Magnetic encoder

The magnetic encoder uses isotropic Nd-Fe-B magnet powder and thermosetting resin to achieve high angular accuracy and reduce magnetic flux variations, addressing the challenges of particle size distribution and cost in rare earth bonded magnets, resulting in enhanced performance and cost-effectiveness.

WO2024203792A1PCT designated stage expired Publication Date: 2024-10-03MINEBEAMITSUMI INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011181
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Magnetic encoders using rare earth bonded magnets face challenges in achieving high angular accuracy and reducing variations in magnetic characteristics due to particle size distribution and resin content, especially with narrow magnetic pole pitches and high costs associated with rare earth magnet powder.

Method used

A magnetic encoder is developed using isotropic Nd-Fe-B magnet powder with a particle size of 45 μm to 75 μm, mixed with a cured thermosetting resin in a specific ratio, and formed into a ring shape with predetermined magnetic pole pitches, ensuring even distribution and high precision, which enhances angular accuracy and reduces magnetic flux variations.

Benefits of technology

The solution achieves high angular accuracy and overwhelming strength in magnetic encoders by controlling the particle size and resin content, improving the magnetic properties and reducing variations, while also potentially lowering costs by optimizing the use of rare earth magnet powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011181_03102024_PF_FP_ABST
    Figure JP2024011181_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This magnetic encoder is a ring-shaped magnetic encoder having a magnetic track that includes a rare earth magnetic powder and a resin cured product of a thermosetting resin, and that is formed by magnetizing a plurality of magnetic poles at a predetermined pitch in a circumferential direction of the surface, wherein: the rare earth magnetic powder is an isotropic Nd-Fe-B based magnetic powder having a particle size of 45 μm or more and less than 75 μm; the resin cured product is contained in an amount of 5 wt. % or more and 6.5 wt. % or less; and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

magnetic encoder

[0001] The present invention relates to a magnetic encoder, and more particularly to a magnetic encoder using a rare earth bonded magnet.

[0002] Conventionally, magnetic encoders have been known to detect the rotational position of devices. A rotation detection device has been proposed that includes two magnetic encoders arranged in concentric rings, each with a different number of magnetic poles, and magnetic sensors that detect the magnetic fields of the magnetic encoders, and that calculates the absolute angle of the magnetic encoders based on the phase difference between the magnetic field signals detected by the magnetic sensors (see, for example, Patent Document 1).

[0003] The magnetic encoder in the rotation detection device of Patent Document 1 is configured as a rubber magnet, for example, by vulcanizing an elastic member mixed with magnetic powder to a magnetic core, and forming magnetic poles alternately in the circumferential direction on this elastic member to form a magnetic track. Another configuration example of a magnetic encoder is also described, in which a resin molded body is formed by molding a resin mixed with magnetic powder onto a magnetic core, and this resin molded body can be used as a resin magnet, with magnetic poles alternately in the circumferential direction to form a magnetic track. Such rubber magnets and resin magnets typically use ferrite magnet powder as the magnetic powder.

[0004] To improve the magnetic properties of a magnetic encoder, it is preferable to have a larger amount of magnetic material in the magnetic encoder, and it is also preferable for the magnetic powder to have higher magnetic properties. For this reason, using rare earth magnetic powder rather than ferrite magnetic powder improves the magnetic properties. Therefore, it is possible to construct the magnetic encoder, which is the object to be magnetized, using a rare earth bonded magnet.

[0005] When magnetizing the multiple magnetic poles (north and south poles) that form the magnetic tracks of a magnetic encoder, a magnetizing device that uses a coil current flow method (so-called pulse magnetization method) is generally used. This coil current flow method magnetizes the object to be magnetized by the magnetic field generated by passing a pulse current through a field magnet part having a coil wound around a magnetizing yoke, for example. However, as described in Patent Document 2, for example, if the magnetic pole width of the magnetic sensor that detects the magnetic track of the magnetic encoder is limited to 1.28 mm, it is difficult to form multiple magnetic poles by saturating magnetization at a magnetic pole pitch as narrow as 1.28 mm using the pulse magnetization method.

[0006] For this reason, a method has been proposed that enables favorable magnetization even in the case of multi-pole magnetization, by heating the object to be magnetized to a temperature equal to or higher than the Curie point of the magnet, and then continuously applying a magnetizing magnetic field to the object to be magnetized using a permanent magnet that serves as a field source while cooling the object to a temperature below the Curie point (see, for example, Patent Document 3).

[0007] The magnetization device in Patent Document 3 describes an isotropic rare earth iron-based bonded magnet that is made by mixing isotropic magnetic powder with epoxy resin, compressing it, and curing it at a predetermined temperature, and is capable of effectively magnetizing multiple poles with a narrow magnetic pole pitch such as 1.28 mm.

[0008] JP 2008-267867 A JP 2017-32327 A JP 2021-093521 A

[0009] In light of the recent rise in the price of rare earth magnetic powder, it is preferable to use an isotropic rare earth bonded magnet, which contains a small amount of rare earth magnetic powder, in a magnetic encoder, although the magnetic properties will be lower than those of an isotropic rare earth iron-based bulk magnet made by sintering magnetic powder at a predetermined temperature.When a rare earth bonded magnet is used, the magnetizing device of Patent Document 3 can be used to magnetize multiple poles with a narrow magnetic pole pitch in an appropriate manner, and cost reductions can be expected.

[0010] Rare earth bonded magnets are made by mixing rare earth magnet powder with a thermosetting resin, compressing the mixture to form a green body, then thermally curing the resin contained in the green body to form a cured body (thermosetting body), and magnetizing the cured body with a predetermined magnetic pole pitch to produce a magnetic encoder.

[0011] Rare earth bonded magnets are composed of rare earth magnetic powder, a thermosetting resin binder, and voids, with the volume ratios of each being approximately 80% magnetic powder, 10% resin, and 10% voids (air holes). Because magnetic powder contains a mixture of magnetic powders with various particle sizes, it is prone to deformation after thermal curing due to variations in compactability when the green body is thinned and variations in the density of the green body. Furthermore, since only the magnetic powder contributes to the magnetic properties of a magnetic encoder, it is important for the magnetic powder to be distributed evenly and for the magnetic properties to be kept to a minimum in order to achieve high accuracy in a magnetic encoder.

[0012] Patent Document 3 describes that isotropic rare earth iron-based bonded magnets can be magnetized favorably even when multiple poles are magnetized with a narrow magnetic pole pitch. However, there is room for further consideration in terms of the angular accuracy of the magnetic encoder.

[0013] SUMMARY OF THE INVENTION Therefore, an object of the present invention is to provide a magnetic encoder using a rare earth bonded magnet that reduces variations in magnetic characteristics and achieves high angular accuracy.

[0014] In order to solve the above-mentioned problems and achieve the object, a magnetic encoder according to one embodiment of the present invention is a ring-shaped magnetic encoder that includes rare earth magnet powder and a cured resin of a thermosetting resin, and has a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of the surface, wherein the rare earth magnet powder is an isotropic Nd—Fe—B-based magnet powder with a particle size of 45 μm or more and less than 75 μm, the cured resin is contained in an amount of 5 wt % or more and 6.5 wt % or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.

[0015] According to one aspect of the present invention, a magnetic encoder with high angular accuracy is obtained.

[0016] FIG. 1 is a diagram for explaining a magnetic encoder according to a first embodiment.

[0017] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to these embodiments. Furthermore, the components in the following embodiments include those that are easily replaceable by those skilled in the art, or those that are substantially the same.

[0018] <Embodiment 1> The magnetic encoder of embodiment 1 is a ring-shaped magnetic encoder that includes rare earth magnet powder and a cured resin of a thermosetting resin, and has a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of the surface, the rare earth magnet powder being an isotropic Nd—Fe—B-based magnet powder with a particle size of 45 μm or more and less than 75 μm, the cured resin being included in an amount of 5 wt % or more and 6.5 wt % or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.

[0019] When using an isotropic rare earth bonded magnet made with Nd—Fe—B-based magnetic powder in a magnetic encoder, if the rare earth magnetic powder contains magnetic powders of various particle sizes, the resulting magnetic encoder will detect variations in the surface magnetic flux from each magnetic pole. This results in variations in the output of the magnetic sensor that detects the magnetic flux from the magnetic poles of the magnetic encoder, making it difficult to improve the angular accuracy of the magnetic encoder. Therefore, we have found that in order to reduce the variation in surface magnetic flux from location to location (from pole to pole) throughout the magnetic encoder and achieve a uniform state, it is effective to reduce the particle size of the rare earth magnetic powder while narrowing its particle size distribution. Note that, generally, the smaller the particle size of the magnetic powder, the lower the static magnetic properties (residual magnetic flux density) of the magnetic powder. However, the magnetic encoder of embodiment 1 prioritizes suppressing variations in static magnetic properties and achieving a uniform state.

[0020] FIG. 1 is a diagram illustrating a magnetic encoder according to a first embodiment. The magnetic encoder 1 has a vernier structure with two concentric magnetic tracks (a main track 11 and a sub-track 12) formed on one axial end face. Specifically, in the axial direction, the main track 11 is magnetized circumferentially at a predetermined magnetic pole pitch on the outer circumferential side, and the sub-track 12 is magnetized circumferentially at a predetermined magnetic pole pitch on the inner circumferential side. If the main track 11 is magnetized with n pole pairs, the sub-track 12 is magnetized with (n-1) pole pairs. When the magnetic pole width of the magnetic sensor detecting the magnetic track of the magnetic encoder is limited, the magnetic pole pitch of the magnetic track formed on the magnetic encoder is set to the same width as the magnetic pole width of the magnetic sensor. For example, the predetermined pitch is 0.4 mm to 2.4 mm, more specifically, 1.28 mm. Furthermore, the magnetic encoder 1 has non-magnetized regions 13 on the end face between the main track 11 and the sub-track 12 and on the inner circumferential side of the sub-track 12.

[0021] The rare earth magnet powder contained in the magnetic encoder of embodiment 1 is an isotropic Nd (neodymium)-Fe (iron)-B (boron) based magnet powder. Examples of the isotropic Nd—Fe—B based magnet powder include MQP-14-12 (product name), MQP-8-5 (product name), MQP-10-8.5HD (product name), MQP-11-8 (product name), and MQP12-8HD (product name) manufactured by Magnequench Corporation.

[0022] Alternatively, for example, Nd—Fe—B magnet powder produced by a rapid cooling method may be used. Specifically, an Nd—Fe—B alloy is melted by high-frequency induction heating under reduced pressure or in an argon atmosphere. The molten alloy is then sprayed onto a rotating copper roll and rapidly cooled (rapidly cooled) to produce ribbon-shaped thin strips. The thin strips are then broken into pieces, for example, several millimeters to several tens of millimeters in size, and pulverized using a grinder or the like to obtain powder. The pulverized powder is then classified using a sieve with a specified mesh and then heat-treated to produce rare earth magnet powder. This rare earth magnet powder is magnetically isotropic because the easy axes of magnetization of the crystal grains are not aligned in a single direction.

[0023] The rare earth magnet powder has a particle size of 45 μm or more and less than 75 μm. This particle size range can be adjusted by classification using a sieve with a predetermined mesh.

[0024] The cured thermosetting resin contained in the magnetic encoder of the first embodiment is specifically a cured epoxy resin.

[0025] In the magnetic encoder of embodiment 1, the cured resin is contained in an amount of 5% by weight to 6.5% by weight, and the rare earth magnet powder is contained in an amount of 93.5% by weight to 95% by weight, based on 100% by weight of the magnetic encoder. In the magnetic encoder of embodiment 1, it is preferable that the rare earth magnet powder and the cured thermosetting resin are uniformly mixed.

[0026] As described above, the magnetic encoder of embodiment 1 has the above thickness and contains rare earth magnet powder within the above particle size range and cured resin in the above ratio, and therefore has excellent angular accuracy and rolling strength.

[0027] Furthermore, from the viewpoint of compression strength, it is preferable that, out of 100% by weight of the magnetic encoder of embodiment 1, the cured resin is contained in an amount of 6% by weight or more and 6.5% by weight or less, and the rare earth magnet powder is contained in an amount of 93.5% by weight or more and 94% by weight or less.

[0028] The magnetic encoder of the first embodiment can be fabricated, for example, as follows. First, the rare earth magnet powder and the components constituting the cured resin in the magnetic encoder (the raw material components of the cured resin) are mixed in a predetermined blending ratio to prepare a compound. The blending ratio of the rare earth magnet powder to the raw material components of the cured resin is considered to be the same as the ratio of the rare earth magnet powder to the cured resin in the fabricated magnetic encoder. The raw material components of the cured resin include a thermosetting resin binder (e.g., epoxy resin) and a curing agent. Furthermore, a small amount of a lubricant (e.g., calcium stearate) may be added when preparing the compound. Specifically, the lubricant may be blended in an amount of 0.02 wt % or more but less than 0.5 wt % relative to 100 wt % of the combined total of the rare earth magnet powder and the raw material components of the cured resin.

[0029] Next, the compound is filled into the cavity of a mold and compressed under a predetermined pressure to produce a donut-shaped green body. The green body is then removed from the mold and placed in an oven where it is thermally cured at a predetermined temperature for a predetermined time to produce a cured body (thermoset body) containing the rare earth magnet powder and the cured resin. It is also preferable to apply a rust prevention measure to the surface of the cured body to prevent oxidation. Rust prevention measures that can be used include known methods such as electrodeposition coating and spray coating.

[0030] Next, as shown in FIG. 1, a vernier system is constructed in which two concentric magnetic tracks are formed on one axial end surface of the cured body. This configuration is also shown in the diagrams of Patent Document 1. Specifically, in the axial direction, a main track is magnetized circumferentially on the outer circumferential side with a predetermined magnetic pole pitch, and a sub-track is magnetized circumferentially on the inner circumferential side with a predetermined magnetic pole pitch. If the main track is magnetized with n pole pairs, the sub-track is magnetized with (n-1) pole pairs. Regarding the magnetic pole pitch, if the magnetic sensor detecting the magnetic track of the magnetic encoder has a limited magnetic pole width, the magnetic track formed on the magnetic encoder is formed with the same magnetic pole pitch as the magnetic sensor's magnetic pole width. Magnetization is so-called magnetization, and the magnetization method can be performed by, for example, heating the object to be magnetized above the Curie point of the magnetic powder and continuously applying a magnetizing magnetic field to the object to be magnetized using a permanent magnet as a field source while cooling it below the Curie point, as disclosed in Patent Document 3. Since the sub-track is located closer to the inner periphery than the main track, the magnetic pole pitch is set to correspond to the inner diameter position of the detection portion of the magnetic sensor for the sub-track. In this way, the magnetic encoder of the first embodiment is obtained.

[0031] <Embodiment 2> The magnetic encoder of embodiment 2 is a ring-shaped magnetic encoder containing rare earth magnet powder and a cured thermosetting resin, and having a magnetic track formed by magnetizing multiple magnetic poles at a predetermined pitch in the circumferential direction of the surface, where the rare earth magnet powder is an isotropic Nd—Fe—B-based magnet powder with a particle size of 45 μm or more and less than 175 μm, the cured resin is contained in an amount of 5 wt % to 6.5 wt %, and the thickness of the ring-shaped magnetic encoder is 0.2 mm to 0.4 mm. Other than the thickness of the ring-shaped magnetic encoder, the configurations and functions of the components of the magnetic encoder of embodiment 2 are the same as those of the magnetic encoder of embodiment 1. Therefore, detailed description will be omitted here.

[0032] The magnetic encoder of embodiment 2 also has the above thickness and contains rare earth magnet powder within the above particle size range and cured resin in the above ratio, so it has excellent angular accuracy and rolling strength.

[0033] <Other embodiments> This embodiment 1 is an axial magnetic encoder having a vernier system in which two magnetic tracks are formed on a donut-shaped (ring-shaped) magnetic encoder as shown in Figure 1, but it may also be a radial magnetic encoder having a vernier system in which two magnetic tracks are formed on the side of a hollow cylindrical magnetic encoder.

[0034] The present invention will be explained in more detail below based on examples, but the present invention is not limited to these examples.

[0035] [Example] <Magnetic Encoder Fabrication> Isotropic Nd—Fe—B magnet powder was used as the rare earth magnet powder. MQP-14-12 (product name) manufactured by Magnequench was prepared as the isotropic Nd—Fe—B magnet powder. The MQP-14-12 particle size was classified into three groups: 75 μm or more and less than 150 μm, 45 μm or more and less than 75 μm, and 32 μm or more and less than 45 μm. The classification was carried out using a sieve with a specified mesh. Next, for each of the three groups, the isotropic Nd—Fe—B magnet powder was mixed with raw materials for a cured resin (manufactured by Pernoc, model number XW2310) containing an epoxy resin binder and a curing agent at a specified blending ratio to prepare a compound. Here, the blending ratios of the raw materials for the cured resin and the rare earth magnet powder were 2.5% by weight and 97.5% by weight, respectively, with the total weight being 100% by weight. Furthermore, compounds were also prepared in the following cases: 5% by weight of the raw materials for the cured resin and 95% by weight of the rare earth magnet powder; 5.5% by weight of the raw materials for the cured resin and 94.5% by weight of the rare earth magnet powder; 6% by weight of the raw materials for the cured resin and 94% by weight of the rare earth magnet powder; 6.5% by weight of the raw materials for the cured resin and 93.5% by weight of the rare earth magnet powder; and 7.5% by weight of the raw materials for the cured resin and 92.5% by weight of the rare earth magnet powder. The compounds were prepared by mixing the raw materials for the cured resin dissolved in a solvent with the rare earth magnet powder, evaporating the solvent, and then crushing and classifying the mixture. All compounds were prepared with the same particle size, and the fluidity conditions for filling the mold cavity were the same. The compound was then filled into the mold cavity and compressed under a predetermined pressure to produce a donut-shaped green body. The green body had an outer diameter of 56 mm, an inner diameter of 41 mm, and a thickness of 1 mm. Green bodies with thicknesses of 0.4 mm and 0.2 mm were also produced. The green body was then removed from the mold and placed in an oven, where it was thermally cured at a predetermined temperature (150°C) for a predetermined time to produce a cured body (thermoset). The cured body had an outer diameter of 56 mm, an inner diameter of 41 mm, and a thickness of 1 mm. Cured bodies with thicknesses of 0.4 mm and 0.2 mm were also produced.As shown, no difference in size was observed between the green body and the cured body. Next, after applying a rust prevention treatment (specifically, electrocoating) to prevent oxidation to the surface of the cured body, a vernier-type structure was formed in which two concentric magnetic tracks were formed on one axial end surface of the thermoset body, as shown in Figure 1. Specifically, in the axial direction, a main track was magnetized circumferentially on the outer circumferential side with a predetermined magnetic pole pitch, and a sub-track was magnetized circumferentially on the inner circumferential side with a predetermined magnetic pole pitch. The main track was magnetized with 32 pole pairs, and the sub-track was magnetized with 31 pole pairs. In this example, since a magnetic sensor with a pole width limited to 1.28 mm was used, the main track of the magnetic encoder was magnetized to 1.28 mm. The magnetization was so-called magnetization, and the magnetization method was, for example, as disclosed in Patent Document 3, a method in which a magnetizing magnetic field is continuously applied to the magnetized object using a permanent magnet as a field source while the object is heated to above the Curie point of the magnetic powder and cooled below the Curie point. Since the sub-track is located more inward than the main track, the magnetic pole pitch was set to correspond to the inner diameter position of the detection part of the magnetic sensor for the sub-track. In this way, ring-shaped magnetic encoders (samples 1 to 54) containing rare earth magnet powder and a cured resin of a thermosetting resin were produced, and having magnetic tracks formed by magnetizing multiple magnetic poles at a predetermined pitch in the circumferential direction of the surface.

[0036] <Evaluation Method> (Moldability) The compound was filled into the cavity of a mold and compression molded into a doughnut-shaped green body, and the handleability when removing it from the mold was evaluated. Specifically, when the green body was removed from the mold with an ejector pin provided on the mold, the state of cracks and chips that occurred in the green body was visually observed and evaluated as moldability. The evaluation criteria were as follows: ○: No cracks or chips ×: Cracks or chips present

[0037] (Thickness Precision) The cured body was removed from the oven and the thickness was measured at eight diagonal positions with a micrometer to evaluate the thickness variation (maximum value - minimum value). The evaluation criteria are as follows: ○: Samples with a variation value of less than 0.06 mm were rated as good. △: Samples with a variation value between 0.06 mm and 0.08 mm were rated as fair. ×: Samples with a variation value of more than 0.08 mm were rejected.

[0038] (Radial crushing strength) The radial crushing strength was measured in accordance with JIS Z2507. The evaluation criteria are as follows: ⊚: The radial crushing strength is 100 MPa or more. ◯: The radial crushing strength is 60 MPa or more and less than 100 MPa. Δ: The radial crushing strength is 50 MPa or more and less than 60 MPa. ×: The radial crushing strength is less than 50 MPa.

[0039] (Angular Accuracy) The angular accuracy of the magnetic encoder magnetized by the above-mentioned method was measured. The evaluation criteria were as follows. To evaluate the angular accuracy, the magnet and IC board were attached to the shaft of a reference servo motor equipped with an optical encoder (angle accuracy of ±10 seconds or less, resolution of 20 bits or more), and the reference motor was driven in 1-degree increments (twice: 360 degrees CW and CCW), and the difference between the angle output from the IC and the reference angle was measured. The difference between the maximum and minimum values ​​was taken as the angular error. ◎: The magnetic flux variation is 0.05 degrees or less. ○: The magnetic flux variation is more than 0.05 degrees and less than 0.07 degrees. △: The magnetic flux variation is more than 0.07 degrees and less than 0.1 degrees. ×: The magnetic flux variation is 0.1 degrees or more.

[0040] (Overall Evaluation) An overall evaluation was performed on Samples 1 to 54. The evaluation criteria are as follows: ○: The evaluation result for each evaluation item was only ◯ or ◎. ×: The evaluation result for each evaluation item included △ or ×. The evaluation results for Samples 1 to 54 are shown in Tables 1 to 3 below. In Table 1, the magnetic powder particle size (μm) of "75-150" indicates that the particle size of the isotropic Nd—Fe—B based magnetic powder was in the range of 75 μm or more and less than 150 μm. In Table 2, the magnetic powder particle size (μm) of "45-75" indicates that the particle size of the isotropic Nd—Fe—B based magnetic powder was in the range of 45 μm or more and less than 75 μm. In Table 3, the magnetic powder particle size (μm) of "32-45" indicates that the particle size of the isotropic Nd—Fe—B based magnetic powder was in the range of 32 μm or more and less than 45 μm.

[0041]

[0042] Table 1 shows the evaluation of the magnetic encoders for Samples 1 to 18. The particle size of the isotropic Nd—Fe—B magnetic powder for Samples 1 to 18 ranged from 75 μm to less than 150 μm. Samples 1 to 3, in which the amount of raw material components in the cured resin was 2.5 wt %, had a fair radial crushing strength. This was due to the low amount of raw material components in the cured resin. When ejecting the sample (green body) from the mold with an ejector pin, chips and cracks occurred on the outer edge. If these chips and cracks extend into the track formation area when magnetizing the sample to form tracks in a subsequent process, the tracks cannot be formed. Furthermore, because Nd—Fe—B magnetic powder is used as the rare earth magnetic powder, the sample is prone to rust. Therefore, a rust-preventive film must be coated on the sample surface to prevent oxidation. However, the areas with chips and cracks do not form a uniform rust-preventive film, which may lead to rust formation. In samples 16 to 18, in which the amount of raw material components of the cured resin was 7.5% by weight, some of the binder leaked from the cavity. Therefore, angular accuracy was not evaluated. This is due to the amount of raw material components of the cured resin being too high. The angular accuracy of samples 22 to 33, described below, was all rated as Excellent. This is due to the particle size of the isotropic Nd—Fe—B magnetic powder being in the range of 45 μm or more and less than 75 μm. This is thought to be due to the smaller particle size range compared to the range of Nd—Fe—B magnetic powder in samples 1 to 18 shown in Table 1, which reduces the variation in the distribution of magnetic powder in a given area (or volume), and therefore reduces the overall variation in magnetic properties for each magnetic pole. The angular accuracy at a sample thickness of 1 mm was rated as poor. This is due to the particle size of the Nd—Fe—B magnetic powder being in the range of 75 μm or more and less than 150 μm. This is thought to be because the particle size of Nd—Fe—B based magnetic powder is large, which results in greater variation in the area occupied by the magnetic powder in the thickness direction within a given area, resulting in greater variation in the magnetic properties of each magnetic pole.

[0043]

[0044] Table 2 shows the evaluation of the magnetic encoders for Samples 19 to 36. The particle size of the isotropic Nd—Fe—B magnet powder in Samples 19 to 36 was in the range of 45 μm or more and less than 75 μm. Samples 19 to 21, in which the raw material component content of the cured resin was 2.5 wt%, had a radial crushing strength of Fair. This is due to the low amount of raw material component in the cured resin. Furthermore, in Samples 34 to 36, in which the raw material component content of the cured resin was 7.5 wt%, some of the binder leaked from the cavity. Therefore, angular accuracy was not evaluated. This is due to the excessive amount of raw material component in the cured resin. Samples 22 to 33, other than the sample with the raw material component content of 2.5 wt%, were evaluated as either ◎ or 〇 in all items. Therefore, the overall evaluation of Samples 22 to 33 shown in Table 2 is 〇. The angular accuracy of Samples 22 to 33 was evaluated as ◎. This is because the particle size of the isotropic Nd—Fe—B magnetic powder is in the range of 45 μm or more and less than 75 μm. This is in a smaller range than the particle size range of the Nd—Fe—B magnetic powder in Samples 1 to 18 shown in Table 1, so there is less variation in the area occupied by the magnetic powder in the thickness direction in a given area, which is thought to be why there is also less variation in the magnetic properties for each magnetic pole.

[0045]

[0046] Table 3 shows the evaluation of the magnetic encoders for Samples 37 to 54. The particle size of the isotropic Nd—Fe—B magnetic powder in Samples 37 to 54 was in the range of 32 μm or more and less than 45 μm. Samples 37 to 39, in which the raw material component content of the cured resin was 2.5 wt%, had a fair radial crushing strength. This is due to the low amount of raw material component in the cured resin. Furthermore, Samples 52 to 54, in which the raw material component content of the cured resin was 7.5 wt%, had some binder leaking from the cavity. Therefore, angular accuracy was not evaluated. This is due to the excessive amount of raw material component in the cured resin. All samples other than the above were evaluated as fair in angular accuracy. This is likely due to the small particle size of the Nd—Fe—B magnetic powder, between 32 μm and 45 μm. The smaller the particle size of the magnetic powder, the poorer the squareness of the demagnetization curve of the magnetic powder itself and the greater the susceptibility to deterioration of magnetic properties due to thermal degradation, oxidative degradation, and other factors. This is thought to be due to the reduced surface magnetic flux from the magnetic encoder. For this reason, the overall evaluation of samples 37 to 54 shown in Table 3 was all rated as x.

[0047] 1 magnetic encoder, 11 main track, 12 sub-track, 13 non-magnetized area, D outer diameter, d inner diameter, t thickness

Claims

1. A ring-shaped magnetic encoder comprising rare earth magnet powder and a cured thermosetting resin, and having a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of the surface, wherein the rare earth magnet powder is an isotropic Nd-Fe-B magnet powder having a particle size of 45 μm or more and less than 75 μm, the cured resin is contained in an amount of 5% by weight or more and 6.5% by weight or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.

2. A ring-shaped magnetic encoder comprising rare earth magnet powder and a hardened thermosetting resin, and having a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of the surface, wherein the rare earth magnet powder is an isotropic Nd-Fe-B magnet powder having a particle size of 45 μm or more and less than 175 μm, the hardened resin is contained in an amount of 5% by weight or more and 6.5% by weight or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 0.4 mm or less.

3. A magnetic encoder according to claim 1 or 2, characterized in that the magnetization is performed in the axial direction.

Citation Information

Patent Citations

  • Permanent-magnet motor and other device applied thereon

    JP2000060080A

  • Method of manufacturing resin-bonded permanent magnet

    JP2006278461A

  • Method of manufacturing bond magnet

    JP2013157506A

  • Rare earth magnet powder, rare earth bonded magnet, and method of manufacturing rare earth bonded magnet

    JP2019102583A

  • Magnetization device and magnetized object

    JP2021093521A