Carbon material, material composition and method for producing carbon material

The development of a high-nitrogen content carbon material with optimized pore structure and supported metals addresses performance limitations in capacitors and catalyst carriers, enhancing capacitance and catalytic activity.

WO2024204299A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/012154
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional carbon materials do not achieve sufficient performance in applications such as capacitors and catalyst carriers due to limitations in nitrogen doping levels and pore structure, leading to inadequate capacitance and catalytic performance.

Method used

A carbon material with a nitrogen content of 9 at% or more, a mesopore volume of 0.30 cm^3/g or more, and a specific surface area of 700 m^2/g or more, featuring a controlled mesopore diameter distribution and supported metals or metal oxides, is developed to enhance performance.

Benefits of technology

The enhanced carbon material improves capacitance and catalytic performance by increasing diffusivity and surface area, supporting higher catalyst loading and activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000025_0000
    Figure 00000025_0000
Patent Text Reader

Abstract

Disclosed is a carbon material which is a porous body containing nitrogen, and which has a nitrogen content ratio of 9 at% or more, a mesopore volume of 0.30 cm3 / g or more, and a specific surface area of 700 m2 / g or more. The standard deviation of the pore diameters of the mesopores is preferably 7 to 10, the molar ratio expressed by (the number of moles of nitrogen) / (the number of moles of carbon) is preferably 0.1 to 0.3, and the ratio of the number of moles of active nitrogen to the total number of moles of nitrogen is preferably 20% to 80%. In addition, it is preferable that the carbon material is in the form of a powder and has an average primary particle diameter of 25 nm to 3,000 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Carbon material, material composition, and method for producing carbon material

[0001] The present invention relates to a carbon material, a material composition, and a method for producing a carbon material. This application claims priority based on Japanese Patent Application No. 2023-049188, filed on March 27, 2023, the contents of which are incorporated herein by reference.

[0002] Porous carbon materials such as activated carbon are used in a variety of applications, including electrode materials, separators, sensors, spacers, reinforcing materials, catalysts, and catalyst supports. The performance of carbon materials is affected by factors such as pore size and pore volume.

[0003] Carbon materials are used, for example, as electrode active materials in capacitor electrodes. For example, Patent Document 1 proposes activated carbon for hybrid capacitors, which has a specific range of basic functional group content based on neutralization titration and a specific range of carbon dioxide adsorption capacity at -196°C. The invention of Patent Document 1 aims to suppress capacity loss at low temperatures.

[0004] Carbon materials are also used as catalyst supports. For example, Patent Document 2 proposes a fuel cell electrode catalyst for a fuel cell that includes a conductive support and at least one of a metal and a metal compound supported on the conductive support and that operates at a temperature of 100°C or higher. The conductive support is nitrogen-doped graphene, which is a heteroelement-doped graphene. The heteroelement-doped graphene has a nitrogen doping amount of 4 atom% or more relative to the carbon on the surface of the heteroelement-doped graphene. Patent Document 2 describes that a predetermined amount of nitrogen doping increases the catalyst loading, resulting in improved catalytic properties.

[0005] Patent No. 6297285 International Publication No. 2022 / 030552

[0006] However, conventional carbon materials have not been sufficient in terms of the intended performance (e.g., the capacitance characteristics of a capacitor using a carbon material as an electrode, or the catalytic performance when a carbon material is used as a catalyst support), and further improvements are desired. Furthermore, Patent Document 2 uses a carbon material with an actual nitrogen doping amount of approximately 2.9 to 7.0 at % as a catalyst support, but the catalyst support amount is insufficient, and the catalytic performance when used as a catalyst support is also unsatisfactory. Therefore, the present invention aims to provide a carbon material that can further improve the intended performance.

[0007] The present invention has the following aspects: <1> A nitrogen-containing porous body, wherein the nitrogen content is 9 at% or more, and the mesopore volume is 0.30 cm 3 / g or more, and the specific surface area is 700 m 2 / g or more. <2> The carbon material according to <1>, wherein the standard deviation of the mesopore diameter is 7 to 10. <3> The carbon material according to <1> or <2>, wherein the molar ratio represented by [moles of nitrogen] / [moles of carbon] is 0.1 to 0.3. <4> The carbon material according to any one of <1> to <3>, wherein the ratio of the number of moles of active nitrogen to the total number of moles of nitrogen is 20 to 80%. <5> The carbon material according to any one of <1> to <4>, which is in the form of a powder and has an average primary particle diameter of 25 to 3,000 nm. <6> The carbon material according to any one of <1> to <5>, wherein at least one selected from a metal and a metal oxide is supported. <7> The carbon material according to any one of <1> to <6>, wherein an organic substance is supported. <8> The carbon material according to any one of <1> to <7>, wherein a metal-organic framework is supported.

[0008] <9> A material composition comprising the carbon material according to any one of <1> to <8>. <10> The material composition according to <9>, which is an electrode material, a separator, a sensor material, a spacer material, a reinforcing material, a gas adsorbent, a liquid adsorbent, an ion adsorbent, a solid adsorbent, a catalyst support, an electromagnetic wave-related material, or an energy storage material.

[0009] <11> A method for producing the carbon material according to any one of <1> to <8>, comprising a step of firing a raw material composition containing a nitrogen-containing metal organic framework.

[0010] The carbon material of the present invention can further improve the desired performance.

[0011] 1 is a graph showing the pore distribution (Log differential pore volume distribution) of the carbon materials used in Examples 1 and 2 and Comparative Examples 1 and 2.

[0012] In this specification and claims, the use of "to" indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits.

[0013] (Carbon Material) The carbon material of the present invention is a porous body having mesopores. The carbon material is preferably a single carbon material. A "single" carbon material means that the carbon substances constituting the carbon material are not a mixture but form a continuous phase. Whether a carbon material is a single carbon material can be confirmed by observation with thermogravimetric analysis (TGA) or scanning electron microscope (SEM), for example. For example, in the case of TGA, the weight loss curve of the carbon material is measured by TGA, and if the obtained weight loss curve has one drop point within the range of 150 to 1500°C, it can be determined that it is a single carbon material. In the case of SEM, if no carbon bodies of different shapes are confirmed, it can be determined that it is a single carbon material.

[0014] The total pore volume of the carbon material is 0.80 m 3 / g or more is preferable, and 1.20m 3 / g or more is more preferable, and 1.60m 3 When the total pore volume is equal to or greater than the above lower limit, the diffusibility of the substance increases, and the target performance (for example, when the carbon material is used as an electrode of a capacitor, the capacitance is increased, and when the carbon material is used as a support for a catalyst, the adsorption of the metal that becomes the active site onto the support is increased, etc.) can be further improved. The upper limit of the total pore volume of the carbon material is 4.0 cm 3When the total pore volume is equal to or less than the upper limit, the specific surface area can be increased, and the desired performance can be improved. The range of the total pore volume of the carbon material is 0.80 to 4.0 cm 3 / g is preferred, and 1.20 to 4.0 cm 3 / g is more preferable, and 1.60 to 4.0 cm 3 / g is even more preferable. The total pore volume, the average pore size, the standard deviation of pore sizes, the mesopore size and distribution, the mesopore volume, and the micropore volume, which will be described later, are calculated by performing nitrogen adsorption / desorption measurements by a gas adsorption method and using the BJH (Barrett-Joyner-Halenda) method from the obtained nitrogen adsorption isotherm. The macropore volume, which will be described later, is calculated by subtracting the sum of the micropore volume and the mesopore volume from the total pore volume. The total pore volume can be adjusted by combining the composition of the carbon material (e.g., the type or amount of metal ions or organic bridging ligands constituting the raw material MOF, which will be described later, and the B / A ratio) and the production conditions (e.g., the calcination temperature and time).

[0015] Mesopores have a pore diameter of 2 nm to 50 nm. The average pore diameter (D50) of the mesopores in the carbon material is preferably 2 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more. When the average pore diameter of the mesopores (average mesopore diameter) is equal to or greater than the above-mentioned lower limit, the diffusibility of substances is increased, and the target performance can be further improved. The upper limit of the average pore diameter is preferably 50 nm or less, more preferably 45 nm or less, and even more preferably 40 nm or less. When the average mesopore diameter is equal to or less than the above-mentioned upper limit, the specific surface area can be further increased, and the target performance can be further improved. The range of the average pore diameter is preferably 2 to 50 nm, more preferably 10 to 45 nm, and even more preferably 15 to 40 nm. The average mesopore diameter can be adjusted by combining the composition of the carbon material (e.g., the type or amount of metal ions or organic bridging ligands constituting the raw material MOF described below, and the B / A ratio) and the production conditions (e.g., the calcination temperature and time).

[0016] The standard deviation of the mesopore diameters of the carbon material is preferably 7 to 15, more preferably 8.2 to 15, and even more preferably 11 to 15. When the standard deviation of mesopore diameters is equal to or greater than the above lower limit, the diffusibility of substances is increased, further improving the target performance. When the standard deviation of mesopore diameters is equal to or less than the above upper limit, the specific surface area is increased, further improving the target performance. The standard deviation of mesopore diameters can be adjusted by combining the composition of the carbon material (e.g., the type or amount of metal ions or organic bridging ligands constituting the raw material MOF described below, and the B / A ratio) and the production conditions (e.g., the firing temperature and time). It is preferable that the mesopore distribution of the pore diameters of the carbon material be a wide pore distribution.

[0017] The mesopore volume of the carbon material is 0.30 cm 3 / g or more, preferably 0.70 cm3 / g or more, and 1.3 cm 3 When the mesopore volume is equal to or greater than the above lower limit, the diffusibility of the substance is increased, and the target performance can be improved. The upper limit of the mesopore volume of the carbon material is not particularly limited, but is, for example, 4.0 cm 3 / g or less is preferable, and 3.7 cm 3 / g or less is more preferable. When the mesopore volume is equal to or less than the above upper limit, the specific surface area can be increased, and the target performance can be further improved. The above upper and lower limits can be combined arbitrarily. For example, the mesopore volume of the carbon material is in the range of 0.30 to 4.0 cm 3 / g is preferred, and 0.70 to 4.0 cm 3 / g is more preferable, and 1.3 to 3.7 cm 3 / g is more preferable. The mesopore volume is the ratio of the volume of mesopores (cm) to the mass (g) of the carbon material. 3 The mesopore volume can be adjusted by combining the composition of the carbon material (e.g., the type or amount of metal ions or organic bridging ligands constituting the raw material MOF, which will be described later, and the B / A ratio) and the production conditions (e.g., the calcination temperature and time).

[0018] The ratio of mesopore volume to total pore volume (mesopore volume ratio) is, for example, preferably 17% by volume or more, more preferably 37% by volume or more, and even more preferably 45% by volume or more. When the mesopore volume ratio is equal to or greater than the above-mentioned lower limit, the diffusibility of substances is increased, and the target performance can be further improved. The upper limit of the mesopore volume ratio is, for example, preferably 50% by volume or less. When the mesopore volume ratio is equal to or less than the above-mentioned upper limit, the specific surface area can be further increased, and the target performance can be further improved. The range of the mesopore volume ratio is, for example, preferably 17 to 50% by volume, more preferably 37 to 50% by volume, and even more preferably 45 to 50% by volume. The mesopore volume ratio can be adjusted by combining the composition of the carbon material (e.g., the type or amount of metal ions or organic bridging ligands constituting the raw material MOF described below, the B / A ratio) and the production conditions (e.g., the firing temperature and time).

[0019] In addition to mesopores, the carbon material may have at least one of micropores and macropores. Micropores are pores with a diameter smaller than that of mesopores. The diameter of micropores is, for example, less than 2 nm. The lower limit of the micropore diameter is the detection limit of a measurement method (e.g., gas adsorption method), and is, for example, 0.3 nm. The ratio of the micropore volume to the total pore volume (micropore volume ratio) is, for example, preferably 7 vol% or more, more preferably 13 vol% or more, and even more preferably 20 vol% or more. When the micropore volume ratio is equal to or greater than the above lower limit, the diffusibility of substances can be enhanced. The upper limit of the micropore volume ratio is, for example, preferably 74 vol% or less. When the micropore volume ratio is equal to or less than the above upper limit, the specific surface area can be further increased. The range of the micropore volume ratio is, for example, preferably 7 to 74 vol%, more preferably 13 to 74 vol%, and even more preferably 20 to 74 vol%.

[0020] Macropores are pores with a pore diameter larger than that of mesopores. The pore diameter of macropores is, for example, greater than 50 nm. The upper limit of the pore diameter of macropores is, for example, 400 nm. The ratio of macropore volume to total pore volume (macropore volume ratio) is, for example, preferably 3 vol% or more, more preferably 13 vol% or more, and even more preferably 20 vol% or more. When the macropore volume ratio is equal to or greater than the above lower limit, the diffusibility of substances can be enhanced. The upper limit of the macropore volume ratio is, for example, preferably 74 vol% or less. When the macropore volume ratio is equal to or less than the above upper limit, the specific surface area can be enhanced. The range of the macropore volume ratio is, for example, preferably 3 to 74 vol%, more preferably 13 to 74 vol%, and even more preferably 20 to 74 vol%.

[0021] The specific surface area of ​​the carbon material is 700 m 2 / g or more, and 2 / g or more is preferable, and 1500m 2 When the specific surface area of ​​the carbon material is equal to or greater than the lower limit, the amount of material adsorbed on the surface is increased, thereby improving the target performance. The upper limit of the specific surface area of ​​the carbon material is 3000 m 2 When the specific surface area of ​​the carbon material is equal to or less than the upper limit, the target performance can be further improved. 2 / g to 3000m 2 / g is preferred, and 1100 to 3000m 2 / g is more preferable, and 1500 to 3000m 2 The specific surface area is a value measured by a gas adsorption / desorption method.

[0022] The carbon material contains nitrogen in its structure. Part or all of the nitrogen contained in the carbon material is in the pyridine or pyrrole form, which is so-called activated nitrogen. The active nitrogen in the carbon material serves as an active site, facilitating proton exchange and increasing polarity, thereby improving the intended performance. The carbon material preferably has a graphene structure. The graphene structure of the carbon material further increases the conductivity.

[0023] The carbon material may have a structure in which nitrogen is introduced into the structure of a known carbon material. Examples of such known carbon materials include activated carbon, carbon black, MOF carbon, graphene oxide, reduced graphene oxide (re-reduced graphene oxide: rGO), and surface-modified graphene (graphene whose surface is modified with functional groups, such as hydroxyl, epoxy, amino, carboxyl, aldehyde, carbonyl, alkyl, methyl, ethyl, propyl, methoxy, ketone, acetyl, sulfo, sulfoxide, and nitro groups). The use of the above materials can achieve both electrical conductivity and metal adsorption. Note that graphene has few functional groups on its surface, which allows metals to easily migrate and aggregate. Therefore, when using a carbon material as a catalyst support, it is preferable to have a structure other than graphene.

[0024] The ratio of the number of nitrogen atoms to the total number of atoms constituting the carbon material is 9 at% or more, preferably 9 to 30 at%, and more preferably 20 to 30 at%. When the ratio of the number of nitrogen atoms is equal to or greater than the above lower limit, the target performance can be further improved. When the ratio of the number of nitrogen atoms is equal to or less than the above upper limit, the pseudocapacitance, conductivity, and ion adsorption amount can be further increased. The ratio of the number of nitrogen atoms in the carbon material is a value measured by energy dispersive X-ray spectroscopy (SEM-EDX), X-ray photoelectron spectroscopy (XPS), CHN elemental analysis (carbon, hydrogen, nitrogen), etc.

[0025] In a carbon material, the molar ratio (N / C ratio), which is the ratio of the number of moles of nitrogen to the number of moles of carbon and is expressed as [number of moles of nitrogen] / [number of moles of carbon], is preferably 0.1 to 0.3, more preferably 0.13 to 0.3, and even more preferably 0.2 to 0.3. When the N / C ratio is equal to or greater than the lower limit, the target performance can be further improved. When the N / C ratio is equal to or less than the upper limit, the diffusibility of the substance can be improved, the wettability with the electrolyte can be further improved, and the catalytic activity can be further improved. The carbon content in the carbon material and the ratio of the number of nitrogen atoms in the carbon material are values ​​measured by SEM-EDX, XPS, CHN elemental analysis, etc.

[0026] The ratio of the content (number of moles) of active nitrogen in the carbon material to the total amount of nitrogen (total number of moles) in the carbon material (active nitrogen ratio) is preferably 20% or more, more preferably 40% or more, and even more preferably 60% or more. When the active nitrogen ratio is equal to or greater than the above lower limit, the target performance can be further improved. The upper limit of the active nitrogen ratio is preferably 80% or less. When the active nitrogen ratio is equal to or less than the above upper limit, the metal adsorption efficiency can be further improved. When the active nitrogen ratio exceeds the above upper limit, the amount of metal adsorbed becomes excessive, which may cause aggregation of metal particles. The range of the active nitrogen ratio is preferably 20 to 80%, more preferably 40 to 80%, and even more preferably 60 to 80%. The active nitrogen is a value measured by XPS.

[0027] Carbon materials also have excellent optical properties in the visible to infrared range, as well as excellent IR properties such as IR absorption and reflection. For example, carbon materials can enhance light absorption in the visible to infrared range (500 to 1000 nm). The absorbance of carbon materials at a wavelength of 700 nm is preferably 0.2 to 1.0 or higher, more preferably 0.4 to 1.0, and even more preferably 0.6 to 1.0. Absorbance above the lower limit enhances photocatalytic activity, while absorbance below the upper limit enhances catalytic efficiency. The absorbance is a value measured by UV-Vis-NIR spectroscopy. Absorbance can be adjusted by combining the composition of the carbon material, manufacturing method, etc.

[0028] The carbon material may support at least one metal (e.g., a supported metal) selected from metals and metal compounds (e.g., metal oxides and metal complexes). That is, the carbon material may be a support in which a supported metal is supported on a nitrogen-containing porous body. Examples of metals such as supported metals include platinum, gold, palladium, rhodium, ruthenium, zinc, iron, nickel, cobalt, titanium, tungsten, vanadium, molybdenum, chromium, manganese, and niobium. Examples of metal oxides such as supported metals include zinc oxide, cobalt oxide, nickel oxide, and iron oxide. Examples of metal complexes include ammine complexes, cyano complexes, halogeno complexes, hydroxy complexes, salen complexes, porphyrin complexes, and phthalocyanine complexes. Examples of other metal compounds include alloys, nitrides, oxynitrides, carbides, phosphates, and fluorides. These metals may be used alone or in combinations of two or more. The amount of the supported metal or the like is, for example, 0.1 to 2 mass % relative to the total mass of the carbon material.

[0029] The carbon material may be supported with an organic substance (supported organic substance). That is, the carbon material may be a support in which a supported organic substance is supported on a nitrogen-containing porous body. Examples of supported organic substances include sugars and proteins. These supported organic substances may be used alone or in combination of two or more. The amount of supported organic substance is, for example, 0.1 to 2 mass % with respect to the total mass of the carbon material.

[0030] The carbon material may be supported with a metal-organic framework (hereinafter, sometimes referred to as "MOF"). That is, the carbon material may be a support in which a nitrogen-containing porous body supports an MOF (hereinafter, the supported MOF may be referred to as a "supported MOF"). Examples of supported MOFs include those similar to the raw MOFs described below. The supported MOF and the raw MOF may be the same or different. Note that the supported MOF does not necessarily need to contain nitrogen. Therefore, a MOF other than the raw MOF described below may also be used. The supported MOF may be, for example, a MOF containing atoms such as fluorine, phosphorus, boron, or sulfur instead of nitrogen, or a MOF containing these atoms and nitrogen. The amount of supported MOF supported is, for example, 0.1 to 2 mass% relative to the total mass of the carbon material.

[0031] The form of the carbon material is not particularly limited, and examples include powder, pellets, and blocks. When the carbon material is a powder, the average primary particle diameter of the carbon material is, for example, preferably 25 to 3,000 nm, more preferably 50 to 400 nm, and even more preferably 80 to 200 nm. When the average primary particle diameter is equal to or greater than the above lower limit, the target performance can be improved. When the average primary particle diameter is equal to or less than the above upper limit, the performance can be improved more uniformly. The average particle diameter of the carbon material is the median diameter measured by dry particle size distribution measurement using laser scattering.

[0032] (Material composition) The material composition includes the carbon material of the present invention. By including the carbon material, the material composition can further improve the intended performance. The material composition may consist of only the carbon material, or may include components other than the carbon material (optional material components). The content of the carbon material in the material composition is determined appropriately taking into consideration the application of the material composition, etc.

[0033] The optional components are determined appropriately depending on the application of the material composition. Examples of applications of the material composition include electrode materials, separation materials, sensor materials, spacer materials, reinforcing materials, gas adsorbents, liquid adsorbents, ion adsorbents, solid adsorbents, catalyst carriers, electromagnetic wave-related materials, and energy storage materials. When the material composition is used for an electrode material, the optional components include conductive aids, binders, and additives. Examples of conductive aids include ketjen black and carbon nanotubes. Examples of binders include polyacrylonitrile, cellulose-based polymers, and polyvinylidene fluoride. Examples of additives include carboxymethyl cellulose. These optional components may be used alone or in combination of two or more. The content of the optional components in the material composition is determined appropriately taking into account the application of the material composition.

[0034] (Method for producing carbon material) The method for producing a carbon material of the present invention includes, for example, a step of calcining a raw material composition (calcination step). The raw material composition includes nitrogen-containing MOFs (MOFs used in the production of carbon materials may be referred to as "raw material MOFs"). By calcining the raw material composition containing the raw material MOFs, a porous body having a large specific surface area, a large mesopore volume, and a high nitrogen content can be easily produced. Hereinafter, the method for producing a carbon material will be described with reference to one embodiment.

[0035] The method for producing a carbon material according to the present embodiment includes a step of preparing a raw material composition (raw material preparation step) and a step of firing the raw material composition (firing step).

[0036] <Raw Material Preparation Step> The raw material preparation step is a step of preparing a raw material composition. The raw material composition contains raw material MOFs and, optionally, other components (optional raw material components). That is, in the raw material preparation step, the raw material composition may be the raw material MOFs, or the raw material MOFs and the optional raw material components may be mixed to prepare the raw material composition.

[0037] MOFs are porous structures in which metal ions and organic bridging ligands (multidentate ligands having two or more coordinating functional groups) are continuously bonded together, and have multiple internal pores. Known MOFs include those with multiple metal, metal oxide, metal cluster, or metal oxide cluster structural units, but the raw MOF is not limited to any of these.

[0038] Examples of metal atoms constituting the raw MOF include zinc, cobalt, niobium, zirconium, cadmium, copper, nickel, chromium, vanadium, titanium, molybdenum, magnesium, iron, and aluminum. However, the metal atoms constituting the MOF are not limited to these. The metal atoms constituting the raw MOF may be one type or two or more types. Suitable metal sources for the raw MOF include complexes containing metal ions such as Zn2+, Cu2+, Ni2+, and Co2+, as well as metal-containing secondary structure units (SBUs).

[0039] The coordinating functional group of the organic bridging ligand used in producing the starting MOF may be any functional group capable of coordinating to a metal atom, such as a carboxyl group, an imidazole group, a hydroxyl group, a sulfonic acid group, a pyridine group, a tertiary amine group, an amide group, or a thioamide group. Among these, an imidazole group is preferred. The two or more coordinating functional groups possessed by the organic bridging ligand may be the same or different. The organic bridging ligand typically has two or more coordinating functional groups substituted on a skeleton having a rigid structure (e.g., an aromatic ring, an unsaturated bond, or the like).

[0040] The organic bridging ligand of the starting MOF contains nitrogen. When the organic bridging ligand contains nitrogen, a nitrogen-containing carbon material can be obtained. Examples of the organic bridging ligand of the starting MOF include compounds having an imidazole structure, such as imidazole, 2-methylimidazole, benzimidazole, 2-nitroimidazole, cyclobenzimidazole, imidazole-2-carboxaldehyde, 4-cyanoimidazole, 6-methylbenzimidazole, and 6-bromobenzimidazole. The organic bridging ligand constituting the starting MOF may be one type or two or more types.

[0041] Specific examples of raw material MOFs are listed below, but the present invention is not limited thereto. IRMOF-3 represented by Zn4O(2-amino-1,4-benzenedicarboxylate)3; ZIF-8 represented by Zn(2-methylimidazolate)2; ZIF-68 represented by Zn(benzimidazolate)(2-nitroimidazolate); ZIF-69 represented by Zn(cyclobenzimidazolate)(2-nitroimidazolate); ZIF-7 represented by Zn(benzimidazolate)2; ZIF-9 represented by Co(benzimidazolate)2; and Zn2(benzimidazolate). ZIF-11 represented by the formula (I); ZIF-90 represented by Zn(imidazolate-2-carboxaldehyde)2; ZIF-82 represented by Zn(4-cyanoimidazolate)(2-nitroimidazolate); ZIF-70 represented by Zn(imidazolate)(2-nitroimidazolate); ZIF-79 represented by Zn(6-methylbenzimidazolate)(2-nitroimidazolate); and ZIF-81 represented by Zn(6-bromobenzimidazolate)(2-nitroimidazolate).

[0042] ZIF, such as ZIF-8, is preferred as the starting MOF. ZIF is a material with a zeolite-like topology that contains zinc or cobalt as the metal and imidazole-based organic bridging ligands (imidazole, benzimidazole, 2-nitroimidazole, 2-methylimidazole, cyclobenzimidazole, imidazole-2-carboxaldehyde, 4-cyanoimidazole, 6-methylbenzimidazole, 6-bromobenzimidazole, etc.). Using ZIF as the starting MOF allows for easy adjustment of the nitrogen content of the carbon material within the desired range, thereby increasing the mesopore volume and specific surface area of ​​the carbon material.

[0043] The raw material MOF typically has a crystalline structure. Because the raw material MOF has an ordered structure, it is easily crystallized and can be easily obtained as a single crystal or polycrystal. The crystal may be a single crystal or a polycrystal. The median size of the crystal structure is preferably 10 nm to 100 μm, more preferably 30 nm to 1 μm. If the median size of the crystal structure is equal to or greater than the above-mentioned lower limit, the specific surface area is superior, and if it is equal to or less than the above-mentioned upper limit, the diffusibility of the substance and the dispersibility of the crystal are superior.

[0044] The median size of the crystal structure of the raw MOF is measured by the following method. An image of the surface of the sample is obtained using a scanning electron microscope or an optical microscope. The magnification is set so that the number of crystals (MOFs) present in the image is 100 to 200. The maximum diameters of all crystals present in the obtained image are measured, and the median (average of the minimum and maximum values) is calculated, and this value is used as the median size of the crystal structure of the MOF.

[0045] The raw MOF may be commercially available or may be produced by a known production method. Examples of methods for producing raw MOFs include those described in International Publication No. 2019 / 039509. Depending on the production method and production conditions of the raw MOF, differences occur in the size of the crystal structure of the produced MOF and the amount of metal oxide contained, resulting in differences in the pore distribution of the raw MOF. Using the method described in International Publication No. 2019 / 039509 as an example, this method involves applying a stimulus to a composition containing a substance (A) (excluding MOFs) containing a metal atom constituting the raw MOF, an organic substance (B) having two or more metal coordination moieties capable of coordinating to the metal atom to produce a crystal, and a coordination promoter (C) that undergoes a reaction or phase transition upon stimulation and can promote the coordination of the metal coordination moiety of the organic substance (B) to the metal atom of the substance (A), thereby producing a MOF. The mixing ratio (B / A ratio) of the organic material (B) to the substance (A) is preferably 1 or more, more preferably 1.2 or more, and even more preferably 1.5 or more, in terms of molar ratio. The upper limit of the B / A ratio is not particularly limited, but is preferably 1.9, for example. When the B / A ratio is equal to or greater than the lower limit, the specific surface area and mesopore volume can be increased, and the nitrogen content of the raw material MOF can be increased.

[0046] In the above method, the type and equivalent amount of the coordination promoter (C) affect the pore distribution of the resulting MOF. For example, when a base (e.g., an amine-borane complex, dicyandiamide, hydrazide, imine, oxazolidine, pyridine, tertiary amine, ketoprofen amine salt, secondary amine, primary amine, or a mixture thereof) is blended as the coordination promoter (C) in an amount equal to or greater than the organic substance (B), the mesopore volume and specific surface area of ​​the carbon material can be further increased. On the other hand, when the blending amount of the base is reduced, the yield of the resulting MOF tends to decrease.

[0047] The raw material MOF has a crystalline structure and therefore has internal pores. Therefore, unlike conventional activated carbon, it can be converted into a carbon material by a calcination process without undergoing a porosity-improving treatment (activation) using chemicals or an activation gas. However, after calcination, a porosity-improving treatment can be performed as needed to further increase the specific surface area. Note that the raw material MOF does not usually have mesopores before calcination. Calcination forms mesopores in the carbon material.

[0048] Examples of optional raw material components that may be mixed with the raw material MOF include common resins, plant-derived carbon sources, and carbon-containing chemical substances. By mixing the optional raw material components, the amount of metal-organic framework used can be reduced, thereby reducing costs. When the raw material composition contains the optional raw material components, the lower limit of the content of the raw material MOF relative to the total mass of the raw material MOF and the optional raw material components is preferably 10% by mass or more, more preferably 50% by mass, and even more preferably 80% by mass or more. The range of the content of the raw material MOF relative to the total mass of the raw material MOF and the optional raw material components is preferably 10 to 100% by mass, more preferably 50 to 100% by mass, and even more preferably 80 to 99.9% by mass. When the content of the raw material MOF is equal to or greater than the above-mentioned lower limit, the desired performance of the carbon material can be further improved. When the content of the raw material MOF is equal to or less than the preferred upper limit, changes in carbon dynamics occur, resulting in a favorable effect on diffusion.

[0049] The raw material composition is preferably crushed. After firing, it becomes a high-density, strong sintered body, which makes it difficult to adjust the particle size by crushing. There are no particular limitations on the crushing method, and the use of a mixer, grinding in a mortar, a ball mill, etc. can be appropriately adopted. Among these, crushing using a mixer is preferred because it is easy to eliminate human error and unevenness in the degree of crushing.

[0050] <Caking Step> In the baking step, the raw material composition is baked to obtain a porous body. The baking method in the baking step is not particularly limited, and any known baking method used in the carbonization of organic materials can be used. Baking is preferably performed in an inert gas. Examples of inert gases include nitrogen gas and argon. The baking temperature (maximum temperature after heating) is preferably 300 to 1000°C, more preferably 600 to 1000°C, and even more preferably 900 to 980°C. Considering the use of the carbon material as an electrode catalyst, baking at a relatively high temperature improves conductivity. From this perspective, the baking temperature (maximum temperature after heating) is preferably 300 to 2000°C, more preferably 600 to 1800°C, and even more preferably 900 to 1500°C. The baking time is preferably 0.5 to 10 hours, more preferably 1 to 5 hours, and even more preferably 1 to 3 hours. By firing within the above range, structural changes as a carbon material are promoted, and the electrical conductivity as a carbon material can be improved.

[0051] The raw material composition is preferably classified after firing. By classifying after firing, coarse particles and fine particles can be removed. Coarse particles can be removed, for example, by using a sieve with a mesh size of 10 to 1000 μm and removing particles that did not pass through this sieve. The range of coarse particles to be removed is determined appropriately depending on the application of the carbon material. For example, when the carbon material is used as an electrode material, it depends on the thickness d of the electrode active material layer of the electrode material using the carbon material as the active material. The thicker the thickness d of the electrode active material layer, the larger the mesh size should be used to remove only larger coarse particles.

[0052] The removal of fine particles can be carried out, for example, by using a sieve with a mesh size of 1 to 50 μm and removing particles that pass through this sieve. The range of fine particles to be removed is adjusted in terms of resistance. By removing the fine particles, when the material is used as an electrode material, the resistance is less likely to increase due to binders and the like. It is preferable to return some of the removed fine particles rather than removing all of them as they are. This makes it easier for the porous carbon powder to maintain good point contact with each other after sintering.

[0053] Of the fine particles once removed by sieving, it is preferable to return 1 to 99% by mass, more preferably 10 to 95% by mass, and even more preferably 30 to 90% by mass. If the proportion of returned particles is equal to or greater than the lower limit, the number of contact points increases and resistance decreases. If the proportion of returned particles is equal to or less than the upper limit, the amount of particles removed can be reduced, resulting in cost savings.

[0054] <Other Steps> The method for producing a carbon material may include steps other than the raw material preparation step and the firing step. Examples of the other steps include a supporting step.

[0055] The loading step is a step of loading a material such as a supported metal, a supported organic material, or a supported MOF onto the porous body obtained in the calcination step. Methods for loading a material onto the porous body include, for example, immersion, compression immersion, AD, and electrolysis.

[0056] (Method for producing material composition) In the method for producing a material composition, the carbon material of the present invention is mixed with any other material component. The method for mixing the carbon material with the other material component is appropriately determined depending on the form of the material composition, and examples thereof include powder mixing and a method for dispersing the carbon material in a liquid dispersion medium.

[0057] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0058] Example 1 Production Example 1 Production of Raw Material MOF-1 Raw material MOF-1 was prepared using 2-methylimidazole as the organic bridging ligand, zinc oxide as the metal raw material, and aqueous ammonia as a reaction accelerator, according to the following procedure. 2-Methylimidazole was added to pure water and stirred until completely dissolved to obtain an organic bridging ligand solution. Separately, zinc oxide and nitric acid were added to pure water and stirred until completely dissolved to obtain a metal raw material solution. The solutions were mixed, and then aqueous ammonia was added and mixed. In the mixed solution, the molar ratio of 2-methylimidazole to zinc oxide (B / A ratio) was 1. When the resulting mixed solution was stirred at room temperature, crystals precipitated. The crystals were then collected by filtration, washed, and dried to obtain the crystalline raw material MOF-1.

[0059] <Production of Carbon Material> The raw material MOF-1 obtained in Production Example 1 above was pulverized using an agate mortar or a Labo Mill II manufactured by Osaka Chemical Co., Ltd. to obtain a pulverized product with an average particle size of 50 μm. The pulverized product obtained was transferred to a quartz glass tubular furnace and heated to 950° C. in an inert atmosphere. After holding for 1 hour, it was allowed to cool naturally to room temperature to obtain the carbon material of this example.

[0060] <Measurement of pore volume and pore distribution> Nitrogen adsorption and desorption measurements were performed on the obtained carbon material at 77 K (-196°C) using a gas adsorption measurement device BELSORP-max manufactured by Microtrac-Bell Corporation. From the obtained nitrogen adsorption isotherm, the total pore volume, specific surface area, pore diameter standard deviation, mesopore volume, and mesopore volume ratio were calculated using the BJH method. In addition, the log differential pore volume distribution was determined from the results of the nitrogen adsorption and desorption measurements. The results are shown in Figure 1. In Figure 1, Dp represents the pore diameter, and dVp / dlogDp represents the log differential pore volume.

[0061] <Measurement of Nitrogen Content> The nitrogen content and carbon content of the obtained carbon material were measured by SEM-EDX measurement using a tabletop microscope Miniscope® TM4000Plus manufactured by Hitachi High-Tech Corporation at an acceleration voltage of 15 kV. The N / C ratio was determined by dividing the amount of nitrogen atoms by the amount of carbon atoms. In addition, the carbon material was subjected to XPS N1s spectrum measurement using an X-ray photoelectron spectrometer AXIS ULTRA2 manufactured by Shimadzu Corporation, and the proportion of active nitrogen was determined by peak separation of the N1s spectrum.

[0062] <Evaluation Method> <Production of Capacitor Electrode Containing Carbon Material> 80 parts by mass of the obtained carbon material, 10 parts by mass of a conductive additive (Ketjen Black), 5 parts by mass of an aqueous binder, 5 parts by mass of a thickener (carboxymethyl cellulose), and 100 parts by mass of pure water were mixed to obtain a paste-like material composition. The obtained material composition was applied to aluminum foil and dried under reduced pressure at 120°C for 1 hour to obtain a capacitor electrode.

[0063] <Evaluation of Capacitor Electrode Capacitance> The obtained capacitor electrodes were placed opposite each other with a separator interposed therebetween, and an organic electrolyte solution (1 M lithium tetrafluoroborate polycarbonate solution) was poured into the electrodes. Charge / discharge measurements were carried out in the range of 0 to 2.5 V to determine the capacitance. The capacitance of each example was shown, with the capacitance of Example 1 being taken as 100%.

[0064] <Evaluation of the amount of metal adsorption onto the carbon material> One part by mass of the obtained carbon material was dispersed in 100 parts by mass of ethanol to prepare a carbon-dispersed ethanol solution. Furthermore, 1 part by mass of a chloroplatinic acid aqueous solution was dissolved in 2,000 parts by mass of pure water, and 0.8 parts by mass of the chloroplatinic acid aqueous solution was added. The mixture was stirred at room temperature for 24 hours, allowing platinum ions to be adsorbed onto the carbon material. The metal filtrate and the metal-adsorbed carbon material were then separated by suction filtration, and the amount of metal contained in the resulting metal filtrate was measured by ICP-MS. The ICP-MS analysis was performed using an Agilent 8900 manufactured by Agilent Technologies.

[0065] (Example 2) A carbon material was obtained in the same manner as in Example 1, except that the B / A ratio was set to 1.5 in Production Example 1. The log differential pore volume distribution and the capacitance of the capacitor electrode of the obtained carbon material were measured.

[0066] Comparative Example 1 Except for using activated carbon that had been activated instead of the carbon material, a carbon material was obtained in the same manner as in Example 1. The obtained carbon material was evaluated for its log differential pore volume distribution, the capacitance of the capacitor electrode, and the amount of metal adsorption onto the carbon material.

[0067] Comparative Example 2 A carbon material was obtained in the same manner as in Example 1, except that a commercially available MOF (manufactured by Aldrich under the trade name "Z1200", ZIF-8) was used instead of MOF-1. The obtained carbon material was evaluated for the log differential pore volume distribution, the capacitance of the capacitor electrode, and the amount of metal adsorption onto the carbon material.

[0068] Comparative Example 3 MOF-1' was obtained in the same manner as in Production Example 1, except that terephthalic acid was used as the organic bridging ligand and dimethylformamide (DMF) was used as the solvent. A carbon material was obtained in the same manner as in Example 1, except that MOF-1' was used instead of MOF-1. The capacitance of a capacitor electrode made of the obtained carbon material was measured.

[0069] Comparative Example 4 MOF-2' was obtained in the same manner as in Production Example 1, except that 4-fluoroimidazole (nitrogen=33 at %, fluorine=17 at %, manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the organic bridging ligand. A carbon material was obtained in the same manner as in Example 1, except that MOF-2' was used instead of MOF-1. The obtained carbon material was evaluated for the capacitance of the capacitor electrode and the amount of metal adsorption onto the carbon material.

[0070]

[0071] As shown in Table 1, Examples 1 and 2 to which the present invention was applied had a performance ratio of 100 to 140%. The "performance ratio" in Table 1 indicates the capacitance rate of each example when the capacitance of the capacitor electrode of Example 1 is taken as 100%. The performance ratio of Comparative Example 1, in which the nitrogen content was 0 at %, was 62.7%. The nitrogen content was 20.4 at % and the specific surface area was 844 m 2 / g, mesopore volume 0.07 cm 3 The performance ratio of Comparative Example 2, in which the nitrogen content was 0 at% / g, was 29%. The performance ratio of Comparative Example 3, in which the nitrogen content was 0 at% was 70%. The performance ratio of Comparative Example 4, in which the nitrogen content was 8.6%, was 80%. These results confirmed that the application of the present invention can improve high-rate cycle characteristics. Furthermore, Example 1, in which the present invention was applied, had an adsorption amount of metal of 0.32 mass%. In contrast, the adsorption amount of metal of Comparative Example 1, in which the nitrogen content was 0 at% was 0.04 mass%. Furthermore, the performance ratio of Comparative Example 2, in which the nitrogen content was 20.4 at% and the specific surface area was 844 m 2 / g, mesopore volume 0.07 cm 3 In Comparative Example 2, where the nitrogen content was 1.0% by mass, and Comparative Example 4, where the nitrogen content was 8.6%, the metal adsorption amounts were 0.02% by mass and 0.10% by mass, respectively. These results demonstrate that when the carbon material of the present invention is used as a catalyst support, it is possible to significantly improve the catalyst support amount.

Claims

1. A porous body containing nitrogen, the nitrogen content is 9 at% or more, and the mesopore volume is 0.30 cm 3 / g or more, and the specific surface area is 700 m 2 / g or more.

2. The carbon material according to claim 1, wherein the standard deviation of the mesopore diameter is 7 to 10.

3. The carbon material according to claim 1, wherein the molar ratio represented by [moles of nitrogen] / [moles of carbon] is 0.1 to 0.

3.

4. The carbon material according to claim 1, wherein the ratio of the number of moles of active nitrogen to the total number of moles of nitrogen is 20 to 80%.

5. The carbon material according to claim 1, which is in the form of a powder and has an average primary particle size of 25 to 3,000 nm.

6. The carbon material according to claim 1, which supports at least one selected from the group consisting of metals and metal oxides.

7. The carbon material according to claim 1, which has an organic substance supported thereon.

8. The carbon material according to claim 1, which has a metal-organic framework supported thereon.

9. A material composition comprising the carbon material according to any one of claims 1 to 8.

10. The material composition according to claim 9, which is an electrode material, a separator, a sensor material, a spacer material, a reinforcing material, a gas adsorbent, a liquid adsorbent, an ion adsorbent, a solid adsorbent, a catalyst support, an electromagnetic wave-related material, or an energy storage material.

11. A method for producing a carbon material according to any one of claims 1 to 8, comprising the step of calcining a raw material composition containing a nitrogen-containing metal organic framework.

Citation Information

Patent Citations

  • Preparation method of nitrogenous porous carbon

    CN103626150A

  • Preparation method of high-specific surface area nitrogen-rich classified porous carbon electrode material for supercapacitor

    CN108584944A

  • Nitrogen-containing porous carbon material, method for producing same, and electric double layer capacitor using the nitrogen-containing porous carbon material

    WO2011065484A1

Cited By

  • Organometallic compounds, methods for producing the same, and carbon materials

    JP2026157759A

  • Carbon materials

    JP2026157850A