Reducing agent, and method for producing gas

A reducing agent with an oxygen carrier composed of specific metal elements enhances the stability and efficiency of carbon dioxide conversion to carbon monoxide at high temperatures, addressing the inefficiencies of conventional methods by ensuring stable oxygen ion conductivity and crystal structure integrity.

WO2024203959A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011495
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for converting carbon dioxide to carbon monoxide, such as the reverse water gas shift reaction, suffer from low conversion efficiency due to chemical equilibrium constraints, and there is a lack of understanding about the stability and conversion rate of oxygen vacancy reactions at high temperatures in chemical looping methods.

Method used

A reducing agent containing an oxygen carrier with oxygen ion conductivity, comprising at least two metal elements from Group 3 or Group 4 of the periodic table, including lanthanides and actinides, is used to stabilize the conversion of carbon dioxide to carbon monoxide at high temperatures, with specific electrical conductivity and X-ray diffraction characteristics that ensure long-term stability and efficient oxygen ion movement.

Benefits of technology

The reducing agent enables stable and efficient conversion of carbon dioxide to carbon monoxide at high temperatures, maintaining performance over a long period and improving the carbon dioxide and hydrogen conversion rates, thus overcoming the limitations of conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000030_0000
    Figure 00000030_0000
  • Figure 00000030_0001
    Figure 00000030_0001
Patent Text Reader

Abstract

[Problem] To provide: a reducing agent which can be used stably for a long period in reactions at high temperatures; and a method for producing a gas using the reducing agent. [Solution] According to one aspect of the present invention, there is provided a reducing agent with which carbon dioxide is reduced to produce a valuable carbon substance. The reducing agent comprises an oxygen carrier having oxygen ion conductivity and containing at least two metal elements selected from metal elements belonging to Group 3 or Group 4 on the periodic table including lanthanoid elements and actinoid elements. The oxygen carrier has electroconductivity of 1×10-7 S / cm or more at a temperature of 700°C under a pure oxygen atmosphere. When the reducing agent is subjected to an X-ray diffraction measurement in the measurement range of 10° to 90.5° inclusive, the full width at half maximum of all of peaks observed in an X-ray diffraction profile is less than 1.5°.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing reducing agent and gas

[0001] The present invention relates to a reducing agent and a method for producing a gas, and more particularly to a reducing agent that can be used in, for example, a chemical looping method, and a method for producing a gas using such a reducing agent.

[0002] In recent years, the concentration of carbon dioxide, a greenhouse gas, has been increasing in the atmosphere. This increase in atmospheric carbon dioxide concentration contributes to global warming. Therefore, it is important to capture carbon dioxide released into the atmosphere. Furthermore, if the captured carbon dioxide could be converted into valuable carbon resources and reused, a carbon-recycling society could be realized. Conventionally, a method using the reverse water-gas shift reaction (RWSR) has been known as a method for producing carbon monoxide from carbon dioxide. However, this conventional RWSR has a problem in that the conversion efficiency (yield) of carbon dioxide to carbon monoxide is low due to constraints of chemical equilibrium, since the products, carbon monoxide and water, coexist in the system.

[0003] To solve the above problem, the chemical looping method is used to convert (synthesize) carbon dioxide into carbon monoxide. The chemical looping method is a method in which the reverse water gas shift reaction is divided into two reactions: a reduction reaction with hydrogen and a production reaction of carbon monoxide from carbon dioxide. These reactions are carried out using an oxygen carrier (e.g., a metal oxide: MO). x ) is used to bridge the gap (see the formula below). 2 + MO x → H 2 O + MO x-1 CO 2 + MO x-1 → CO + MO x In the above formula, MO x-1 indicates a state in which the metal oxide is partially or completely reduced.

[0004] In the chemical looping method, because the substrates for the reverse reaction, water and carbon monoxide, do not coexist during each reaction, it is possible to obtain a higher conversion efficiency of carbon dioxide to carbon monoxide than the chemical equilibrium of the reverse water-gas shift reaction. Conventionally, in the chemical looping method, the reaction of converting carbon dioxide to carbon monoxide via oxygen vacancies formed in the oxygen carrier is carried out at a temperature of 650°C or less (see Patent Document 1).

[0005] Ind. Eng. Chem. Res. 2013, 52, 8416-8426

[0006] According to the studies of the present inventors, since the reaction of hydrogen to generate oxygen vacancies in the crystal structure of the oxygen carrier is an endothermic reaction, it has been found that in order to efficiently generate these oxygen vacancies, it is better to carry out the reaction at a higher temperature. However, until now, there has been insufficient research into the conversion rate and stability of the reaction of generating oxygen vacancies in the high temperature range (temperatures above 650°C). In view of the above circumstances, the present invention aims to provide a reducing agent that can be used stably for a long period of time in a reaction at a high temperature, and a method for producing a gas using such a reducing agent.

[0007] According to one aspect of the present invention, there is provided a reducing agent for reducing carbon dioxide to produce carbon valuables. The reducing agent contains an oxygen carrier having oxygen ion conductivity, which contains at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides. The oxygen carrier has an oxygen ion conductivity of 1×10 in a pure oxygen atmosphere at a temperature of 700° C. -7 The reducing agent has an electrical conductivity of 20 S / cm or more, and when X-ray diffraction measurement is performed on the reducing agent in a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°.

[0008] According to this embodiment, a reducing agent that can be stably used for a long period of time in a reaction at high temperature can be obtained.

[0009] FIG. 1( a) is an example of an image obtained by STEM-EDS measurement of a reducing agent in which an oxygen carrier and a sub-compound exist independently, and FIG. 1( b) is a graph showing a line profile of the mapping of each element along the white line in FIG. 1( a). FIG. 2( a) is an example of an image obtained by STEM-EDS measurement of a reducing agent in which an oxygen carrier and a sub-compound exist as a solid solution, and FIG. 2( b) is a graph showing a line profile of the mapping of each element along the white line in FIG. 2( a). FIG. 3 is a graph showing an example of the change in electrical conductivity with changes in oxygen partial pressure. FIG. 4 is an X-ray diffraction profile of the reducing agent obtained in Example 2. FIG. 5 is an X-ray diffraction profile of the reducing agent obtained in Example 4. FIG. 6 is an X-ray diffraction profile of the reducing agent obtained in Example 5. FIG. 7 is an X-ray diffraction profile of the reducing agent obtained in Example 6. FIG. 8 is an X-ray diffraction profile of the reducing agent obtained in Comparative Example 2.

[0010] The reducing agent and gas production method of the present invention will be described in detail below based on preferred embodiments. [Reducing Agent] The reducing agent of this embodiment is used when producing a product gas containing carbon monoxide (carbon valuable) by reducing carbon dioxide by contacting a raw material gas containing carbon dioxide with the reducing agent (by causing the reducing agent to act on the raw material gas) (i.e., used in the gas production method of this embodiment). Furthermore, the reducing agent oxidized by contact with carbon dioxide can be reduced (regenerated) by contacting it with a reducing gas containing hydrogen (reducing substance). In this case, preferably, the raw material gas and the reducing gas are passed alternately through a reaction tube (reaction vessel) filled with the reducing agent of this embodiment, whereby the carbon dioxide is converted to carbon monoxide by the reducing agent and the oxidized reducing agent is regenerated by the reducing gas.

[0011] The reducing agent of this embodiment contains an oxygen carrier with oxygen ion conductivity. Here, the oxygen carrier is a compound capable of generating reversible oxygen deficiency. The oxygen carrier itself loses oxygen element through reduction, but when it comes into contact with carbon dioxide in an oxygen-deficient state (reduced state), it acts to remove oxygen element from carbon dioxide and reduce it. The oxygen carrier of this embodiment contains at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides. The inclusion of two or more metal elements in this oxygen carrier creates distortion in the crystal lattice, facilitating the transfer of oxygen element between the oxygen carrier and a counter substance (e.g., carbon dioxide, hydrogen). This improves the conversion efficiency of carbon dioxide to carbon monoxide (also referred to as the carbon dioxide conversion rate) and the conversion efficiency of hydrogen to water (also referred to as the hydrogen conversion rate). The carbon dioxide conversion rate and hydrogenation rate can be determined by the methods described in the examples.

[0012] The oxygen carrier is 1×10 in a pure oxygen atmosphere at a temperature of 700°C. -7 The reducing agent containing the oxygen carrier having such electrical conductivity can sufficiently increase the migration speed of oxygen ions in the oxygen carrier, so that oxygen elements are efficiently released by contact with the reducing gas, oxygen vacancies are smoothly induced, and the induced oxygen vacancies facilitate the removal of oxygen elements from carbon dioxide. The electrical conductivity in a pure oxygen atmosphere at a temperature of 700°C is 1 x 10 -7 S / cm or more is sufficient, but 1×10 -6 S / cm or more, and preferably 1×10 -5 S / cm or more is more preferable, and 1×10 -4 It is more preferable that the electrical conductivity is 1×10 S / cm or more in a pure oxygen atmosphere at a temperature of 700°C. -1 S / cm or less, and may be 1×10 -2 In this specification, the pure oxygen atmosphere refers to a condition in which the oxygen concentration is 99% by volume or more.

[0013] Furthermore, when the reducing agent of this embodiment is subjected to X-ray diffraction measurement in a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°. This indicates that the crystal lattice in the oxygen carrier has grown sufficiently, meaning that the crystal has high stability. Therefore, such a reducing agent can maintain its performance even when used for a long period of time. The full width at half maximum of all peaks may be less than 1.5°, but is preferably 1.25° or less, and more preferably 1° or less. The full width at half maximum of the peaks is preferably 0.1° or more, and more preferably 0.5° or more. Furthermore, the reducing agent to be subjected to X-ray diffraction measurement can be accurately measured if it has a mass of approximately 50 mg. Note that the timing for measuring the electrical conductivity and the X-ray diffraction measurement is both before the reducing agent is used in a reaction with a gas.

[0014] The reducing agent of this embodiment preferably further contains an element belonging to Groups 6 to 14 of the periodic table. The element belonging to Groups 6 to 14 of the periodic table may be, for example, indium (In), tin (Sn), technetium (Tc), silver (Ag), or the like, or may be an element exemplified below. The element belonging to Groups 6 to 14 of the periodic table more preferably includes an element belonging to Groups 8 to 12 of the periodic table, and more preferably includes iron (Fe), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), or silicon (Si). These elements may be used alone or in combination of two or more. Furthermore, when the oxygen carrier has an electrical conductivity of σA [S / cm] in a pure oxygen atmosphere at a temperature of 700°C and an electrical conductivity of σB [S / cm] in an argon gas atmosphere containing 1% by volume of carbon monoxide, the ratio σB / σA is preferably less than 85. In this case, as shown in Figure 3, the difference in electrical conductivity of the oxygen carrier under atmospheres of different oxygen partial pressures is small, which means that the reactivity change of the oxygen carrier is small. Therefore, a reducing agent containing such an oxygen carrier can exist stably and maintain its performance even when used for a long period of time. σB / σA may be less than 85, but is preferably 80 or less, and more preferably 60 or less. σB / σA may be 10 or more, or may be 20 or more.

[0015] The reducing agent of this embodiment preferably contains an element belonging to Groups 6 to 14 of the periodic table as a secondary compound containing the element. Examples of the secondary compound include oxides, nitrides, oxynitrides, and carbides. Examples of the secondary compound include NiO, Fe, 2 O 3 , SiC, etc. By using these secondary compounds, the time for which the carbon dioxide conversion rate and hydrogen conversion rate of the reducing agent are maintained can be sufficiently extended. Among these, oxides are preferred as the secondary compounds. Oxides have high affinity with oxygen carriers, and therefore can increase the mechanical strength of the reducing agent as a whole. In addition, part of the oxygen element in the oxide can be utilized as oxygen ions, which provides an excellent effect in maintaining the carbon dioxide conversion rate and hydrogen conversion rate of the reducing agent.

[0016] When this reducing agent is subjected to scanning transmission electron microscope-energy dispersive X-ray spectroscopy (STEM-EDS) measurement, the oxygen carrier and the sub-compounds are observed individually, as shown in FIG. 1, and the sub-compounds are preferably in the form of particles in contact with the oxygen carrier. This produces a spillover effect, in which hydrogen elements activated by the sub-compounds move smoothly within the oxygen carrier. This allows the reactivity of oxygen elements and hydrogen elements within the crystal lattice of the oxygen carrier to be sufficiently enhanced. As a result, the carbon dioxide conversion rate and hydrogen conversion rate of the reducing agent can be further improved. Note that when the oxygen carrier and the sub-compounds form a solid solution, they cannot be observed individually, as shown in FIG. 2.

[0017] Furthermore, when X-ray diffraction measurement is performed on this reducing agent, the peaks derived from the oxygen carrier and the peaks derived from the sub-compounds observed in the X-ray diffraction profile are preferably shifted by less than 0.3° in 2θ relative to the peaks observed in the X-ray diffraction profile when X-ray diffraction measurement is performed on the oxygen carrier alone and the sub-compound alone, respectively. This means that solid solution of the oxygen carrier and the sub-compound is suppressed, and the particles thereof exist individually (independently). Therefore, in such a reducing agent, the function of the oxygen carrier and the function of the sub-compound are exhibited in a balanced manner. This shift amount is more preferably 0.25° or less, even more preferably 0.2° or less, and particularly preferably 0.15° or less. The shift amount may be 0.05° or more, or may be 0.1° or more.

[0018] The average particle size of the particles of the secondary compound is preferably 1 nm or more and 10 μm or less, more preferably 3 nm or more and 8 μm or less, and even more preferably 5 nm or more and 6 μm or less. This increases the area of ​​the interface formed between the particles of the secondary compound and the oxygen carrier, allowing hydrogen elements activated by the secondary compound to move more smoothly through the oxygen carrier. This sufficiently enhances the reactivity between oxygen elements and hydrogen elements in the crystal lattice of the oxygen carrier. The average particle size of the particles can be determined by acquiring volume-based particle size distribution data using a laser diffraction / scattering particle size distribution analyzer (e.g., "Partica LA-960" manufactured by Horiba, Ltd.) and processing the data. Measurement is usually performed wet.

[0019] As described above, it is believed that the crystal structure of the oxygen carrier is stabilized and the heat resistance temperature is increased by the sufficient solid solution of each metal element. As a result, the reducing agent of this embodiment can be used even at high temperatures exceeding 650°C. Furthermore, at high temperatures exceeding 650°C, the metal elements constituting the oxygen carrier are alloyed and tend to form a stable crystal structure, so that the initial activity can be easily maintained even if the reducing agent is repeatedly subjected to oxidation-reduction.

[0020] The packing density of the reducing agent is preferably 4 g / mL or less, more preferably 0.5 g / mL to 3 g / mL or less, and even more preferably 1 g / mL to 2.5 g / mL or less. If this packing density is too low, the gas passage rate becomes too fast, and the contact time between the reducing agent and the raw material gas and the reducing gas decreases. As a result, the carbon dioxide conversion rate and hydrogen conversion rate by the reducing agent tend to decrease. On the other hand, if this packing density is too high, the gas passage rate becomes too slow, making it difficult for the reaction to proceed or requiring a long time to produce the product gas.

[0021] The pore volume of the reducing agent is 0.1 cm 3 / g or more, and 3 / g or more 30cm 3 / g or less, and more preferably 5 cm 3 / g or more 20cm 3 / g or less is even more preferable. If this pore volume is too small, it becomes difficult for the raw material gas and reducing gas to penetrate into the inside of the reducing agent. As a result, the contact area between the reducing agent and the raw material gas and reducing gas decreases, and the carbon dioxide conversion rate and hydrogen conversion rate by the reducing agent tend to decrease. On the other hand, even if the pore volume is increased beyond this upper limit, no further increase in effect can be expected, and depending on the type of reducing agent, mechanical strength tends to decrease.

[0022] The shape of the reducing agent is not particularly limited, but is preferably granular, for example. Granular reduces the packing density within the above range. Here, granular is a concept that includes powder, particles, lumps, pellets, etc., and the form may be any of spherical, plate-like, polygonal, crushed, columnar, needle-like, and scale-like. The average particle size of the reducing agent is preferably 1 μm or more and 5 mm or less, more preferably 10 μm or more and 1 mm or less, and even more preferably 20 μm or more and 0.5 mm or less. A reducing agent having such an average particle size can easily adjust its packing density within the above range.

[0023] In this specification, the term "average particle size" refers to the average value of the particle sizes of 200 randomly selected reducing agents in one field of view observed under an electron microscope. In this case, "particle size" refers to the maximum length of the distance between two points on the contour line of the reducing agent. When the reducing agent is columnar, the maximum length of the distance between two points on the contour line of its end face is taken as the "particle size." Furthermore, when the reducing agent is, for example, in a blocky form where primary particles are aggregated, the average particle size refers to the average particle size of secondary particles. The BET specific surface area of ​​the reducing agent is 1 m 2 / g or more 500m 2 / g or less, and 2 / g or more 450m 2 / g or less is more preferable, and 5m 2 / g or more 400m 2 / g or less is more preferable. When the BET specific surface area is within the above range, it becomes easier to improve the carbon dioxide conversion rate and hydrogen conversion rate of the reducing agent. The BET specific surface area can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method in accordance with the BET method (preferably the BET multipoint method).

[0024] Furthermore, in this embodiment, because each metal element is stably dissolved in the oxygen carrier, the oxygen capacity of the reducing agent can be maintained at a high level over a wide temperature range from low temperatures (approximately 400°C) to high temperatures (approximately 850°C). That is, the reducing agent of this embodiment can efficiently convert carbon dioxide to carbon monoxide over a wide temperature range, and can be efficiently reduced by a reducing gas containing hydrogen. The oxygen capacity of the oxygen carrier contained in the reducing agent at 400°C is preferably 0.1% by mass or more and 40% by mass or less, and more preferably 0.5% by mass or more and 30% by mass or less. If the oxygen capacity of the oxygen carrier contained in the reducing agent at low temperatures is within the above range, this means that the oxygen capacity is sufficiently high even at temperatures during actual operation (temperatures above 650°C), and it can be said that the reducing agent has extremely high carbon dioxide conversion rates and hydrogen conversion rates.

[0025] [Method for Producing Reducing Agent] Next, a method for producing a reducing agent will be described. The method for producing a reducing agent is not particularly limited, but examples thereof include a sol-gel method, a co-precipitation method, a solid-phase method, and a hydrothermal synthesis method. As an example, the reducing agent can be produced as follows. First, a salt of a metal element constituting the reducing agent is dissolved in water to prepare an aqueous solution. Next, this aqueous solution is gelled, and then dried and baked. That is, the reducing agent of this embodiment can be produced easily and reliably by the so-called sol-gel method. Note that, to prepare the aqueous solution, acidic water adjusted to an acidic state with, for example, citric acid, acetic acid, malic acid, tartaric acid, hydrochloric acid, nitric acid, or a mixture thereof may be used.

[0026] Examples of salts of metal elements include nitrates, sulfates, chlorides, hydroxides, carbonates, and composites thereof, with nitrates being preferred. Furthermore, hydrates of metal element salts may be used as needed. The gel is dried at a temperature of preferably 20°C or higher and 200°C or lower, more preferably 50°C or higher and 150°C or lower, for a time of preferably 0.5 hours or higher and 20 hours or lower, more preferably 1 hour or higher and 15 hours or lower. By drying in this manner, the gel can be dried uniformly.

[0027] The gel is preferably fired at a temperature of 300°C to 1200°C, more preferably 700°C to 1000°C, for a time of preferably 1 hour to 24 hours, more preferably 1.5 hours to 20 hours. The gel is preferably converted into an oxide by firing, but firing under the above firing conditions can easily convert it into a reducing agent. Furthermore, firing under the above firing conditions can prevent excessive particle growth of the reducing agent. The temperature should be increased at a rate of 1°C / min to 20°C / min, preferably 2°C / min to 10°C / min, until the firing temperature is reached. This promotes particle growth of the reducing agent and also prevents cracking of the crystals (particles).

[0028] The reducing agent can also be produced as follows. First, oxides containing each of the metal elements constituting the reducing agent are mixed and pulverized. For pulverization, for example, a ball mill, a bead mill, a jet mill, a hammer mill, a rod mill, or the like can be used. This pulverization can be carried out either dry or wet. Next, the pulverized aggregate is pulverized and then calcined. This calcination is preferably carried out at a temperature of 300°C to 1200°C, more preferably 700°C to 1000°C, for a time period of preferably 1 hour to 24 hours, more preferably 1.5 hours to 20 hours. The calcined aggregate is then pulverized in the same manner as above to obtain the reducing agent. The reducing agent containing a minor compound may be produced by adding the minor compound to the aqueous solution or by mixing the minor compound with the oxide, but the former is preferred.

[0029] [Method of Using the Reducing Agent] As described above, the reducing agent of this embodiment can be used, for example, in a chemical looping method. Furthermore, as described above, the reducing agent of this embodiment can be used in applications in which carbon dioxide is reduced by contact to produce carbon monoxide (carbon valuables). More specifically, a reduction reaction of carbon dioxide and a reduction reaction of the reducing agent are preferably carried out, and the reducing agent is preferably used so as to circulate between the reduction reaction of carbon dioxide and the reduction reaction of the reducing agent. In the reduction reaction of the reducing agent, a reducing gas containing another reducing substance is used.

[0030] The reducing agent of this embodiment is preferably used in a so-called reverse water gas shift reaction. The reverse water gas shift reaction is a reaction that produces carbon monoxide and water from carbon dioxide and hydrogen. When the chemical looping method is applied to the reverse water gas shift reaction, the reaction is carried out separately into a reduction reaction of the reducing agent (first process) and a reduction reaction of carbon dioxide (second process). The reduction reaction of the reducing agent is the reaction shown in formula (A) below, and the reduction reaction of carbon dioxide is the reaction shown in formula (B) below.

[0031] H 2 (Gas) + MO x (Solid) → H 2 O (gas) + MO x-1 (solid)   (A) CO 2 (Gas) + MO x-1 (solid) → CO (gas) + MO x (Solid) (B) In formulas (A) and (B), x is usually 2. That is, in the reduction reaction of the reducing agent, hydrogen, which is a type of reducing substance, is oxidized to produce water. Also, in the reduction reaction of carbon dioxide, carbon dioxide is reduced to produce carbon monoxide, which is a type of carbon valuable.

[0032] The reaction temperature in the reduction reaction of the reducing agent (contact temperature of the reducing agent with the reducing gas) may be any temperature at which the reduction reaction can proceed, but is preferably a temperature above 650°C, more preferably 700°C or higher, even more preferably 750°C or higher, and particularly preferably 800°C or higher. Within this temperature range, the reduction reaction of the reducing agent can proceed efficiently. The upper limit of this reaction temperature is preferably 1050°C or lower, more preferably 1000°C or lower, even more preferably 950°C or lower, particularly preferably 900°C or lower, and most preferably 850°C or lower. Setting the upper limit of the reaction temperature within the above range can improve economic efficiency. The lower limit and upper limit can be combined in any way to define the reaction temperature range.

[0033] Furthermore, during the reduction reaction of the reducing agent, the amount of hydrogen (reducing gas) brought into contact with the oxidized reducing agent is preferably 1 mmol to 50 mmol, more preferably 2.5 mmol to 35 mmol, and even more preferably 5 mmol to 20 mmol, per 1 g of reducing agent. The reducing agent of this embodiment has a high hydrogen utilization rate because oxygen elements can be smoothly introduced and removed. Therefore, the reducing agent of this embodiment is sufficiently reduced (regenerated) with a small amount of hydrogen. This reduces the energy required to generate hydrogen, and ultimately contributes to reducing carbon dioxide generated when obtaining energy. The hydrogen utilization rate (%) is a value expressed as a percentage of the amount of carbon monoxide produced (number of moles) relative to the amount of hydrogen input (number of moles) brought into contact with 1 g of reducing agent.

[0034] Furthermore, the reaction temperature (contact temperature of the reducing agent with carbon dioxide) in the carbon dioxide reduction reaction is preferably above 650°C, more preferably 700°C or higher, even more preferably 750°C or higher, and particularly preferably 800°C or higher. Within this temperature range, the carbon dioxide reduction reaction can proceed efficiently. The upper limit of this reaction temperature is preferably 1050°C or lower, more preferably 1000°C or lower, even more preferably 950°C or lower, particularly preferably 900°C or lower, and most preferably 850°C or lower. Since the reducing agent can efficiently reduce carbon dioxide to carbon monoxide even at low temperatures, the carbon dioxide reduction reaction can be set to a relatively low temperature. Furthermore, setting the upper limit of the reaction temperature within the above range not only facilitates waste heat utilization but also further improves economic efficiency. The lower limit and upper limit can be combined in any way to define the reaction temperature range.

[0035] Furthermore, during the carbon dioxide reduction reaction, the amount of carbon dioxide brought into contact with the reducing agent is preferably 1 mmol to 50 mmol, more preferably 2.5 mmol to 30 mmol, and even more preferably 5 mmol to 20 mmol, per 1 g of reducing agent. The reducing agent of this embodiment allows smooth transfer of oxygen elements. Therefore, the reducing agent of this embodiment has a high carbon dioxide conversion rate (and therefore produces a large amount of carbon monoxide), which also contributes to reducing carbon dioxide from this perspective. Meanwhile, since the reduction reaction is efficiently carried out using a reducing gas containing hydrogen, the reducing agent can be regenerated with a small amount of hydrogen. The amount of carbon monoxide produced by the reducing agent of this embodiment is preferably approximately 0.3 mmol to 1 mmol per 1 g of reducing agent.

[0036] In this embodiment, the reduction product (carbon valuable product) obtained by the carbon dioxide reduction reaction contains carbon monoxide. However, it may also contain substances other than carbon monoxide, or may be a mixture of carbon monoxide and other substances. Specific examples of other substances include methane. Preferably, the reduction products, such as carbon monoxide, obtained by the carbon dioxide reduction reaction are further converted into organic substances by microbial fermentation or the like. Examples of microbial fermentation include anaerobic fermentation. Examples of the resulting organic substances include methanol, ethanol, acetic acid, butanol, derivatives thereof, mixtures thereof, and C5 or higher compounds such as isoprene. Furthermore, reduction products such as carbon monoxide may be converted into C1 to C20 compounds, including hydrocarbons and alcohols conventionally synthesized by petrochemical methods, using metal oxides or the like. Specific examples of the resulting compounds include methane, ethane, propylene, methanol, ethanol, propanol, acetaldehyde, diethyl ether, acetic acid, butyric acid, diethyl carbonate, and butadiene.

[0037] [Characteristics of the Reducing Agent] The reducing agent of this embodiment preferably has the following characteristics. That is, when a stainless steel reaction tube having an inner diameter of 8 mm and a pressure gauge disposed in the flow path is filled with the reducing agent to a height of 40 cm and nitrogen gas having a concentration of 100% by volume is passed through at a rate of 30 mL / min, the pressure increase over 10 minutes is preferably 0.03 MPaG or less, and more preferably 0.01 MPaG or less. A reducing agent exhibiting such characteristics can be determined to have a packing density and pore volume that satisfy the above ranges, and can sufficiently increase the carbon dioxide conversion rate and the hydrogen conversion rate.

[0038] According to the above-described embodiment, it is possible to provide a reducing agent that can be stably used for a long period of time in a reaction at high temperatures, and a method for producing a gas using this reducing agent. Because the reducing agent of this embodiment can withstand use at high temperatures, it enables more efficient conversion of carbon dioxide to carbon monoxide (a carbon valuable) through a chemical looping reaction at high temperatures. Furthermore, the reducing agent may be provided in the following aspects.

[0039] (1) A reducing agent for reducing carbon dioxide to generate carbon valuables, the reducing agent comprising an oxygen carrier having oxygen ion conductivity and containing at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides, and the oxygen carrier has an oxygen ion conductivity of 1×10 in a pure oxygen atmosphere at a temperature of 700°C. -7 A reducing agent having an electrical conductivity of 10 S / cm or more, and when X-ray diffraction measurement is performed on the reducing agent in a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°.

[0040] (2) The reducing agent according to (1) above, further comprising an element belonging to Groups 6 to 14 of the periodic table, wherein the oxygen carrier has a σB / σA ratio of less than 85 at a temperature of 700°C, where σA [S / cm] is the electrical conductivity in a pure oxygen atmosphere and σB [S / cm] is the electrical conductivity in an argon gas atmosphere containing 1% by volume of carbon monoxide.

[0041] (3) The reducing agent according to (2) above, further comprising a sub-compound containing an element belonging to Groups 6 to 14 of the periodic table, wherein when the reducing agent is subjected to scanning transmission electron microscopy-energy dispersive X-ray spectroscopy (STEM-EDS) measurement, the oxygen carrier and the sub-compound are observed individually, and the sub-compound is in the form of particles and in contact with the oxygen carrier.

[0042] (4) The reducing agent according to (3) above, wherein, when X-ray diffraction measurement is performed on the reducing agent, the peaks attributable to the oxygen carrier and the peaks attributable to the minor compound observed in the X-ray diffraction profile are shifted by less than 0.3° in 2θ relative to the peaks observed in the X-ray diffraction profiles when X-ray diffraction measurement is performed on the oxygen carrier alone and the minor compound alone, respectively.

[0043] (5) The reducing agent according to (3) or (4) above, wherein the average particle size of the particles of the secondary compound is 1 nm or more and 10 μm or less.

[0044] (6) The reducing agent according to any one of (1) to (5) above, wherein the reaction with carbon dioxide is carried out at a temperature exceeding 650°C.

[0045] (7) The reducing agent according to any one of (1) to (6) above, wherein the reducing agent oxidized by the carbon dioxide is reduced by a reducing gas containing hydrogen.

[0046] (8) The reducing agent according to (7) above, wherein the reaction with the hydrogen-containing reducing gas is carried out at a temperature exceeding 650°C.

[0047] (9) A gas production method for producing a product gas containing carbon valuables by reducing a source gas containing carbon dioxide with a reducing agent, the reducing agent containing at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides, and an oxygen carrier having oxygen ion conductivity, the oxygen carrier having oxygen ion conductivity of 1×10 -7 A method for producing a gas in which the reducing agent has an electrical conductivity of 100 S / cm or more, and when X-ray diffraction measurement is performed on the reducing agent over a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°. Of course, this is not limited to this. For example, "containing a metal element" does not simply mean containing a single metal element, but may also mean two or more metal elements in an alloy state, or the metal element in a compound state. Here, "compound" includes various states such as oxides, nitrides, chlorides, sulfides, and salts including nitrates.

[0048] As described above, various embodiments of the present invention have been described, but these are presented as examples and do not limit the scope of the invention in any way. The novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. Such embodiments and their modifications are intended to be included within the scope and spirit of the invention, as well as within the scope of the inventions and their equivalents as set forth in the claims.

[0049] For example, the reducing agent and gas manufacturing method of the present invention may have any other additional components compared to the above-mentioned embodiments, may be replaced with any components that exhibit similar functions, or may omit some components. In the above-mentioned embodiments, a gas containing hydrogen has been described as a representative reducing gas, but the reducing gas may also use a gas containing at least one selected from hydrocarbons (e.g., methane, ethane, acetylene, etc.) and ammonia as a reducing substance instead of or in addition to hydrogen.

[0050] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. 1. Preparation of reducing agent materials The following compounds were prepared as reducing agent materials. (Oxygen carrier precursors) Cerium (III) nitrate hexahydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 98.0%) Zirconium nitrate dihydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 97.0%) Samarium nitrate hexahydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.5%) Copper (II) nitrate trihydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.0%) Iron (III) nitrate nonahydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%) Lanthanum (III) nitrate hexahydrate (Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%) (Minor compounds) Silicon carbide (High Purity Chemical Laboratory Co., Ltd., purity: 99.0%) Nickel (II) oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%)

[0051] 2. Preparation of Reducing Agent (Example 1) First, predetermined amounts of cerium (III) nitrate hexahydrate and zirconium nitrate dihydrate were weighed. Next, 6.06 g of citric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.5%) was weighed and dissolved in 96 mL of deionized water to obtain a citric acid aqueous solution. The precursor (metal nitrate salt) was then added to the citric acid aqueous solution at room temperature while stirring to prepare a precursor aqueous solution. The Ce:Zr (molar ratio) in the precursor aqueous solution was set to 0.9:0.1. After 30 minutes, 2.15 g of ethylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.5%) was added to the precursor aqueous solution, and the temperature was raised to 80°C.

[0052] The temperature was maintained at 80°C with continuous stirring until a viscous gel was formed. The gel was then transferred to a drying oven. The gel was dried at 120°C for 5 hours. The resulting swollen mass of organic and inorganic compounds was pulverized and heated from room temperature to 450°C at a rate of 8°C / min in an air atmosphere, followed by calcination at 450°C for 4 hours. The temperature was then further increased to 950°C at a rate of 8°C / min, followed by calcination at 950°C for 8 hours. Finally, the calcined mass was mechanically pulverized to obtain the target reducing agent composed solely of the oxygen carrier. The reducing agent was in granular form. For ease of loading into the reactor or to satisfy the pressure increase requirements described in the "Properties of the Reducing Agent" section, the reducing agent was optionally compressed into tablets for testing.

[0053] (Examples 2 to 6 and Comparative Examples 1 and 2) Reducing agents composed of an oxygen carrier alone or an oxygen carrier and a sub-compound were produced in the same manner as in Example 1, except that the type and amount of the oxygen carrier precursor used was changed and / or a sub-compound was added. The sub-compound was added in the form of particles to the precursor aqueous solution. The resulting reducing agents were granular.

[0054] 2. Measurement and Evaluation 2-1. X-ray Diffraction Measurements Prior to X-ray diffraction measurements, a reducing agent sample was prepared. First, approximately 100 mg of reducing agent was weighed into a mortar and ground using a pestle. The reducing agent was then uniformly filled into the sample-filling hole of the sample plate, and the surface of the sample plate and the surface of the reducing agent were adjusted to be flush with each other. X-ray diffraction measurements were performed using an X-ray diffractometer (PANanalytical, "Aeris") using the focusing method. A ceramic tube was used as the anticathode, and CuKα characteristic X-rays (Kα1 wavelength (λ) = 1.54056 Å (0.154056 nm), Kα2 wavelength (λ) = 1.54439 Å (0.154439 nm), Kα2 ratio = 0.50000) were used for diffraction. The diffractometer was set to a divergence slit of 1 / 2°, a divergence longitudinal limiting slit of 10 mm, a scattering slit of 2°, and a receiving slit of 0.15 mm. The goniometer radius was 145 mm.

[0055] The prepared reducing agent sample was then irradiated with X-rays under conditions of a tube voltage of 40 kV and a tube current of 15 mA. The measurement was performed with the goniometer scanning angle set to a range of 10° to 90.5°, a scanning speed of 3.5° / min, and a measurement step of 0.01. The measurement was performed in air at room temperature. After the measurement was completed, the data obtained without separation of Kα1 and Kα2 was analyzed. Software (High Score, manufactured by PANanalytical) was used for data analysis. If it is difficult to distinguish the baseline, correction may be performed using the software. The value with the highest intensity of the diffraction peak was defined as the apex, and the distance between the two points at half the intensity of the maximum peak value at this time was defined as the full width at half maximum.

[0056] 2-2. STEM-EDS Measurement The reducing agent was ultrasonically dispersed in ethanol, dropped onto a grid, and then dried. Afterwards, observation was performed with STEM and EDS analysis was carried out (mapping → line profiling). For the line profile, a line was drawn so that it intersected with the interface between the oxygen carrier and the sub-compound observed in the elemental mapping of the STEM-EDS measurement, and the count number of each element at a certain point on that line was plotted. - Manufacturer and model number of the STEM-EDS device used in this measurement STEM: Hitachi (HD-2700) STEM-EDS: EDAX (TEAM) - Parameters Acceleration voltage: 200 kV EDS mapping resolution: 256 x 200 Dwell: 200

[0057] 2-3. Particle size distribution measurement (wet type) Particle size distribution measurement was performed using a laser diffraction / scattering particle size distribution analyzer (Horiba, Ltd., "Partica LA-960") and a wet flow cell. The flow cell was made of synthetic quartz, and the light source was a semiconductor laser (650 nm) 5 mW and an LED (405 nm) 3 mW, and the detector was a ring-shaped silicon photodiode. The measurement was performed at a temperature of 25°C and a humidity of 20% on a dispersion prepared by dispersing approximately 10 mg of reducing agent in approximately 180 mL of purified water (pH 6.8 to 7.2). The measurement was performed at least three times, and the median particle diameters obtained by each particle size distribution measurement were arithmetically averaged to obtain the average particle diameter.

[0058] 2-4. Measurement of electrical conductivity of oxygen carrier Samples were prepared before measuring electrical conductivity. The oxygen carrier was fired at 1300°C to produce a sintered body, which was then cut into a rectangular parallelepiped and connected to platinum electrodes with Pt paste. Electrical conductivity was measured using an A&D 7461P Digimol and a Hokuto Denko Galvanostat HA101, and DC four-terminal conductivity was measured. The measurement temperature was 700°C, and the sample was placed in a pure oxygen atmosphere (O 2The measurements were performed under a high-purity (99.9% by volume) oxygen atmosphere and a carbon monoxide-containing atmosphere (argon gas atmosphere containing 1% by volume of carbon monoxide). The electrical conductivity measured in the pure oxygen atmosphere was designated "σA," and the electrical conductivity measured in the carbon monoxide-containing atmosphere was designated "σB." Data were analyzed using software (Microsoft's "Excel") . For reducing agents that did not contain a secondary compound, a reducing agent consisting only of an oxygen carrier was used as is for electrical conductivity measurement. For reducing agents that contained a secondary compound, an oxygen carrier was separately produced in the same manner as above, without adding the secondary compound to the precursor aqueous solution, and this oxygen carrier was used for electrical conductivity measurement.

[0059] 2-5. Measurement of Carbon Dioxide Conversion Rate and Hydrogen Conversion Rate Measurement Using a rapid catalyst evaluation system equipped with a fixed-bed flow reactor and a quadrupole mass spectrometer directly connected to the reactor, the amount of carbon monoxide produced by the reducing agent was measured according to the following procedure. Specifically, a quartz reaction tube with an inner diameter of 6 mm was prepared and filled with a powdered reducing agent so that the filling amount was 500.0 mg.

[0060] Next, while flowing helium gas at a flow rate of 5 mL / min, the temperature was increased to 850°C at a rate of 15°C / min, and the mixture was heated at the same temperature for 5 minutes to stabilize the temperature. Next, to activate the reducing agent, hydrogen gas (reducing gas) was flowed at a flow rate of 5 mL / min for 20 minutes to carry out a reduction reaction of the reducing agent (first process), thereby reducing the reducing agent. At this time, the gas discharged from the outlet contained water vapor. Thereafter, for gas exchange, helium gas was flowed at a flow rate of 5 mL / min for 10 minutes, and then carbon dioxide gas was flowed at a flow rate of 5 mL / min for 20 minutes to carry out a reduction reaction of carbon dioxide (second process), thereby reducing the carbon dioxide gas (raw material gas). At this time, the product gas discharged from the outlet contained carbon monoxide.

[0061] Next, for this test, the following process was performed. First, for gas exchange, helium gas was flowed at a flow rate of 5 mL / min for 10 minutes. Next, hydrogen gas (reducing gas) was flowed at a flow rate of 5 mL / min for 7 minutes to carry out a reduction reaction of the reducing agent (first process), thereby reducing the reducing agent. At this time, the gas discharged from the outlet contained water vapor.

[0062] Thereafter, for gas exchange, helium gas was flowed at a flow rate of 5 mL / min for 5 minutes, and then carbon dioxide gas was flowed at a flow rate of 5 mL / min for 7 minutes to carry out a carbon dioxide reduction reaction (second process) to reduce the carbon dioxide gas (raw material gas). At this time, the product gas discharged from the outlet contained carbon monoxide. In the above process, the temperature of the reducing agent was maintained at 850°C and the process was carried out under atmospheric pressure conditions when any of the gases was flowed.

[0063] The conversion rate was calculated from the time when the amount of carbon monoxide produced per unit second after starting to flow carbon dioxide gas (feed gas) reached 0 mmol or more until the value of the following formula calculated based on the signal detected by the quadrupole mass spectrometer fell below 80. The average value of the values ​​calculated during this period was defined as the carbon dioxide conversion rate. Note that the region where the amount of carbon monoxide produced was 0 mmol or less was not used in calculating the conversion rate. Carbon dioxide conversion rate [%] = (amount of carbon monoxide detected per unit second) ÷ (amount of carbon monoxide detected per unit second + amount of carbon dioxide detected per unit second) × 100 Hydrogen conversion rate [%] = (amount of carbon monoxide detected [mmol] in the range where the carbon dioxide conversion rate is 80% or more) ÷ (hydrogen flow rate [mL / min] × hydrogen flow time [min] ÷ volume of 1 mol of gas under standard conditions [mL / mmol]) × 100

[0064] 2-6. Measurement of Relative Carbon Dioxide Conversion Amount Using a catalyst evaluation system equipped with a fixed-bed flow reactor and an NDIR (GMS810 manufactured by SICK) directly connected to the reactor, the amount of carbon monoxide produced by the reducing agent was measured according to the following procedure. Specifically, a quartz reaction tube with an inner diameter of 7 mm was prepared and filled with a cylindrical reducing agent molded to a major axis of 3 mm so that the filling amount was 9 g to 16 g (filling height: 12 cm to 15 cm). Next, while flowing nitrogen gas at a flow rate of 100 mL / min, the temperature was increased to 850 °C at a heating rate of 15 °C / min, and the temperature was then stabilized for 5 minutes.

[0065] 2-6-1. Life cycle Next, for this test, the following process was carried out. First, in order to activate the reducing agent, hydrogen gas (reducing gas) was flowed at a flow rate of 100 mL / min for 4 minutes to carry out a reduction reaction of the reducing agent (first process), thereby reducing the reducing agent. At this time, the gas discharged from the outlet contained water vapor. Then, carbon dioxide gas was flowed at a flow rate of 100 mL / min for 4 minutes to carry out a reduction reaction of carbon dioxide (second process), thereby reducing the carbon dioxide gas (raw material gas). At this time, the product gas discharged from the outlet contained carbon monoxide. In addition, in the above processes, the temperature of the reducing agent was maintained at 850°C when flowing any of the gases, and the processes were carried out under atmospheric pressure conditions.

[0066] The above process was counted as one cycle, and the amount of carbon monoxide produced for every 1000 cycles was calculated according to the method described in the next section "2-6-2. Measurement cycle."

[0067] 2-6-2. Measurement Cycle First, hydrogen gas (reducing gas) was flowed at a flow rate of 100 mL / min for 4 minutes to carry out a reduction reaction of the reducing agent (first process), thereby reducing the reducing agent. At this time, the gas discharged from the outlet contained water vapor. Subsequently, for gas exchange, nitrogen gas was flowed at a flow rate of 100 mL / min for 5 minutes, and then carbon dioxide gas was flowed at a flow rate of 100 mL / min for 4 minutes to carry out a reduction reaction of carbon dioxide (second process), thereby reducing the carbon dioxide gas (raw material gas). At this time, the product gas discharged from the outlet contained carbon monoxide. Note that in all of the above processes, the temperature of the reducing agent was maintained at 850°C and the processes were carried out under atmospheric pressure conditions when flowing any of the gases.

[0068] Measurement of the amount of carbon monoxide produced in each cycle began when the carbon monoxide concentration detected by NDIR (non-dispersive infrared) reached 2.0% or higher after carbon dioxide gas (feed gas) began to flow. The carbon monoxide concentration detected by NDIR was recorded every 5.0 seconds, and the amount of carbon monoxide produced was calculated by the quadrature by division method from the carbon monoxide concentrations recorded during this period. Note that regions where the carbon monoxide concentration was less than 2.0% were not used in calculating the amount of carbon monoxide produced. The relative value of the carbon dioxide conversion amount was calculated based on the following formula: Relative value of carbon dioxide conversion amount = (amount of carbon monoxide produced in each cycle) ÷ (amount of carbon monoxide produced in the first cycle) × 100

[0069] The results are shown in the following Table 1. In the evaluation column, ⊚ indicates the most preferable, ◯ indicates the preferable, and × indicates the unpreferable.

[0070] The full width at half maximum of all peaks observed in the X-ray diffraction profiles of the reducing agents obtained in each Example is less than 1.5°. In contrast, the full width at half maximum of at least one peak observed in the X-ray diffraction profiles of the reducing agents obtained in each Comparative Example is 1.5° or greater. The X-ray diffraction profiles of the reducing agents obtained in Examples 2, 4, 5, and 6 and Comparative Example 2 are shown in Figures 4 to 8, respectively. Furthermore, the peaks derived from the oxygen carrier and the peaks derived from the minor compounds observed in the X-ray diffraction profiles of the reducing agents obtained in each Example are shifted by less than 0.3° in 2θ relative to the peaks observed in the X-ray diffraction profiles of the oxygen carrier alone and the minor compounds alone, respectively. Furthermore, when STEM-EDS measurements are performed on the reducing agents obtained in Examples 4 and 6, images similar to the image shown in Figure 1 are obtained.

Claims

1. A reducing agent for reducing carbon dioxide to generate carbon values, comprising an oxygen carrier having oxygen ion conductivity containing at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides, and the oxygen carrier has an oxygen ion conductivity of 1×10 in a pure oxygen atmosphere at a temperature of 700° C. -7 The reducing agent has an electrical conductivity of 10 S / cm or more, and when X-ray diffraction measurement is performed on the reducing agent in a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°.

2. The reducing agent according to claim 1, further comprising an element belonging to Groups 6 to 14 of the periodic table, wherein the oxygen carrier has an electrical conductivity of σB / σA of less than 85 at a temperature of 700°C, where σA [S / cm] is electrical conductivity in a pure oxygen atmosphere and σB [S / cm] is electrical conductivity in an argon gas atmosphere containing 1% by volume of carbon monoxide.

3. The reducing agent according to claim 2, further comprising an auxiliary compound containing an element belonging to Groups 6 to 14 of the periodic table, wherein when the reducing agent is subjected to a scanning transmission electron microscope-energy dispersive X-ray spectroscopy (STEM-EDS) measurement, the oxygen carrier and the auxiliary compound are observed separately, and the auxiliary compound is in contact with the oxygen carrier in the form of particles.

4. The reducing agent according to claim 3, wherein, when X-ray diffraction measurement is performed on the reducing agent, a peak derived from the oxygen carrier and a peak derived from the minor compound observed in the X-ray diffraction profile are shifted by less than 0.3° in 2θ relative to the peaks observed in the X-ray diffraction profiles when X-ray diffraction measurement is performed on the oxygen carrier alone and the minor compound alone, respectively.

5. The reducing agent according to claim 3 or 4, wherein the average particle size of the particles of the secondary compound is 1 nm or more and 10 μm or less.

6. The reducing agent according to any one of claims 1 to 5, wherein the reaction with carbon dioxide is carried out at a temperature above 650°C.

7. The reducing agent according to any one of claims 1 to 6, wherein the reducing agent oxidized by the carbon dioxide is reduced by a reducing gas containing hydrogen.

8. The reducing agent according to claim 7, wherein the reaction with the reducing gas containing hydrogen is carried out at a temperature above 650°C.

9. A gas production method for producing a product gas containing carbon valuables by reducing a raw material gas containing carbon dioxide with a reducing agent, the reducing agent containing at least two metal elements belonging to Group 3 or Group 4 of the periodic table, including lanthanides and actinides, and an oxygen carrier having oxygen ion conductivity, the oxygen carrier having an oxygen ion conductivity of 1×10 -7 and when X-ray diffraction measurement is performed on the reducing agent in a measurement range of 10° to 90.5°, the full width at half maximum of all peaks observed in the X-ray diffraction profile is less than 1.5°.

Citation Information

Patent Citations

  • Facile co2 sequestration and fuel production from a hydrocarbon

    US20210284540A1

  • Method for producing carbon monoxide and production apparatus

    WO2012057162A1

  • Reducing agent, and method for producing gas

    WO2021192871A1

  • Reducing agent, and gas production method

    WO2021192872A1

  • Reducing agent, and gas production method

    WO2023167287A1