Plating device for insoluble anodes
The plating apparatus addresses the challenge of maintaining copper concentration and reducing additive consumption by using a diaphragm and copper oxide powder supply system, ensuring continuous and uniform copper plating on high-aspect-ratio features.
Patent Information
- Application Number
- PCT/JP2024/011624
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Current plating equipment using insoluble anodes faces challenges in maintaining uniform copper plating on fine vias and trenches with high aspect ratios due to fluctuations in copper concentration and additive consumption, particularly when using a copper sulfate solution, leading to difficulties in achieving continuous and good copper plating processes.
The plating apparatus incorporates a diaphragm with a through hole and an inclined liquid supply pipe, along with a copper oxide powder supply system that maintains copper concentration through static electricity removal and controlled addition of copper oxide powder, ensuring stable copper plating solutions and minimizing additive consumption.
This setup allows for continuous and uniform copper plating on fine vias and trenches by maintaining copper concentration within a predetermined range, reducing additive consumption and preventing solution mixing, thereby enhancing the plating process efficiency.
Smart Images

Figure JP2024011624_03102024_PF_FP_ABST
Abstract
Description
Insoluble anode plating equipment
[0001] The present invention relates to a plating apparatus for an insoluble anode.
[0002] Conventionally, various plating processes have been performed on substrates such as semiconductor wafers, printed wiring boards, etc. When performing plating processes on such substrates, a so-called jet-type plating apparatus is known.
[0003] This jet-type plating apparatus generally comprises an opening on which the object to be plated can be placed, a liquid supply pipe that supplies plating solution toward the object to be plated, and an anode positioned opposite the object to be plated, and plating is performed while supplying plating solution from the liquid supply pipe toward the object to be plated. Jet-type plating apparatuses can perform uniform plating on the surface of the object to be plated, and can sequentially replace the objects to be plated placed in the opening for plating, so they are widely used as suitable for small-lot production and automated plating.
[0004] Although this jet-type plating apparatus has the advantages described above, when a soluble anode is used, a film formed on the anode surface, such as a black film, may peel off and become an impurity in the plating solution. This may then flow along with the plating solution being supplied to the object to be plated, adversely affecting the plating process.
[0005] Furthermore, air mixed in the solution or bubbles generated from the anode may reach the surface to be plated and hinder a good plating process. For this reason, a method is known in which a diaphragm is placed in the plating tank to separate the object to be plated from the anode in this jet-type plating apparatus (see Patent Documents 1 and 2).
[0006] The use of insoluble anodes in jet-type plating equipment equipped with a diaphragm offers various advantages over the use of soluble anodes, such as reduced consumption of additives in the plating solution and improved productivity by eliminating the need for maintenance such as anode replacement, which is required with soluble anodes.
[0007] However, although jet-type plating equipment using insoluble anodes offers various advantages over soluble anodes, their use within the plating industry has not progressed much except for precious metal plating and copper plating.
[0008] When a diaphragm is placed in a plating tank of a jet-type plating apparatus, an upper isolation chamber is formed above the diaphragm by the diaphragm and the object to be plated placed in the opening, and a lower isolation chamber is formed below the diaphragm by the plating tank and the diaphragm. Because the insoluble anode is placed in the lower isolation chamber, a large amount of bubbles appear below the diaphragm during plating due to gas generation caused by electrolysis of water. Therefore, it is necessary to efficiently remove the bubbles that appear below the diaphragm. To obtain the benefits of using an insoluble anode, different types of solutions may be supplied separately to the upper and lower isolation chambers. However, the diaphragm placed in the plating tank must prevent the different types of solutions supplied to the upper and lower isolation chambers from mixing.
[0009] In the prior art of Patent Document 1, when supplying a solution to the upper isolation chamber, a large pressure loss occurs during supply, making it difficult to increase the supply flow rate to the lower isolation chamber, and it tends to be difficult to sufficiently discharge the large amount of bubbles generated from the insoluble anode. Also, in Patent Document 2, although bubbles can be efficiently discharged in the lower isolation chamber, it is not possible to separate the solutions supplied to the upper and lower isolation chambers, and therefore the benefits of the insoluble anode cannot be fully realized.
[0010] In order to solve the problems of such jet-type insoluble anode plating apparatuses in which a diaphragm is disposed in a plating tank, the prior art described in Patent Document 3 (WO 2022 / 107551) has been proposed. In Patent Document 3, the solutions supplied to the upper and lower isolation chambers do not mix with each other, and bubbles generated from the insoluble anode in the lower isolation chamber can be efficiently discharged, thereby fully realizing the benefits of the insoluble anode.
[0011] In plating apparatuses using insoluble anodes, for example, when performing copper plating, it is necessary to adjust the copper concentration in the plating solution consumed during the plating process. One method for adjusting the copper concentration is proposed using copper oxide powder (Patent Document 4). This prior art proposes that copper oxide powder with a specified content of impurities such as sodium is used and periodically added to the plating solution to control the copper concentration in the plating solution within a predetermined range, thereby enabling good copper plating of semiconductor substrates such as wafers.
[0012] Japanese Patent Application Laid-Open No. 2000-273693 Japanese Patent Application Laid-Open No. 2007-169773 International Publication No. WO2022 / 107551 Japanese Patent Application Laid-Open No. 2018-62453
[0013] As described above, plating apparatuses using insoluble anodes offer various advantages over those using soluble anodes, and various plating processing techniques that can fully utilize these advantages have been proposed. However, further technological development is required for plating apparatuses using insoluble anodes.
[0014] Copper plating is used to fill small vias in semiconductor wafers and other substrates. Recently, electronic substrates and other devices have become increasingly lighter, thinner, and smaller. This has led to remarkable miniaturization of vias, creating a demand for plating equipment capable of uniformly and effectively plating fine vias with high aspect ratios, such as vias with a diameter of 5 μm and a depth of 100 μm. When performing such fine copper plating using an insoluble anode plating system, controlling the concentration of copper and additives in the plating solution is extremely important. Specifically, when copper plating semiconductor wafers using a copper sulfate solution, additives known as accelerators, suppressors, and levelers (commercially available products) are added to the plating solution. These additives tend to be consumed during the plating process, and this consumption also occurs in insoluble anode plating systems equipped with a diaphragm. In an insoluble anode plating apparatus equipped with a diaphragm, a copper sulfate solution is supplied as a cathode plating solution to the upper isolated chamber formed by the diaphragm. As copper plating continues, the copper concentration in the cathode plating solution decreases. In a copper sulfate solution with a decreased copper concentration, sulfate ions (SO 4 2- ) increases. In a copper sulfate solution with a relatively elevated sulfate ion concentration, additives in the solution tend to be consumed more rapidly, making it difficult to perform uniform and satisfactory copper plating. In particular, when copper plating is performed on fine vias or trenches with high aspect ratios, the copper plating thickness is extremely thin. Therefore, in order to perform uniform and continuous copper plating of thin thicknesses, it is necessary to minimize fluctuations in the copper concentration in the plating solution and consumption of additives. In other words, there is a demand for a plating apparatus for an insoluble anode that enables continuous copper plating while minimizing fluctuations in the copper concentration of the copper sulfate solution used as the plating solution.
[0015] The present invention has been made in light of the above-mentioned circumstances, and has an object to provide an insoluble anode plating apparatus equipped with a diaphragm, which, when copper plating is performed on a substrate such as a semiconductor wafer using an insoluble anode plating apparatus, minimizes fluctuations in the copper concentration in the cathode plating solution, suppresses consumption of additives contained in the cathode plating solution, and enables continuous, satisfactory, uniform copper plating of fine vias and trenches with high aspect ratios.
[0016] In order to solve the above problems, the present invention provides a plating tank having an opening for placing an object to be plated, a liquid supply pipe for supplying plating solution toward the object to be plated, an insoluble anode arranged so as to face the object to be plated, and a diaphragm for separating the object to be plated and the insoluble anode, wherein the diaphragm has an outer peripheral edge fixed to the inner wall of the plating tank and a peripheral edge of a through hole provided in the center of the diaphragm is fixed to the liquid supply pipe, so that an inclination rising from the liquid supply pipe toward the outer periphery is given, and the liquid supply pipe is connected to an upper isolation chamber in the plating tank formed by the diaphragm and the placed object to be plated, and a control tank storing a cathode plating solution is connected to the liquid supply pipe. The insoluble anode plating apparatus supplies a cathode plating solution to a lower isolation chamber formed below a diaphragm, and supplies the anode solution from an anode solution tank storing the anode solution therein. The insoluble anode plating apparatus is characterized in that it includes copper oxide powder supply means for supplying copper oxide powder together with a carrier gas to a control tank via a supply tube having static electricity removal capabilities, and the upper cover of the control tank is provided with a powder supply cylinder having static electricity removal capabilities, the tip of which is positioned near the liquid surface of the cathode plating solution stored in the control tank, and the supply tube is connected to the powder supply cylinder.
[0017] According to the present invention, by supplying copper oxide powder to the cathode plating solution in an amount equivalent to the amount of copper used in the plating process, it is possible to continuously maintain the copper concentration within a set range, thereby reliably suppressing additive consumption due to fluctuations in copper concentration caused by the plating process. As a result, it is possible to continuously perform satisfactory and uniform copper plating even on fine vias and fine trenches with high aspect ratios. In the present invention, the copper oxide powder is supplied to the cathode plating solution from a powder supply cylinder with static electricity removal capabilities, the tip of which is positioned near the liquid surface of the cathode plating solution stored in the control tank, in order to ensure that powdered copper oxide is introduced into the cathode plating solution. If the tip of the powder supply cylinder is separated from the liquid surface of the cathode plating solution stored in the control tank, a large amount of copper oxide powder supplied from the powder supply cylinder will scatter into the space above the liquid surface of the cathode plating solution, making it difficult to adjust the copper concentration. Furthermore, if the tip of the powder supply cylinder comes into contact with the liquid surface, the copper oxide powder will aggregate and adhere to the tip, making it difficult to supply the copper oxide powder. Therefore, in the present invention, the tip of the powder supply cylinder is positioned near the liquid surface of the cathode plating solution stored in the control tank. Near refers to a distance where the tip does not come into contact with the liquid surface and where the copper oxide powder supplied from the tip does not scatter into the space above the liquid surface of the cathode plating solution. The distance between the tip of the powder supply cylinder and the liquid surface of the cathode plating solution can be adjusted appropriately depending on the physical properties of the copper oxide powder used, such as the average particle shape, but is preferably 50 to 100 mm.
[0018] The present invention also provides a plating tank having an opening for placing an object to be plated, a liquid supply pipe for supplying a plating solution toward the object to be plated, an insoluble anode arranged to face the object to be plated, and a diaphragm for separating the object to be plated and the insoluble anode, wherein the diaphragm has an outer peripheral edge fixed to an inner wall of the plating tank and a peripheral edge of a through-hole provided in the center of the diaphragm fixed to the liquid supply pipe, so that an upward slope is provided from the liquid supply pipe toward the outer periphery, and a cathode plating solution is supplied from a control tank storing a cathode plating solution through the liquid supply pipe to an upper isolated chamber in the plating tank formed by the diaphragm and the placed object to be plated, The insoluble anode plating apparatus is configured to supply an anode solution from an anode solution tank storing the anode solution to a lower isolated chamber within a plating tank formed below a diaphragm, the insoluble anode plating apparatus comprising: a copper concentration adjustment tank for adjusting the copper concentration of the cathode plating solution; the copper concentration adjustment tank has a copper oxide powder supply device that transports copper oxide powder together with a carrier gas through a supply tube having static electricity removal capabilities; an upper lid of the copper concentration adjustment tank is provided with a powder supply cylinder having static electricity removal capabilities, with its tip positioned near the surface of the cathode plating solution stored in the copper concentration adjustment tank; the copper concentration adjustment tank is provided with stirring means for stirring the cathode plating solution, and the supply tube is connected to the powder supply cylinder; the copper oxide powder is supplied to the copper concentration adjustment tank to adjust the copper concentration of the cathode plating solution in the copper concentration adjustment tank; and the cathode plating solution with the adjusted copper concentration is supplied from the copper concentration adjustment tank to a control tank.
[0019] The insoluble anode plating apparatus of the present invention is suitable for copper plating of semiconductor wafers and other substrates, but because the manufacture of semiconductor wafers and other substrates is carried out in a so-called clean room, it is conceivable that substances that are prone to scattering, such as copper oxide powder, would contaminate the clean room. Therefore, by locating a copper concentration adjustment tank outside the clean room, adjusting the copper concentration in the copper concentration adjustment tank using copper oxide powder, and supplying the adjusted cathode plating solution to the control tank, contamination inside the clean room can be reliably prevented.
[0020] In the present invention, the copper oxide powder has an average particle size of 25 to 40 μm and a compacted bulk density of 1.7 g / cm 3 Preferably, the compacted bulk density is less than 1.7 g / cm 3 If the concentration is more than this, the dissolution of the copper oxide powder into the cathode plating solution tends to be slow. 3 or more and less than 1.7 g / cm3. The packed bulk density refers to the bulk density measured after gently filling a specified container with copper oxide powder, applying a constant vibration to the container to fill the gaps between the powder particles, and then refilling the container. The packed bulk density in the present invention is a value measured using a measuring cylinder. Furthermore, the copper oxide powder in the present invention preferably has a relatively small angle of repose (10° to 12.5°). This angle of repose is obtained by dropping 100 mL of copper oxide powder, the packed bulk density of which has been measured using a measuring cylinder, from a height of 15 cm to create a mountain-shaped mass of copper oxide powder and measuring the angle of the base of the mountain-shaped mass. Copper oxide powder with a large angle of repose tends to have a slower dissolution rate. This angle of repose is an indicator of the fluidity of the copper oxide powder, and copper oxide powder with an angle of repose of 10° to 12.5° has high solubility. The gaps between powder particles are generated due to geometrical factors of the particle shape and surface characteristics such as adhesive force. According to the findings of the present inventors, the bulk density of copper oxide powder is 1.6 g / cm 3 It has been found that when the copper oxide powder has a particle shape of about 10° to 12.5°, dissolution of the copper oxide powder proceeds rapidly in the cathode plating solution. Furthermore, it has also been found that when the copper oxide powder has a granular particle shape, dissolution of the copper oxide powder proceeds rapidly. This is thought to be related to the relatively small angle of repose of the copper oxide powder (10° to 12.5°).
[0021] The powder supply cylinder in the present invention has static electricity removal properties, and is preferably made of a grounded titanium material or a powder supply cylinder connected to an ionizer. If static electricity occurs in the powder supply cylinder, the copper oxide powder is likely to agglomerate, making it difficult to steadily supply the copper oxide powder.
[0022] In the present invention, nitrogen gas or argon gas is preferably used as a carrier gas suitable for supplying copper oxide powder from a copper oxide powder supplying device through a supply tube having static electricity removal properties. The use of nitrogen gas or argon gas suppresses aggregation of the copper oxide powder, thereby reducing adhesion of the copper oxide powder to the supply tube and reliably preventing clogging.
[0023] In the plating apparatus for insoluble anodes according to the present invention, it is preferable to provide a switching means in the supply tube that can switch between supplying a carrier gas and copper oxide powder and supplying only carrier gas. When stopping the supply of copper oxide powder, supplying only carrier gas to the supply tube prevents aggregation of the copper oxide powder in the supply tube and reliably prevents adhesion or clogging of the copper oxide powder.
[0024] In the plating apparatus for insoluble anodes according to the present invention, it is preferable to provide a powder flow meter in the supply tube for monitoring the supply status of the copper oxide powder, and to provide a powder supply control means for adjusting the supply rate of the copper oxide powder and controlling the stop of supply. By monitoring the supply status with the powder flow meter, it is possible to fine-tune the supply rate of the copper oxide powder and appropriately stop the supply of the copper oxide powder in the event of an abnormality. Furthermore, as a means for confirming that the copper concentration in the copper plating solution has been reliably adjusted, it is preferable to install copper concentration meters in the piping before and after the copper concentration adjustment tank to monitor whether the copper used in the plating process has been accurately replenished.
[0025] In the insoluble anode plating apparatus according to the present invention, in order to prevent the separate solutions supplied to the lower isolation chamber and the upper isolation chamber from directly mixing with each other, it is preferable to attach a silicon ring to the outer peripheral edge of the diaphragm and to the periphery of the through-hole in the diaphragm. When attaching the silicon ring to the diaphragm, it is preferable to use a method called simultaneous casting of the silicon ring. Simultaneous casting of the silicon ring involves fixing the diaphragm to a mold that has a central through-hole and that allows the outer peripheral edge of the diaphragm and the periphery of the through-hole to be pressed from above and below. An adhesive (primer) is applied to the outer peripheral edge and the periphery of the hole where the silicon ring will be attached. Silicon is then injected into the adhesive-applied area, and the mold is then pressed. After the silicon hardens, the mold is removed, leaving the silicon ring attached to the outer peripheral edge of the diaphragm and the periphery of the through-hole in the diaphragm. A diaphragm having such a silicone ring fixed thereto can reliably prevent leakage of the solution from the outer peripheral edge of the diaphragm that is fixed to the inner wall of the plating tank and from the peripheral edge of the through-hole in the center of the diaphragm that is fixed to the solution supply pipe. There are no particular restrictions on the material of the diaphragm that can be used, and it may be selected taking into consideration liquid permeability and plating solution resistance. However, it is preferable to use a diaphragm whose diaphragm base material is polyethylene terephthalate resin and whose diaphragm material is a polyvinylidene fluoride resin-based material. In addition, the water permeability should be 0.1 mL / min / cm. 2 It is preferable that:
[0026] Although the insoluble anode plating apparatus of the present invention is intended for copper plating, it can also be used for any plating process in which the plating metal or plating solution components can be supplied as powder. For example, in non-cyanide gold plating containing gold sulfite, the insoluble anode plating apparatus of the present invention can be used to supply sulfite powder to replenish the sulfite consumed during the plating process. The insoluble anode plating apparatus of the present invention can also be used in electrolytic nickel plating using an insoluble anode.
[0027] According to the present invention, in an insoluble anode plating apparatus equipped with a diaphragm, the copper concentration of the cathode plating solution can be continuously maintained within a predetermined range, thereby suppressing consumption of additives contained in the cathode plating solution and enabling continuous, satisfactory, uniform copper plating of fine vias and fine trenches with high aspect ratios.
[0028] Schematic cross-sectional view of an insoluble anode plating apparatus according to the present embodiment. Schematic cross-sectional view of a plating tank of an insoluble anode plating apparatus according to the present embodiment. Schematic cross-sectional view of an insoluble anode plating apparatus equipped with a copper concentration adjustment tank according to the present embodiment. SEM observation photograph of copper oxide powder A. SEM observation photograph of copper oxide powder B. Cross-sectional observation photograph of a via that has been embedded with copper plating.
[0029] An embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a schematic cross-sectional view of an insoluble anode plating apparatus according to this embodiment, and Fig. 2 is a schematic cross-sectional view of a plating tank.
[0030] The insoluble anode plating apparatus in Figure 1 is composed of a plating tank 1, a control tank 2, and an anode solution tank 3. A copper oxide powder feeder 4 is disposed near the control tank 3.
[0031] First, the plating tank 1 shown in Fig. 1 will be described with reference to Fig. 2. A donut-shaped diaphragm 11 having a through-hole in the center is installed in the plating tank 1. The outer peripheral edge of the diaphragm 11 is fixed to the inner wall 12 of the plating tank, and the peripheral edge of the through-hole is fixed to the tip of a solution supply pipe 13, so that the diaphragm 11 is inclined upward from the solution supply pipe 13 toward the periphery. An annular flow path 14 is provided on the outer periphery of the solution supply pipe 13. A mesh-like insoluble anode 15 is disposed at the bottom of the plating tank 1.
[0032] When a wafer W to be plated is placed in the opening of plating tank 1, an upper isolated chamber U and a lower isolated chamber D are formed in plating tank 1. A cathode plating solution is supplied to upper isolated chamber U through solution supply pipe 13. An anode solution from an anode solution tank 3 is supplied to lower isolated chamber D through an annular flow path 14.
[0033] The cathode plating solution stored in the management tank 2 is supplied from the solution supply pipe 13 to the upper isolated chamber U in the plating tank 1, and is discharged from the outer peripheral edge side of the diaphragm 11 to return to the management tank 2. A copper oxide powder supplyer 4 disposed near the management tank 1 supplies copper oxide powder from a powder storage chamber 41 together with a carrier gas G through a supply tube 42 into the management tank 1 from a powder supply cylinder 43 attached to the upper lid 21 of the management tank 1. The tip of the powder supply cylinder 43 is disposed near the liquid surface of the cathode plating solution.
[0034] The supply tube 42 of the copper oxide powder supply device 4 is equipped with a switching device 44 that can switch between supplying a carrier gas and copper oxide powder and supplying only carrier gas, and a powder supply control device 45 that has a powder flow meter that monitors the supply state of the copper oxide powder and controls the adjustment of the supply amount of copper oxide powder and the stop of supply.
[0035] Although not shown, the control tank 2 is equipped with a magnetic stirrer function as a liquid stirring means, and when copper oxide powder is supplied to the control tank 2, the liquid is stirred to quickly dissolve the copper oxide powder. Also, although not shown, the control tank 2 is equipped with a copper concentration meter so that the copper concentration of the cathode plating solution can be measured at all times. If the copper concentration of the cathode plating solution falls outside the set range due to plating processing, the copper concentration meter signals to operate the copper oxide powder supplyer 4, which is controlled to supply the required amount of copper oxide powder to the control tank 2.
[0036] Figure 3 shows an insoluble anode plating apparatus equipped with a copper concentration adjustment tank. The copper concentration adjustment tank 5 is configured to send the cathode plating solution, the copper concentration of which has been adjusted, to the control tank 2 and to recover the cathode plating solution from the control tank 2. A copper oxide powder supplier 4 is located near the copper concentration adjustment tank 5. The right side of the thick dashed line in Figure 3 is inside the clean room, and the left side of the thick dashed line is outside the clean room. Because the copper concentration adjustment tank 5 and the copper oxide powder supplier 4 are located outside the clean room, it is possible to reliably prevent contamination of the clean room with copper oxide powder.
[0037] Although not shown, the copper concentration adjustment tank 5 in Fig. 3 is equipped with a magnetic stirrer function as a liquid stirring means, so that when copper oxide powder is supplied to the copper concentration adjustment tank 5, the liquid is stirred to quickly dissolve the copper oxide powder. Although not shown, the copper concentration adjustment tank 5 is also equipped with a copper concentration meter so that the copper concentration of the cathode plating solution can be constantly measured. When the copper concentration of the cathode plating solution stored in the control tank 2 falls outside the set range and decreases, the copper oxide powder supply unit 4 is activated by a signal from the copper concentration meter attached to the control tank 2, and is controlled to supply the required amount of copper oxide powder to the copper concentration adjustment tank 5. The plating tank 1, anode solution tank 2, and copper oxide powder supply unit 4 in Fig. 3 are the same as those described in Fig. 1.
[0038] <Solubility of Copper Oxide Powder> Next, the results of examining the solubility of the copper oxide powder of the present invention will be described. The following three types of copper oxide powder were used for evaluation. Copper oxide powder A: average particle size 30 μm (FCO-M6, manufactured by Furukawa Chemicals Co., Ltd.) Copper oxide powder B: average particle size 3.7 μm (FCO-500, manufactured by Furukawa Chemicals Co., Ltd.) Copper oxide powder C: average particle size 1 μm (YS-808, manufactured by Kunshan Tokuken New Materials Technology Co., Ltd.)
[0039] The dissolution rate, compacted bulk density, and angle of repose were measured for each copper oxide powder. The test conditions were as follows: Dissolution rate: A copper sulfate solution (MF-Cu525, manufactured by EEJA Corporation) was used as the plating solution. A predetermined amount of copper oxide powder was added to a beaker containing 1 L of plating solution (liquid temperature: 22°C). The time required for the black copper sulfate solution to return to its original color due to complete dissolution of the copper oxide powder was measured, and the copper concentration of the plating solution after a predetermined time had elapsed was then measured. The amount of dissolution was measured from the copper concentration before and after the addition of the copper oxide powder, and the dissolution rate of the copper oxide powder was measured from the time required for complete dissolution. Compacted bulk density: A small amount of copper oxide powder was added to a 200 mL measuring cylinder, and the powder was compacted by hitting the bottom of the measuring cylinder against a table three times. This compaction process was repeated, and copper oxide powder was added until the volume reached 100 mL. The weight of the added copper oxide powder was measured, and the compacted bulk density was measured. Angle of repose: Copper oxide powder (100 mL) filled in the 200 mL measuring cylinder in which the packed bulk density was measured as described above was dropped onto a table from a height of 15 cm to create a mountain-shaped mass of copper oxide powder, and the angle of the base of the mountain-shaped mass was measured.
[0040] The results of measuring the dissolution rate, packed bulk density, and angle of repose for each copper oxide powder are shown in Table 1.
[0041]
[0042] As shown in Table 1, copper oxide powder A had the fastest dissolution rate and a bulk density of 1.6. On the other hand, copper oxide powder B, which had the slowest dissolution rate, had a bulk density of 2.23 and a large angle of repose of 22.5. Copper oxide powder C had a slower dissolution rate than A, but had a bulk density of 1.22 and an angle of repose of 15. This suggests that the bulk density was 1.6 g / cm. 3 It was found that copper oxide powder with an angle of repose of about 12.5° had a fast dissolution rate.
[0043] The results of SEM observation of particle morphology and specific surface area measurement for copper oxide powders A and B will be described. Figure 4 shows an SEM photograph of copper oxide powder A, and Figure 5 shows an SEM photograph of copper oxide powder B. In Figures 4 and 5, the upper row is an observation photograph at 1000x magnification, and the lower row is an observation photograph at 50,000x magnification. As shown in Figure 4, at 1000x magnification, many particles of 20 μm or more in diameter were observed in copper oxide powder A. Furthermore, at 50,000x magnification, fine particles with diameters of sub-μm or less were observed across the entire field of view in copper oxide powder A. Furthermore, as shown in Figure 5, many particles of 2-3 μm in diameter were observed in copper oxide powder B at both 1000x and 50,000x magnification. The specific surface area of copper oxide powder A was 23 m 2 / g, and the specific surface area of copper oxide powder A is 0.8 m 2 / g. Considering the results of the SEM observation and the specific surface area measurement, it is clear that although the average particle size of copper oxide powder A is large at 30 μm, particles with this average particle size are formed by agglomeration of fine particles. Since copper oxide powder A is a granular powder composed of fine particles, it is thought that the powder has good fluidity and a relatively small angle of repose.
[0044] <Copper Plating Test> Next, the results of a copper plating test in which copper plating was performed using a copper sulfate plating solution using the plating apparatus of this embodiment will be described. This copper plating test was performed using the insoluble anode plating apparatus described in Figure 1. A commercially available apparatus (MX-750, manufactured by Kinboshi Co., Ltd.) was used as the copper oxide powder feeder.
[0045] In this test, copper sulfate plating solution containing three types of additives (commercially available products) called accelerator, suppressor, and leveler was supplied to the upper isolated chamber on the cathode side, while copper sulfate plating solution containing no additives was supplied to the lower isolated chamber on the anode side. The solution composition is shown below.
[0046] *Liquid supplied to upper isolation chamber: Copper sulfate plating solution (commercially available Microfab Cu525 / manufactured by EEJA Corporation) Copper concentration: 60 g / L Sulfuric acid concentration: 30 g / L Accelerator 5W (accelerator): 3 mL / L Suppressor (inhibitor): 10 mL / L Leveler (smoothing agent): 10 mL / L Liquid temperature: 22-23°C Liquid volume: 40 L Supply flow rate: 25 L / min *Liquid supplied to lower isolation chamber: Copper sulfate plating solution (commercially available Microfab Cu525 / manufactured by EEJA Corporation, same liquid as the upper isolation chamber) Liquid temperature: 22-25°C Liquid volume: 20 L Supply flow rate: 5 L / min
[0047] The plating equipment used a mesh-shaped insoluble anode made of Pt-Ti, and the diaphragm was a commercially available product (membrane material: fluorine-based resin, thickness: 0.12 mm, water permeability: 0.08 mL / min / cm 2 The substrate used was an 8-inch PCB wafer. This PCB wafer was made by attaching copper foil to a glass epoxy substrate and processing it into a circular wafer shape.
[0048] In this copper plating test, a running test was conducted in which copper plating and copper oxide powder were supplied to examine the change in the concentration of additives contained in the upper isolation chamber supply solution. The copper oxide powder used was the copper oxide powder A described above, and nitrogen gas was used as the carrier gas. The supply tube was made of PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer) with an inner diameter of 1 mm and an outer diameter of 2 mm, and the powder supply cylinder was made of PFA with an inner diameter of 20.4 mm and an outer diameter of 25 mm. The tip of the powder supply cylinder (the copper oxide powder outlet side) was positioned approximately 80 mm above the plating solution surface in the control tank.
[0049] The copper plating conditions were as follows: plating current was supplied at an average current density of 0.91 A / dm2 (plating time 44 min) so that the amount of Cu deposited per wafer was 0.45 g. Furthermore, when copper plating was performed on one wafer, 0.5625 g of copper oxide powder A was supplied to the plating solution in the control tank. The nitrogen gas flow rate was 0.06 L / min (equivalent to a copper oxide powder A supply rate of 0.3 g / min). Furthermore, in the control tank to which copper oxide powder A was supplied, the solution was stirred using a magnetic stirrer.
[0050] Copper plating was performed on four wafers in sequence, and the plating solution in the upper isolation chamber was sampled after each plating process to analyze the additive concentrations. The copper concentration after each plating process was also analyzed. The results confirmed that the concentrations of the three additives in the copper sulfate plating solution supplied to the upper isolation chamber hardly fluctuated. Furthermore, the copper concentration in the copper sulfate plating solution supplied to the upper isolation chamber was also maintained at a nearly constant level. Analysis of the copper sulfate plating solution in the lower isolation chamber after each plating process revealed no traces of the three additives. This confirmed that the additives in the copper sulfate plating solution in the upper isolation chamber had not migrated to the lower isolation chamber.
[0051] Next, the results of the copper via-filling plating test will be described. In this test, a Si wafer with a via formed therein, 30 μm in diameter and 70 μm in depth, was used. Copper was filled into this via, and a pad, 12 μm thick and 80 μm in diameter, was continuously formed on top of the via by copper plating. The copper sulfate plating solution, copper oxide powder A, and other equipment conditions used were the same as those used in the running test for investigating changes in additive concentration described above.
[0052] Before copper embedding plating, the Si wafer was placed in a reduced pressure atmosphere, then pickled and washed with pure water, and copper embedding plating of the vias was performed. The plating conditions were: initial treatment current density 0.9 A / dm 2 , 0.5 mi, first stage treatment current density 0.9 A / dm 2 , 19.5 min, second stage treatment current density 1.36 A / dm 2 The first stage corresponds to filling the vias, and the second stage corresponds to copper plating on the top of the vias.
[0053] 6 shows a cross-sectional photograph of a via after copper plating. It was confirmed that the via was completely filled with copper plating. It was found that the plating apparatus of this embodiment can reliably perform copper plating to fill a fine via with a diameter of 30 μm and a depth of 70 μm.
[0054] REFERENCE SIGNS LIST 1 Plating tank 11 Diaphragm 12 Plating tank inner wall 13 Liquid supply pipe 14 Annular flow path 15 Insoluble anode 2 Control tank 21 Upper lid 3 Anode solution tank 4 Copper oxide powder supply device 41 Powder storage chamber 42 Supply tube 43 Powder supply cylinder 44 Switching device 45 Powder supply control device 5 Copper concentration adjustment tank 51 Upper lid U Upper isolation chamber D Upper isolation chamber W Wafer G Carrier gas
Claims
1. An insoluble anode plating apparatus comprising a plating tank having an opening for placing an object to be plated, a liquid supply pipe for supplying plating solution toward the object to be plated, an insoluble anode arranged to face the object to be plated, and a diaphragm for isolating the object to be plated and the insoluble anode, the diaphragm is arranged so that an outer peripheral edge is fixed to the inner wall of the plating tank and the peripheral edge of a through hole provided in the center of the diaphragm is fixed to the liquid supply pipe so as to be inclined upward from the liquid supply pipe toward the outer periphery, the liquid supply pipe supplies cathode plating solution from a control tank storing cathode plating solution to an upper isolation chamber in the plating tank formed by the diaphragm and the placed object to be plated, and the anode solution is supplied from an anode solution tank storing anode solution to a lower isolation chamber in the plating tank formed below the diaphragm, the apparatus comprising: a copper oxide powder supply means for supplying copper oxide powder together with a carrier gas to the control tank via a supply tube having static electricity removing performance, The plating apparatus for insoluble anodes is characterized in that a powder supply cylinder having a static electricity removing function and a tip of which is positioned near the liquid level of the cathode plating solution stored in the management tank is provided on the upper lid of the management tank, and a supply tube is connected to the powder supply cylinder.
2. An insoluble anode plating device comprising a plating tank having an opening for placing an object to be plated, a liquid supply pipe for supplying plating solution toward the object to be plated, an insoluble anode arranged to face the object to be plated, and a diaphragm for isolating the object to be plated and the insoluble anode, the diaphragm is arranged so that an inclination ascending from the liquid supply pipe toward the outer periphery is given to the diaphragm by fixing the outer peripheral edge to the inner wall of the plating tank and fixing the peripheral edge of a through hole provided in the center of the diaphragm to the liquid supply pipe, the cathode plating solution is supplied from the liquid supply pipe to an upper isolation chamber in the plating tank formed by the diaphragm and the placed object to be plated from a control tank storing cathode plating solution, and the anode solution is supplied from an anode solution tank storing anode solution to a lower isolation chamber in the plating tank formed below the diaphragm, the device comprising a copper concentration adjustment tank for adjusting the copper concentration of the cathode plating solution, the copper concentration adjustment tank has a copper oxide powder supply device that transports copper oxide powder together with a carrier gas through a supply tube having static electricity removal capability, an upper cover of the copper concentration adjustment tank is provided with a powder supply cylinder having static electricity removal capability and whose tip is located near the liquid surface of the cathode plating solution stored in the copper concentration adjustment tank, and the copper concentration adjustment tank is provided with a stirring means for stirring the cathode plating solution, the supply tube is connected to the powder supply cylinder, and the copper concentration of the cathode plating solution in the copper concentration adjustment tank is adjusted by supplying copper oxide powder to the copper concentration adjustment tank, and the cathode plating solution with the adjusted copper concentration is supplied from the copper concentration adjustment tank to a control tank.
3. The copper oxide powder has an average particle size of 25-40 μm and a bulk density of 1.7 g / cm 3 3. The insoluble anode plating apparatus according to claim 1 or 2, wherein the insoluble anode plating temperature is less than 100° C.
4. An insoluble anode plating apparatus according to claim 1 or 2, wherein the powder supply cylinder is made of a grounded titanium material or is connected to a static eliminator.
5. An insoluble anode plating apparatus according to claim 1 or 2, wherein the carrier gas is nitrogen gas or argon gas.
6. An insoluble anode plating apparatus as described in claim 1 or 2, wherein the supply tube is provided with a switching means capable of switching between supplying a carrier gas and copper oxide powder and supplying only a carrier gas.
7. A plating apparatus for insoluble anodes as described in claim 1 or claim 2, wherein the supply tube has a powder flow meter for monitoring the supply state of the copper oxide powder and is provided with a powder supply control means for adjusting the supply amount of the copper oxide powder and controlling the stopping of the supply.
Citation Information
Patent Citations
JP1974033193U
Method of eliminating electrostatic powder fluid
JP1979009597A
Feeder of powder and granular material
JP2014118215A
Plating system and plating method
JP2018178141A
Copper oxide solids used for plating circuit board, production method of copper oxide solids, and apparatus for supplying plating solution to plating tank
JP2020029590A