Polyester-based shrink film

The use of motion capture technology in polyester shrink films allows for precise control and measurement of heat shrinkage rates, addressing the issue of uneven shrinkage and wrinkles on non-circular containers by ensuring uniform heat distribution and accurate measurement.

WO2024204502A1PCT designated stage expired Publication Date: 2024-10-03C I TAKIRON CORP +1

Patent Information

Application Number
PCT/JP2024/012579
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional polyester shrink films face challenges in achieving uniform heat shrinkage rates, leading to wrinkles and color unevenness on non-circular, complex-shaped containers like PET bottles, due to variations in heat distribution and measurement inaccuracies.

Method used

A polyester shrink film with a predetermined heat shrinkage rate is produced using motion capture technology, which sets measurement positions and calculates the shrinkage rate based on distance changes measured by inertial sensors and infrared light, ensuring a standard deviation of 15% or less and thickness variation within 10 μm, allowing for precise control of heat shrinkage characteristics.

Benefits of technology

This approach enables quick and accurate measurement and control of heat shrinkage rates, reducing wrinkles and ensuring uniform shrinkage across the film, enhancing the film's applicability to complex container shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012579_03102024_PF_FP_ABST
    Figure JP2024012579_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a polyester-based shrink film having a predetermined heat shrinkage rate in a main shrinkage direction etc. as measured using motion capture. The polyester-based shrink film having a predetermined heat shrinkage rate as measured using motion capture is characterized in that, when two measurement positions are set in the main shrinkage direction, the distance between the two measurement positions is L, and the distance measured using motion capture after heat shrinkage is L'1, the heat shrinkage rate (temperature: 70-98°C, time: 1-60 seconds), based on the distance between L1 and L'1 etc., in the main shrinkage direction is 20% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester shrink film

[0001] The present invention relates to a polyester shrink film, and more particularly to a polyester shrink film having a predetermined thermal shrinkage rate, etc., which is measured quickly and accurately using motion capture.

[0002] Conventionally, shrink films have been widely used as base films for labels on PET bottles and the like. Polyester-based resins, in particular, are widely used due to their excellent transparency and strength. These shrink films are thermally shrunk by passing them through a tunnel that generates hot air or steam, and then attached to a container. However, shrinkage variations (unevenness) may occur during the heat shrinkage, resulting in wrinkles and color unevenness. Therefore, various heat-shrinkable polyester films have been proposed to prevent wrinkles and color unevenness due to shrinkage variations (unevenness) during the heat shrinkage.

[0003] For example, a heat-shrinkable polyester film has been proposed in which the proportion of alcohol components other than ethylene glycol is controlled, or the amount of naphthalenedicarboxylic acid component or alkali metal salt of sulfobenzenedicarboxylic acid is strictly controlled within the total acid components (see Patent Document 1). More specifically, the polyester resin is characterized in that the proportion of acid components other than terephthalic acid (A mol %) within the total acid components and the proportion of alcohol components other than ethylene glycol (B mol %) within the total alcohol components are in the range of 5 mol %≦A+B≦40 mol %, and the total acid components contain 1 to 30 mol % of naphthalenedicarboxylic acid component and 0.3 to 3 mol % of alkali metal salt of sulfobenzenedicarboxylic acid. The heat shrinkage rate of such a polyester film is preferably 5% or more in the longitudinal direction of the film when immersed in hot water at 60°C for 60 seconds, and 30% or more when immersed in hot water at 80°C for 60 seconds.

[0004] Furthermore, a heat-shrinkable polyester film has been proposed in which the amount of amorphous components in the total polyester resin components is strictly controlled, and the hot water heat shrinkage rate at 80°C and 90°C in the longitudinal direction of the film and the hot water heat shrinkage rate at 90°C in the width direction of the film are limited (see Patent Document 2). More specifically, this heat-shrinkable polyester film contains ethylene terephthalate as a main component and one or more monomer components that can become amorphous components in the total polyester resin components, the total amount of which is 15 mol% or more. The hot water heat shrinkage rate of the polyester film in the longitudinal direction of the film is 30% or more when treated at 80°C for 10 seconds, and 40% or more when treated at 90°C for 10 seconds, and the hot water shrinkage rate in the width direction of the film is 10% or less when treated at 90°C for 10 seconds.

[0005] Also proposed is a heat-shrinkable polyester film that specifies the heat shrinkage rate in one direction and the heat shrinkage rate in the direction perpendicular thereto, and that has a predetermined range of average heat shrinkage rate coefficient in a temperature range of 70 to 120°C (see Patent Document 3). More specifically, the heat-shrinkable polyester film is a homopolymer of polyethylene terephthalate or a copolymer containing a dicarboxylic acid component other than terephthalic acid, and / or a diol component other than ethylene glycol, and / or an oxycarboxylic acid. The heat shrinkage rate in at least one direction is 30% or more, and the average heat shrinkage rate coefficient in at least that direction in a temperature range of 70 to 120°C is in the range of 0.1 to 0.5% / sec·°C.

[0006] A shrink label has also been proposed that specifies the maximum heat shrinkage rate measured under specified conditions (see Patent Document 4). More specifically, it is a heat-shrinkable shrink label that includes at least one film layer containing a polylactic acid polymer as an essential component and a printed layer. The label is characterized by a heat shrinkage rate in the main orientation direction of 3 to 23% 1 second after the start of heat shrinkage in 75°C hot water, and a heat shrinkage rate in the main orientation direction of 40 to 84% at 90°C for 10 seconds. Alternatively, the label is characterized by a maximum heat shrinkage rate in the main orientation direction of 7 to 40% / second in 75°C hot water, and a heat shrinkage rate in the main orientation direction of 40 to 84% at 90°C for 10 seconds.

[0007] JP 08-027259 A (claims, etc.) JP 2007-016120 A (claims, etc.) JP 8-323859 A (claims, etc.) JP 2008-1098 A (claims, etc.)

[0008] However, in the heat-shrinkable films described in Patent Documents 1 and 2, although the heat shrinkage rate at a predetermined temperature and in a predetermined shrinkage direction is limited to a predetermined range, it is necessary to measure the film by immersing it in warm water and then removing it from the warm water, which can easily cause uneven heat distribution and large variations in the measured values. Therefore, it is difficult to obtain a polyester film having a desired heat shrinkage rate from a polyester film having a heat shrinkage rate measured in this way, and it is sometimes difficult to control the heat shrinkage rate characteristics quickly and accurately. Therefore, particularly in the case of PET bottles in which the bottle diameter of the body is not uniform and the horizontal cross-sectional shape of the body is not circular in some parts but has a complex shape, the heat shrinkability is likely to be uneven, which has caused a problem that it is extremely difficult to suppress the occurrence of fine wrinkles.

[0009] Furthermore, in the heat-shrinkable film described in Patent Document 3, although the amount of change in the heat shrinkage rate with time is specified, the heat shrinkage rate coefficient (% / (sec·°C)) averaged before and after heat shrinkage is specified, and there is no intention to measure the heat shrinkage rate (mm / sec) from before heat shrinkage until a predetermined time, let alone its maximum value. Therefore, it was not possible to accurately measure the heat shrinkage rate (mm / sec) at a timing when the heat-shrinkable film changes significantly in a short period of time during heat shrinkage.

[0010] Furthermore, the shrink label described in Patent Document 4 specifies the heat shrinkage rate (%) one second after the start of heat shrinkage, but this is a heat shrinkage rate limited to a certain time period, and no attempt is made to apply it to shrink labels with different heat shrink timing. Furthermore, while the maximum heat shrinkage rate (% / sec) is also mentioned, this is a measurement of the actual instantaneous heat shrinkage rate measured at 0.1-second intervals, and there is no intention to measure the maximum heat shrinkage rate (mm / sec) from before heat shrinkage until a specified time. Therefore, when converted to the maximum heat shrinkage rate from before heat shrinkage until a specified time, it is limited to a very narrow range.

[0011] The inventors of the present invention have therefore discovered that heat shrinkage properties can be controlled quickly and accurately by measuring the heat shrinkage rate in the main shrinkage direction, etc. using motion capture and controlling the value, and have completed the present invention. That is, an object of the present invention is to provide a polyester shrink film having a predetermined heat shrinkage rate in the main shrinkage direction, etc., which can be measured quickly and accurately using a predetermined simple measurement method.

[0012] The present invention provides a polyester shrink film having a predetermined heat shrinkage rate, which is obtained using motion capture. Two measurement positions are set in the TD direction, which is the main shrinkage direction of the polyester shrink film as the object to be measured, the distance between the two measurement positions is L1, and the distance between the two measurement positions after the polyester shrink film has been heat-shrunk is L'1, as measured using motion capture. This polyester shrink film has a heat shrinkage rate in the main shrinkage direction of the polyester shrink film (temperature: 70 to 98°C, time: 1 to 60 seconds) of 20% or more, as calculated according to the following formula (1), thereby solving the above-mentioned problems.

[0013]

[0014] That is, by using motion capture and corresponding inertial sensors and infrared light to measure the distance traveled at a specific location, the thermal shrinkage rate at the specific location can be calculated quickly and accurately.

[0015] Furthermore, in constructing the polyester shrink film of the present invention, it is preferable to set the standard deviation of the heat shrinkage percentage to 15% or less, because by controlling the standard deviation of the heat shrinkage percentage in this way, the heat shrinkage percentage of the polyester shrink film can be controlled more accurately.

[0016] In forming the polyester shrink film of the present invention, it is preferable that the thickness of the polyester shrink film be in the range of 10 to 200 μm, and that the difference between the maximum thickness and the average thickness be within 10 μm. By controlling the thickness of the polyester shrink film in this way, the difference between the maximum thickness and the average thickness in the transverse direction becomes small, and thus the thermal shrinkage rate in the transverse direction can be controlled more quickly and accurately.

[0017] In addition, when constructing the polyester shrink film of the present invention, it is preferable to set two measurement positions at multiple locations and use the average of the heat shrinkage values ​​in the TD direction obtained at the multiple locations as the heat shrinkage value in the TD direction. By calculating the heat shrinkage values ​​in the TD direction at multiple locations in this way, the heat shrinkage value in the TD direction can be controlled more quickly and accurately.

[0018] Furthermore, when constructing the polyester shrink film of the present invention, it is preferable that the motion capture device is an image-based motion capture device that detects information from predetermined markers. By selecting and using an image-based motion capture device from various types of motion capture devices, the positions of the predetermined markers can be calculated efficiently, allowing the thermal shrinkage rate to be measured quickly and accurately.

[0019] In constructing the polyester shrink film of the present invention, it is preferable that the motion capture device is equipped with a camera for recording the thermal shrinkage state of the polyester shrink film. By taking into consideration image data showing the thermal shrinkage state captured by the camera, the state of thermal shrinkage in the TD direction can be accurately confirmed, and the thermal shrinkage rate in the TD direction can be measured more quickly and accurately.

[0020] In preparing the polyester shrink film of the present invention, the heat shrinkage rate of the polyester shrink film is preferably measured using at least one heat shrinkage device selected from the group consisting of a thermostatic bath, a steam bath, a hot water bath, a fluorine-containing liquid bath, and an infrared irradiation device. By measuring using such a heat shrinkage device, the heat shrinkage rate can be controlled more quickly, accurately, and simply depending on the intended use of the polyester shrink film.

[0021] Furthermore, in constructing the polyester-based shrink film of the present invention, the direction perpendicular to the main shrinkage direction of the polyester-based shrink film to be measured is defined as the MD direction, and the heat shrinkage in the MD direction is preferably measured using motion capture at the same time as measuring the heat shrinkage in the TD direction, and the heat shrinkage in the MD direction is preferably set to a value within the range of -5 to 5%. By simultaneously measuring the heat shrinkage in the MD direction using motion capture in this way, the heat shrinkage properties of the polyester-based shrink film when actually used can be controlled depending on the application, etc. of the polyester-based shrink film.

[0022] In preparing the polyester shrink film of the present invention, it is preferable to prepare a calibration curve in advance showing the relationship between the heat shrinkage temperature and heat shrinkage time in the main shrinkage direction of the polyester shrink film to be measured and the heat shrinkage percentage in the TD direction, and then compare and verify the calibration curve with the heat shrinkage percentage obtained based on the formula (1), so that the heat shrinkage percentage obtained based on the formula (1) is within ±10% of the heat shrinkage percentage in the TD direction obtained from the calibration curve. By comparing the measured heat shrinkage percentage with the previously prepared calibration curve, a polyester shrink film can be obtained that has a heat shrinkage percentage, etc. that is more rapid, accurate, and reproducible, even when motion capture is used.

[0023] FIGS. 1(a) to 1(c) are diagrams illustrating the configuration of polyester-based shrink films. FIGS. 2(a) to 2(c) are diagrams illustrating a method for measuring the thermal shrinkage of polyester-based shrink films using motion capture or the like. FIGS. 3(a) to 3(b) are diagrams illustrating the positional movement of a predetermined marker accompanying the thermal shrinkage of a polyester-based shrink film. FIGS. 4(a) to 4(b) are diagrams illustrating a method for measuring the thermal shrinkage rate of polyester-based shrink films using motion capture or the like. FIGS. 5(a) to 5(c) are diagrams illustrating an example of the configuration of a fixture used in measuring the thermal shrinkage rate using motion capture. FIGS. 6(a) to 6(b) are diagrams illustrating the thermal shrinkage rate and thermal shrinkage rate. FIG. 7 is a diagram illustrating the relationship between time (seconds) and the change in distance (mm) in a predetermined section for the polyester-based shrink films of Examples 1 and 2 and Comparative Examples 2 and 3. Figures 8(a) and 8(b) are diagrams illustrating the relationship between time (seconds) and heat shrinkage rate (mm / sec) for the polyester shrink films of Examples 1 and 2, and Figure 8(c) is a diagram illustrating the relationship between time and heat shrinkage rate (% / sec). Figures 9(a) and 9(b) are diagrams illustrating the relationship between time (seconds) and heat shrinkage rate (mm / sec) for the polyester shrink films of Comparative Examples 2 and 3, and Figure 9(c) is a diagram illustrating the relationship between time and heat shrinkage rate (% / sec). Figure 10(a) is a diagram illustrating the relationship between time (seconds) and intermediate heat shrinkage rate (mm / sec) for the polyester shrink film of Example 1, and Figure 10(b) is a diagram illustrating the relationship between time and intermediate heat shrinkage rate (% / sec). FIG. 11(a) is a diagram illustrating the relationship between time (seconds) and intermediate heat shrinkage rate (mm / second) for the polyester shrink film of Example 2, and FIG. 11(b) is a diagram illustrating the relationship between time and intermediate heat shrinkage rate (% / second).Fig. 12(a) is a diagram illustrating the relationship between time (seconds) and the intermediate heat shrinkage speed (mm / sec) for the polyester shrink film of Comparative Example 2, and Fig. 12(b) is a diagram illustrating the relationship between time and the intermediate heat shrinkage rate (% / sec). Fig. 13(a) is a diagram illustrating the relationship between time (seconds) and the intermediate heat shrinkage speed (mm / sec) for the polyester shrink film of Comparative Example 3, and Fig. 13(b) is a diagram illustrating the relationship between time and the intermediate heat shrinkage rate (% / sec). Fig. 14(a) is a diagram illustrating multiple measurement samples (W, C, E) taken along the TD direction from a roll of polyester shrink film, and Fig. 14(b) is a diagram illustrating the state in which a motion capture device is attached to one of the measurement samples (W, C, E). Fig. 15 is a diagram illustrating the relationship between the immersion time in 95°C water for 1 to 20 seconds and the thermal shrinkage (%) in the TD direction measured using motion capture for Example 1 (line A) and Comparative Example 1 (line B). Fig. 16 is a diagram illustrating the relationship between the thickness (μm) of a polyester shrink film when immersed in 95°C water for 20 seconds and the thermal shrinkage (%) in the TD direction measured using motion capture. Fig. 17(a) is a diagram (photograph) illustrating the appearance of a cylindrical label corresponding to Example 1 when no wrinkles have occurred, and Figs. 17(b) to (d) are enlarged views of the appearance regions P, Q, and R shown in Fig. 17(a). Figure 18(a) corresponds to Comparative Example 1 and is a diagram (photograph) showing the appearance of a cylindrical label when wrinkles occur, and Figures 18(b) to (d) are enlarged views of the appearance areas S, T, and U shown in Figure 18(a).

[0024] [First Embodiment] The first embodiment is a polyester shrink film 10 as shown in Fig. 1, which has a predetermined heat shrinkage rate and is measured using a motion capture device 14 as shown in Figs. 2(a) to (c). As shown in Fig. 3, two measurement positions are set in the TD direction, which is the main shrinkage direction of the polyester shrink film as the object to be measured. The distance between the two measurement positions is L1. After the polyester shrink film has been heat-shrunk, the distance between the two measurement positions is L'1, measured using the motion capture device. The polyester shrink film has a heat shrinkage rate in the main shrinkage direction (temperature: 70 to 98°C, time: 1 to 60 seconds) of 20% or more, as calculated according to the following formula (1):

[0025]

[0026] Hereinafter, the polyester shrink film of the first embodiment will be specifically described by dividing it into its components and the like, with reference to the drawings as appropriate.

[0027] 1. Polyester Resin The polyester resin constituting the polyester shrink film of the first embodiment may be of any type, but is typically preferably a polyester resin composed of a polyalcohol and a dicarboxylic acid, a polyester resin composed of a polyalcohol and a hydroxycarboxylic acid, a polyester resin composed of a polyalcohol dicarboxylic acid and a hydroxycarboxylic acid, or a mixture of these polyester resins.

[0028] Here, examples of the polyalcohol, which is a compound component of the polyester resin, include at least one diol such as an aliphatic diol such as ethylene glycol, diethylene glycol, propanediol, butanediol, neopentyl glycol, or hexanediol, an alicyclic diol such as 1,4-hexanedimethanol, or an aromatic diol. Therefore, among these, ethylene glycol, diethylene glycol, and 1,4-hexanedimethanol are particularly preferred.

[0029] Furthermore, it is more preferable to use a mixture containing at least ethylene glycol as the polyalcohol. By limiting the type of polyalcohol, which is one of the polymerization components of the polyester resin, in this way, it is possible to adjust the proportion of the amorphous portion and, ultimately, obtain good wearability. Furthermore, when preparing a mixture containing a predetermined amount of ethylene glycol, it is preferable to use at least one other polyalcohol, such as a diol having an alicyclic structure (e.g., 1,4-cyclohexanedimethanol), an aliphatic diol (e.g., diethylene glycol, propanediol, butanediol, neopentyl glycol, or hexanediol), or an aromatic diol, in combination with ethylene glycol. This is because the use of such a polyalcohol allows for an appropriate reaction with the polycarboxylic acid, making it easier to obtain an amorphous polyester resin with at least controlled crystallinity / amorphousness.

[0030] Similarly, examples of dicarboxylic acids as a compound component of polyester resins include at least one of aliphatic dicarboxylic acids such as adipic acid, sebacic acid, and azelaic acid; aromatic dicarboxylic acids such as terephthalic acid, naphthalenedicarboxylic acid, and isophthalic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and ester-forming derivatives thereof. Among these, terephthalic acid is particularly preferred. Similarly, examples of hydroxycarboxylic acids as a compound component of polyester resins include at least one of lactic acid, hydroxybutyric acid, and polycaprolactone.

[0031] Furthermore, it is also preferable to use a non-crystalline polyester resin in part or in whole as the polyester resin. For example, a non-crystalline polyester resin composed of a dicarboxylic acid containing at least 80 mol% of terephthalic acid and a diol containing 50 to 80 mol% of ethylene glycol and 20 to 50 mol% of one or more diols selected from 1,4-cyclohexanedimethanol, neopentyl glycol, and diethylene glycol can be suitably used. If necessary, other dicarboxylic acids and diols, or hydroxycarboxylic acids, may be used to change the properties of the film. Furthermore, each of these may be used alone or in combination.

[0032] On the other hand, examples of crystalline polyester resins include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polybutylene naphthalate, and polypropylene terephthalate, and these may be used alone or in combination.

[0033] Furthermore, when the polyester resin is a mixture of an amorphous polyester resin and a crystalline polyester resin, it is also preferable to blend a predetermined amount of the amorphous polyester resin with the resin constituting the polyester shrink film in order to obtain good heat resistance, shrinkage rate, etc. That is, the blending amount of the amorphous polyester resin relative to the total amount (100% by weight) of the resin constituting the polyester shrink film is usually preferably in the range of 70 to 100% by weight, more preferably in the range of 80 to 98% by weight, and even more preferably in the range of 85 to 95% by weight.

[0034] 2. Heat Shrinkage Rate Measured Using Motion Capture (1) Basic Configuration The heat shrinkage rate in the main shrinkage direction measured using motion capture is typically calculated from the distance traveled by measuring at least two measurement positions in the TD direction, the main shrinkage direction of the polyester shrink film being measured, before and after heat shrinkage using an inertial sensor or optical techniques. That is, the change in the distance between the two measurement positions is measured using an inertial sensor or infrared light corresponding to the motion capture, and the heat shrinkage rate is calculated from this distance. More specifically, the distance between the two measurement positions is designated L1, and the distance between the two measurement positions after heat shrinkage under predetermined heat shrinkage conditions at a predetermined heat shrinkage temperature and for a predetermined heat shrinkage time is measured using motion capture, and this distance is designated L'1. The heat shrinkage rate is then calculated based on the above-mentioned formula (1). The polyester shrink film of the present invention is characterized in that the predetermined heat shrinkage rate (temperature: 70 to 98°C, time: 1 to 60 seconds) is 20% or greater. The reason for this is that the heat shrinkage characteristics of the polyester shrink film can be controlled quickly and accurately by having such a predetermined heat shrinkage ratio. Therefore, the predetermined heat shrinkage ratio (temperature: 70 to 98°C, time: 1 to 60 seconds) is preferably set to a value of 30 to less than 95%, more preferably a value of 40 to less than 90%, and even more preferably a value of 50 to less than 85%.

[0035] The value of the distance L1 (mm) between the two measurement positions is preferably selected appropriately depending on the size of the polyester shrink film, the type of motion capture, etc., but is preferably set to a value within the range of 3 to 300 mm, for example. The reason for this is that such a distance allows the difference in distance between the film before and after shrinkage to be clearly recognized, allowing for faster and more accurate measurement of the thermal shrinkage rate in the TD direction. Therefore, it is more preferable to set the distance L1 (mm) between the measurement positions to a value within the range of 5 to 100 mm, and even more preferably to a value within the range of 8 to 30 mm.

[0036] The measurement positions are provided on the polyester shrink film to indicate coordinate position information for measuring the behavior of the polyester shrink film during thermal shrinkage. That is, as shown in Figures 4(a) and 4(b), a predetermined section M between two measurement positions is preferably marked with a predetermined marker such as a dot, line, cross, circle, arrow, L-shape, T-shape, or check mark. This configuration allows the shrinkage of the polyester shrink film to be easily observed from the surrounding area.

[0037] (2) Thickness Variation It has also been found that the thermal shrinkage rate in the transverse direction measured using motion capture can be affected by the thickness of the polyester-based shrink film. Therefore, it is preferable to set the thickness of the polyester-based shrink film in the range of 10 to 200 μm, and to set the difference between the maximum thickness and the average thickness (hereinafter sometimes referred to as thickness variation) within 10 μm. The reason for this is that by controlling the thickness and thickness variation of the polyester-based shrink film, it becomes easier to control the thermal shrinkage rate in the transverse direction, and ultimately, the thermal shrinkage rate in the transverse direction can be controlled more quickly and accurately.

[0038] However, if the thickness variation is too small, the manufacturing yield will be extremely low, which may be economically disadvantageous. Therefore, it is more preferable to set the thickness variation to a value within the range of 0.01 to 5 μm, and even more preferable to set it to a value within the range of 0.1 to 3 μm. The thickness of polyester shrink films is usually within the range of 10 to 200 μm, but it is more preferable to set it to a value within the range of 20 to 100 μm, and even more preferable to set it to a value within the range of 30 to 60 μm.

[0039] Furthermore, it is preferable to calculate the thickness variation of a polyester shrink film by selecting multiple different locations (e.g., n = 3 to 30 locations) on the same film and measuring the maximum and average thicknesses. This is because calculating the thickness in this manner allows for faster and more accurate evaluation of the film. Therefore, it is more preferable to select 4 to 20 different measurement locations on the same film, and even more preferable to select 5 to 10 measurement locations.

[0040] (3) Heat Shrinkage at Multiple Locations It is also preferable to set multiple distances between two measurement locations, calculate the thermal shrinkage in the TD direction at the multiple locations, and use the average value as the heat shrinkage in the TD direction. That is, it is preferable to select multiple different locations (e.g., n = 3 to 30 locations) on the same film, and use the average of the measured heat shrinkages (temperature: 70 to 98°C, time: 1 to 60 seconds) as the heat shrinkage in the TD direction. This is because calculating the heat shrinkage in the TD direction at multiple locations allows for more rapid and accurate measurement of the heat shrinkage in the TD direction. Therefore, it is more preferable to select at least 4 to 20 measurement locations, and even more preferable to select 5 to 10 measurement locations, in the TD direction of a polyester shrink film.

[0041] (4) Standard Deviation of Thermal Shrinkage in the TD (σ1) Furthermore, when a polyester shrink film is heat-shrunk at a predetermined temperature for a predetermined time, it is preferable that the standard deviation of the thermal shrinkage in the TD be within 15%. This is because such a standard deviation allows for more accurate control of the thermal shrinkage of the polyester shrink film. Therefore, it is more preferable that the standard deviation of the thermal shrinkage in the TD be within 10%, and even more preferable that it be within 5%.

[0042] (5) Motion Capture 1) Basic Configuration The interval between measurement positions on a polyester shrink film is preferably calculated based on position information of the measurement positions obtained by motion capture. This is because the use of such motion capture allows the interval between measurement positions on the film to be quickly and accurately acquired as digital data. Here, motion capture is a technology for converting the movement of a measurement target into digital data, and is primarily a technology for tracking the position of a predetermined marker on the measurement target and recording it as coordinate data.

[0043] Specifically, the type of motion capture is not particularly limited, but any of the following motion captures can be used: image-based motion capture, inertial-based motion capture, optical-based motion capture, or a combination of these. However, in the case of polyester shrink film, since it is heat-treated by immersion in warm water or the like, there are many spatial limitations, and it is easier to make the device smaller and simpler, so it can be said that it is more preferable to use image-based or inertial-based motion capture.

[0044] Therefore, as shown in FIG. 2( a), it is preferable to use an optical camera as an image-based motion capture device 14 to capture video of the polyester shrink film 10 being measured during thermal shrinkage, and then image-analyze the captured data to measure the thermal shrinkage rate. That is, it is preferable to first mark the polyester shrink film with multiple scales (e.g., 2 to 30 scales) spaced at intervals L1 using a predetermined marker such as an oil-based marker. Next, it is preferable to place the polyester shrink film on a flat surface, and then capture video before and after thermal shrinkage from vertically above using an optical camera. Furthermore, it is preferable to calculate the spacing between each scale before thermal shrinkage from the captured video data based on the relationship between the number of pixels and actual measurements, and then use the average value to determine the thermal shrinkage rate. Specifically, for example, in an embodiment where scales are lined up on the left and right, it is preferable to draw a horizontal imaginary line that intersects with each scale, and use the point where the scale and the imaginary line intersect as the measurement position. The reason for this is that by continuously recording the thermal shrinkage state as video data, the thermal shrinkage rate in the TD direction can be measured more quickly, accurately, and efficiently. Furthermore, by recording in this manner, even in cases where there are many spatial limitations, the device can be made smaller and simpler, and the thermal shrinkage rate can be measured more efficiently. The type of the predetermined marker may be any type that is easily visible to an optical camera, but it is preferable that it be composed of, for example, an oil-based marker, a groove, or the like.

[0045] Furthermore, the motion capture is preferably configured as an inertial position measurement device that can obtain acceleration, angular velocity, and orientation information from an inertial sensor attached to a polyester shrink film using a device such as an IMU, and accurately identify the position (center of gravity, etc.) of the marker. In other words, it is preferable for the motion capture to be an inertial type motion capture device equipped with a 9-axis inertial sensor that combines an accelerometer and an angular velocity meter (gyro sensor), or further, a combination of these with a geomagnetometer.

[0046] On the other hand, it is also preferable to use optical motion capture as the motion capture. That is, it is preferable that the motion capture is a type of optical position measurement device that irradiates radiation such as infrared rays toward an optical marker (such as a retroreflective marker) and detects the reflected light. Such motion capture performs predetermined image processing based on the obtained reflected light and can identify the position (center of gravity, etc.) of the marker in two dimensions. Furthermore, by using multiple motion captures in combination, it is a measurement device that can identify the position in three dimensions.

[0047] 2(b)-(c), it is preferable to use predetermined optical cameras 14a and 14b in combination with the inertial motion capture device 14 to capture images of the heat shrinkage state of the polyester shrink film 10, and use the captured images as image data for reference when measuring the heat shrinkage rate. This is because continuously recording the heat shrinkage state in combination with the camera images makes it possible to confirm the heat shrinkage state in the TD direction as image data, thereby enabling more efficient and accurate measurement of the heat shrinkage rate in the TD direction. More specifically, it is preferable to prepare one or more optical cameras and capture image data of the heat shrinkage state of the polyester shrink film from the front, side, top, back, or oblique direction of the polyester shrink film as the object to be measured.

[0048] 3) Heat Shrinkage Conditions The heat shrinkage temperature is preferably set to a value within the range of 70 to 98°C and the heat shrinkage time is preferably set to a value within the range of 1 to 60 seconds. This is because such heat shrinkage conditions allow for easy comparison and verification with the heat shrinkage characteristics of polyester shrink films when actually used. Therefore, because these heat shrinkage conditions approximate actual heat shrinkage conditions and can be measured in a relatively short time, it is more preferable to set the heat shrinkage temperature to a value within the range of 75 to 95°C and the heat shrinkage time to a value within the range of 5 to 30 seconds, and even more preferable to set the heat shrinkage temperature to a value within the range of 80 to 90°C and the heat shrinkage time to a value within the range of 8 to 15 seconds. Furthermore, it has been found that when the accuracy of motion capture is improved, the heat shrinkage rate of polyester shrink films can be measured accurately even within the range of 1 to 5 seconds or even within the range of 1 to 3 seconds.

[0049] 4) Heat Shrinkage Device The heat shrinkage device is preferably at least one of a thermostatic bath (oven), a steam bath, a hot water bath, a hot air heater, a liquid bath of a fluorine-containing compound, a vapor bath of a fluorine-containing compound, and an infrared irradiation device. The reason for this is that when motion capture is used, various types of heat shrinkage devices such as these can be used depending on the application of the polyester shrink film, and thus the heat shrinkage rate can be measured more quickly, accurately, and simply.

[0050] As an example, it is preferable to use a hot water bath as the heat shrinkage device. This is because the use of such a heat shrinkage device makes it easy to maintain a constant hot water temperature, allowing for more precise control of the heat shrinkage temperature. Furthermore, using a hot water bath allows the polyester shrink film to be floated and heated evenly in a flat manner, making it easier to capture the behavior of the polyester shrink film during heat shrinkage from above using an optical camera or the like.

[0051] Specifically, when a single motion capture is used, the thermal shrinkage rate can be measured and calculated from two-dimensional measurement points, but when multiple motion captures are used, there is an advantage that the positional relationship of three-dimensional measurement points can be measured, and then the thermal shrinkage rate can be measured and calculated.

[0052] For example, when a flat hot plate is used as the heat shrinkage device, the heat shrinkage can be measured easily and quickly in three dimensions not only in the horizontal direction but also when it is tilted along the direction of gravity or even when it is placed vertically so as to be parallel to the direction of gravity. Therefore, when a single or multiple motion capture devices are used, various heat shrinkage devices can be used, and therefore the heat shrinkage can be measured more easily and quickly depending on the application of the polyester shrink film.

[0053] As another example, it is preferable to use a hot air heater as the heat shrinking device. That is, it is preferable to use a device that blows air supplied by a compressed air pump or fan, etc., onto an object via a heat source such as an electric heating wire or oil heater. Specifically, for example, the heat shrinking device is preferably configured to blow hot air vertically from above a polyester shrink film placed flat on a belt conveyor or a mounting table to thermally shrink the polyester shrink film. This is because the use of such a heat shrinking device allows for greater freedom in the placement of the device, allowing it to be placed above the polyester shrink film manufacturing equipment, and hot air can be blown onto the cut-off end, etc., making it easier to measure the heat shrinkage rate in-line. Therefore, when using such a hot air heater, it is preferable to configure the polyester shrink film to receive hot air within a tunnel-shaped housing made of stainless steel, aluminum, glass, etc., in order to effectively transfer the heat of the hot air to the polyester shrink film.

[0054] 2(a) to 2(c), a hot water bath 20 containing hot water 22 maintained at a predetermined temperature by a heater 22a is preferably prepared, and the polyester shrink film is immersed in the hot water at a heat shrinkage temperature of 70 to 98°C for a shrinkage time of 1 to 60 seconds to heat shrink the polyester shrink film in the main shrinkage direction. In this case, a mesh-like fixing jig 12 made of stainless steel wire or the like is preferably prepared, and the polyester shrink film 10 is preferably partially housed within the fixing jig, as shown in FIGS. 2(a) to 2(b).

[0055] Furthermore, when thermally shrinking a polyester-based shrink film, it is preferable to use a frame-shaped fixture that maintains the orientation of the polyester-based shrink film without interfering with its shrinkage. That is, as illustrated in Figures 5(a) to 5(c), the fixture 12 is preferably composed of a frame member and has at least a mounting portion 13a for mounting and holding the polyester-based shrink film, a guide portion 13b for controlling the shrinkage direction of the polyester-based shrink film, and a regulating portion 13c for preventing misalignment during thermal shrinkage. Furthermore, from the viewpoint of improved ease of handling, the fixture 12 is preferably provided with a handle portion 13d that protrudes obliquely upward and is located at the end of the mounting portion 13a in the main shrinkage direction. Specifically, the fixture 12 is preferably composed of a frame member made of metal wire such as stainless steel, iron, aluminum, or copper, or resin. This configuration allows for stable placement of the polyester-based shrink film and reduces wobble during thermal shrinkage, allowing for more accurate measurement of the thermal shrinkage rate.

[0056] Furthermore, from the viewpoints of ease of handling and uniform heating of the polyester shrink film, the mounting portion is preferably a substantially flat frame-like portion and, when viewed vertically from above, is preferably composed of at least two rail-like portions parallel to the main shrinkage direction. Furthermore, when viewed vertically from above, the guide portion is preferably arranged parallel to the mounting portion and is preferably a portion curved in a wavy pattern up and down in the vertical direction. Additionally, the restricting portion is arranged so as to bridge the guide portion in a direction perpendicular to the main shrinkage direction, and is a portion provided along the frame of the guide portion so as to be movable up and down, and is a portion that clamps the polyester shrink film placed on the mounting portion between the mounting portion and the restricting portion. This configuration prevents displacement of the polyester shrink film during thermal shrinkage and stabilizes the center position of shrinkage, allowing for accurate measurement of the thermal shrinkage rate by motion capture. Furthermore, by curving the guide portion in a wavy shape, for example, when a hot water bath is used as the heat shrinking device during heat shrinking, the device can be placed on the bottom of the water bath by adjusting the height of the guide portion to the water level, and measurements can be made by placing the device on the bottom of the water bath.

[0057] 6) Heat Shrinkage in MD The heat shrinkage in the direction perpendicular to the main shrinkage direction of the polyester shrink film to be measured (B1) is preferably measured using motion capture at the same time as the heat shrinkage in the TD direction. By simultaneously measuring the heat shrinkage in the MD direction using motion capture, it is possible to compare the heat shrinkage characteristics of the polyester shrink film with those of the actual use, depending on the intended use of the polyester shrink film. The heat shrinkage in the MD direction is preferably set to a value within the range of -5 to 5%.

[0058] 7) Calibration Curve It is preferable to prepare a calibration curve in advance showing the relationship between the heat shrinkage temperature and heat shrinkage time in the main shrinkage direction of the polyester shrink film to be measured, and the heat shrinkage percentage in the TD direction obtained using motion capture, and then compare the calibration curve with the heat shrinkage percentage obtained based on formula (1). By comparing the results with the previously prepared calibration curve, a polyester shrink film can be obtained that has a heat shrinkage percentage that is more rapid, accurate, and reproducible.

[0059] 3. Thermal Properties of Polyester-Based Shrink Films (1) Structure (a) The polyester-based shrink film to be measured preferably has the following structural requirement: (a) the polyester-based shrink film of the first embodiment has a main shrinkage direction in the TD direction, and the heat shrinkage percentage A1 in the TD direction when shrunk at 95°C for 1 second is 30 to less than 95%. The reason for this is that limiting the 95°C heat shrinkage percentage A1 to 30 to less than 95% ensures that the polyester-based shrink film achieves a good heat shrinkage percentage during heat shrinkage, and thus facilitates the achievement of maximum shrinkage stress. Therefore, for structure (a), it is more preferable to set the 95°C heat shrinkage percentage A1 to a value in the range of 40 to less than 90%, and even more preferable to set it to a value in the range of 50 to less than 85%.

[0060] Furthermore, the polyester shrink film to be measured preferably has a configuration (a') in which the main shrinkage direction is the TD direction and the heat shrinkage percentage A'1 in the TD direction when shrunk at 95°C for 10 seconds is within the range of 60 to less than 95%. The reason for this is that by limiting the 95°C heat shrinkage percentage A'1 to 60 to less than 95%, the polyester shrink film can achieve a good heat shrinkage percentage during heat shrinkage, and thus the maximum shrinkage stress can also be easily achieved. Therefore, for configuration (a'), it is more preferable to set the 95°C heat shrinkage percentage A'1 to a value within the range of 65 to less than 90%, and even more preferably within the range of 70 to less than 85%.

[0061] Furthermore, the polyester shrink film to be measured preferably has a structure (a2) in which the main shrinkage direction is the TD direction and the heat shrinkage percentage A2 in the TD direction when shrunk at 80°C for 1 second is within the range of 10 to less than 80%. The reason for this is that by setting the 80°C heat shrinkage percentage A2 within the specified range, the polyester shrink film can achieve a better heat shrinkage percentage during heat shrinkage, and thus the maximum shrinkage stress can be more easily achieved. Therefore, for structure (a2), the 80°C heat shrinkage percentage A2 is more preferably within the range of 15 to less than 70%, and even more preferably within the range of 20 to less than 50%.

[0062] Furthermore, for the polyester shrink film to be measured, the main shrinkage direction is the TD, and the heat shrinkage percentage A'2 in the TD direction when shrunk at 80°C for 10 seconds is preferably set to a value within the range of 10 to less than 85%. The reason for this is that by setting the 80°C heat shrinkage percentage A'2 within a predetermined range, a better heat shrinkage percentage can be obtained, and ultimately, the maximum shrinkage stress can be more easily achieved. Therefore, for the structure (a'2), the 80°C heat shrinkage percentage A'2 is more preferably set to a value within the range of 20 to less than 75%, and even more preferably to a value within the range of 30 to 65%.

[0063] (2) Structure (b) Furthermore, as structure (b), it is preferable to have a structural requirement that the maximum shrinkage stress in the TD direction of the polyester shrink film at a shrinkage temperature of 95°C is B, and that this B is a value within the range of 2 to 10 MPa. The reason for this is that by specifically limiting B to a value within this specified range, it is possible to suppress wrinkles that can occur due to an excess or deficiency of the maximum shrinkage stress. Therefore, as structure (b), it is more preferable that the maximum shrinkage stress B at a shrinkage temperature of 95°C is a value within the range of 2.5 to 9.5 MPa, and even more preferably a value within the range of 3 to 9 MPa.

[0064] (3) Structure (c) Preferably, structure (c) has the requirement that the value expressed by B / A1, based on the maximum shrinkage stress B and the thermal shrinkage rate A1, is within the range of 0.08 to 0.15 MPa / %. The reason for this is that by specifically limiting B / A1 to a value within the specified range in this way, even if the values ​​of structures (a) and (b) vary somewhat, the causes of the specified influencing factors can be reduced, and non-uniform shrinkage due to a sudden thermal response in the polyester-based shrink film during heat shrinkage can be suppressed, and as a result, the occurrence of fine wrinkles can also be suppressed.

[0065] (4) Structure (d) Preferably, structure (d) has the requirement that the ratio of the maximum shrinkage stress B of the polyester shrink film to its thickness t (μm), expressed as B / t, be within the range of 0.05 to 0.4 MPa / μm. This is because specifically limiting B / t to a value within the specified range makes it easier to control the value expressed as B / A1 within the specified range. This reduces the factors that influence the polyester shrink film during heat shrinkage, thereby suppressing uneven shrinkage due to a sudden thermal response, and as a result, effectively suppressing the occurrence of fine wrinkles.

[0066] (5) Structure (e) Furthermore, structure (e) preferably includes a structural requirement regarding the stretch ratio in the MD direction of the polyester shrink film before shrinkage (average MD stretch ratio, sometimes simply referred to as the MD stretch ratio). A preferred embodiment of this MD stretch ratio is a value within the range of 100 to 200%. The reason for this is that by specifically limiting the MD stretch ratio to a value within a predetermined range and specifically limiting the predetermined thermal shrinkage rate and other factors to values ​​within their respective predetermined ranges, the occurrence of fine wrinkles can be further suppressed. Therefore, as structure (e), it is more preferable to set the MD stretch ratio to a value within the range of 105 to 180%, and even more preferably to a value within the range of 110 to 160%.

[0067] (6) Structure (f) Furthermore, as structure (f), it is preferable to have a structural requirement regarding the stretch ratio in the TD direction of the polyester-based shrink film before heat shrinkage (average TD stretch ratio, sometimes simply referred to as the TD stretch ratio). The TD stretch ratio is preferably set to a value within a range of 300 to 700%, more preferably a value within a range of 350 to 600%, and even more preferably a value within a range of 400 to 550%. The reason for this is that by specifically limiting the TD stretch ratio to a value within a predetermined range and specifically limiting the predetermined heat shrinkage rate, etc., to values ​​within their respective predetermined ranges, the occurrence of fine wrinkles can be further suppressed.

[0068] (7) Feature (g) Feature (g) preferably includes the requirement that the haze value of the polyester shrink film before heat shrinkage, measured in accordance with JIS K 7105, be 7% or less. The reason for this is that by specifically limiting the haze value to a value within a predetermined range, the transparency of the polyester shrink film can be easily controlled quantitatively, and since the transparency is good, versatility can be further enhanced. More specifically, if the haze value of the film before heat shrinkage exceeds 7%, transparency decreases, which may make it difficult to apply the film to decorative applications such as PET bottles. On the other hand, if the haze value of the film before heat shrinkage is excessively low, stable control becomes difficult, which may significantly reduce production yield. Therefore, as feature (g), it is more preferable that the haze value of the film before heat shrinkage be within the range of 0.1 to 5%, and even more preferably within the range of 0.5 to 3%.

[0069] (8) Structure (h) Structure (h) is a constituent requirement for a polyester-based shrink film that contains an amorphous polyester resin in the range of 90 to 100 wt% of the total weight. This is because specifically limiting the content of the amorphous polyester resin in this manner makes it easier to adjust the thermal shrinkage rate and maximum shrinkage stress near the shrinkage temperature to the desired range, and also makes it easier to quantitatively control the haze value and other parameters. More specifically, if the content of the amorphous polyester resin is less than 90 wt%, it may be difficult to control the shrinkage rate and maximum shrinkage stress near the shrinkage temperature of the polyester-based shrink film. Furthermore, if the content of the crystalline polyester resin is excessively high, the range in which the effects of certain influencing factors can be reduced may be significantly narrowed. Therefore, as structure (h), it is more preferable to set the content of the amorphous polyester resin in the range of 91 to 100 wt% of the total weight, and even more preferable to set it in the range of 92 to 100 wt%.

[0070] 4. Composition of Polyester-Based Shrink Films It is preferable to incorporate various additives into or attach them to one or both surfaces of a polyester-based shrink film. More specifically, at least one of a hydrolysis inhibitor, an antistatic agent, an ultraviolet absorber, an infrared absorber, a colorant, an organic filler, an inorganic filler, an organic fiber, or an inorganic fiber is incorporated in an amount of preferably 0.01 to 10% by weight, more preferably 0.1 to 1% by weight, based on the total weight of the polyester-based shrink film.

[0071] 1(b), it is also preferable to laminate other resin layers 10a, 10b containing at least one of these various additives on one or both sides of the polyester shrink film 10. In this case, it is generally preferable that the single layer thickness or total thickness of the additional resin layers be within a range of 0.1 to 10%, assuming the thickness of the polyester shrink film to be 100%.

[0072] The resin as the main component constituting the other resin layer may be a polyester resin similar to that of a polyester shrink film, or preferably at least one of a different acrylic resin, an olefin resin, a urethane resin, a rubber resin, etc.

[0073] Furthermore, it is also preferable to form the polyester shrink film into a multilayer structure to further prevent hydrolysis and provide mechanical protection, or to provide a shrinkage-adjusting layer 10c on the surface of the polyester shrink film 10 so that the shrinkage rate of the polyester shrink film is uniform within the plane, as shown in Figure 1(c). Such a shrinkage-adjusting layer can be laminated using an adhesive, a coating method, heat treatment, or the like, depending on the shrinkage characteristics of the polyester shrink film.

[0074] More specifically, the thickness of the shrinkage rate adjusting layer is in the range of 0.1 to 3 μm, and if the shrinkage rate of the polyester-based shrink film at a predetermined temperature is excessively large, it is preferable to laminate a shrinkage rate adjusting layer of a type that suppresses this. Also, if the shrinkage rate of the polyester-based shrink film at a predetermined temperature is excessively small, it is preferable to laminate a shrinkage rate adjusting layer of a type that increases it. Thus, the shrinkage rate adjusting layer is used to achieve a desired shrinkage rate for the polyester-based shrink film, without having to create various shrink films with different shrinkage rates.

[0075] 5. Measurement of Other Thermal Properties (1) Heat Shrinkage Speed ​​When a polyester shrink film is heat shrunk in the main shrinkage direction at a predetermined temperature T for a predetermined time t1, it is preferable to use a predetermined correlation between the distance information of a predetermined section measured by motion capture and the measurement time to adjust the maximum heat shrinkage speed calculated based on equation (2) to fall within a predetermined range. That is, as shown in Figure 6(a), it is preferable to set the maximum heat shrinkage speed that can be calculated based on equation (2) to 3 mm / sec or more, where PL0 is the distance of the predetermined section measured by motion capture before heat shrinkage, and PL1 is the distance of the predetermined section measured by motion capture at a predetermined time t2 shorter than the predetermined time t1.

[0076]

[0077] The reason for this is that by setting the heat shrinkage rate at this maximum, it is possible to precisely adjust the balance between the amount of change at which the polyester shrink film changes most significantly and the time required, thereby effectively preventing the occurrence of wrinkles and the like when the polyester shrink film is used on an object. Therefore, it is more preferable to set the maximum heat shrinkage rate to 3.5 mm / sec or more, and even more preferable to set it to 4 mm / sec or more. It is also preferable that the distance PL0 of the predetermined section before heat shrinkage be the same as L1, etc.

[0078] Referring to FIG. 7 , the relationship between time (seconds) and distance change (mm) in a predetermined section will be described. Specifically, for Examples 1 and 2 and Comparative Examples 2 and 3 described below, measurements were taken at 0.1-second intervals and graphed, with time (seconds) on the horizontal axis and the maximum distance change (mm) in six predetermined sections spaced 10 mm apart along the main shrinkage direction on the vertical axis. From this graph, it can be seen that Examples 1 and 2 show a uniform increase between 0 and 2 seconds, followed by a gradual increase thereafter. It can also be seen that Comparative Example 2 shows a portion where the distance change in the predetermined section decreases between 0 and 1 second. On the other hand, it can be seen that Comparative Example 3 shows a gradual increase in distance change in the predetermined section between 0 and 1 second, a sudden increase between 1 and 2 seconds, and then a small decrease thereafter. Furthermore, it can be seen that Comparative Example 3 shows approximately 1 / 3 to 1 / 2 of the other relationship curves at 1 second after the start of thermal shrinkage.

[0079] 8(a)-(b) and 9(a)-(b), the relationship between time (seconds), heat shrinkage speed (mm / second), and heat shrinkage percentage speed (% / second) will be described. Specifically, for Examples 1 and 2 and Comparative Examples 1 and 2 described below, the horizontal axis represents time (seconds), and the vertical axis represents the heat shrinkage speed with the smallest maximum value among six predetermined sections set at 10 mm intervals along the main shrinkage direction. The graphs were plotted at 0.1-second intervals. From FIGS. 8(a)-(b), it can be seen that the heat shrinkage speeds of Examples 1 and 2 increased relatively steadily immediately after the start of heat shrinkage, exceeded 3 mm / second after about 1 second, and then decreased to 3 mm / second or less within 1 to 2 seconds. 9(a) and 9(b), it can be seen that the heat shrinkage speed in Comparative Examples 2 and 3 does not increase significantly immediately after the start of heat shrinkage, and does not exceed 3 mm / sec even after 1 second has passed since the start of heat shrinkage. In the cases of Fig. 8(c) and Fig. 9(c), a heat shrinkage speed of 1 mm / sec corresponds to a heat shrinkage rate of 10% / sec.

[0080] (2) Heat Shrinkage Rate Furthermore, as shown in FIG. 6(a), it is preferable that the maximum heat shrinkage rate of a polyester shrink film in the main shrinkage direction calculated based on the following formula (3) is 30% / sec or more.

[0081]

[0082] The reason for this is that by setting such a heat shrinkage rate, it is possible to accurately adjust the balance between the amount of change at which the polyester-based shrink film changes most significantly and the time required, thereby effectively preventing the occurrence of wrinkles and the like when the polyester-based shrink film is used on an object. Furthermore, by measuring the amount of change in the heat shrinkage rate, it is possible to evaluate the polyester-based shrink film without depending on the distance of a specified section. Therefore, it is more preferable that the maximum heat shrinkage rate be 3.5% / sec or more, and even more preferable that it be 4% / sec or more.

[0083] (3) Standard Deviation of Maximum Heat Shrinkage Rate Furthermore, when a polyester shrink film is divided into multiple predetermined sections and the heat shrinkage rate from the start of heat shrinkage to a predetermined time t1 is calculated every 0.1 seconds, it is preferable that the standard deviation of the maximum heat shrinkage rate for each predetermined section be 3.5 mm / sec or less. This is because such a standard deviation allows for accurate adjustment of the shrinkage rate per time during heat shrinkage, resulting in more stable behavior during heat shrinkage. Therefore, it is more preferable that the standard deviation of the maximum heat shrinkage rate be 1 mm / sec or less, and even more preferable that it be 0.3 mm / sec or less. The standard deviation is the square root of the sum of the squares of the deviations divided by the number of data points minus 1.

[0084] (4) Heat Shrinkage Speed ​​in a Predetermined Period (Intermediate Heat Shrinkage Speed) As shown in FIG. 6(b), a polyester-based shrink film is provided with a predetermined section along the main shrinkage direction of the polyester-based shrink film in a state where it can shrink in at least one of the longitudinal and transverse directions, and is heat-shrunk at a predetermined temperature T for a predetermined time t1. From the change in distance between the distance PL0 of the predetermined section before heat shrinkage, the distance PL1 of the predetermined section at a predetermined time t2 that is shorter than the predetermined time t1, and the distance PL2 of the predetermined section at a predetermined time t3 that is shorter than the predetermined time t1 but longer than the predetermined time t2, it is preferable that the heat shrinkage speed in the main shrinkage direction in a predetermined period (hereinafter sometimes referred to as the intermediate heat shrinkage speed) be 20 mm / sec or less.

[0085]

[0086] The reason for this is that by using such an intermediate heat shrinkage speed, a predetermined correlation can be utilized between the change in distance over a predetermined section of the polyester shrink film during heat shrinkage and position information obtained by motion capture or the like. Ultimately, the heat shrinkage speed of the polyester shrink film can be adjusted to a value within a predetermined range, allowing the polyester shrink film to exhibit stable, excellent heat shrinkability. Therefore, the heat shrinkage speed during the measurement period is more preferably 18 mm / sec or less, and even more preferably 15 mm / sec or less. The intermediate heat shrinkage speed is defined as positive in the shrinkage direction of the polyester shrink film, and is defined as negative in cases where the polyester shrink film elongates in reaction to shrinkage or where the film is three-dimensionally distorted due to rapid heat shrinkage and then returns to a flat state.

[0087] Furthermore, for polyester shrink films, it is preferable to set the measurement period t3-t2 to a value of 3 seconds or less. The reason for this is that such a measurement period allows for more accurate measurement of behavior during thermal shrinkage. Therefore, it is more preferable to set the measurement period t3-t2 to a value of 2 seconds or less, and even more preferable to set it to a value of 1 second or less. On the other hand, from the viewpoint of preventing an increase in measurement errors due to an excessively high time resolution, it is preferable to set the measurement period t3-t2 to a value of 0.1 seconds or more.

[0088] Furthermore, it is preferable that the intermediate heat shrinkage rate always be a positive value during heat shrinkage. However, even if the rate becomes negative, it has been found that this does not pose a problem for the intended use of the polyester-based shrink film as long as the value is small. Therefore, it is preferable that the minimum intermediate heat shrinkage rate of a polyester-based shrink film over a specified period be kept at -2.5 mm / sec or greater. By preventing the intermediate heat shrinkage rate of a polyester-based shrink film from becoming negative, wrinkles and other problems can be more effectively prevented when the polyester-based shrink film is used as a polyester-based shrink film. Therefore, it is more preferable that the minimum intermediate heat shrinkage rate be -1.5 mm / sec or greater, and even more preferable that it be 0 mm / sec or greater.

[0089] Here, referring to FIGS. 10(a) to 13(a), the relationship between time (seconds) and the intermediate heat shrinkage speed (mm / second) will be described. Specifically, for Examples 1 and 2 and Comparative Examples 2 and 3 described below, the horizontal axis represents time (seconds) and the vertical axis represents the intermediate heat shrinkage speed (mm / second) for the highest maximum value among six predetermined sections set at 10 mm intervals along the main shrinkage direction. The graphs were plotted at 0.1-second intervals. FIGS. 10(a) to 11(a) show that in Examples 1 and 2, the intermediate heat shrinkage speed reaches its maximum value between 0 and 1 second and then decreases to approximately 0 mm / second by about 1 second after the start of heat shrinkage. On the other hand, FIG. 12(a) shows that in Comparative Example 2, the intermediate heat shrinkage speed reaches its maximum value between 0 and 1 second, but then varies significantly between 1 and 2 seconds after 0 mm / second. 13(a), it can be seen that in Comparative Example 3, the intermediate heat shrinkage speed was 5 mm / sec or less between 0 and 1 second, increased to over 20 mm / sec after about 1 second, and then decreased to 5 mm / sec or less between 1.1 and 1.5 seconds. In the cases of FIGS. 10(b) to 13(b), a heat shrinkage speed of 1 mm / sec corresponds to a heat shrinkage rate of 10% / sec.

[0090] (5) Standard Deviation of the Maximum Intermediate Heat Shrinkage Speed ​​Furthermore, when a polyester shrink film is divided into multiple predetermined sections and the heat shrinkage rate from the start of heat shrinkage to a predetermined time t1 is calculated every 0.1 seconds, it is preferable that the standard deviation of the maximum intermediate heat shrinkage rate for each predetermined section be 4.5 mm / sec or less. This is because such a standard deviation allows for accurate adjustment of the shrinkage rate within a predetermined time during heat shrinkage, resulting in more stable behavior during heat shrinkage. Therefore, it is more preferable that the standard deviation of the maximum intermediate heat shrinkage rate be 3.5 mm / sec or less, and even more preferable that it be 3 mm / sec or less. The standard deviation is the square root of the sum of the squares of the deviations divided by the number of data points minus 1.

[0091] (6) Heat Shrinkage Rate in a Predetermined Period (Intermediate Heat Shrinkage Rate) When a polyester shrink film is heat-shrunk at a predetermined temperature T for a predetermined time t1 as shown in FIG. 6(b), the intermediate heat shrinkage rate in the main shrinkage direction (hereinafter sometimes referred to as the intermediate heat shrinkage rate) is preferably 200% / second or less, as calculated from the change in distance between the distance PL0 of a predetermined section before heat shrinkage, the distance PL1 of a predetermined section at a predetermined time t2 that is shorter than the predetermined time t1, and the distance PL2 of a predetermined section at a predetermined time t3 that is shorter than the predetermined time t1 but longer than the predetermined time t2, according to the following formula (5):

[0092]

[0093] The reason for this is that such an intermediate heat shrinkage rate allows the heat shrinkage rate of the polyester-based shrink film to be adjusted more accurately regardless of the size of the polyester-based shrink film. Therefore, the intermediate heat shrinkage rate is more preferably 180% / sec or less, and even more preferably 150% / sec or less.

[0094] On the other hand, from the viewpoint of preventing defects due to excessively small shrinkage in a short period of time, the intermediate heat shrinkage rate is preferably 60% / sec or more, more preferably 80% / sec or more, and even more preferably 90% / sec or more. Note that, like the intermediate heat shrinkage rate, it is preferable that the intermediate heat shrinkage rate is always a positive value, but even if it becomes a negative value, it has been found that there is no problem for the intended use of the polyester-based shrink film as long as the value is small.

[0095] Therefore, it is preferable that the minimum intermediate heat shrinkage rate of a polyester-based shrink film be −2.5% / sec or higher. By preventing the intermediate heat shrinkage rate of a polyester-based shrink film from becoming negative, wrinkles and other problems can be more effectively prevented when the polyester-based shrink film is used. Therefore, it is more preferable that the minimum intermediate heat shrinkage rate be −1.5% / sec, and even more preferable that it be 0% / sec or higher.

[0096] Furthermore, when calculating the heat shrinkage rate, it is preferable that the predetermined times t2 and t3 be 5 seconds or less. This is because such predetermined times allow for more detailed measurement of the behavior of the polyester shrink film during heat shrinkage. Therefore, it is more preferable that the predetermined times t2 and t3 be 4 seconds or less, and even more preferable that they be 3 seconds or less.

[0097] Furthermore, it is preferable that the time when the intermediate heat shrinkage speed reaches its maximum be 1 second or less. This is because, by configuring the polyester shrink film in this way, the timing at which the polyester shrink film shrinks significantly can be controlled, and the heat shrinkage characteristics can be adjusted more accurately. Therefore, it is more preferable that the time when the intermediate heat shrinkage speed reaches its maximum be 0.8 seconds or less, and even more preferable that it be 0.6 seconds or less.

[0098] (7) Difference in Heat Shrinkage Rate Rate Per Second Furthermore, when a polyester-based shrink film has a predetermined section along the main shrinkage direction of the polyester-based shrink film and is heat-shrunk along the main shrinkage direction at a predetermined temperature T for a predetermined time t1, the distance of the predetermined section before heat shrinkage is defined as PL0, the distance of the predetermined section at a predetermined time t2 shorter than the predetermined time t1 is defined as PL1, and the distance of the predetermined section at a predetermined time t3 shorter than the predetermined time t1 and longer than the predetermined time t2 is defined as PL2, and the measurement period t3-t2 is defined as 1 second. The difference in heat shrinkage rate rate per second calculated based on the following formula (6) is usually preferably 100% / second or less under predetermined conditions (predetermined temperature T: 70 to 98°C, predetermined time t1: longer than 5 seconds).

[0099]

[0100] The reason for this is that such a difference in heat shrinkage rate allows the polyester-based shrink film to shrink more stably. Therefore, the difference in heat shrinkage rate is more preferably 80% / sec or less, and even more preferably 50% / sec or less.

[0101] Second Embodiment The second embodiment relates to a method for producing the polyester shrink film of the first embodiment using motion capture.

[0102] 1. Preparation and Mixing of Raw Materials First, it is preferable to prepare the raw materials, such as base materials and additives, such as crystalline polyester resin, amorphous polyester resin, rubber-based resin, antistatic agent, hydrolysis inhibitor, etc. Next, it is preferable to charge the prepared crystalline polyester resin, amorphous polyester resin, etc. into a stirring vessel while weighing them, and mix and stir them using a stirring device until they become uniform.

[0103] 2. Raw Sheet Preparation Process Next, the uniformly mixed raw materials are preferably dried to an absolutely dry state. Next, typically, extrusion molding is preferably performed to prepare a raw sheet of a predetermined thickness. More specifically, for example, extrusion molding is performed using an extruder (manufactured by Tanabe Plastic Machinery Co., Ltd.) with an L / D of 24 and an extrusion screw diameter of 50 mm under conditions of an extrusion temperature of 260°C, to obtain a raw sheet of a predetermined thickness (usually 10 to 100 μm).

[0104] 3. Preparation of Polyester-Based Shrink Film Next, the obtained raw sheet is heated and pressed while moving on or between rolls using a shrink film manufacturing device to produce a polyester-based shrink film. That is, it is preferable to stretch the film in a predetermined direction while heating and pressing it at a predetermined stretching temperature and stretching ratio, while basically expanding the film width, thereby crystallizing the polyester molecules that make up the polyester-based shrink film into a predetermined shape. Then, by solidifying it in that state, a heat-shrinkable polyester-based shrink film can be produced that can be used for decorations, labels, etc.

[0105] 4. Measurement of Heat Shrinkage Rate Using Motion Capture Typically, it is preferable to measure the heat shrinkage rate according to the following steps.

[0106] (1) A polyester shrink film is prepared as a test object. It is preferable to confirm that the thickness of the polyester shrink film is within a predetermined range. It is also preferable to measure the haze, glass transition temperature, and various thermal properties of the polyester shrink film in advance.

[0107] (2) Next, as shown in Figure 3(a), a step of setting two measurement positions (P1 and P2) in the TD direction, which is the main shrinkage direction of the polyester shrink film 10 before heat shrinkage, is carried out. The distance between the two measurement positions (P1 and P2) in the TD direction before heat shrinkage is defined as L1. Here, when the polyester shrink film has a rectangular or square planar shape, the two measurement positions (P1 and P2) in the TD direction are preferably located at positions typically 5 mm or more from the end so that both ends are free.

[0108] 3(a), it is preferable to carry out a step of setting two measurement positions (P3 and P4) in addition to the two measurement positions (P1 and P2) described above in the MD direction, which is the direction perpendicular to the main shrinkage direction. The distance between the two measurement positions (P3 and P4) in the MD direction before heat shrinkage is preferably L2. Here, when the polyester shrink film has a rectangular or square planar shape, the two measurement positions (P3 and P4) in the MD direction are preferably located at positions typically 5 mm or more from the edge, similar to the measurement positions in the TD direction.

[0109] (3) Next, the polyester-based shrink film is subjected to a heat shrinking process. Specifically, as shown in Figures 2(a) to 2(c), a hot water bath 20 containing hot water 22 maintained at a predetermined temperature by a heater 22a is prepared. The polyester-based shrink film is then immersed in the hot water at a heat shrinkage temperature of 70 to 98°C and a shrinkage time of 1 to 60 seconds, causing the polyester-based shrink film to heat shrink in the TD direction. As shown in Figure 2(b), a mesh-like fixture 12 made of, for example, stainless steel wire is prepared so that the polyester-based shrink film is uniformly immersed and heated. The polyester-based shrink film 10 is partially housed within the fixture 12. Furthermore, the fixture 12 preferably has openings 12' of predetermined sizes corresponding to measurement points P1 and P2, allowing the shrinkage rate to be measured using motion capture or the like without stretching the polyester-based shrink film 10 in the thickness direction.

[0110] To further allow the polyester shrink film to be uniformly immersed and heated for a predetermined period of time, at least two linear objects 26 are preferably attached to both ends of the polyester shrink film 10 via stainless steel fixtures 12. That is, these linear objects 26, such as wires, are further connected to a lifter 24, which preferably winds up and unwinds the linear objects 26, moving up and down at a constant speed while maintaining the horizontal orientation of the polyester shrink film 10.

[0111] In order to prevent temperature variations, the process of thermally shrinking a polyester shrink film is preferably performed by immersing the polyester shrink film 10 in a hot water bath 20 as shown in Fig. 2(b). On the other hand, in order to perform measurements more quickly and simply, it is also preferable to thermally shrink the polyester shrink film 10 by floating it on the surface of hot water 22 maintained at a predetermined temperature in the hot water bath 20 as shown in Figs. 2(a) and 2(c).

[0112] (4) Next, as shown in FIG. 3(b), a measurement step is performed using a motion capture device 14, with the distance between two measurement positions (P1' and P2') in the TD direction of the heat-shrunk polyester shrink film 10' defined as the second distance. That is, as shown in FIGS. 3(b) and 14, a predetermined motion capture device 14 and an inertial sensor 14' are preferably prepared, and the distance between two measurement positions on the polyester shrink film heat-shrunk under predetermined conditions is preferably measured using the motion capture device as L'1 (sometimes referred to as the second distance). Furthermore, when measurement samples are cut out from three locations (W, C, E) along the TD direction as shown in FIG. 14 to obtain multiple samples, it is preferable to attach predetermined markers to the two measurement positions on each measurement sample (W, C, E) and perform the measurements. On the other hand, it is also preferable to measure the distance between two measurement positions continuously (for example, at time intervals of 0.01 to 1 second) using a motion capture device or the like before or during the heat shrinkage of such a polyester-based shrink film.

[0113] Furthermore, the inertial sensor 14' shown in Figure 14 is a combination of a major axis sensor and several minor axis sensors that intersect the major axis sensor at equal intervals at 90°, and preferably has at least two measurement points at a predetermined interval somewhere in the sensor. However, the inertial sensor 14' is not limited to these combinations, and it is also preferable that the planar shape be at least one of a circle, a triangle, a square, a polygon, or an irregular shape. Note that, here, an inertial motion capture is used as the motion capture to measure the intervals between the inertial sensors that are placed at predetermined intervals, but it is also preferable to use an image-based motion capture to measure a predetermined marker such as an oil-based marker.

[0114] 3(b), it is preferable to perform a measurement process using motion capture, with the distance between two measurement positions (P3' and P4') in the MD direction defined as the second distance. The distance between the two measurement positions (P3' and P4') in the MD direction after thermal shrinkage is defined as L'2. That is, it is preferable to measure the second distance in the MD direction in the same way as measuring the second distance in the TD direction.

[0115] (5) Next, a step of calculating the thermal shrinkage percentage in the TD direction is carried out using L1, the distance between the two points before heat shrinkage, and L'1, the distance between the two points after heat shrinkage, based on formula (1). It is then preferable to confirm that the thermal shrinkage percentage in the TD direction of the polyester shrink film is 20% or more.

[0116] Here, referring to FIG. 15 , the relationship between the immersion time (seconds) and the thermal shrinkage (%) in the TD direction measured using motion capture for Example 2 and Comparative Example 1 when the samples were immersed in 95°C water for 1 to 20 seconds will be described. That is, the horizontal axis of FIG. 15 represents the immersion time (seconds), and the vertical axis represents the thermal shrinkage (%) in the TD direction measured using motion capture. For the characteristic curve of Example 2 (line A), an immersion time of approximately 1 second results in a thermal shrinkage (%) that is approximately the same as that obtained after 20 seconds. In contrast, for the characteristic curve of Comparative Example 1 (line B), a comparison of the thermal shrinkage (%) obtained after immersion for 1 second and after immersion for 20 seconds shows a tendency for the thermal shrinkage (%) to increase with increasing immersion time. Therefore, it is preferable to determine the immersion time taking into consideration the PET resin used, the thickness and thermal properties of the polyester shrink film obtained from it, and the manufacturing conditions.

[0117] Furthermore, referring to Figure 16, the relationship between the thickness (µm) of a polyester-based shrink film and the thermal shrinkage (%) in the TD direction measured using motion capture when immersed in 95°C hot water for 20 seconds will be described. That is, the horizontal axis of Figure 16 represents the thickness (µm) of the polyester-based shrink film, and the vertical axis represents the thermal shrinkage (%) in the TD direction measured using motion capture. Therefore, in the case of the characteristic curve (line C), it can be seen that the thicker the polyester-based shrink film, the lower the thermal shrinkage (%), and there is a certain correlation (linear relationship). Therefore, it can be said that it is preferable to adjust the thermal shrinkage (%) taking into account the thickness and thermal properties of the polyester-based shrink film.

[0118] It is also preferable to carry out a step of calculating the heat shrinkage percentage in the MD direction from L2, the distance between the two points before heat shrinkage, and L'2, the distance between the two points after heat shrinkage, in the same manner as the heat shrinkage percentage in the TD direction. It is also preferable to confirm that the heat shrinkage percentage in the MD direction of the polyester-based shrink film is within the range of -5 to 5%. The reason for this is that by simultaneously measuring the heat shrinkage percentage in the MD direction in this way, the heat shrinkage characteristics of the polyester-based shrink film during actual use can be more easily controlled depending on the application, etc., of the polyester-based shrink film.

[0119] (6) Next, it is preferable to carry out a step of comparing the obtained data on the heat shrinkage rate and thickness with a calibration curve. That is, it is preferable to confirm that the thickness of the polyester shrink film confirmed in step (1) and the heat shrinkage rate obtained in step (5) each match with a calibration curve prepared in advance, which shows the relationship between the thickness of the polyester shrink film and the heat shrinkage rate measured using motion capture.

[0120] (7) Next, it is also preferable to carry out a predetermined adjustment step. That is, if the thermal shrinkage rate in the TD direction is below 20%, it is preferable to adjust the thermal shrinkage rate to within a predetermined range by reducing the thickness of the polyester-based shrink film or by changing the raw materials or manufacturing conditions of the polyester-based shrink film.

[0121] (8) Next, it is preferable to have another predetermined adjustment step of adjusting the standard deviation of the heat shrinkage. That is, if the standard deviation of the heat shrinkage in the TD direction exceeds 15%, it is preferable to adjust the standard deviation of the heat shrinkage within a predetermined range by reducing the thickness of the polyester shrink film or by changing the raw materials or manufacturing conditions of the polyester shrink film.

[0122] (9) Next, as other steps, it is preferable to include a step of calculating, by motion capture, other heat shrinkage characteristics in the first embodiment, such as the heat shrinkage rate, the standard deviation of the heat shrinkage speed, the intermediate heat shrinkage rate, the intermediate heat shrinkage rate speed, the difference in the intermediate heat shrinkage rate speed per second, etc. It is also preferable to include a step of adjusting each measured value to fall within a predetermined range.

[0123] (10) Finally, it is also preferable to carry out other inspection processes. That is, it is preferable to provide a predetermined inspection process in which the following properties are measured continuously or intermittently for the produced polyester shrink film. By measuring the following properties and confirming that they fall within the predetermined ranges through such predetermined inspection processes, it is possible to obtain a polyester shrink film with more uniform shrinkage properties. 1) Visual inspection of the appearance of the polyester shrink film 2) Measurement of thickness variation 3) Haze measurement 4) Measurement of glass transition point 5) Measurement of melting point and heat of fusion 6) Measurement of tensile modulus 7) Measurement of tear strength 8) Measurement of viscoelastic properties using SS curves

[0124] [Third Embodiment] The third embodiment relates to a method for using a polyester shrink film having a thermal shrinkage rate measured using motion capture. That is, any known method for using shrink films can be suitably applied. For example, when carrying out the method for using a polyester shrink film, the polyester shrink film is first cut to an appropriate length and width and formed into a long cylindrical object. The long cylindrical object is then fed to an automatic labeling device (shrink labeler), further cut to the required length, and finally fitted onto a PET bottle or the like filled with a content.

[0125] Next, the polyester shrink film wrapped around the PET bottle or the like is heated by passing it through a hot air tunnel or steam tunnel at a predetermined temperature. These tunnels provide radiant heat such as infrared radiation or heated steam at approximately 90°C, which uniformly heats and heat-shrinks the polyester shrink film. Therefore, when the thermal shrinkage rate in the TD is 20% or more, the film can be quickly adhered to the outer surface of the PET bottle or the like, thereby producing a labeled container, as shown in Figures 17(a) to 17(d). On the other hand, when the thermal shrinkage rate in the TD is less than 20%, the label cannot conform to the shape of the bottle from the top to the bottom of the bottle body, as shown in Figures 18(a) to 18(d). Furthermore, significant wrinkling is observed.

[0126] The present invention will be described in detail below based on examples. However, the scope of the present invention will not be narrowed by the description of the examples without any particular reason. The polyester resins used in Example 1 etc. are as follows.

[0127] (PETG1) Amorphous polyester (glass transition temperature: 69°C) consisting of dicarboxylic acid: 100 mol% terephthalic acid, diol: 69 mol% ethylene glycol, 20 mol% 1,4-cyclohexanedimethanol, and 11 mol% diethylene glycol

[0128] (PETG2) Amorphous polyester (glass transition temperature: 69°C) consisting of dicarboxylic acid: 100 mol% terephthalic acid, diol: 63 mol% ethylene glycol, 24 mol% 1,4-cyclohexanedimethanol, and 13 mol% diethylene glycol.

[0129] (PETG3) Amorphous polyester (glass transition temperature: 75°C) consisting of dicarboxylic acid: 100 mol% terephthalic acid, diol: 68 mol% ethylene glycol, 30 mol% neopentyl glycol, and 2 mol% diethylene glycol

[0130] (PETG4) Amorphous polyester (glass transition temperature: 69°C) consisting of dicarboxylic acid: 100 mol% terephthalic acid, diol: 70 mol% ethylene glycol, 28 mol% 1,4-cyclohexanedimethanol, and 2 mol% diethylene glycol.

[0131] [Example 1] 1. Preparation of polyester shrink film 100 parts by weight of amorphous polyester resin (PETG1) was placed in a stirring vessel. Next, this raw material was dried and extruded at an extrusion temperature of 260°C using an extruder with an L / D of 24 and an extrusion screw diameter of 50 mm (manufactured by Tanabe Plastic Machinery Co., Ltd.) to obtain a raw sheet with a thickness of 200 μm.

[0132] Next, using a shrink film manufacturing device, a polyester shrink film having a thickness of 40 μm was produced from the raw sheet at a preheating temperature of 75°C, a stretching temperature of 75°C, a stretching ratio (MD direction: 105%, TD direction: 500%), and a heat setting temperature of 60°C.

[0133] 2. Evaluation of Polyester-Based Shrink Films (1) Evaluation 1: Thickness Variation The thickness of the obtained polyester-based shrink films was measured using a micrometer (n=6) and evaluated according to the following criteria: Excellent: Thickness variation was within 3 μm. Good: Thickness variation was within 5 μm. Fair: Thickness variation was within 10 μm. Bad: Thickness variation was greater than 10 μm.

[0134] (2) Evaluation 2: Thermal Shrinkage Ratio (A1) in the TD Direction The obtained polyester shrink film was immersed in 95°C hot water for 1 second using a hot water bath to allow thermal shrinkage. Next, as shown in FIG. 2(a), while capturing image data with an optical camera, the thermal shrinkage ratio (A1) in the TD direction was calculated from the change in marker distance before and after heat treatment, obtained using an image-based motion capture device 14, according to formula (1). The thermal shrinkage ratio (A1) was evaluated according to the following criteria: ◎: The thermal shrinkage ratio (A1) was within the range of 50 to less than 85%. ○: The thermal shrinkage ratio (A1) was 30 to less than 50%, or 85% to less than 90%. △: The thermal shrinkage ratio (A1) was 20 to less than 30%, or 90% to less than 95%. ×: The thermal shrinkage ratio (A1) was less than 20% or more than 95%.

[0135] (3) Evaluation 3: Standard deviation (σ1) of thermal shrinkage rate (A1) in TD direction The standard deviation (σ1) was calculated from the values ​​(n=6) of thermal shrinkage rate (A1) in TD direction obtained using image motion capture in Evaluation 2, and evaluated according to the following criteria. ⊚: The standard deviation of the thermal shrinkage rate (A1) is within 5%. ◯: The standard deviation of the thermal shrinkage rate (A1) is within 10%. △: The standard deviation of the thermal shrinkage rate (A1) is within 15%. ×: The standard deviation of the thermal shrinkage rate (A1) is more than 20%.

[0136] (4) Evaluation 4: Thermal Shrinkage Ratio (A'1) in TD The obtained polyester shrink film was immersed in 95°C hot water for 10 seconds in a hot water bath to cause thermal shrinkage. The dimensional change before and after the heat treatment was then calculated based on the data, and the thermal shrinkage ratio (A'1) in TD was calculated according to formula (1). The evaluation was based on the following criteria: Excellent: The thermal shrinkage ratio (A'1) was in the range of 70 to 85%. Good: The thermal shrinkage ratio (A'1) was 65 to less than 70%, or 85 to less than 90%. Fair: The thermal shrinkage ratio (A'1) was 60 to less than 65%, or 90 to less than 95%. Bad: The thermal shrinkage ratio (A'1) was less than 60% or more than 95%.

[0137] (5) Evaluation 5: Haze The haze value of the obtained polyester shrink film was measured in accordance with JIS K 7105 and evaluated according to the following criteria: Excellent: Haze is 3% or less. Good: Haze is 5% or less. Fair: Haze is 7% or less. Bad: Haze is more than 7%.

[0138] (6) Evaluation 6: Thermal Shrinkage Ratio (A2) in the TD Direction The obtained polyester shrink film was immersed in 80°C hot water for 1 second using a hot water bath to allow thermal shrinkage. Next, as shown in FIG. 2(a), while capturing image data with an optical camera, the thermal shrinkage ratio (A2) in the TD direction was calculated from the change in marker distance before and after heat treatment, obtained by an image-based motion capture device 14 according to formula (1), and evaluated according to the following criteria: ◎: The thermal shrinkage ratio (A2) was within the range of 20 to less than 50%. ○: The thermal shrinkage ratio (A1) was 15 to less than 20%, or 50% to less than 70%. △: The thermal shrinkage ratio (A1) was 10 to less than 15%, or 70% to less than 80%. ×: The thermal shrinkage ratio (A1) was less than 10% or more than 80%.

[0139] (7) Evaluation 7: Standard deviation (σ2) of thermal shrinkage rate (A2) in TD direction The standard deviation (σ2) was calculated from the values ​​(n=6) of thermal shrinkage rate (A2) in TD direction obtained using image motion capture in Evaluation 6, and evaluated according to the following criteria. ◎: The standard deviation of the thermal shrinkage rate (A2) is within 4%. ○: The standard deviation of the thermal shrinkage rate (A2) is within 8%. △: The standard deviation of the thermal shrinkage rate (A2) is within 12%. ×: The standard deviation of the thermal shrinkage rate (A2) is more than 16%.

[0140] (8) Evaluation 8: Thermal Shrinkage Ratio (A'2) in the TD Direction The obtained polyester shrink film was immersed in 80°C hot water for 10 seconds using a hot water bath to allow thermal shrinkage. Next, as shown in FIG. 2(a), while capturing image data with an optical camera, the thermal shrinkage ratio (A'2) in the TD direction was calculated from the change in marker distance before and after heat treatment, obtained by an image-based motion capture device 14 according to formula (1), and evaluated according to the following criteria: ⊚: The thermal shrinkage ratio (A'2) was a value within the range of 30 to less than 65%. ◯: The thermal shrinkage ratio (A'2) was 20 to less than 30%, or 65% to less than 75%. △: The thermal shrinkage ratio (A'2) was 10 to less than 20%, or 75% to less than 85%. ×: The thermal shrinkage ratio (A'2) was less than 10% or more than 85%.

[0141] (9) Evaluation 9: Standard deviation (σ'2) of thermal shrinkage rate (A'2) in TD direction The standard deviation (σ'2) was calculated from the values ​​(n=6) of thermal shrinkage rate (A2') in TD direction obtained using image motion capture in Evaluation 8, and evaluated according to the following criteria. ⊚: The standard deviation of thermal shrinkage rate (A'2) is within 2.5%. ◯: The standard deviation of thermal shrinkage rate (A'2) is within 5%. △: The standard deviation of thermal shrinkage rate (A'2) is within 7.5%. ×: The standard deviation of thermal shrinkage rate (A'2) is more than 10%.

[0142] (10) Evaluation 10: Heat Shrinkage Rate The obtained polyester shrink film was floated in 80°C hot water in a hot water bath for 10 seconds and heat-shrunk for at least 10 seconds while being measured using an image-based motion capture system. That is, while capturing image data with an optical camera, the heat shrinkage rate in the main shrinkage direction was calculated from the change in distance of a predetermined marker before and after a predetermined time, obtained by image-based motion capture, according to formula (2), and evaluated according to the following criteria. In calculating the heat shrinkage rate, the distance PL0 of a predetermined section before heat shrinkage was set to 10 mm, and measurements were taken at 0.1-second intervals. Excellent: The heat shrinkage rate was 4 mm / sec or more. ◯: The heat shrinkage rate was 3 mm / sec or more but less than 4 mm / sec. △: The heat shrinkage rate was 2 mm / sec or more but less than 3 mm / sec. ×: The heat shrinkage rate was less than 2 mm / sec.

[0143] (11) Evaluation 11: Minimum Intermediate Heat Shrinkage Speed ​​The obtained polyester shrink film was thermally shrunk by floating it on 80°C hot water in a hot water bath for 10 seconds. Next, while capturing image data with an optical camera, the thermal shrinkage rate in the main shrinkage direction (number of predetermined sections n = 6) was obtained by image-based motion capture. The intermediate heat shrinkage speed was calculated according to formula (4). The minimum intermediate heat shrinkage speed in the section with the largest maximum intermediate heat shrinkage speed among the predetermined sections was used to evaluate the film according to the following criteria. The distance PL0 of the predetermined section before heat shrinkage was set to 10 mm, and the measurement period t3-t2 was set to 0.1 seconds. Excellent: The minimum intermediate heat shrinkage speed was 0 mm / sec or greater. Good: The minimum intermediate heat shrinkage speed was -1.5 mm / sec or greater. Fair: The minimum intermediate heat shrinkage speed was -2.5 mm / sec or greater. ×: The minimum value of the intermediate heat shrinkage speed is less than −2.5 mm / sec.

[0144] [Example 2] 1. Preparation of Polyester-Based Shrink Film In Example 2, a raw sheet having a thickness of 200 μm was prepared in the same manner as in Example 1, except that 100 parts by weight of amorphous polyester resin (PETG2) was used in the stirring vessel as shown in Table 1. Next, a polyester-based shrink film having a thickness of 40 μm was prepared from the raw sheet using a shrink film manufacturing device at a preheating temperature of 75°C, a stretching temperature of 75°C, a stretch ratio (MD direction: 105%, TD direction: 500%), and a heat setting temperature of 60°C.

[0145] 2. Evaluation of Polyester-Based Shrink Film In Example 2, the thickness variation of the obtained polyester-based shrink film (Evaluation 1), the thermal shrinkage rate in the transverse direction measured by image-based motion capture (Evaluation 2 and Evaluation 4), and the standard deviation of the thermal shrinkage rate in the transverse direction measured by image-based motion capture (Evaluation 3) were measured and evaluated in the same manner as in Example 1. The results are shown in Tables 2 and 3.

[0146] Comparative Example 1 1. Preparation of Polyester-Based Shrink Film In Comparative Example 1, a raw sheet having a thickness of 200 μm was prepared in the same manner as in Example 1, except that 50 parts by weight of amorphous polyester resin (PETG3) and 50 parts by weight of amorphous polyester resin (PETG4) were used in the stirring vessel as shown in Table 1. Next, using a shrink film manufacturing device, a polyester-based shrink film having a thickness of 40 μm was prepared from the raw sheet at a preheating temperature of 90°C, a stretching temperature of 90°C, a stretch ratio (MD direction: 105%, TD direction: 500%), and a heat setting temperature of 60°C.

[0147] 2. Evaluation of Polyester-Based Shrink Film In Comparative Example 1, the obtained polyester-based shrink film was evaluated for thickness variation (Evaluation 1), thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 2 and Evaluation 4), and standard deviation of thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 3), in the same manner as in Example 1. The results are shown in Tables 2 and 3.

[0148] Comparative Example 2 1. Preparation of Polyester-Based Shrink Film In Comparative Example 2, a raw sheet having a thickness of 200 μm was prepared in the same manner as in Example 1, except that 100 parts by weight of amorphous polyester resin (PETG4) was used in the stirring vessel as shown in Table 1. Next, a polyester-based shrink film having a thickness of 40 μm was prepared from the raw sheet using a shrink film manufacturing device at a preheating temperature of 90°C, a stretching temperature of 90°C, a stretch ratio (MD direction: 105%, TD direction: 500%), and a heat setting temperature of 60°C.

[0149] 2. Evaluation of Polyester-Based Shrink Film In Comparative Example 2, the obtained polyester-based shrink film was evaluated for thickness variation (Evaluation 1), thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 2 and Evaluation 4), and standard deviation of thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 3), in the same manner as in Example 1. The results are shown in Tables 2 and 3.

[0150] Comparative Example 3 1. Preparation of Polyester-Based Shrink Film In Example 2, a raw sheet having a thickness of 200 μm was prepared in the same manner as in Example 1, except that 100 parts by weight of amorphous polyester resin (PETG3) was used in the stirring vessel as shown in Table 1. Next, using a shrink film manufacturing device, a polyester-based shrink film having a thickness of 40 μm was prepared from the raw sheet at an extrusion temperature of 260°C, a preheating temperature of 90°C, a stretching temperature of 90°C, a stretch ratio (MD direction: 105%, TD direction: 500%), and a heat setting temperature of 60°C.

[0151] 2. Evaluation of Polyester-Based Shrink Film In Comparative Example 3, the obtained polyester-based shrink film was evaluated for thickness variation (Evaluation 1), thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 2 and Evaluation 4), and standard deviation of thermal shrinkage in the transverse direction measured by image-based motion capture (Evaluation 3), in the same manner as in Example 1. The results are shown in Tables 2 and 3.

[0152]

[0153]

[0154]

[0155] According to the present invention, by using motion capture to limit at least the heat shrinkage rate measured under predetermined conditions to a predetermined range, it is possible to quickly and accurately evaluate and provide polyester shrink films and the like that exhibit excellent wrinkle resistance. Therefore, the polyester shrink film of the present invention can be applied to various PET bottles and the like, significantly expanding its versatility and having extremely high industrial applicability.

Claims

1. A polyester-based shrink film having a predetermined heat shrinkage rate obtained using motion capture, wherein two measurement positions are set in the TD direction, which is the main shrinkage direction of the polyester-based shrink film as the object to be measured, the distance between the two measurement positions is L1, and the distance between the two measurement positions after the polyester-based shrink film is heat shrunk is L'1 measured using the motion capture, the polyester-based shrink film has a heat shrinkage rate in the main shrinkage direction (temperature: 70-98°C, time: 1-60 seconds) of 20% or more, calculated based on the following formula (1):

2. The polyester shrink film according to claim 1, characterized in that the standard deviation of the heat shrinkage rate is 15% or less.

3. A polyester-based shrink film as described in claim 1 or 2, characterized in that the thickness of the polyester-based shrink film is in the range of 10 to 200 μm, and the difference between the maximum thickness and the average thickness is within 10 μm.

4. A polyester-based shrink film as described in claim 1 or 2, characterized in that the two measurement positions are set in multiple locations, and the average of the thermal shrinkage rates in the TD direction obtained at the multiple locations is taken as the thermal shrinkage rate in the TD direction.

5. A polyester shrink film according to claim 1 or 2, characterized in that the motion capture is an image-type motion capture that detects information from a specified marker.

6. A polyester shrink film as described in claim 1 or 2, characterized in that the motion capture device is equipped with a camera for recording the thermal shrinkage state of the polyester shrink film.

7. A polyester-based shrink film as described in claim 1 or 2, characterized in that the heat shrinkage rate of the polyester-based shrink film is measured using at least one heat shrinkage device selected from the group consisting of a constant temperature bath, a steam bath, a hot water bath, a liquid bath for a fluorine-containing compound, a steam bath for a fluorine-containing compound, and an infrared irradiation device.

8. A polyester-based shrink film as described in claim 1 or 2, characterized in that the thermal shrinkage rate in a direction perpendicular to the main shrinkage direction of the polyester-based shrink film as the measured object is measured using the motion capture at the same time as measuring the thermal shrinkage rate in the TD direction, and the thermal shrinkage rate in the MD direction is set to a value within the range of -5 to 5%.

9. A polyester-based shrink film as described in claim 1 or 2, characterized in that a calibration curve showing the relationship between the heat shrinkage temperature and heat shrinkage time in the main shrinkage direction of the polyester-based shrink film as the object to be measured, and the heat shrinkage rate in the TD direction is prepared in advance, and the calibration curve is compared and verified with the heat shrinkage rate obtained based on formula (1), and the heat shrinkage rate obtained based on formula (1) is set to a value within ±10% of the heat shrinkage rate in the TD direction obtained from the calibration curve.

Citation Information

Patent Citations

  • Heat-shrinkable polyester-based film

    JP2010100002A

  • Method for measuring heat shrinkage behavior of film

    JP2011075372A

  • Labeled container and method for manufacturing labeled container

    JP2022087090A

Cited By

  • Polyester-based heat-shrinkable film and method for manufacturing polyester-based resin film

    JP7793256B1

  • Polyester-based heat-shrinkable film and method for producing polyester-based resin film

    WO2025197668A1

  • Polyester-based heat-shrinkable film and method for producing polyester-based heat-shrinkable film

    WO2025197669A1