Composite particles

Composite particles with a tailored breaking strength and molecular weight range address the high electrical resistance issue in electrochemical devices, improving electrode performance by forming a conductive network and reducing internal resistance.

WO2024203558A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010606
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional composite particles for electrochemical device electrodes exhibit high electrical resistance, limiting the performance of electrochemical devices such as lithium-ion batteries.

Method used

Composite particles with a specific range of breaking strength (0.40 mN to 1.60 mN when compressed at 0.04 mN/sec) are developed, comprising an electrode active material, a conductive material, and a binder with a weight average molecular weight between 0.1×10^5 and 10.0×10^5, which are spray-dried and pressure-molded to form a uniform electrode composite material layer.

Benefits of technology

The composite particles achieve low electrical resistance, enhancing the performance and efficiency of electrochemical devices by maintaining a balance between strength and brittleness, allowing for effective conductive network formation and reduced internal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010606_03102024_PF_FP_ABST
    Figure JP2024010606_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides composite particles having low electrical resistance.  The composite particles contain an electrode active material, a conductive material, and a binder. The composite particles have a fracture point test force of 0.40 mN to 1.60 mN when compressed at a loading rate of 0.04 mN / sec by using a micro-compression tester.
Need to check novelty before this filing date? Find Prior Art

Description

composite particles

[0001] The present invention relates to composite particles, and more particularly to composite particles for use in dry molding of electrodes for electrochemical devices.

[0002] Electrochemical devices such as lithium-ion secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications.

[0003] In order to improve the performance of electrochemical devices, various improvements have been made to the materials that form the electrodes for electrochemical devices. Electrodes for electrochemical devices have a structure in which an electrode mixture layer containing an electrode active material as a main component and, as necessary, other components such as a conductive material and a binder to impart specific functions such as conductivity, adhesion, and flexibility to the electrode is disposed on an electrode substrate. From the viewpoint of improving the performance of electrochemical devices, it is preferable that the electrode active material and other components are uniformly dispersed in the electrode mixture layer.

[0004] As methods for forming an electrode mixture layer, various methods have been considered in the past, including a method of applying a slurry composition containing an electrode active material, a conductive material, a binder, and a solvent onto an electrode substrate and drying the slurry composition to form an electrode mixture layer, and a method of spray-drying a slurry composition containing an electrode active material, a conductive material, a binder, and a solvent to obtain composite particles, and then pressure-molding the obtained composite particles onto an electrode substrate to form an electrode mixture layer.

[0005] Known composite particles for electrochemical element electrodes are produced by spray-drying a slurry containing an electrode active material, a conductive material, and a binder to form granules, and then heating the particles to crosslink and harden the binder, resulting in a weight-average particle size of 0.1 to 1,000 μm and a particle size displacement rate of 5 to 70% when compressed to a maximum load of 9.8 mN at a loading rate of 0.9 mN / sec using a microcompression tester (see, for example, Patent Document 1). Also known are composite particles for electrochemical element electrodes that contain a positive electrode active material, a conductive additive, a binder resin, and water-insoluble polysaccharide polymer fibers (see, for example, Patent Document 2).

[0006] JP 2006-310628 A International Publication No. 2014 / 185365

[0007] However, there is still room for improvement in the properties of the conventional granulated particles, in the electrodes formed using the obtained granulated particles, and in the properties of the electrochemical devices provided with such electrodes.

[0008] Therefore, an object of the present invention is to provide composite particles having low electrical resistance.

[0009] The present inventors have conducted extensive research to solve the above problems, and have newly discovered that composite particles having a breaking strength within a predetermined range have low electrical resistance, thereby completing the present invention.

[0010]

[0010] The present invention aims to advantageously solve the above-mentioned problems, and provides: [1] a composite particle for use in dry molding of an electrode for an electrochemical device, which contains an electrode active material, a conductive material, and a binder, and has a test force of 0.40 mN or more and 1.60 mN or less at the breaking point when compressed at a loading rate of 0.04 mN / sec using a micro-compression tester. Such composite particles have low electrical resistance.

[0011] [2] Here, in the composite particles of [1] above, the binder has a weight average molecular weight of 0.1 × 10 5 Above 10.0 x 10 5 It is preferable that:

[0012] According to the present invention, composite particles having low electrical resistance can be provided.

[0013] 1 is a top view showing an example of a granulation tank that can be used to produce composite particles of the present invention.

[0014] DETAILED DESCRIPTION OF THE INVENTION The present invention will be described in detail below with reference to exemplary embodiments. The composite particles of the present invention can be advantageously used as a compounding component of an electrode mixture layer provided in an electrode of an electrochemical device such as a secondary battery.

[0015] (Composite Particles) The composite particles of the present invention are used in dry molding of electrodes for electrochemical devices. These composite particles contain an electrode active material, a conductive material, and a binder. Furthermore, the test force at the breaking point (hereinafter also referred to as breaking strength) when the composite particles are compressed at a loading rate of 0.04 mN / sec using a microcompression tester must be 0.40 mN or more and 1.60 mN or less. When the composite particles contain an electrode active material, a conductive material, and a binder and have the above-mentioned predetermined breaking strength, the electrical resistance is sufficiently low. Although the reason for this is unclear, composite particles having a breaking strength within the above range have low strength compared to conventional composite particles, but are not excessively fragile. Therefore, for example, as described in the examples below, the electrical resistance can be reduced when a predetermined pressure is applied.

[0016] <Test force at breaking point (breaking strength)> The breaking strength of the composite particles must be 0.40 mN or more and 1.60 mN or less, preferably 1.30 mN or less, and more preferably 1.00 mN or less. If the breaking strength is equal to or greater than the above lower limit, it is possible to effectively prevent the composite particles from collapsing during the formation of the electrode mixture layer, thereby improving production efficiency and effectively reducing the internal resistance of the resulting electrode mixture layer. If the breaking strength is equal to or less than the above upper limit, it is presumed that this is because the composite particles can be appropriately deformed during the formation of the electrode mixture layer, and a conductive network between the particles is well formed in the resulting electrode mixture layer, thereby effectively reducing the internal resistance of the electrode mixture layer.

[0017] <Electrode Active Material> The electrode active material is not particularly limited, and a positive electrode active material and a negative electrode active material that can be used when manufacturing an electrochemical element can be used. Specifically, the positive electrode active material is not particularly limited, and for example, lithium-containing cobalt oxide (lithium cobalt oxide, LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium-containing nickel oxide (LiNiO 2 ), Co—Ni—Mn lithium-containing composite oxide (Li(Co Mn Ni)O 2), lithium-containing composite oxide of Ni-Mn-Al, lithium-containing composite oxide of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO 4 ), olivine-type lithium manganese phosphate (LiMnPO 4 ), Li 2 MnO 3 -LiNiO 2 system solid solution, Li 1+x Mn 2-x O 4 (0<X<2) Lithium-excess spinel compound represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 Examples of known positive electrode active materials include: carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials that are combinations of these.

[0018] The volume-average particle diameter of the electrode active material is preferably 0.03 μm or more, more preferably 0.1 μm or more, even more preferably 0.5 μm or more, and preferably 500 μm or less, more preferably 200 μm or less, and even more preferably 30 μm or less. The particle diameter of the electrode active material can be measured by laser diffraction. More specifically, in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution analyzer, the particle diameter D50 at which the cumulative volume calculated from the smallest diameter side is 50% is defined as the volume-average particle diameter, and this value preferably falls within the above particle diameter range. If the particle diameter of the electrode active material is equal to or less than the above upper limit, the composition within the composite particle can be made more homogeneous. Furthermore, if the particle diameter of the electrode active material is equal to or less than the above upper limit, the electrode density of the obtained electrode can be increased, and the specific surface area of ​​the electrode active material is sufficiently large, thereby optimizing the electrochemical reaction when forming an electrochemical element. When the particle size of the electrode active material is equal to or greater than the lower limit, the handling property during production of the composite particles is improved, and the productivity of the composite particles is improved. Furthermore, when the particle size of the electrode active material is equal to or greater than the lower limit, deterioration of the electrode active material during repeated charging and discharging of the electrochemical device can be effectively suppressed.

[0019] <Conductive Material> The conductive material is not particularly limited, and examples thereof include carbon black (e.g., acetylene black, Ketjen Black (registered trademark), furnace black, etc.), single-walled or multi-walled carbon nanotubes (multi-walled carbon nanotubes include cup-stacked types), carbon nanohorns, vapor-grown carbon fibers, milled carbon fibers obtained by calcining and then crushing polymer fibers, and single-walled or multi-walled graphene. These may be used alone or in combination.

[0020] When the conductive material is carbon black, the volume average particle diameter of the conductive material is preferably 5 nm or more, more preferably 12 nm or more, and preferably 500 nm or less, more preferably 100 nm or less. When the volume average particle diameter of the conductive material is equal to or greater than the above-mentioned lower limit, a good conductive network can be formed, and the electrical resistance of the composite particles can be effectively reduced. Therefore, it is believed that the use of such composite particles can further reduce the resistance of the resulting electrode. Furthermore, when the volume average particle diameter of the conductive material is equal to or less than the above-mentioned upper limit, it is believed that the composition within the composite particles can be made more homogeneous and the electrode density of the resulting electrode can be increased. The volume average particle diameter of the conductive material refers to the particle diameter (D50) at which the cumulative volume calculated from the smallest diameter side in the particle size distribution (volume basis) measured by laser diffraction is 50%.

[0021] The blend ratio of the electrode active material and the conductive material is not particularly limited, and may be a general blend ratio of these materials contained in an electrode for an electrochemical element.

[0022] <Binder> The binder is not particularly limited, and for example, a conjugated diene polymer, an acrylic polymer, an aromatic vinyl block polymer, a fluorine-containing polymer, a cellulose polymer, a cyclic olefin polymer, etc. can be used. As the binder, one type may be used alone, or two or more types may be used in combination. Among these, an aromatic vinyl block polymer is preferred.

[0023] The conjugated diene polymer refers to a polymer containing a conjugated diene monomer unit. Specific examples of the conjugated diene polymer include, but are not limited to, a copolymer containing an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit, such as styrene-butadiene copolymer (SBR), butadiene rubber (BR), acrylic rubber (NBR) (a copolymer containing an acrylonitrile unit and a butadiene unit), and hydrogenated products thereof.

[0024] The acrylic polymer is not particularly limited, and examples thereof include a polymer containing a crosslinkable monomer unit, a (meth)acrylic acid ester monomer unit, and an acidic group-containing monomer unit. The proportion of the (meth)acrylic acid ester monomer unit in the acrylic polymer is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 58% by mass or more, and is preferably 98% by mass or less, more preferably 97% by mass or less, and even more preferably 96% by mass or less.

[0025] Examples of aromatic vinyl block polymers include block polymers containing block regions composed of aromatic vinyl monomer units. Examples of aromatic vinyl monomers include styrene, styrene sulfonic acid and its salts, α-methylstyrene, p-t-butylstyrene, butoxystyrene, vinyltoluene, chlorostyrene, and vinylnaphthalene, with styrene being preferred. Examples of aromatic vinyl block polymers include styrene-isoprene-styrene block copolymers, styrene-butadiene-styrene copolymers, and hydrogenated versions of these. Among these, preferred aromatic vinyl block polymers are styrene-ethylene-butylene-styrene block copolymers, which are hydrogenated versions of styrene-butadiene-styrene copolymers.

[0026] The term "fluorine-containing polymer" refers to a polymer that contains fluorine-containing monomer units and may further contain fluorine-free monomer units (fluorine-free monomers). Examples of fluorine-containing monomers include, but are not limited to, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, vinyl trifluoride, vinyl fluoride, trifluoroethylene, trifluorochloroethylene, 2,3,3,3-tetrafluoropropene, and perfluoroalkyl vinyl ether. Examples of fluorine-containing polymers include, but are not limited to, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, perfluoroalkoxy fluororesin, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, and vinylidene fluoride-hexafluoropropylene copolymer (vinylidene fluoride-hexafluoropropylene copolymer).

[0027] The cellulose-based polymer is not particularly limited, and examples thereof include cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose.

[0028] The cyclic olefin polymer is not particularly limited, and examples thereof include a polymer (addition polymer or ring-opening polymer) synthesized using a cyclic olefin compound as a monomer and its hydrogenated product, and a hydrogenated polymer using an aromatic vinyl compound as a monomer. Among them, a hydrogenated ring-opening polymer using a cyclic olefin compound as a monomer and a hydrogenated polymer using an aromatic vinyl compound as a monomer are preferred because the electrolyte swelling degree and glass transition temperature can be easily adjusted to appropriate levels.

[0029] The cyclic olefin compound is not particularly limited, and examples thereof include: norbornene, 5-methylnorbornene, 5-ethylnorbornene, 5-butylnorbornene, 5-hexylnorbornene, 5-decylnorbornene, 5-cyclohexylnorbornene, 5-cyclopentylnorbornene, and other unsubstituted or alkyl group-containing norbornenes; norbornenes having an alkenyl group, such as 5-ethylidenenorbornene, 5-vinylnorbornene, 5-propenylnorbornene, 5-cyclohexenylnorbornene, and 5-cyclopentenylnorbornene; norbornenes having an aromatic ring, such as 5-phenylnorbornene; Norbornenes having a polar group containing an oxygen atom, such as 5-methoxycarbonylnorbornene, 5-ethoxycarbonylnorbornene, 5-methyl-5-methoxycarbonylnorbornene, 5-methyl-5-ethoxycarbonylnorbornene, norbornenyl-2-methylpropionate, norbornenyl-2-methyloctanate, 5-hydroxymethylnorbornene, 5,6-di(hydroxymethyl)norbornene, 5,5-di(hydroxymethyl)norbornene, 5-hydroxy-i-propylnorbornene, 5,6-dicarboxynorbornene, and 5-methoxycarbonyl-6-carboxynorbornene; norbornenes having a polar group containing a nitrogen atom, such as 5-cyanonorbornene; polycyclic norbornenes having three or more rings and not containing an aromatic ring structure, such as dicyclopentadiene, methyldicyclopentadiene, and tricyclo[5.2.1.02,6]dec-8-ene; Polycyclic norbornenes having three or more aromatic rings, such as tetracyclo[9.2.1.02,10.03,8]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene) and tetracyclo[10.2.1.02,11.04,9]pentadeca-4,6,8,13-tetraene (also known as 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene);unsubstituted or alkyl group-containing tetracyclododecenes such as tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-cyclohexyltetracyclododecene, 8-cyclopentyltetracyclododecene, 8-methoxycarbonyl-8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene; tetracyclododecenes having an exocyclic double bond such as 8-methylidenetetracyclododecene, 8-ethylidenetetracyclododecene, 8-vinyltetracyclododecene, 8-propenyltetracyclododecene, 8-cyclohexenyltetracyclododecene, 8-cyclopentenyltetracyclododecene; tetracyclododecenes having an aromatic ring such as 8-phenyltetracyclododecene; Tetracyclododecenes having a substituent containing an oxygen atom, such as 8-methoxycarbonyltetracyclododecene, 8-methyl-8-methoxycarbonyltetracyclododecene, 8-hydroxymethyltetracyclododecene, 8-carboxytetracyclododecene, tetracyclododecene-8,9-dicarboxylic acid, and tetracyclododecene-8,9-dicarboxylic anhydride; tetracyclododecenes having a substituent containing a nitrogen atom, such as 8-cyanotetracyclododecene and tetracyclododecene-8,9-dicarboxylic imide; tetracyclododecenes having a substituent containing a halogen atom, such as 8-chlorotetracyclododecene; tetracyclododecenes having a substituent containing a silicon atom, such as 8-trimethoxysilyltetracyclododecene; hexacycloheptadecenes such as Diels-Alder adducts of the above-mentioned tetracyclododecenes and cyclopentadiene; and the like.

[0030] Among these, non-polar norbornene-based monomers are preferred as the cyclic olefin compound, and more preferred are unsubstituted or alkyl group-containing norbornenes (e.g., norbornene, 8-ethyltetracyclododecene), alkenyl group-containing norbornenes (e.g., ethylidenetetracyclododecene (8-ethylidenetetracyclododecene)), dicyclopentadiene, aromatic ring-containing norbornene derivatives (e.g., tetracyclo[9.2.1.02,10.03,8]tetradeca-3,5,7,12-tetraene (also referred to as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene)), and unsubstituted or alkyl group-containing tetracyclododecenes (e.g., tetracyclododecene, 8-methoxycarbonyl-8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene).

[0031] The polymer using a cyclic olefin compound as a monomer, which can be optionally hydrogenated, may be a polymer using only a cyclic olefin compound as a monomer, or may be a polymer using a cyclic olefin compound and a copolymerizable compound other than a cyclic olefin compound as monomers, but is preferably a polymer using only a cyclic olefin compound as a monomer.

[0032] The polymer using a cyclic olefin compound as a monomer, which can be optionally hydrogenated, is preferably a polymer using tetracyclododecene, dicyclopentadiene, and norbornene as monomers, and more preferably a ring-opening polymer using tetracyclododecene, dicyclopentadiene, and norbornene as monomers.

[0033] Here, the binder has a weight average molecular weight of 0.1 × 10 5 It is preferable that the ratio is 0.5×10 or more. 5 More preferably, it is 1.0 × 10 or more. 5 More preferably, it is 1.3 × 10 or more. 5 It is particularly preferable that the value is 10.0×10 or more. 5 Preferably, it is 5.0 × 10 or less. 5 More preferably, it is 3.0 × 10 or less.5 It is more preferable that the weight average molecular weight of the binder is within the above range. It is presumed that the breaking strength of the composite particles can be efficiently controlled within a suitable range.

[0034] <Other Compounding Components> The composite particles may contain, if necessary, other compounding components in addition to those described above, although there are no particular limitations thereon.

[0035] <Method for producing composite particles> The composite particles of the present invention can be efficiently produced in a granulation tank equipped with two or more stirring blades with different stirring shafts. Then, by using the above-mentioned granulation tank, a composition containing a binder and a solvent is added to the electrode active material in a stirred state, thereby efficiently producing the above-mentioned composite particles of the present invention.

[0036] <Granulation tank> The granulation tank needs to be equipped with two or more stirring blades with different stirring shafts. By providing two or more stirring blades with different stirring shafts, the uniformity of the composition of the obtained composite particles is increased. An example of a granulation tank that can be used to produce the composite particles of the present invention will be described with reference to Figures 1 and 2. Figure 1 is a top view of the granulation tank 1, and Figure 2 is a cross-sectional view taken along the A-A section line shown in Figure 1. The granulation tank 1 is equipped with a main stirring blade 2 and a sub-stirring blade 3 with a stirring shaft different from that of the main stirring blade 2. The number of stirring blades is not particularly limited, as long as there are two or more. By providing two or more stirring blades, the uniformity of the composition of the composite particles can be increased.

[0037] Furthermore, although not shown, the granulation tank 1 is equipped with at least one supply means capable of supplying a liquid composition. Examples of such supply means include a spray nozzle configured to supply a mist of liquid and a dropping funnel. The number of supply means is not particularly limited, but multiple supply means may be arranged discretely depending on the size of the granulation tank. Furthermore, although not shown, the granulation tank 1 may be equipped with a supply port for a powder material such as an electrode active material and a discharge port configured to discharge the formed composite particles.

[0038] In FIG. 2, the agitation shaft of the main agitator blade 2 is shown by a dashed line as the first agitation shaft RA1, and the agitation shaft of the sub-agitator blade is shown by a dashed line as the second agitation shaft RA2. In FIG. 2, the angle θ between the first agitation shaft RA1 and the second agitation shaft RA2 is approximately 90 degrees. Note that the angle between the first agitation shaft RA1 and the second agitation shaft RA2 refers to the acute angle between these two axes. Here, in this specification, "different agitation shafts" means that the angle θ between the agitation shafts is 20° or more and 90° or less. The angle θ between the agitation shafts is preferably 30° or more, more preferably 45° or more, and even more preferably 85° or more. If the angle θ between the agitation shafts is within the above range, the powder material can be effectively agitated, and the coarsening of the particle size of the resulting composite particles and the increase in the coefficient of variation can be well controlled. The "coefficient of variation" refers to the coefficient of variation of the particle size distribution of the composite particles, and is the percentage obtained by dividing the standard deviation of the area-equivalent diameters of the composite particles by the average value of the area-equivalent diameters.

[0039] The shape of the granulation tank is not particularly limited as long as it can accommodate the powder material containing the electrode active material therein for a predetermined period of time and can be stirred by at least two stirring blades. For example, the shape of the granulation tank may be cylindrical, with circular bottom and top surfaces and a tapered upper portion in the height direction, as in granulation tank 1 shown in Figures 1 and 2. In addition, when the granulation tank has a predetermined cylindrical shape as shown in Figures 1 and 2, one of the at least two stirring shafts may coincide with the central axis of the cylinder, and the other stirring shaft may coincide with a direction perpendicular to the central axis.

[0040] The main agitating blade 2 has three main blades 21. The shape and number of the main blades 21 are not particularly limited. The auxiliary agitating blade 3 has two auxiliary blades 31. The auxiliary blades 31 are illustrated as anchor blades in FIGS. 1 and 2, but are not limited to this. The number of auxiliary blades 31 is also not limited to the illustrated form and may be one, or three or more. Furthermore, the granulation tank 1 may be equipped with a ventilation mechanism (not shown) configured to ventilate air and thereby prevent powder material from being mixed into the drive parts of the main agitating blade 2 and the auxiliary agitating blade 3.

[0041] Examples of granulation vessels that satisfy the above conditions include a high-speed mixer manufactured by EarthTechnica Co., Ltd., a Henschel mixer manufactured by Mitsui Mining Co., Ltd. (now an FM mixer manufactured by Nippon Coke Company), a vertical granulator manufactured by Powrex Corporation, a CF granulator manufactured by Freund Corporation, a high-speed stirring and mixing granulator manufactured by Nara Machinery Works, Ltd., an SP granulator manufactured by Dalton Corporation, and a balance granulator manufactured by Freund Corporation.

[0042] An example of the procedure for producing the composite particles of the present invention using the above-described granulation tank will now be described.

[0043] First, the electrode active material is charged into a granulation tank. A dispersion containing a conductive material, a binder, and a solvent is prepared separately. Agitation of the granulation tank is initiated to agitate the electrode active material in the granulation tank, and the dispersion is added to the granulation layer. The addition method is not particularly limited as long as it is not limited to batch addition. Examples include continuous addition and intermittent addition with one or more intervening periods of suspension. Of these, continuous addition is preferred. In an atmosphere in which the electrode active material and the dispersion (including the binder and conductive material) are all in a state of agitation, composite particles of the electrode active material, binder, and conductive material are gradually formed, and particle size regulation can occur due to collisions between the particles and between the particles and the solvent. In other words, during agitation, the formation of composite particles and the regulation of particle size can occur simultaneously in the presence of a solvent.

[0044] As described above, examples of the means for adding the composition containing the binder and the solvent to the powder material include a spray nozzle and a dropping funnel. Among these, it is preferable to use a spray nozzle from the viewpoint of efficiency.

[0045] Here, the solvent that can be used when preparing the dispersion containing the soluble resin and conductive material is not particularly limited, and any solvent can be used as long as it can dissolve the above-mentioned binder. For example, organic solvents such as N-methyl-2-pyrrolidone, cyclohexane, n-hexane, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, methylene chloride, and chloroform can be used as the solvent. Among these, from the viewpoint of efficiently removing the solvent in the granulation tank and reducing the drying energy required to form the composite particles, it is preferable to use a non-aqueous solvent having a boiling point of 95°C or less at 1 atm. Furthermore, from the viewpoint of more effectively achieving the above-mentioned effects, it is more preferable that the boiling point of the non-aqueous solvent be 90°C or less, and even more preferably 85°C or less at 1 atm. The lower limit of the boiling point of the non-aqueous solvent at 1 atm is not particularly limited, but from the viewpoint of improving stability when forming the composite particles, it is preferably 50°C or higher. Examples of solvents that satisfy these conditions include cyclohexane, n-hexane, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, methylene chloride, and chloroform. These may be used alone or in combination of two or more in any ratio.

[0046] The solids concentration of the dispersion containing the conductive material, binder, and solvent continuously added to the granulation tank is not particularly limited, but is preferably 2.0% by mass or more, more preferably 3.0% by mass or more, and is preferably 20.0% by mass or less, more preferably 8.0% by mass or less, and even more preferably 6.5% by mass or less. By setting the solids concentration of the dispersion containing the conductive material and binder within the above range, the particle size and coefficient of variation of the obtained composite particles can be well controlled. In addition, the stirring time is not particularly limited, but can be, for example, 5 minutes to 60 minutes.

[0047] Furthermore, the temperature inside the granulation tank is preferably less than 50° C., more preferably not more than 45° C., and even more preferably not more than 40° C. By satisfying such temperature conditions, deterioration of the electrode active material contained in the obtained composite particles can be effectively suppressed.

[0048] The composite particles thus produced can be subjected to a dry molding process such as pressure molding to form an electrode mixture layer. The pressure molding is not particularly limited, and for example, the composite particles of the present invention can be subjected to a roll press and roll-pressed on an electrode substrate to pressure-mold the composite particles on the electrode substrate to form an electrode mixture layer. The pressure during pressing can be appropriately set according to the desired electrode density.

[0049] The electrode substrate is made of a material that is conductive and electrochemically durable. Specifically, the electrode substrate may be made of a current collector made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. One of the above materials may be used alone, or two or more may be used in combination in any ratio.

[0050] The electrochemical device formed using the electrode for electrochemical devices obtained as described above is not particularly limited and may be, for example, a lithium ion secondary battery, an electric double layer capacitor, or a lithium ion capacitor, and preferably a lithium ion secondary battery. An electrochemical device including an electrode for electrochemical devices formed using the composite particles of the present invention has excellent battery performance.

[0051] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. Furthermore, in a polymer produced by copolymerizing multiple types of monomers, the proportion of a repeating unit (monomer unit) formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of that certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the measurement and evaluation of various attributes were carried out according to the following methods.

[0052] <Test Force at Breaking Point (Breaking Strength)> The composite particles produced in the Examples and Comparative Examples were used as test samples. A very small amount of the test sample was scattered on the lower pressure plate of a micro-compression tester (Shimadzu Corporation, "MCT-510"), and a compression test was performed on each particle. The flat diameter of the upper pressure indenter was 100 μm. The surface detection mode was soft surface detection mode, the test force was 2.0 mN, and the loading rate was 0.04 mN / sec. The particle diameter of the test sample was approximately 50 μm. The test force and compression displacement were monitored while applying a load at the above loading rate. When the horizontal axis is plotted as displacement (indenter travel distance [μm]) and the vertical axis is plotted as test force (particle compressing force [mN]), a point is detected where the test force on the vertical axis remains constant even when the displacement on the horizontal axis changes. The test force at this point was defined as the "test force at breaking point" for each test sample. Five tests were performed on each test sample, and the average value was defined as the test force at breaking point for each test sample.

[0053] <Powder Resistivity of Composite Particles> The powder resistivity of the composite particles produced in the Examples and Comparative Examples was measured. For the measurement, 4.0 g of the composite particles prepared in the Examples and Comparative Examples was placed in a probe unit of a powder resistivity measurement system MCP-PD51 manufactured by Mitsubishi Chemical Analytech Co., Ltd., and the powder resistivity was measured when a pressure of 20 kN was applied. The measurement results were then evaluated according to the following criteria. A: 18.0 Ω or less B: More than 18.0 Ω and 22.0 Ω or less C: More than 22.0 Ω and 24.5 Ω or less D: More than 24.5 Ω

[0054] <Weight-average molecular weight of binder> The weight-average molecular weight of the binder was measured as follows: GPC apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Column: TSKgel guard column HHR-H (6.0 mm I.D. × 4 cm) × 1 + TSKgel GMHHR-H (7.8 mm I.D. × 30 cm) × 2 (manufactured by Tosoh Corporation) Eluent: THF Detector: differential refractometer (RI detector), polarity = (+) Flow rate: 1.0 mL / min Column temperature: 40°C Sample concentration: 1 mg / mL Sample injection amount: 100 μL Calibration curve: three-dimensional approximation curve using standard polystyrene manufactured by Tosoh Corporation

[0055] Example 1 <Production of Binder> A hydrogenated styrene-butadiene-styrene block copolymer was produced as a binder in the following manner. 270 parts of dehydrated cyclohexane and 0.53 parts of ethylene glycol dibutyl ether were placed in a reactor equipped with a stirrer and the inside of which had been thoroughly purged with nitrogen, and 0.47 parts of n-butyllithium (15% cyclohexane solution) was further added. While stirring the entire contents at 60°C, 12.5 parts of dehydrated styrene were continuously added to the reactor over a period of 40 minutes. After the addition was completed, the entire contents were stirred for an additional 20 minutes at 60°C. When the reaction solution was measured by gas chromatography, the polymerization conversion rate at this point was 99.5%. Next, 200 parts of dehydrated butadiene were continuously added to the reaction solution over a period of 100 minutes, and stirring was continued for 20 minutes after the addition was completed. The polymerization conversion rate at this point was 99.5%. Thereafter, 50 parts of dehydrated styrene were continuously added over 60 minutes, and after completion of the addition, the entire solution was stirred for 30 minutes. At this point, the polymerization conversion rate was nearly 100%. Then, 0.5 parts of isopropyl alcohol was added to the reaction solution to terminate the reaction. Of all the butadiene-derived structural units in the resulting block copolymer, the proportion of structural units derived from 1,2- and 3,4-addition polymerization was 58%. Next, the polymer solution was transferred to a pressure-resistant reactor equipped with a stirrer, and 7.0 parts of a diatomaceous earth-supported nickel catalyst (manufactured by JGC Catalysts and Chemicals, product name "E22U," nickel loading 60%) as a hydrogenation catalyst and 80 parts of dehydrated cyclohexane were added and mixed. The inside of the reactor was purged with hydrogen gas, and hydrogen was further supplied while stirring the solution, and the hydrogenation reaction was carried out at a temperature of 190°C and a pressure of 4.5 MPa for 6 hours. After completion of the hydrogenation reaction, the reaction solution was filtered to remove the hydrogenation catalyst, and then 1.0 part of a xylene solution containing 0.1 part of pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Koyo Chemical Research Institute, product name "Songnox 1010"), a phenolic antioxidant, was added to the filtrate and dissolved. Cyclohexane was further added to prepare a copolymer solution with a concentration of 10% by mass. The weight-average molecular weight of the prepared copolymer was 2.2 × 10 5 It was.

[0056] <Preparation of Composite Particles> A granulator having the following configuration was used (referred to as "Granulator Type A" in Table 1). This granulator had a cylindrical vessel with an inner diameter of 180 mm and a capacity of 2 L serving as a granulation tank. The axial direction of the cylindrical vessel was the vertical direction, and stirring blades were attached to two axes, one vertical and one horizontal (the main stirring blade was attached vertically, and the auxiliary stirring blade was attached horizontally). The main stirring blade was an inclined paddle with three main blades each having a diameter of 170 mm, and the auxiliary stirring blade had a V-shaped anchor blade with a diameter of 30 mm. The main stirring blade and the auxiliary stirring blade each had a mechanism for sealing by ventilating air to prevent raw materials from being mixed into the drive parts of the main stirring blade and the auxiliary stirring blade. Composite particles were prepared using the above granulator. First, 97.3 parts by mass of NMC (average particle diameter 6 μm) as a positive electrode active material for lithium-ion batteries was added to the granulation tank. Acetylene black (BET specific surface area: 133 m) was added as a conductive material. 2 Two parts of a conductive material, binder, and solvent (2 parts by weight, volume average particle diameter: 23 nm) were mixed with 0.7 parts of a binder (solids content equivalent), and cyclohexane was added as a solvent to prepare a mixture of conductive material, binder, and solvent with a solids concentration of 3.5% by mass. The resulting mixture was then dispersed twice using a Nanovater (NVC-ES008A, manufactured by Yoshida Kikai Kogyo) at a discharge pressure of 100 MPa to prepare a dispersion containing conductive material, binder, and solvent. Next, room temperature sealing air was circulated at 20 L / min (airflow rate: 10 / min), and 2 parts by mass of a composition containing conductive material, binder, and solvent (solids content) was continuously added by two-fluid spraying over 50 minutes under operating conditions of a main stirring impeller with a peripheral speed of 6 m / s and a secondary stirring impeller with a peripheral speed of 7 m / s. Upon confirming completion of addition, the operation of the main stirring impeller and secondary stirring impeller was stopped to obtain composite particles. The above measurements were performed on the prepared composite particles. The results are shown in Table 1.

[0057] (Example 2) In <Preparation of Composite Particles>, the solid content concentration of the dispersion containing the conductive material, binder, and solvent was adjusted to 5 mass %. Except for this, composite particles were obtained in the same manner as in Example 1, and the obtained composite particles were subjected to the same measurements as in Example 1. The results are shown in Table 1.

[0058] Comparative Example 1 In the preparation of composite particles, the binder mixed in the dispersion containing the conductive material, binder, and solvent was changed to one with a smaller weight-average molecular weight. This binder was a hydrogenated styrene-butadiene-styrene block copolymer produced as follows, and had a weight-average molecular weight of 1.0 × 10 5The results were as follows. Except for using the binder thus obtained, composite particles were obtained in the same manner as in Example 2, and the same measurements as in Example 1 were carried out on the obtained composite particles. The results are shown in Table 1. <Production of Binder> 270 parts of dehydrated cyclohexane and 0.53 parts of ethylene glycol dibutyl ether were placed in a reactor equipped with a stirrer and the inside of which had been thoroughly purged with nitrogen, and 0.47 parts of n-butyllithium (15% cyclohexane solution) was further added. While stirring the entire contents at 60°C, 12.5 parts of dehydrated styrene were continuously added to the reactor over a period of 40 minutes. After the addition was completed, the entire contents were stirred for an additional 20 minutes at 60°C. When the reaction solution was measured by gas chromatography, the polymerization conversion rate at this point was 99.5%. Next, 75 parts of dehydrated butadiene was continuously added to the reaction solution over a period of 100 minutes, and stirring was continued for 20 minutes after the addition was completed. The polymerization conversion rate at this point was 99.5%. Thereafter, 12.5 parts of dehydrated styrene were continuously added over 60 minutes, and after completion of the addition, the entire solution was stirred for 30 minutes. At this point, the polymerization conversion rate was nearly 100%. Then, 0.5 parts of isopropyl alcohol was added to the reaction solution to terminate the reaction. Of all the butadiene-derived structural units in the resulting block copolymer, the proportion of structural units derived from 1,2- and 3,4-addition polymerization was 58%. Next, the polymer solution was transferred to a pressure-resistant reactor equipped with a stirrer, and 7.0 parts of a diatomaceous earth-supported nickel catalyst (manufactured by JGC Catalysts and Chemicals, product name "E22U," nickel loading 60%) as a hydrogenation catalyst and 80 parts of dehydrated cyclohexane were added and mixed. The inside of the reactor was purged with hydrogen gas, and hydrogen was further supplied while stirring the solution, and the hydrogenation reaction was carried out at a temperature of 190°C and a pressure of 4.5 MPa for 6 hours. After completion of the hydrogenation reaction, the reaction solution was filtered to remove the hydrogenation catalyst, and then 1.0 part of a xylene solution containing 0.1 part of pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Koyo Chemical Research Institute, product name "Songnox 1010"), a phenolic antioxidant, was added to the filtrate and dissolved. Cyclohexane was further added to prepare a copolymer solution with a concentration of 10% by mass.

[0059] Comparative Example 2 Composite particles were obtained in the same manner as in Example 2, except that the granulator used was changed to one in which the rotation axis of the auxiliary stirring blade was in the vertical direction (referred to as "Granulator Type B" in Table 1), and the obtained composite particles were subjected to the same measurements as in Example 1. The results are shown in Table 1.

[0060]

[0061] From Table 1, it can be seen that the composite particles of Examples 1 and 2, whose breaking strengths (test force at breaking point) were within the predetermined range, had sufficiently low electrical resistance. It can also be seen that the composite particles of Comparative Examples 1 and 2, whose breaking strengths (test force at breaking point) were outside the predetermined range, had higher electrical resistance than the composite particles produced in Examples 1 and 2.

[0062] According to the present invention, composite particles having low electrical resistance can be provided.

[0063] REFERENCE SIGNS LIST 1 Granulation tank 2 Main stirring blade 21 Main blade 3 Sub-stirring blade 31 Sub-blade RA1 First stirring shaft RA2 Second stirring shaft

Claims

1. Composite particles containing an electrode active material, a conductive material, and a binder, the test force at the breaking point when compressed at a load rate of 0.04 mN / sec using a micro-compression tester being 0.40 mN or more and 1.60 mN or less, for use in dry molding of electrodes for electrochemical elements.

2. The binder has a weight average molecular weight of 0.1×10 5 Above 10.0 x 10 5 2. The composite particle of claim 1, wherein:

Citation Information

Patent Citations

  • Composite particles for electrochemical element electrode, method for manufacturing composite particles for electrochemical element electrode, electrochemical element electrode, and electrochemical element

    WO2014185365A1

  • Composite particle for electrode of electrochemical device

    JP2006310628A

  • Electrode for electrochemical element and method for manufacturing the same

    JP2008251965A

  • Electro-chemical element electrode

    WO2006118235A1