening methods include sandblasting and solvent treatment. These surface treatments are selected appropriately depending on the type of substrate layer, but in consideration of the effect of the surface treatment and operability, corona discharge treatment is generally preferred.

[0090] When the substrate layer is a laminate, an adhesive layer or a primer layer may be disposed between adjacent layers to improve the adhesion between the layers.

[0091] The thickness of the substrate layer is not particularly limited and is appropriately selected depending on the material of the substrate layer. In the case of a substrate layer containing a resin, the thickness of the substrate layer is, for example, 10 μm or more and 300 μm or less, or may be 20 μm or more and 200 μm or less, or may be 40 μm or more and 100 μm or less. In addition, in the case where the substrate layer is a paper substrate, the basis weight is, for example, 20 g / m 2 150g / m or more 2 less than 30 g / m 2 More than 100g / m 2 It may be the following:

[0092] 5. Other Layers As shown in Figure 1, the decorative sheet of the present disclosure has at least a base layer 1, a design layer 2, a protective layer 3, and a raised layer 4. However, the decorative sheet of the present disclosure may have other layers in addition to these layers. Examples of other layers include a transparent resin layer, an adhesive layer, a separator layer, and a primer layer.

[0093] (1) Transparent Resin Layer The decorative sheet of the present disclosure may have a transparent resin layer between the protective layer and the design layer. The transparent resin layer can increase the strength of the decorative sheet.

[0094] The transparent resin layer may be transparent enough to allow the design layer to be visually recognized, and may be colorless and transparent, colored and transparent, or translucent.

[0095] Examples of resins constituting the transparent resin layer include polyolefin resins, polyester resins, polycarbonate resins, acrylonitrile-butadiene-styrene resins (hereinafter also referred to as "ABS resins"), acrylic resins, and vinyl chloride resins. In consideration of processability, polyolefin resins and vinyl chloride resins are preferred. The resins may be used alone or in combination of two or more.

[0096] The transparent resin layer may contain additives as needed. Examples of the additives include weather-resistant agents such as ultraviolet absorbers and light stabilizers. The weather-resistant agents may be appropriately selected from those described above.

[0097] Considering processability, the thickness of the transparent resin layer is, for example, 20 μm to 150 μm, or may be 40 μm to 120 μm, or may be 60 μm to 100 μm.

[0098] Examples of methods for forming the transparent resin layer include a method of applying a resin composition and a method of laminating a resin film by dry lamination.

[0099] (2) Back Adhesive Layer The decorative sheet of the present disclosure may have a back adhesive layer on the side of the base layer opposite the design layer. The back adhesive layer is, for example, a member for attaching the decorative sheet to an adherend.

[0100] The back adhesive layer may be transparent or opaque.

[0101] Examples of adhesives used for the back surface adhesive layer include curing adhesives and pressure-sensitive adhesives. Specific examples include urethane adhesives, acrylic adhesives, epoxy adhesives, and rubber adhesives. Optically clear adhesive (OCA) or optically clear resin (OCR) can also be used for the back surface adhesive layer.

[0102] From the viewpoint of efficiently obtaining the desired adhesive strength, the thickness of the back surface adhesive layer is, for example, 5 μm or more and 100 μm or less, or may be 10 μm or more and 75 μm or less, or may be 20 μm or more and 50 μm or less.

[0103] Examples of methods for forming the backside adhesive layer include a method of applying an adhesive composition and a method of laminating an adhesive film by dry lamination.

[0104] (3) Primer Layer The decorative sheet of the present disclosure may have a primer layer to improve interlayer adhesion between the multiple layers that make up the decorative sheet. The primer layer may be disposed between any of the layers.

[0105] The primer layer is mainly composed of a binder resin, and may contain additives such as an ultraviolet absorber and a light stabilizer, if necessary.

[0106] Examples of binder resins include urethane resins, acrylic polyol resins, acrylic resins, ester resins, amide resins, butyral resins, styrene resins, urethane-acrylic copolymers, polycarbonate-based urethane-acrylic copolymers (urethane-acrylic copolymers derived from polymers (polycarbonate polyols) having carbonate bonds in the polymer main chain and two or more hydroxyl groups at the terminals and side chains), vinyl chloride-vinyl acetate copolymer resins, vinyl chloride-vinyl acetate-acrylic copolymer resins, chlorinated propylene resins, nitrocellulose resins (nitrocellulose), and cellulose acetate resins. These can be used alone or in combination of two or more.

[0107] The binder resin may be a resin obtained by crosslinking and curing the above-mentioned resin with the addition of a curing agent such as an isocyanate-based curing agent or an epoxy-based curing agent. For example, a resin obtained by crosslinking and curing a polyol-based resin such as an acrylic polyol resin with an isocyanate-based curing agent is preferred, and a resin obtained by crosslinking and curing an acrylic polyol resin with an isocyanate-based curing agent is more preferred.

[0108] The thickness of the primer layer is, for example, 0.5 μm or more, or may be 1 μm or more, or 2 μm or more, and the thickness of the primer layer is, for example, 10 μm or less, or may be 8 μm or less, or may be 6 μm or less.

[0109] The primer layer can be formed by applying a resin composition, and then drying and curing it as necessary.

[0110] (4) Separator Layer The decorative sheet of the present disclosure may have a separator layer on the surface of the back adhesive layer opposite the base material layer. The separator layer is a member that protects the back adhesive layer and is peeled off when the decorative sheet is attached to an adherend. Conventionally known separator layers can be used.

[0111] B. Decorative Member The decorative member of the present disclosure has a base and the above-described decorative sheet. Figure 5 is a schematic cross-sectional view illustrating an example of a decorative member of the present disclosure. The decorative member 100 shown in Figure 5 has, in this order, a base 50, an adhesive layer 40, and the above-described decorative sheet 10. As shown in Figure 5, the raised layer 4 of the decorative sheet 10 constitutes the outermost layer of the decorative member 100. The decorative sheet 10 is arranged so that the surface on the base layer 1 side faces the base 50 side.

[0112] According to the present disclosure, the decorative member has the decorative sheet described above, and thus has a strong feel and a genuine appearance.

[0113] 1. Decorative Sheet The decorative sheet in the present disclosure is the same as that described above in "A. Decorative Sheet," and therefore will not be described here.

[0114] 2. Base The base in the present disclosure is a member to be decorated with a decorative sheet. An example of a base is a resin member. Examples of resins used in resin members include vinyl chloride resins, acrylic resins, ester resins, styrene resins, olefin resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), phenolic resins, cellulose resins, and rubber. Another example of a base is a wood member. Examples of wood members include wood veneers, wood plywood, particle board, and wood fiberboard. Examples of wood used in wood members include cedar, cypress, pine, and lauan.

[0115] Another example of the substrate is a metal member. Examples of metals used for the metal member include iron, iron alloys (e.g., carbon steel and stainless steel), and aluminum. Another example of the substrate is a ceramic member. The material of the ceramic member may be ceramics such as glass or porcelain, a non-cement ceramic material such as gypsum, or a non-ceramic ceramic material such as ALC (lightweight aerated concrete).

[0116] The shape of the substrate is not particularly limited, and examples thereof include a plate, a sheet, and a three-dimensional shape. The substrate may have a flat surface, a curved surface, or both a flat surface and a curved surface. The substrate may have at least one of a convex portion, a concave portion, a ridge portion, a groove portion, and a through portion.

[0117] 3. Adhesive Layer The decorative member of the present disclosure may have an adhesive layer (second adhesive layer) between the substrate and the decorative sheet. The second adhesive layer disposed between the substrate and the decorative sheet may be made of, for example, the same resin as the back adhesive layer described above. Furthermore, when the decorative sheet has the back adhesive layer described above, the decorative sheet and the substrate may be in direct contact.

[0118] 4. Decorative Members The decorative member of the present disclosure has the decorative sheet and substrate described above. The uses of the decorative member of the present disclosure are not particularly limited, and examples thereof include architectural components such as walls, ceilings, floors, roofs, eaves, fences, and gates; fixtures or fittings such as window frames, doors, handrails, baseboards, moldings, and other building components; general furniture such as chests of drawers, shelves, and desks; kitchen furniture such as dining tables and sinks; various types of furniture used in wet areas such as kitchens, toilets, bathrooms, and washbasins; surface decorative panels for cabinets and the like for home appliances and office equipment; and interior or exterior components for vehicles. Furthermore, the decorative material of the present disclosure may be a component for outdoor use (exterior component) or a component for indoor use (interior component).

[0119] The decorative member of the present disclosure can be obtained, for example, by laminating a decorative sheet and a substrate. Specifically, the surface of the substrate (the surface requiring decoration) and the surface of the decorative sheet facing the base layer are laminated together.

[0120] As a method for manufacturing a decorative member, for example, a method can be mentioned in which a decorative sheet is attached to a substrate so that the back adhesive layer of the decorative sheet of the present disclosure is in direct contact with the surface of the substrate. Another method for manufacturing a decorative member can be mentioned in which a decorative sheet is laminated to a substrate via a second adhesive layer so that the surface of the decorative sheet of the present disclosure facing the base layer faces the surface of the substrate.

[0121] Methods for laminating a substrate and a decorative sheet include, for example, lamination, wrapping, and vacuum forming. In lamination, for example, a decorative sheet is pressed onto a plate-shaped substrate with a pressure roller. In wrapping, for example, while the decorative sheet is being supplied, the decorative sheet is sequentially pressure-bonded to multiple sides of the substrate using multiple rollers oriented in different directions. When a hot melt adhesive (heat-sensitive adhesive) is used to laminate the decorative sheet and the substrate, the heating temperature is, for example, 150°C or higher and 200°C or lower. Furthermore, when a reactive hot melt adhesive is used, the heating temperature is, for example, 100°C or higher and 130°C or lower.

[0122] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included within the technical scope of the present disclosure.

[0123] [Example 1] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2 A 5-μm thick substrate (manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing an acrylic resin as a binder and titanium white, red iron oxide, and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising a solid layer and a design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protrusion layer ink 1 (formulated as follows) was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Example 1. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0124] <Ink 1 for raised layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 33 parts by weight (spherical urethane beads, average particle size 50 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0125] [Example 2] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was prepared on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and yellow lead as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising a solid layer and a design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 2 (formula 2) with the following formulation was applied to a portion of the protective layer and dried to form a protruding layer with multiple protruding portions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Example 2. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0126] <Ink 2 for raised layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 11 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles 9 parts by weight (silica particles, average particle diameter 3 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0127] [Example 3] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was prepared on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and yellow lead as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer on the substrate, including a solid layer and a design layer. A protective layer ink containing a two-component curable resin (base: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protrusion layer ink 3 with the following formulation was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Example 3. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0128] <Ink 3 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 11 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles 4.5 parts by weight (silica particles, average particle diameter 12 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0129] [Example 4] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was prepared on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising the solid layer and the design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protrusion layer ink 4 with the following formulation was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Example 4. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0130] <Ink 4 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Inorganic particles 28 parts by weight (silica particles, average particle size 3 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0131] [Example 5] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was formed on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising a solid layer and a design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 8 μm. Next, a protruding layer ink 5 with the following formulation was applied to a portion of the protective layer and dried to form a protruding layer with multiple protruding portions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Example 5. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0132] <Ink 5 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 7.6 parts by weight (spherical polymethyl methacrylate particles, average particle size 50 μm) Inorganic particles 15 parts by weight (silica particles, average particle size 6 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0133] [Example 6] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5 μm thick solid layer was formed on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising a solid layer and a design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 1 μm. Next, a protrusion layer ink 6 with the following formulation was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. This was followed by heat curing at 70°C for 24 hours to obtain the decorative sheet of Example 6. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 1.

[0134] <Ink 6 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 7.6 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles 15 parts by weight (silica particles, average particle diameter 8 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0135] [Comparative Examples 1 to 3] (Preparation of decorative sheets) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was formed on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising the solid layer and the design layer on the substrate. A protective layer ink containing a two-component curable resin (base: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 3 μm. Next, a protrusion layer ink 7 with the following formulation was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. Thereafter, heat curing was carried out at 70°C for 24 hours to obtain the decorative sheets of Comparative Examples 1 to 3. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 2.

[0136] <Ink 7 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 16 parts by weight (spherical polymethyl methacrylate particles, average particle size 50 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0137] [Comparative Example 4] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was formed on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising the solid layer and the design layer on the substrate. A protective layer ink containing a two-component curable resin (main component: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 3 μm. Next, a protrusion layer ink 8 with the following formulation was applied to a portion of the protective layer and dried to form a protrusion layer with multiple protrusions. Thereafter, the sheet was heat-cured at 70°C for 24 hours to obtain the decorative sheet of Comparative Example 4. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness of the raised layers were the values ​​shown in Table 2.

[0138] <Ink 8 for protruding layer> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles 16 parts by weight (spherical polymethyl methacrylate particles, average particle size 30 μm) Solvent appropriate amount (butyl acetate, ethyl acetate)

[0139] [Comparative Example 5] (Preparation of decorative sheet) As a substrate, colored base paper for building materials ("CHPS45 (model number)", basis weight: 45 g / m 2A 5-μm thick solid layer was prepared on one side of the substrate by gravure printing using a resin composition containing acrylic resin as a binder and titanium white, red iron oxide, and lead yellow as colorants. A wood grain patterned design layer was then formed on the solid layer using a resin composition containing soluble nitrocellulose as a binder and a red iron oxide-based colorant. This resulted in a design layer comprising the solid layer and the design layer on the substrate. A protective layer ink containing a two-component curable resin (base: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by weight per 100 parts by weight of the protective layer resin components) was then applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, the protruding layer ink 7, formulated as described above, was applied to a portion of the protective layer and dried to form a protruding layer with multiple protruding portions. Thereafter, heat curing was carried out at 70°C for 24 hours to obtain the decorative sheet of Comparative Example 5. The raised portions were formed so that the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction, the average spacing between adjacent raised portions, and the average thickness T4 of the raised layer were the values ​​shown in Table 2.

[0140] [60° Gloss Values ​​of Protective Layer and Prominent Layer] The 60° gloss values ​​of the prominence layer and protective layer of the decorative sheets obtained in the Examples and Comparative Examples were measured using the following method. The results are shown in Tables 1 and 2. (Measurement Method) The decorative sheet was placed with the prominence layer side facing up, and the 60° specular gloss of the prominence layer was measured from the prominence layer side using a gloss meter ("Microgloss (model name)" manufactured by BYK Gardner) in accordance with Method 3 of JIS Z 8741:1997. The 60° gloss value of the prominence layer was taken as the average of the measurements taken at 10 arbitrary prominence locations. At each measurement location, the prominence was located at the center of the gloss meter's measurement area, and measurements were taken so that at least 50% of the area of ​​the measurement area overlapped with the prominence. The 60° specular gloss of the protective layer was also measured using the same method.

[0141] [Evaluation of Realism] A total of 20 subjects, five each from their 20s, 30s, 40s, and 50s, evaluated the realism of the decorative sheets obtained in the Examples and Comparative Examples. Visual observation was made from the raised layer side of the decorative sheet to evaluate the realism created by the raised layer and protective layer. The evaluation was performed under fluorescent lighting indoors, blocking out external light, and based on the following evaluation criteria. The evaluation criteria for realism were whether the difference in gloss between the raised and non-raised areas was sufficiently noticeable and whether the difference in gloss was too great. (Evaluation Criteria) A: 15 or more out of 20 subjects answered that the realism was present. B: Between 11 and 14 out of 20 subjects answered that the realism was present. C: Between 5 and 10 out of 20 subjects answered that the realism was present. D: Fewer than 4 out of 20 subjects answered that the realism was present.

[0142] [Evaluation of Tactile Feeling] A total of 20 subjects, five each from their 20s, 30s, 40s, and 50s, evaluated the tactile feel of the decorative sheets obtained in the Examples and Comparative Examples. Each subject touched the surface of the raised layer of the decorative sheet with the pad of the index finger of their dominant hand and evaluated whether or not the tactile feel was high. The evaluation criteria for tactile feel were "whether or not the unevenness was strongly felt."

[0143] (Evaluation criteria) A: 15 or more people out of 20 answered that they could feel the texture. B: 11 to 14 people out of 20 answered that they could feel the texture. C: 5 to 10 people out of 20 answered that they could feel the texture. D: 4 or less people answered that they could feel the texture.

[0144] [Abrasion Resistance Evaluation] For the decorative sheets obtained in the Examples and Comparative Examples, an abrasion resistance test was carried out on the surface of the raised layer by a method conforming to the provisions of JIS K7204. The test conditions were a load of 500 g for each of the two abrasion wheels (CS-10) and a rotation speed of 250 rpm. After the abrasion test, the decorative sheets were visually observed to determine the pattern retention rate, which was evaluated according to the following evaluation criteria.

[0145] (Evaluation criteria) A: Pattern remaining rate 90% or more B: Pattern remaining rate 70% or more but less than 90% C: Pattern remaining rate 50% or more but less than 70% D: Pattern remaining rate less than 50%

[0146] [Evaluation of Cellotape Resistance] For the decorative sheets obtained in the Examples and Comparative Examples, Cellotape (registered trademark) (manufactured by Nichiban Co., Ltd., 24 mm width) was adhered to the surface of the raised layer side in an area of ​​60 mm x 24 mm. Next, it was rapidly peeled off at an angle of 45°. This was repeated 10 times, and the presence or absence of peeled areas after the test was evaluated. A: No peeling B: Peeling

[0147]

[0148]

[0149] As shown in Table 1, the decorative sheets obtained in Examples 1 to 6 were confirmed to have a strong tactile sensation and a sense of authenticity. On the other hand, as shown in Table 2, the decorative sheets obtained in Comparative Examples 1 to 5 used organic particles with a large average particle size in the raised layer, and therefore had a high gloss value for the raised layer, confirming a poor sense of authenticity. Furthermore, the decorative sheets obtained in Comparative Examples 3 and 4 were confirmed to lack a strong tactile sensation due to the short average spacing between the raised portions.

[0150] Thus, the present disclosure provides, for example, the following inventions.

[0151] [1] A decorative sheet having, in this order in the thickness direction, a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, wherein the 60° gloss value of the protective layer is smaller than the 60° gloss value of the raised layer, and the 60° gloss value of the raised layer is 20 or less, the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction is 10% or more, and the average spacing between adjacent raised portions is 1.6 mm or more.

[0152] [2] The decorative sheet according to [1], wherein the 60° gloss value of the protective layer is 3 or less.

[0153] [3] The decorative sheet according to [1] or [2], wherein the 60° gloss value of the raised layer is 4 or more.

[0154] [4] The decorative sheet according to any one of [1] to [3], wherein the average distance between adjacent raised portions is 4.0 mm or less.

[0155] [5] The decorative sheet according to any one of [1] to [4], wherein the average thickness of the raised layer is at least twice the average thickness of the protective layer.

[0156] [6] The decorative sheet according to any one of [1] to [5], wherein the average thickness of the raised layer is 15 μm or more.

[0157] [7] The decorative sheet according to any one of [1] to [6], wherein the average thickness of the protective layer is 5 μm or more.

[0158] [8] The decorative sheet according to any one of [1] to [7], wherein the raised portion contains a filler.

[0159] [9] The decorative sheet according to [8], wherein the filler is inorganic particles.

[0160]

[10] The decorative sheet according to [9], wherein the content of the inorganic particles in the raised portion is 2 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of the raised portion.

[0161]

[11] The decorative sheet according to [9] or

[10] , wherein the inorganic particles have an average particle size of 2 μm or more and 12 μm or less.

[0162]

[12] The decorative sheet according to [8], wherein the filler is organic particles.

[0163]

[13] The decorative sheet according to

[12] , wherein the content of the organic particles in the raised portion is 7 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of the raised portion.

[0164]

[14] The decorative sheet according to

[12] or

[13] , wherein the average particle size of the organic particles is 20 μm or more and 60 μm or less.

[0165]

[15] A decorative member comprising: a substrate; and the decorative sheet according to any one of [1] to

[14] .

[0166] REFERENCE SIGNS LIST 1... base layer 2... design layer 3... protective layer 4... raised layer 4a... raised portion 10... decorative sheet

Claims

1. A decorative sheet having, in that order in the thickness direction, a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, wherein the 60° gloss value of the protective layer is smaller than the 60° gloss value of the raised layer, the 60° gloss value of the raised layer is 20 or less, the ratio of the area of ​​the raised layer to the area of ​​the protective layer in the thickness direction is 10% or more, and the average spacing between adjacent raised portions is 1.6 mm or more.

2. The decorative sheet according to claim 1, wherein the 60° gloss value of said protective layer is 3 or less.

3. The decorative sheet according to claim 1, wherein the 60° gloss value of said raised layer is 4 or more.

4. The decorative sheet according to claim 1, wherein the average distance between adjacent raised portions is 4.0 mm or less.

5. The decorative sheet according to claim 1, wherein the average thickness of said raised layer is at least twice the average thickness of said protective layer.

6. The decorative sheet according to claim 1, wherein the average thickness of said raised layer is 15 μm or more.

7. The decorative sheet according to claim 1, wherein the average thickness of said protective layer is 5 μm or more.

8. The decorative sheet according to claim 1, wherein the raised portion contains a filler.

9. The decorative sheet according to claim 8, wherein said filler is inorganic particles.

10. The decorative sheet according to claim 9, wherein the content of said inorganic particles in said raised portion is 2 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of said raised portion.

11. The decorative sheet according to claim 9, wherein the average particle size of the inorganic particles is 2 μm or more and 12 μm or less.

12. The decorative sheet according to claim 8, wherein said filler is an organic particle.

13. The decorative sheet according to claim 12, wherein the content of said organic particles in said raised portion is 7 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of said raised portion.

14. The decorative sheet according to claim 12, wherein the average particle size of the organic particles is 20 μm or more and 60 μm or less.

15. A decorative member comprising: a substrate; and a decorative sheet according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Decorative sheet

    JP2008087158A

  • Decorative sheet, decorative material, plate, and manufacturing method for decorative sheet

    WO2022064974A1

  • Cosmetic sheet and cosmetic material

    WO2022209492A1

  • Decorative sheet and decorative material

    WO2022209516A1

  • Decorative sheet and decorative material

    WO2023176981A1