Active energy ray-curable composition, adhesive, and adhesive sheet
The polyester-based active energy ray-curable composition addresses thermal stability and adhesive strength issues by using polyhydric carboxylic acids and photoreactive compounds, offering improved curability and environmental sustainability.
Patent Information
- Application Number
- PCT/JP2024/012740
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional active energy ray-curable adhesives face challenges with thermal stability and adhesive strength due to the inclusion of unsaturated groups, which lead to increased viscosity and gelation during hot-melt processing, and existing solvent-based adhesives have environmental concerns.
A polyester-based active energy ray-curable composition incorporating structural units from polyhydric carboxylic acids, polyhydric alcohols, and compounds with photoreactive groups, minimizing the use of unsaturated groups and optimizing thermal stability and adhesive strength.
The solution provides excellent active energy ray curability, thermal stability, and adhesive strength without the need for unsaturated groups, making it suitable for solvent-free adhesives and reducing environmental impact.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Active energy ray-curable composition, adhesive, and adhesive sheet
[0001] The present invention relates to an active energy ray-curable composition, and an adhesive and adhesive sheet which are cured products of the active energy ray-curable composition. More specifically, the present invention relates to an active energy ray-curable composition, an adhesive, and an adhesive sheet which have excellent curability by active energy rays without having an unsaturated group, and further an adhesive sheet produced using the same which has excellent heat resistance, adhesive strength, and holding power.
[0002] Polyesters have been used in a wide range of applications, such as films, PET bottles, fibers, toners, electrical components, adhesives, and pressure-sensitive adhesives, due to their excellent heat resistance, chemical resistance, durability, and mechanical strength. In addition, polyesters have high polarity due to their polymer structure, and are known to exhibit excellent adhesion to polar polymers such as polyester, polyvinyl chloride, polyimide, and epoxy resin, as well as to metal materials such as copper and aluminum.
[0003] Solvent-based adhesives, in which adhesive polymers are dissolved in a solvent, have traditionally been used as adhesives for adhesive sheets such as adhesive labels and adhesive tapes. In recent years, solvent-free adhesives, which do not use organic solvents, have been attracting attention as a way to reduce environmental impact through VOC (Volatile Organic Compounds) regulations and greenhouse gas emissions reductions. Examples of solvent-free adhesives include water-based adhesives, in which the adhesive is dispersed or dissolved in water, and active energy ray-curable adhesives, which are cured by active energy rays such as ultraviolet light. Water-based adhesives have performance issues, such as a larger amount of energy required to volatilize water compared to solvent-based adhesives and poorer water resistance compared to solvent-based adhesives due to the influence of emulsifiers contained in the base resin. Furthermore, in order to increase the cohesive strength of an active energy ray-curable adhesive, it is necessary to incorporate into the structure unsaturated groups that react with active energy rays to become crosslinking points, or to contain a compound with an unsaturated group in the adhesive, but there have been problems with thermal stability, such as the unsaturated groups reacting with heat during hot melt coating, increasing viscosity, causing gelation, etc. For this reason, solvent-free adhesives used in hot melt coating are required to have high thermal stability and adhesive performance equal to or better than that of solvent-based adhesives.
[0004] Patent Document 1 discloses a photocrosslinkable polyester-based pressure-sensitive adhesive composition comprising a polyester having an unsaturated group, a photoinitiator, and a crosslinking agent.
[0005] Furthermore, Patent Document 2 discloses a photocrosslinkable pressure sensitive adhesive for optical members, which comprises a polyester, an unsaturated group-containing compound, a polymerization initiator, and a crosslinking agent.
[0006] Patent Document 3 discloses a radiation-curable, removable pressure-sensitive adhesive sheet comprising polyester, a radiation-curable resin having an unsaturated group, a radiation reaction initiator, and a crosslinking agent.
[0007] Furthermore, Patent Document 4 discloses an ultraviolet-curable composition comprising an epoxidized oil or fat having an ultraviolet-active site and a polycarboxylic acid.
[0008] JP 2009-102476 A JP 2009-209279 A JP 2010-59336 A JP 2022-535379 A
[0009] In recent years, there has been a demand for environmentally friendly adhesives, such as biomass adhesives made from plant-derived materials and solvent-free adhesives that do not use organic solvents, in order to reduce the environmental impact.Conventional heat-curing adhesives are made from petroleum-based materials and are diluted with organic solvents, which poses environmental challenges due to the generation of VOCs that can cause environmental pollution and the CO2 emissions that occur when they are burned and disposed of.
[0010] Furthermore, conventionally used active energy ray-curable adhesives have required the introduction of unsaturated groups into the adhesive as active energy ray-curable components, the incorporation of unsaturated group-containing compounds, or the inclusion of thermosetting crosslinking agents, etc. Because the unsaturated groups and crosslinking agent components undergo a reaction due to heat, their use in solvent-free adhesive applications involving high-temperature heating processes such as hot melt adhesives has been difficult due to problems with thermal stability, such as an increase in viscosity during the manufacturing process, gelation, and thermal decomposition.
[0011] For example, Patent Document 1 discloses a technique related to a polyester-based photocrosslinkable pressure-sensitive adhesive composition, and since the polyester-based resin has an unsaturated group derived from (meth)acrylate as a photocrosslinking component, there remains a problem with thermal stability.
[0012] Furthermore, Patent Document 2 discloses a technology relating to a photo- and / or thermally crosslinkable pressure-sensitive adhesive for optical components, and since an unsaturated group-containing compound and a thermosetting crosslinking agent are used as the pressure-sensitive adhesive composition, crosslinking proceeds due to heat, which causes problems with thermal stability and leaves room for improvement in hot-melt coating suitability.
[0013] Patent Document 3 discloses a technology relating to a radiation-curable removable pressure-sensitive adhesive sheet, which contains a large amount of a radiation-curable resin having an unsaturated group, and therefore has problems with thermal stability and adhesive strength.
[0014] Patent Document 4 discloses a technique related to an ultraviolet-curable composition comprising an epoxidized oil or fat having an ultraviolet-active site and a polycarboxylic acid. Although the composition does not contain an unsaturated group as an active energy ray-curable component, the composition contains an epoxy group, which reacts with a carboxy group due to heat, and ring-opening polymerization of the epoxy group progresses, so that there remains a problem in thermal stability at high temperatures.
[0015] In view of the above, the present invention provides an active energy ray-curable composition, a pressure-sensitive adhesive, and a pressure-sensitive adhesive sheet that are excellent in adhesive strength, holding power, and thermal stability.
[0016] However, the present inventors have conducted extensive research in light of these circumstances and have found that an active energy ray-curable composition containing a polyester having a structural unit derived from a polycarboxylic acid, a structural unit derived from a polyhydric alcohol, and a structural unit derived from a compound having a photoreactive group does not contain an unsaturated group that causes a decrease in thermal stability, and provides a composition that is excellent in active energy ray curability, and further has excellent thermal stability, adhesive strength, and holding power.
[0017] Furthermore, the present inventors have conducted extensive research in light of the above circumstances and have found that an active energy ray-curable pressure-sensitive adhesive composition containing a polyester having a structural unit derived from a polyvalent carboxylic acid and a structural unit derived from a polyhydric alcohol, and a compound having a photoreactive group, has excellent active energy ray curability without containing unsaturated groups that cause a decrease in thermal stability, and further has excellent thermal stability, adhesive strength, and holding power.
[0018] That is, the gist of the present invention is the following [1] to
[16] . [1] An active energy ray-curable composition containing a polyester (A) having structural units derived from a polycarboxylic acid (α) and structural units derived from a polyhydric alcohol (β), wherein the polyester (A) further comprises a polyester (A1) having structural units derived from a compound (B) having a photoreactive group. [2] An active energy ray-curable composition containing a polyester (A) having structural units derived from a polycarboxylic acid (α) and a polyhydric alcohol (β), and a compound (B) having a photoreactive group, wherein the content of the polymerizable unsaturated group-containing compound (C) contained in the active energy ray-curable composition is less than 15 parts by mass per 100 parts by mass of the polyester (A). [3] The active energy ray-curable composition according to [1], further comprising a polyester (A2) having structural units derived from a polycarboxylic acid (α) and a polyhydric alcohol (β), but not having structural units derived from a compound (B) having a photoreactive group. [4] The active energy ray-curable composition according to [1] or [3], wherein the compound (B) having a photoreactive group is a compound (b1) having a hydrogen abstraction type photoreactive group and / or a compound (b2) having a cleavage type photoreactive group. [5] The active energy ray-curable composition according to any one of [1], [3], and [4], wherein a structural unit derived from the compound (B) having a photoreactive group is incorporated into the main chain of the polyester (A1) via an ester bond. [6] The active energy ray-curable composition according to any one of [1] and [3] to [5], wherein the compound (B) having a photoreactive group is a polycarboxylic acid (α). [7] The active energy ray-curable composition according to [2], wherein the compound (B) having a photoreactive group is a hydrogen abstraction type photopolymerization initiator. [8] The active energy ray-curable composition according to [2] or [7], wherein the compound (B) having a photoreactive group does not have a carboxy group or a hydroxy group as a functional group. [9] The active energy ray-curable composition according to any one of [1] to [8], wherein the glass transition temperature of the polyester (A) is −80 to 30° C.
[10] The active energy ray-curable composition according to any one of [1] to [9], wherein the weight average molecular weight of the polyester (A) is 5,000 to 500,000.
[11] The active energy ray-curable composition according to any one of [1] to
[10] , wherein the unsaturated group concentration of the polyester (A) is 1 mmol / g or less.
[12] The active energy ray-curable composition according to any one of [1] to
[11] , wherein the melt viscosity change rate before and after heating at 200°C for 3 hours is 20 to 500%.
[13] The active energy ray-curable composition according to any one of [1] to
[12] , wherein the content of organic solvent in the active energy ray-curable composition is less than 10 mass%.
[14] A pressure-sensitive adhesive which is a cured product of the active energy ray-curable composition according to any one of [1] to
[13] .
[15] The pressure-sensitive adhesive according to
[14] , wherein the gel fraction of the pressure-sensitive adhesive is 1 to 100%.
[16] A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive according to
[14] or
[15] .
[0019] The active energy ray-curable composition of the present invention can form a pressure-sensitive adhesive that is excellent in active energy ray curability, adhesive strength, holding power, and thermal stability, and is particularly effective as a solventless pressure-sensitive adhesive used for pressure-sensitive adhesive tapes and pressure-sensitive adhesive labels.
[0020] Generally, in order to improve the active energy ray curability, adhesive strength, and holding power of an active energy ray-curable composition, it has been necessary to include an unsaturated group-containing compound in the composition as a component curable by active energy rays. However, when an unsaturated group is present, polymerization is initiated by heat, and therefore viscosity increase and gelation occur in the hot-melt process of a solventless pressure-sensitive adhesive, which requires melting the resin at high temperatures, resulting in a problem of thermal stability and making it unusable.
[0021] In the present invention, by using a polyester having a photoreactive group, the composition has excellent active energy ray curability without containing unsaturated groups that become crosslinking points when exposed to active energy rays, and further has excellent thermal stability, adhesive strength, and holding power.
[0022] Furthermore, in the present invention, the active energy ray-curable composition contains a polyester and a compound having a photoreactive group, and therefore the composition does not contain an unsaturated group or a crosslinking agent that become a crosslinking point when exposed to active energy rays, which have been essential in the past, and therefore the composition has excellent active energy ray curability, as well as excellent thermal stability, adhesive strength, and holding power.
[0023] The configuration of the present invention will be described in detail below, but these are merely examples of preferred embodiments. In the present invention, the term "class" added after the name of a compound is a concept that encompasses not only the compound but also derivatives of the compound. For example, the term "carboxylic acid class" includes not only carboxylic acid but also carboxylic acid derivatives such as carboxylic acid salts, carboxylic acid anhydrides, carboxylic acid halides, and carboxylic acid esters. In the present invention, "structural unit derived from" does not only mean the structural unit of the compound, but also a structural unit chemically derived from the compound other than the structural unit of the compound. Furthermore, "X and / or Y (X and Y are optional structures)" means at least one of X and Y, and can mean three possibilities: X only, Y only, or X and Y.
[0024] An active energy ray-curable composition according to one embodiment of the present invention (hereinafter referred to as "the present composition 1") contains a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and the polyester (A) is a polyester (A1) which further has a structural unit derived from a compound (B) having a photoreactive group.
[0025]
[0033] Furthermore, an active energy ray-curable composition according to another embodiment of the present invention (hereinafter referred to as "the present composition 2") contains a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, and the content of the polymerizable unsaturated group-containing compound (C) contained in the present composition 2 is less than 15 parts by mass relative to 100 parts by mass of the polyester (A).
[0026] Hereinafter, the present compositions 1 and 2 may be collectively referred to simply as “the present compositions.” First, the polyester (A) will be described.
[0027] <Polyester (A)> As described above, the polyester (A) contains a structural unit derived from a polycarboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β) in the molecule. Such a polyester (A) is usually obtained by ester bonding the polycarboxylic acid (α) and the polyhydric alcohol (β).
[0028] Examples of the polyester (A) include polyester (A1) having a structural unit derived from a polycarboxylic acid (α), a structural unit derived from a polyhydric alcohol (β), and a structural unit derived from a compound (B) having a photoreactive group, and polyester (A2) having a structural unit derived from a polycarboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), but not having a structural unit derived from a compound (B) having a photoreactive group.
[0029] The present composition 1 contains the polyester (A1), and by containing the polyester (A1), the present composition 1 has excellent active energy ray curability, adhesive strength, holding power, tackiness, and thermal stability.
[0030] In addition, from the viewpoints of adhesive strength, holding power, and thermal stability, it is preferable that the composition 1 further contains a polyester resin (A2).
[0031] The present composition 2 contains a polyester (A), and the polyester (A) contained in the present composition 2 is preferably a polyester (A2) that does not contain a photoreactive group.
[0032] The content of the polyester (A) in the composition is 50% by mass or more, more preferably 60 to 99.5% by mass, even more preferably 70 to 99% by mass, particularly preferably 80 to 98.5% by mass, and especially preferably 85 to 98% by mass.
[0033] The content of the polyester (A1) is usually 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and may be 100% by mass, based on the amount of the polyester (A).
[0034] Furthermore, when the present composition contains polyester (A1) and polyester (A2), the mass ratio thereof [(A1) / (A2)] is usually 99 / 1 to 1 / 99, preferably 90 / 10 to 5 / 95, more preferably 80 / 20 to 10 / 90, even more preferably 70 / 30 to 15 / 85, and particularly preferably 60 / 40 to 20 / 80. When these mass ratios are within the above ranges, the composition tends to have excellent active energy ray curability, adhesive strength, holding power, and thermal stability.
[0035] [Polycarboxylic Acid (α)] Examples of the polycarboxylic acid (α) include aliphatic polycarboxylic acids (α1), aromatic polycarboxylic acids (α2), and alicyclic polycarboxylic acids (α3). The polycarboxylic acids (α) can be used alone or in combination. Among them, aliphatic polycarboxylic acids (α1) are preferred because they have excellent active energy curability and adhesive strength, and can reduce the melt viscosity when the polymer is further increased in molecular weight, resulting in excellent coating suitability.
[0036] Examples of the aliphatic polycarboxylic acid (α1) include saturated aliphatic dicarboxylic acids (α1-1) such as malonic acids, succinic acids, glutaric acids, adipic acids, trimethyladipic acids, pimelic acids, 3-methylglutaric acids, 2,2-dimethylglutaric acids, azelaic acids, sebacic acids, thiodipropionic acids, diglycolic acids, 1,9-nonanedicarboxylic acids, and hydrogenated dimer acids obtained by hydrogenating dimer acids derived from unsaturated monocarboxylic acids such as oleic acid, linoleic acid, linolenic acid, and erucic acid; and unsaturated aliphatic dicarboxylic acids (α1-2) such as fumaric acids, maleic acids, itaconic acids, and dimer acids derived from unsaturated monocarboxylic acids such as oleic acid, linoleic acid, linolenic acid, and erucic acid. Among these, saturated aliphatic dicarboxylic acids (α1-1) are preferred because of their excellent thermal stability, and succinic acids, adipic acids, azelaic acids, sebacic acids, and hydrogenated dimer acids are more preferred because of their excellent active energy ray curability, adhesive strength, and coatability.
[0037] Examples of the aromatic polycarboxylic acid (α2) include aromatic dicarboxylic acids such as terephthalic acids, isophthalic acids, orthophthalic acids, naphthalenedicarboxylic acids, biphenyldicarboxylic acids, furandicarboxylic acids, and thiophenedicarboxylic acids, trimellitic acids, trimesic acids, ethylene glycol bis(anhydrotrimellitates), glycerol tris(anhydrotrimellitates), pyromellitic acids, oxydiphthalic acids, 3,3',4,4'-benzophenonetetracarboxylic acids, 3,3',4,4'-diphenyltetracarboxylic acids, 3,3',4,4'-diphenylsulfonetetracarboxylic acids, 4,4'-(hexafluoroisopropylidene)diphthalic acids, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propanes, and other trivalent or higher aromatic polycarboxylic acids. Among these, aromatic dicarboxylic acids are preferred from the viewpoint of excellent hydrolysis resistance and cohesive strength, terephthalic acids, isophthalic acids, orthophthalic acids, naphthalenedicarboxylic acids, and furandicarboxylic acids are more preferred, and isophthalic acids, orthophthalic acids, and furandicarboxylic acids are particularly preferred from the viewpoint of reducing the crystallinity of the polyester and thereby improving tackiness and adhesive strength. The aromatic polycarboxylic acid (α2) also includes some compounds of the compound (B) having a photoreactive group, which will be described later.
[0038] Examples of the alicyclic polycarboxylic acid (α3) include cyclohexanedicarboxylic acids, cyclohexanediacetic acids, tetrahydrophthalic acids, and hexahydrophthalic acids.
[0039] When the polyester (A) has structural units derived from an aliphatic polycarboxylic acid (α1), the content of the structural units derived from the aliphatic polycarboxylic acid (α1) relative to the structural units derived from the polycarboxylic acid (α) is preferably 20 mol% or more, more preferably 30 to 100 mol%, even more preferably 40 to 98 mol%, particularly preferably 50 to 95 mol%, especially preferably 60 to 93 mol%, and most preferably 70 to 90 mol%. If the content of the structural units derived from the aliphatic polycarboxylic acid (α1) is too low, the active energy ray curability tends to decrease, the melt viscosity tends to increase, the hot melt coatability tends to deteriorate, and the glass transition temperature tends to increase, resulting in insufficient adhesive strength and tackiness. If the content is too high, the cohesive strength tends to be insufficient, resulting in insufficient holding power.
[0040] When the polyester (A) has structural units derived from saturated aliphatic dicarboxylic acid (α1-1), the content of the structural units derived from saturated aliphatic dicarboxylic acid (α1-1) relative to the structural units derived from polycarboxylic acid (α) is preferably 20 mol% or more, more preferably 30 to 100 mol%, even more preferably 40 to 98 mol%, particularly preferably 50 to 95 mol%, especially preferably 60 to 93 mol%, and most preferably 70 to 90 mol%. If the content of structural units derived from saturated aliphatic dicarboxylic acid (α1-1) is too low, the active energy ray curability tends to decrease, the melt viscosity tends to increase, which deteriorates hot melt coatability, and the glass transition temperature tends to increase, resulting in insufficient adhesive strength and tackiness. If the content is too high, the cohesive strength tends to be insufficient, resulting in insufficient holding power.
[0041] When the polyester (A) has structural units derived from an unsaturated aliphatic dicarboxylic acid (α1-2), the content of the structural units derived from the unsaturated aliphatic dicarboxylic acid (α1-2) relative to the structural units derived from the polycarboxylic acid (α) is preferably 30 mol % or less, more preferably 15 mol % or less, even more preferably 10 mol % or less, particularly preferably 5 mol % or less, especially preferably 3 mol % or less, and most preferably 0 mol %. If the content of the structural units derived from the unsaturated aliphatic dicarboxylic acid (α1-2) is too high, the thermal stability tends to be insufficient.
[0042] When the polyester (A) has structural units derived from an aromatic polycarboxylic acid (α2), the content of the structural units derived from the aromatic polycarboxylic acid (α2) relative to the structural units derived from the polycarboxylic acid (α) is preferably 80 mol% or less, more preferably 1 to 60 mol%, even more preferably 3 to 50 mol%, particularly preferably 5 to 40 mol%, and especially preferably 10 to 30 mol%. If the content of the structural units derived from the aromatic polycarboxylic acid (α2) is too low, the cohesive strength tends to be insufficient, and the holding power, heat resistance, and moist heat resistance tend to be insufficient. If the content is too high, the active energy ray curability tends to be reduced, the melt viscosity tends to be increased, which deteriorates the suitability for hot melt coating, and the glass transition temperature tends to be increased, which tends to result in insufficient tackiness and adhesive strength.
[0043] When the polyester (A) has structural units derived from alicyclic polycarboxylic acid (α3), the ratio of the structural units derived from alicyclic polycarboxylic acid (α3) to the structural units derived from polycarboxylic acid (α) is preferably 80 mol% or less, more preferably 1 to 60 mol%, even more preferably 3 to 50 mol%, particularly preferably 5 to 40 mol%, and especially preferably 10 to 30 mol%. If the content of the structural units derived from alicyclic polycarboxylic acid (α3) is too low, the cohesive strength tends to be insufficient, and the holding power, heat resistance, and moist heat resistance tend to be insufficient. If the content is too high, the active energy ray curability tends to be reduced, the melt viscosity tends to be increased, which deteriorates the suitability for hot melt coating, and the glass transition temperature tends to be increased, which tends to result in insufficient tackiness and adhesive strength.
[0044] The content ratio (molar ratio) of the structural units derived from aliphatic polycarboxylic acids (α1) to the structural units derived from aromatic polycarboxylic acids (α2) in the structural units derived from polycarboxylic acids (α) is preferably (structural units derived from aliphatic polycarboxylic acids (α1) / structural units derived from aromatic polycarboxylic acids (α2))=100 / 0 to 20 / 80, more preferably 99 / 1 to 40 / 60, particularly preferably 97 / 3 to 50 / 50, even more preferably 95 / 5 to 60 / 40, particularly preferably 93 / 7 to 65 / 35, and most preferably 90 / 10 to 70 / 30.
[0045] Furthermore, the content ratio (molar ratio) of the structural units derived from aliphatic polycarboxylic acids (α1) to the structural units derived from alicyclic polycarboxylic acids (α3) in the structural units derived from polycarboxylic acids (α) is preferably (structural units derived from aliphatic polycarboxylic acids (α1) / structural units derived from alicyclic polycarboxylic acids (α3))=100 / 0 to 20 / 80, more preferably 99 / 1 to 40 / 60, particularly preferably 97 / 3 to 50 / 50, even more preferably 95 / 5 to 60 / 40, particularly preferably 93 / 7 to 65 / 35, and most preferably 90 / 10 to 70 / 30.
[0046] The polyester (A) may contain, as structural units derived from the polyvalent carboxylic acid (α), for example, structural units derived from aromatic dicarboxylic acids having a sulfonic acid group, such as sulfoterephthalic acids, 5-sulfoisophthalic acids, 4-sulfophthalic acids, 4-sulfonaphthalene-2,7-dicarboxylic acids, and 5(4-sulfophenoxy)isophthalic acids, and structural units derived from aromatic dicarboxylic acid salts having a sulfonate group, such as metal salts or ammonium salts thereof. From the viewpoint of the moist heat resistance of the polyester (A), the content of these structural units is preferably 10 mol % or less, more preferably 5 mol % or less, particularly preferably 3 mol % or less, even more preferably 1 mol % or less, and most preferably 0 mol %, relative to the structural units derived from the polyvalent carboxylic acids (α).
[0047] [Polyhydric alcohol (β)] Examples of the polyhydric alcohol (β) include aliphatic polyhydric alcohol (β1), alicyclic polyhydric alcohol, and aromatic polyhydric alcohol. One or more types of polyhydric alcohol (β) can be used. Among them, aliphatic polyhydric alcohol (β1) is preferred because it has excellent active energy curability and adhesive strength, and can reduce the melt viscosity when the molecular weight is increased, resulting in excellent coating suitability.
[0048] Examples of the aliphatic polyhydric alcohol (β1) include linear aliphatic polyhydric alcohols (β1-1) such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and 1,10-decanediol, 1,2-propylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 2-ethyl-2-butylpropanediol. Examples of suitable polyhydric alcohols include dimer diols, which are reduced forms of dimer acids derived by dimerizing unsaturated monocarboxylic acids such as pentanediol, oleic acid, linoleic acid, linolenic acid, and erucic acid, and branched aliphatic polyhydric alcohols (β1-2) having a hydrocarbon group on at least one side chain, such as 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. Among these, linear aliphatic polyhydric alcohols (β1-1) are preferred because they lower the glass transition temperature and provide excellent adhesive strength and tackiness, with ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,5-pentanediol being more preferred, and ethylene glycol, 1,3-propanediol, and 1,4-butanediol being particularly preferred. Among these, branched aliphatic polyhydric alcohols (β1-2) having a hydrocarbon group in at least one side chain are preferred, and particularly preferred are 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and dimer diol, from the viewpoints of excellent active energy ray curability, hydrolysis resistance, and tackiness due to reduced crystallinity.
[0049] When the polyester (A) has a structural unit derived from a linear aliphatic polyhydric alcohol (β1-1), the content of the structural unit derived from the linear aliphatic polyhydric alcohol (β1-1) relative to the structural unit derived from the polyhydric alcohol (β) is preferably 10 to 100 mol%, more preferably 20 to 95 mol%, particularly preferably 30 to 90 mol%, even more preferably 35 to 85 mol%, and particularly preferably 40 to 80 mol%. If the content of the structural unit derived from the linear aliphatic polyhydric alcohol (β1-1) is too low, the adhesive strength, tackiness, and substrate adhesion tend to be insufficient, while if it is too high, the crystallinity of the polyester tends to be high, resulting in insufficient adhesive strength, tackiness, and active energy ray curability.
[0050] When the polyester (A) has structural units derived from a branched aliphatic polyhydric alcohol (β1-2) having a hydrocarbon group in at least one side chain, the proportion of structural units derived from the branched aliphatic polyhydric alcohol (β1-2) relative to the structural units derived from the polyhydric alcohol (β) is preferably 5 to 100 mol%, more preferably 10 to 90 mol%, particularly preferably 15 to 80 mol%, even more preferably 20 to 70 mol%, and particularly preferably 25 to 60 mol%. If the content of structural units derived from the branched aliphatic polyhydric alcohol (β1-2) is too low, the crystallinity of the polyester tends to be high, resulting in insufficient adhesive strength, tackiness, and active energy ray curability, while if the content is too high, the adhesive strength, tackiness, and substrate adhesion tend to be insufficient.
[0051] The content ratio (molar ratio) of the structural units derived from the linear aliphatic polyhydric alcohol (β1-1) to the structural units derived from the branched aliphatic polyhydric alcohol (β1-2) in the structural units derived from the polyhydric alcohol (β) is preferably structural units derived from the linear aliphatic polyhydric alcohol (β1-1) / structural units derived from the branched aliphatic polyhydric alcohol (β1-2) = 100 / 0 to 10 / 90, more preferably 95 / 5 to 20 / 80, particularly preferably 90 / 10 to 30 / 70, even more preferably 85 / 15 to 35 / 65, and particularly preferably 80 / 20 to 40 / 60.
[0052] Examples of the alicyclic polyhydric alcohol include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediol, tricyclodecanedimethanol, and spiroglycol.
[0053] Examples of the aromatic polyhydric alcohol include paraxylene glycol, metaxylene glycol, orthoxylene glycol, 1,4-phenylene glycol, ethylene oxide adducts of 1,4-phenylene glycol, bisphenols such as bisphenol A, bisphenol B, bisphenol E, bisphenol F, bisphenol AP, bisphenol BP, bisphenol P, bisphenol PH, bisphenol S, bisphenol Z, 4,4′-dihydroxybenzophenone, and bisphenol fluorene, and hydrogenated products thereof, as well as glycols such as ethylene oxide adducts and propylene oxide adducts obtained by adding 1 to several moles of ethylene oxide or propylene oxide to the hydroxyl groups of bisphenols.
[0054] Furthermore, in order to easily obtain a polymer having a desired molecular weight, the polyhydric alcohol (β) may be, for example, a polyester diol, a polyether diol, a polycaprolactone diol, a polycarbonate diol, a hydrogenated polybutadiene diol, or a hydrogenated polyisoprene diol.
[0055] Examples of the polyester diol include structural units derived from polyester diols obtained by dehydrating a diol component such as ethylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,10-decanediol, or octadecanediol with a dicarboxylic acid component such as succinic acid, methylsuccinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, 1,12-dodecanoic acid, 1,14-tetradecanedioic acid, terephthalic acid, isophthalic acid, or an acid anhydride or lower alkyl ester thereof, or a derivative thereof, either alone or in a mixture.
[0056] Commercially available polyester diols include, for example, polyester diols of 3-methyl-1,5-pentanediol and adipic acid, trade names of which are "Kuraray Polyol P-510," "Kuraray Polyol P-1010," "Kuraray Polyol P-2010," "Kuraray Polyol P-3010," and "Kuraray Polyol P-5010" (all manufactured by Kuraray Co., Ltd.).
[0057] Examples of the polyether diol include structural units derived from polyethylene glycol, polypropylene glycol, polytetramethylene glycol obtained by ring-opening polymerization of ethylene oxide, propylene oxide, tetrahydrofuran, etc., and copolyether glycol obtained by copolymerization of these.
[0058] Commercially available polyether diols include, for example, polyether diols obtained by adding propylene oxide to propylene glycol, such as trade names "ADEKA POLYETHER P-400," "ADEKA POLYETHER P-1000," "ADEKA POLYETHER P-2000," and "ADEKA POLYETHER P-3000" (all manufactured by ADEKA Corporation).
[0059] Examples of the polycaprolactone diol include structural units derived from caprolactone-based polyester diols obtained by ring-opening polymerization of cyclic ester monomers such as ε-caprolactone and δ-valerolactone.
[0060] Examples of commercially available polycaprolactone diols include those under the trade names "PLACCEL L205AL," "PLACCEL L212AL," "PLACCEL L220AL," "PLACCEL L220PL," and "PLACCEL L230AL" (all manufactured by Daicel Chemical Industries, Ltd.).
[0061] Examples of the polycarbonate diol include structural units derived from carbonate diols such as propylene carbonate diol, hexamethylene carbonate diol, and 3-methylpentene carbonate diol, and polycarbonate diols obtained by dealcoholization reaction of polyhydric alcohols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, and 1,9-nonanediol with dialkyl carbonates such as diethylene carbonate and dimethyl carbonate.
[0062] Examples of commercially available polycarbonate diols include those under the trade names "PLACCEL CD205," "PLACCEL CD210," "PLACCEL CD220," "PLACCEL CD205PL," "PLACCEL CD210PL," and "PLACCEL CD220PL" (all manufactured by Daicel Chemical Industries, Ltd.).
[0063] Examples of the hydrogenated polybutadiene polyol include structural units derived from hydrogenated polybutadiene polyols such as 1,2-polybutadiene polyols and 1,4-polybutadiene polyols in which the double bonds are saturated with hydrogen, halogen, or the like.
[0064] Examples of commercially available hydrogenated polybutadiene polyols include those under the trade names "GI-1000," "GI-2000," and "GI-3000" (all manufactured by Nippon Soda Co., Ltd.).
[0065] Examples of the hydrogenated polyisoprene polyol include structural units such as hydrogenated polyisoprene polyols in which the double bonds of polyisoprene polyols are saturated with hydrogen, halogen, or the like.
[0066] Examples of commercially available hydrogenated polyisoprene polyols include those under the trade name "Epole" (manufactured by Idemitsu Kosan Co., Ltd.).
[0067] [Trifunctional or higher polycarboxylic acid and trifunctional or higher polyhydric alcohol] For the purpose of improving cohesive strength by introducing a branched skeleton and enhancing curability by active energy rays, the polyester (A) preferably has a structural unit derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol described in the polycarboxylic acid (α) and polyhydric alcohol (β). In particular, when a crosslinked structure is formed by active energy rays, the polyester (A) having a branched skeleton increases the number of crosslinking points of the polyester (A), and a pressure-sensitive adhesive with high cohesive strength can be efficiently obtained with a small amount of active energy ray irradiation.
[0068] Examples of the trifunctional or higher polyvalent carboxylic acids include trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tris(anhydrotrimellitate), trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride. Examples of trifunctional or higher polyhydric alcohols include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. These trifunctional or higher polyvalent carboxylic acids and trifunctional or higher polyhydric alcohols can each be used alone or in combination.
[0069] When the polyester (A) contains structural units derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol as a branched skeleton, the content of the structural units derived from a trifunctional or higher polycarboxylic acid relative to the structural units derived from the polycarboxylic acid (α) and the content of the structural units derived from a trifunctional or higher polyhydric alcohol relative to the structural units derived from the polyhydric alcohol (β) are each preferably 0.1 to 5 mol%, more preferably 0.3 to 4 mol%, even more preferably 0.5 to 3 mol%, and particularly preferably 1 to 2.5 mol%. If the content of both or either one is too high, the mechanical properties such as elongation at break of the coating film formed by application of the pressure-sensitive adhesive tend to decrease, resulting in a decrease in adhesive strength, and gelation also tends to occur during polymerization.
[0070] When the polyester (A) contains structural units derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol as a branched skeleton, the content of the structural units derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol relative to 100% by mass of all structural units in the polyester (A) is preferably 0.1 to 3% by mass, more preferably 0.2 to 4% by mass, particularly preferably 0.3 to 3% by mass, even more preferably 0.4 to 2% by mass, or 0.5 to 1.5% by mass. If the content of the structural units derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol is too high, the mechanical properties such as elongation at break of the coating film formed by application of the pressure-sensitive adhesive tend to decrease, resulting in a decrease in adhesive strength, and gelation also tends to occur during polymerization.
[0071] [Compound (B) Having a Photoreactive Group] The polyester (A1) contained in the present composition 1 further contains, in addition to the structural unit derived from the polycarboxylic acid (α) and the structural unit derived from the polyhydric alcohol (β), a structural unit derived from the compound (B) having a photoreactive group, so that the polyester (A1) itself can be crosslinked by active energy rays.
[0072] Examples of the compound (B) having a photoreactive group include a compound (b1) having a hydrogen abstraction type photoreactive group and a compound (b2) having a cleavage type photoreactive group. These may be used alone or in combination of two or more. Among them, the compound (b1) having a hydrogen abstraction type photoreactive group is preferred because of its excellent active energy ray curability. However, the photoreactive group does not include ethylenically unsaturated groups such as vinyl groups, allyl groups, and acryloyl groups.
[0073] Furthermore, the compound (B) having a photoreactive group used in the polyester (A1) containing a photoreactive group preferably has one or more carboxy groups and / or hydroxy groups, more preferably two or more carboxy groups and / or hydroxy groups, and even more preferably two or more carboxy groups. Having two or more carboxy groups in the molecule is preferable in that the photoreactive group is incorporated into the main chain of the polyester through an ester bond, resulting in excellent active energy ray curability, thermal stability, and adhesive strength. That is, the compound (B) having a photoreactive group is preferably the polycarboxylic acid (α).
[0074] [Compound (b1) Having a Hydrogen Abstraction Reactive Group] The compound (b1) having a hydrogen abstraction photoreactive group is not particularly limited as long as it generates a radical by abstracting hydrogen from a hydrogen donor upon irradiation with active energy rays, and conventionally known compounds can be used. Examples of the compound (b1) having a hydrogen abstraction photoreactive group include benzophenones (b1-1), thioxanthones (b1-2), anthraquinones (b1-3), ketocoumarins, and camphorquinones. These compounds may be used alone or in combination of two or more. Among these, benzophenones (b1-1) are preferred because of their excellent active energy ray curability.
[0075] When the polyester (A1) contains a structural moiety derived from the compound (b1) having a hydrogen abstraction type photoreactive group, the polyester (A1) itself can undergo a hydrogen abstraction reaction in response to active energy rays without the need for an unsaturated group that can react with active energy rays and / or heat, a crosslinking agent, etc., and therefore a pressure-sensitive adhesive having excellent not only adhesive strength and holding power but also thermal stability and hot-melt coatability can be obtained. Furthermore, the hydrogen abstraction type photoreactive group possessed by the polyester (A1) is also preferred in that it can repeatedly function as an active species by re-irradiating with light even after being used in a photocuring reaction once.
[0076] The benzophenones (b1-1) are not particularly limited, but examples thereof include compounds represented by the following general formula (1).
[0077] The compound represented by the general formula (1) has at least one carboxy group or hydroxy group in the molecule.
[0078] Specific examples thereof include monofunctional hydroxybenzophenones having one hydroxy group in the molecule, such as 3-hydroxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 5-bromo-2-hydroxybenzophenone, 2-hydroxy-5-methylbenzophenone, and 4-chloro-4'-hydroxybenzophenone; monofunctional carboxybenzophenones having one carboxy group in the molecule, such as benzophenone-2-carboxylic acid, benzophenone-4-carboxylic acid, and 3',4'-dimethylbenzophenone-2-carboxylic acid; 2,3,4-tricarboxylic acid; Examples of suitable hydroxybenzophenones include polyhydroxybenzophenones having two or more hydroxy groups in the molecule, such as hydroxybenzophenone, 2,2'-dihydroxybenzophenone, 4,4'-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2,4,4'-trihydroxybenzophenone, and polycarboxybenzophenones having two or more carboxy groups in the molecule, such as benzophenone-2,4'-dicarboxylic acid, benzophenone-4,4'-dicarboxylic acid, and 3,3',4,4'-benzophenonetetracarboxylic dianhydride. Among these, polyhydroxybenzophenones and polycarboxybenzophenones are preferred, more preferably polycarboxybenzophenone, and particularly preferably 3,3',4,4'-benzophenonetetracarboxylic dianhydride, because of their excellent esterification reactivity and excellent active energy ray curability when incorporated into the main chain of the polyester (A).
[0079] The thioxanthones (b1-2) are not particularly limited, but examples thereof include compounds represented by the following general formula (2).
[0080] The compound represented by the general formula (2) has at least one carboxy group or hydroxy group in the molecule.
[0081] Specific examples include thioxanthone-2,3-dicarboxylic acid, thioxanthone-2,7-dicarboxylic acid, thioxanthone-2,6-dicarboxylic acid, and 2,2',3,3'-thioxanthonetetracarboxylic dianhydride.
[0082] The anthraquinones (b1-3) are not particularly limited, but examples thereof include compounds represented by the following general formula (3).
[0083] The compound represented by the general formula (3) has at least one carboxy group or hydroxy group in the molecule.
[0084] Specific examples include anthraquinone-2,3-dicarboxylic acid, anthraquinone-2,7-dicarboxylic acid, anthraquinone-2,6-dicarboxylic acid, and 2,2',3,3'-anthraquinonetetracarboxylic dianhydride.
[0085] [Compound (b2) having a cleavable photoreactive group] The compound (b2) having a cleavable photoreactive group is not particularly limited as long as it is photocleaved to generate a radical by irradiation with active energy rays, and conventionally known compounds can be used. Examples of the compound (b2) having a cleavable photoreactive group include benzoins, benzil ketals, hydroxyacetophenones, aminoacetophenones, and acylphosphine oxides. These may be used alone or in combination of two or more.
[0086] When the polyester (A1) contains a structural moiety derived from the compound (b2) having a cleavable photoreactive group, the polyester (A1) itself can react with active energy rays without the need for an unsaturated group or a crosslinking agent that can react with active energy rays and / or heat, and therefore a pressure-sensitive adhesive that is excellent not only in adhesive strength and holding power but also in thermal stability and hot-melt coatability can be obtained. In addition, the cleavable photoreactive group possessed by the polyester (A1) is also preferred in that it can repeatedly function as an active species by re-irradiating with light even after being used in a photocuring reaction once.
[0087] The compound (B) having a photoreactive group may be incorporated into the structure of the polyester (A) by chemical bonding with any functional group possessed by the polyester (A), but it is preferred that the structural unit derived from the compound (B) having a photoreactive group is incorporated into the main chain of the polyester (A1) by an ester bond. The method for incorporating the compound (B) having a photoreactive group into the polyester (A) can be any conventionally known chemical reaction, and among these, it is preferred to carry out an esterification reaction with the functional group derived from the polycarboxylic acid (α) and / or polyhydric alcohol (β) of the polyester (A) (excluding the epoxy ester bond formed by the reaction of an epoxy group with a carboxy group). Furthermore, when the compound (B) having a photoreactive group is a polycarboxylic acid (α), it is possible to carry out an esterification reaction between the polycarboxylic acid (α) containing the compound (B) having a photoreactive group and the polyhydric alcohol (β).
[0088] The content of the structural units derived from the compound (B) having a photoreactive group relative to 100 mol% of all structural units in the polyester (A1) is preferably 0.001 to 30 mol%, more preferably 0.01 to 15 mol%, particularly preferably 0.05 to 10 mol%, even more preferably 0.1 to 5 mol%, particularly preferably 0.2 to 3 mol%, more preferably 0.3 to 1.5 mol%, more preferably 0.4 to 1.25 mol%, and more preferably 0.5 to 1.0 mol%. If the content of the structural units derived from the compound (B) having a photoreactive group is too low, the active energy ray curability, adhesive strength, and holding power tend to be insufficient, while if it is too high, the crosslinking density of the polyester (A1) tends to be high, resulting in insufficient adhesive strength and tackiness, or the melt viscosity tends to be high, resulting in insufficient coatability.
[0089] Furthermore, the content of the structural units derived from the compound (B) having a photoreactive group relative to 100% by mass of all structural units in the polyester (A1) is preferably 0.001 to 30% by mass, more preferably 0.01 to 15% by mass, particularly preferably 0.1 to 10% by mass, even more preferably 0.2 to 5% by mass, particularly preferably 0.3 to 3% by mass, most preferably 0.4 to 1.5% by mass, and more preferably 0.5 to 1.0% by mass. If the content of the structural units derived from the compound (B) having a photoreactive group is too low, the active energy ray curability, adhesive strength, and holding power tend to be insufficient, whereas if it is too high, the crosslinking density of the polyester (A1) tends to be high, resulting in insufficient adhesive strength and tackiness, or the melt viscosity tends to be high, resulting in insufficient coatability.
[0090] [Cyclic Ester] The polyester (A) may contain, in addition to the structural unit derived from the polycarboxylic acid (α), the structural unit derived from the polyhydric alcohol (β), and the structural unit derived from the compound (B) having a photoreactive group, a structural unit derived from a cyclic ester in order to adjust the melt viscosity and glass transition temperature or to impart biodegradability, within a range that does not impair the effects of the present invention.
[0091] Examples of the cyclic ester include aliphatic lactones such as lactide, β-propiolactone, β-butyrolactone, γ-butyrolactone, γ-hexanolactone, γ-octanolactone, δ-valerolactone, δ-hexalanolactone, δ-octanolactone, ε-caprolactone, δ-dodecanolactone, α-methyl-γ-butyrolactone, β-methyl-δ-valerolactone, glycolide, and lactide. Of these, ε-caprolactone is preferred because of its excellent adhesive strength and biodegradability. These cyclic ester compounds may be used alone or in combination.
[0092] The structural units derived from the cyclic ester in the polyester (A) are preferably less than 140 mol%, more preferably less than 100 mol%, particularly preferably less than 60 mol%, even more preferably less than 30 mol%, particularly preferably less than 15 mol%, and most preferably 0 mol%, relative to 100 mol% of the structural units derived from the polycarboxylic acid (α). If the content of the structural units derived from the cyclic ester is too high, the polyester (A) tends to crystallize, resulting in a decrease in the active energy curability and adhesive strength, and an increase in melt viscosity, which deteriorates the suitability for hot melt coating.
[0093] Furthermore, the polyester (A) may contain a structural unit derived from a compound having both a carboxylic acid and a hydroxyl group in the molecule in order to adjust the melt viscosity and the glass transition temperature or to impart biodegradability, within a range that does not impair the effects of the present invention.
[0094] Examples of the compound having both a carboxylic acid and a hydroxyl group in the molecule include glycolic acid, lactic acid, hydroxybutyric acid, and hydroxyhexanoic acid. Among these, lactic acid and hydroxybutyric acid are particularly preferred because they increase the ester bond concentration and provide excellent adhesive strength and biodegradability. One or more of these compounds having a structural unit derived from a compound having both a carboxylic acid and a hydroxyl group in the molecule can be used.
[0095] In the polyester (A), the structural units derived from the compound having both a carboxylic acid and a hydroxyl group in the molecule are preferably 100 mol% or less, more preferably 80 mol% or less, particularly preferably 60 mol% or less, even more preferably 40 mol% or less, particularly preferably 20 mol% or less, and most preferably 10 mol% or less, relative to 100 mol% of the structural units derived from the polycarboxylic acid (α). If the content of the structural units derived from the compound having both a carboxylic acid and a hydroxyl group in the molecule is too high, the polyester (A) tends to crystallize, resulting in reduced activity energy curability and adhesive strength, and an increased melt viscosity, which deteriorates hot-melt coating suitability.
[0096] [Production of Polyester (A)] The polyester (A) can be produced by a known method. For example, in the case of polyester (A1), a polycarboxylic acid (α), a polyhydric alcohol (β), and a compound (B) having a photoreactive group are subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, followed by polycondensation to obtain a polyester, and further, if necessary, introducing a hydroxyl value and an acid value. In addition, in the case of polyester (A2), a polycarboxylic acid (α) and a polyhydric alcohol (β) are subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, followed by polycondensation to obtain a polyester, and further, if necessary, introducing a hydroxyl value and an acid value.
[0097] The temperature in the esterification reaction is usually 180 to 280° C., and the reaction time is usually 60 minutes to 8 hours.
[0098] The temperature in the polycondensation is usually 220 to 280° C., and the reaction time is usually 20 minutes to 4 hours. The polycondensation is preferably carried out under reduced pressure.
[0099] Examples of methods for introducing an acid value into a polyester include methods for introducing a carboxy group into a polyester by an acid addition method or a depolymerization method after an esterification reaction or reduced-pressure polycondensation. Among these, when a carboxy group is introduced into the main chain terminal of a polyester, the depolymerization method is particularly preferred because it allows for efficient introduction of a carboxy group. Furthermore, when a carboxy group is introduced into a side chain of a polyester, the acid addition method is preferred.
[0100] When a carboxy group is introduced into the main chain end of a polyester by the depolymerization method, in the case of polyester (A1), for example, a polycarboxylic acid (α), a polyhydric alcohol (β), and a compound (B) having a photoreactive group may be subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, followed by polycondensation and further depolymerization.In the case of polyester (A2), for example, a polycarboxylic acid (α) and a polyhydric alcohol (β) may be subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, followed by polycondensation and further depolymerization.
[0101] For depolymerization, it is preferable to use a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride groups from the viewpoint of adhesive strength. Examples of trivalent or higher polycarboxylic acids having 0 or 1 acid anhydride groups include compounds such as trimellitic acid, trimellitic anhydride, hydrogenated trimellitic anhydride, and trimesic acid. Preferred are trivalent or higher polycarboxylic acids having 1 acid anhydride group from the viewpoint of suppressing molecular weight reduction, such as trimellitic anhydride and hydrogenated trimellitic anhydride, with trimellitic anhydride being particularly preferred.
[0102] The temperature for depolymerization is usually 200 to 260° C., and the reaction time is usually 10 minutes to 3 hours.
[0103] When producing polyester (A) by depolymerization, if the content of structural units derived from a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride groups exceeds 20 mol% relative to 100 mol% of structural units derived from the polycarboxylic acid (α), the molecular weight of the resin tends to decrease significantly. Therefore, the content of structural units derived from a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride groups relative to 100 mol% of structural units derived from the polycarboxylic acid (α) is preferably 20 mol% or less, more preferably 1 to 15 mol%, particularly preferably 2 to 10 mol%, and even more preferably 3 to 8 mol%.
[0104] When the carboxyl group is introduced into the side chain of the polyester by the acid addition method, for example, a polycarboxylic acid (α) other than a polycarboxylic anhydride, a polyhydric alcohol (β), and a compound (B) having a photoreactive group are subjected to an esterification reaction to obtain a prepolymer, and then the resulting hydroxyl group-containing prepolymer is reacted with a polycarboxylic anhydride to perform acid addition. Note that, when a monocarboxylic acid, a dicarboxylic acid, or a polyfunctional carboxylic acid compound is used in the acid addition method, a decrease in molecular weight may occur due to ester exchange, so it is preferable to use a compound having at least one carboxylic anhydride.
[0105] Furthermore, methods for depolymerization and acid addition include direct addition in a bulk state and addition of a solution of the polyester. The reaction in the bulk state is fast, but gelation may occur if a large amount is added, and the reaction occurs at a high temperature, so care must be taken to prevent oxidation by blocking oxygen gas. On the other hand, addition in a solution state is slow, but allows for the stable introduction of a large number of carboxyl groups.
[0106] Examples of the polycarboxylic acid anhydride include succinic anhydride, maleic anhydride, orthophthalic anhydride, 2,5-norbornene dicarboxylic acid anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, 3,3',4,4'-diphenyltetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic acid dianhydride, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride.
[0107] When producing the polyester (A) by the acid addition method, if 15 mol % or more of the structural units derived from the polycarboxylic acid (α) are added with acid, gelation may occur. Therefore, it is preferable to add less than 15 mol % of the structural units with acid, based on 100 mol % of the structural units derived from the polycarboxylic acid (α).
[0108] [Compositional Ratio of Polyester (A)] The ratio of structural moieties derived from each component of the polyester (A) (compositional ratio) can be determined by a known method using NMR, for example, a method using a resonant frequency of 400 MHz. 1 H-NMR measurement (proton nuclear magnetic resonance spectroscopy), 13 It can be determined by C-NMR measurement (carbon-type nuclear magnetic resonance spectroscopy) or the like.
[0109] [Glass Transition Temperature of Polyester (A)] The glass transition temperature of the polyester (A) is preferably −80 to 30° C., more preferably −75 to 10° C., even more preferably −70 to −10° C., particularly preferably −65 to −20° C., even more preferably −60 to −30° C., especially preferably −55 to −35° C., and most preferably −50 to −40° C. If the glass transition temperature is too high, tackiness and adhesive strength tend to be insufficient, and the melt viscosity tends to increase, resulting in poor hot-melt coatability, while if the glass transition temperature is too low, holding power and heat resistance tend to be insufficient.
[0110] The glass transition temperature can be measured using a differential scanning calorimeter as follows: the measurement temperature range is −90 to 100° C., and the temperature rise rate is 10° C. / min.
[0111] [Acid value of polyester (A)] The acid value of the polyester (A) is preferably 30 mgKOH / g or less, more preferably 10 mgKOH / g or less, particularly preferably 5 mgKOH / g or less, even more preferably 3 mgKOH / g or less, particularly preferably 1 mgKOH / g or less, and most preferably 0.5 mgKOH / g or less. If the acid value is too high, the wet heat resistance tends to be insufficient, or the heat resistance tends to be reduced, making thermal decomposition more likely to proceed.
[0112] The definition and measurement method of the acid value are as follows. The acid value (mg KOH / g) can be determined by dissolving 1 g of polyester (A) in 30 g of a mixed solvent of toluene / methanol (for example, toluene / methanol = 7 / 3 by volume) and performing neutralization titration in accordance with JIS K 0070. In the present invention, the acid value of polyester (A) is determined by the content of carboxy groups in the resin.
[0113] [Hydroxyl value of polyester (A)] The hydroxyl value of the polyester (A) is preferably 50 mgKOH / g or less, particularly 1 to 30 mgKOH / g, further 2 to 20 mgKOH / g, more preferably 3 to 15 mgKOH / g, particularly preferably 4 to 10 mgKOH / g, and most preferably 5 to 8 mgKOH / g. If the hydroxyl value is too high, the active energy ray curability tends to decrease and the cohesive strength and holding power tend to be insufficient, while if the hydroxyl value is too low, the adhesive strength and adhesion tend to be insufficient and the compatibility with the tackifier resin tends to be poor.
[0114] The hydroxyl value of the polyester (A) is determined by neutralization titration in accordance with JIS K 0070.
[0115] [Isocyanate concentration of polyester (A)] The isocyanate concentration of the polyester (A) is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, particularly preferably 0.5% or less, especially preferably 0.3% or less, and most preferably 0.1% or less. The lower limit is 0%, and it is preferable that the polyester (A) does not contain an isocyanate group. If the isocyanate concentration is too high, the reaction proceeds due to the heat load during the production of the polyester (A) or during hot-melt coating, which tends to result in poor pot life, poor coating appearance, and reduced adhesive strength.
[0116] [Oxirane Oxygen Concentration of Polyester (A)] The oxirane oxygen concentration of the polyester (A) is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, particularly preferably 0.5% or less, especially preferably 0.3% or less, and most preferably 0.1% or less. The lower limit is 0%, and it is preferable that no oxirane oxygen (epoxy group) is contained. If the oxirane concentration is too high, the reaction proceeds due to the heat load during the production of polyester (A) or hot-melt coating, which tends to result in poor pot life, poor coating appearance, and reduced adhesive strength.
[0117] The oxirane oxygen concentration of the polyester (A) can be determined by titration using a solution of hydrogen bromide in acetic acid in accordance with ASTM-1652.
[0118] [Ester Bond Concentration of Polyester (A)] The ester bond concentration of the polyester (A) is preferably 2 to 14 mmol / g, more preferably 3 to 13 mmol / g, even more preferably 4 to 12 mmol / g, particularly preferably 5 to 11 mmol / g, especially preferably 5.5 to 10 mmol / g, and most preferably 6 to 9 mmol / g. If the ester bond concentration is too high, the melt viscosity tends to increase and the coatability tends to be insufficient, whereas if the ester bond concentration is too low, the heat resistance, substrate adhesion, and adhesive strength tend to be insufficient.
[0119] The definition and measurement method of the ester bond concentration are as follows. The ester bond concentration (mmol / g) refers to the number of moles of ester bonds in 1 g of polyester (A), and can be calculated, for example, from the amounts charged. This calculation is the value obtained by dividing the number of moles of the smaller of the charged amounts of polycarboxylic acid (α) and polyhydric alcohol (β) by the total mass of polyester (A), and an example of the calculation formula is shown below. Note that when the charged amounts of polycarboxylic acid (α) and polyhydric alcohol (β) are equal in molar amount, either of the calculation formulas below may be used. Furthermore, when a monomer having both a carboxyl group and a hydroxyl group is used, or when polyester is produced from caprolactone or the like, the calculation method will be changed appropriately.
[0120] (When the amount of polycarboxylic acid (α) is less than the amount of polyhydric alcohol (β)) Ester group concentration (mmol / g) = [(P1 / p1 × m1 + P2 / p2 × m2 + P3 / p3 × m3 ...) / Z] × 1000 P: Amount of polycarboxylic acid (α) charged (g) p: Molecular weight of polycarboxylic acid (α) m: Number of carboxy groups per molecule of polycarboxylic acid (α) Z: Finished mass (g)
[0121] (When the amount of polyhydric alcohol (β) is less than the amount of polycarboxylic acid (α)) Ester group concentration (mmol / g) = [(Q1 / q1 × n1 + Q2 / q2 × n2 + Q3 / q3 × n3 ...) / Z] × 1000 Q: Amount of polyhydric alcohol (β) charged (g) q: Molecular weight of polyhydric alcohol (β) n: Number of hydroxyl groups per molecule of polyhydric alcohol (β) Z: Finished mass (g)
[0122] The ester bond concentration can be measured by a known method using NMR or the like, for example, 1 H-NMR measurement (proton nuclear magnetic resonance spectroscopy), 13 It can also be measured by C-NMR measurement (carbon-type nuclear magnetic resonance spectroscopy).
[0123] [Unsaturated Group Concentration of Polyester (A)] The unsaturated group concentration of the polyester (A) is preferably less than 1.5 mmol / g per 1 g of polyester (A), more preferably 1.0 mmol / g or less, particularly preferably 0.5 mmol / g or less, even more preferably 0.3 mmol / g or less, particularly preferably 0.1 mmol / g or less, and most preferably 0.01 mmol / g or less. The lower limit is 0 mmol / g. If the unsaturated group concentration of the polyester (A) is too high, the unsaturated groups will react due to the heat load during the production of the polyester (A) or during hot melt coating, which will tend to result in poor pot life and coating appearance, and reduced adhesive strength. The unsaturated group concentration contained in the polyester (A) is 1 H-NMR measurement 13 It can be determined from a spectrum obtained by C-NMR measurement.
[0124] [Epoxy Group Concentration of Polyester (A)] The epoxy group concentration of the polyester (A) is preferably 5 mmol / g or less, more preferably 3 mmol / g or less, particularly preferably 2 mmol / g or less, even more preferably 1 mmol / g or less, particularly preferably 0.5 mmol / g or less, and most preferably 0.1 mmol / g or less, per 1 g of polyester (A). The lower limit is 0 mmol / g. If the epoxy group concentration of the polyester (A) is too high, the epoxy groups may react due to heat load during the production of the polyester (A) or hot melt coating, resulting in poor pot life, poor coating appearance, and reduced adhesive strength. The epoxy group concentration can be determined by taking the reciprocal of the epoxy equivalent calculated according to JIS K 7236.
[0125] [Peak Top Molecular Weight (Mp), Number Average Molecular Weight (Mn), and Weight Average Molecular Weight (Mw) of Polyester (A)] The peak top molecular weight (Mp) of the polyester (A) is preferably 5,000 to 150,000, more preferably 10,000 to 120,000, particularly preferably 20,000 to 100,000, even more preferably 30,000 to 90,000, and particularly preferably 40,000 to 80,000. If the peak top molecular weight (Mp) is too low, the active energy ray curability tends to decrease, the cohesive strength tends to be insufficient, and the heat resistance and wet heat durability tend to be insufficient. On the other hand, if the peak top molecular weight (Mp) is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coatability.
[0126] The number average molecular weight (Mn) of the polyester (A) is preferably 1,000 to 150,000, more preferably 2,500 to 120,000, particularly preferably 5,000 to 100,000, even more preferably 10,000 to 80,000, and particularly preferably 20,000 to 60,000. If the number average molecular weight (Mn) is too low, the active energy ray curability tends to decrease, the cohesive strength tends to be insufficient, and the heat resistance and wet heat durability tend to be insufficient. On the other hand, if the number average molecular weight (Mn) is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coatability.
[0127] The weight-average molecular weight (Mw) of the polyester (A) is preferably 5,000 to 500,000, more preferably 10,000 to 300,000, particularly preferably 20,000 to 200,000, even more preferably 30,000 to 150,000, particularly preferably 50,000 to 130,000, and most preferably 70,000 to 110,000. If the weight-average molecular weight (Mw) is too low, the active energy ray curability tends to decrease, the cohesive strength tends to be insufficient, and the heat resistance and wet heat durability tend to be insufficient. On the other hand, if the weight-average molecular weight (Mw) is too high, the substrate adhesion and adhesive strength tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coatability.
[0128] The peak top molecular weight (Mp), number average molecular weight (Mn), and weight average molecular weight (Mw) were measured as follows: Peak top molecular weight (Mp), number average molecular weight (Mn), and weight average molecular weight (Mw) were measured using a high performance liquid chromatograph (manufactured by Tosoh Corporation, "HLC-8320GPC") with a column (TSKgel SuperMultipore HZ-M (exclusion limit molecular weight: 2 × 10 6 The theoretical number of plates: 16,000 plates / plate, filler material: styrene-divinylbenzene copolymer, filler particle size: 4 μm) are measured in series, and the molecular weight can be calculated in terms of standard polystyrene.
[0129] The polydispersity of the polyester (A) is preferably 0.5 or more, more preferably 1 to 30, particularly preferably 1.5 to 20, even more preferably 2 to 15, especially preferably 2.5 to 10, and most preferably 3 to 8. If the polydispersity is too low, the active energy ray curability tends to decrease, the cohesive force tends to be insufficient, and the heat resistance and wet heat durability tend to be insufficient. If the polydispersity is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coatability. The polydispersity is calculated using the following formula: Polydispersity = Weight average molecular weight (Mw) / Number average molecular weight (Mn)
[0130] The melt viscosity (130°C) of the polyester (A) is preferably 500 Pa s or less, more preferably 1 to 400 Pa s or less, even more preferably 3 to 300 Pa s or less, particularly preferably 5 to 200 Pa s or less, particularly preferably 10 to 150 Pa s or less, and most preferably 15 to 100 Pa s. If the melt viscosity is too low, the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, while if it is too high, streaks tend to appear in the coating film appearance, resulting in insufficient coatability.
[0131] Furthermore, when the polyester (A) is a polyester (A1) containing a photoreactive group, its melt viscosity (160°C) is preferably 200 Pa s or less, more preferably 1 to 150 Pa s or less, even more preferably 2 to 100 Pa s or less, particularly preferably 3 to 80 Pa s or less, especially preferably 4 to 60 Pa s or less, and most preferably 5 to 40 Pa s. If the melt viscosity is too low, the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, while if it is too high, the coating film tends to have streaks in its appearance, resulting in insufficient coatability.
[0132] The melt viscosity is measured using a flow tester "CFT-500EX" (manufactured by Shimadzu Corporation) by a constant temperature method, at a test temperature of 130°C or 160°C, a residence time of 3 minutes, a test force of 30 (load of 3 kg), a die diameter of 1.0 mm, a die length of 10 mm, and a stroke of 20 mm, when the polyester is extruded from the nozzle.
[0133] From the viewpoint of thermal stability and coatability, it is preferable that the polyester (A) has a small rate of change in melt viscosity before and after thermal history (200°C x 3 hours, under air conditions). The rate of change in melt viscosity is preferably 20 to 500%, more preferably 30 to 400%, even more preferably 40 to 300%, particularly preferably 50 to 250%, especially preferably 60 to 200%, and most preferably 70 to 150%. If the rate of change in melt viscosity before and after thermal history is outside the above range, the adhesive may gel or decompose, resulting in insufficient coatability, adhesive strength, and adhesion.
[0134] In addition, the polyester (A) is preferably a non-crystalline polyester in terms of active energy ray curability, tackiness, optical properties, etc. If the polyester (A) is crystalline, the active energy ray curability, tackiness, molding stability, optical properties, etc. tend to be insufficient. The non-crystalline nature can be confirmed by a differential scanning calorimeter, and refers to, for example, a case in which no endothermic peak due to crystalline melting is observed when measured at a measurement temperature range of −90 to 400°C and a temperature rise rate of 10°C / min. The measurement temperature range and temperature rise rate can be changed appropriately depending on the sample.
[0135] The heat of crystalline fusion of the polyester (A) is preferably 0 J / g from the viewpoints of active energy ray curability, tackiness, optical properties, etc., but when crystallizing, it is 50 J / g or less, preferably 30 J / g or less, particularly preferably 10 J / g or less, especially preferably 5 J / g or less, more preferably 3 J / g or less, and most preferably 1 J / g or less.
[0136] Furthermore, the polyester (A) is preferably made from plant-derived raw materials and has a biomass degree in order to reduce the burden on the global environment. The biomass degree of the polyester (A) is preferably 10% or more, more preferably 20% or more, particularly preferably 30% or more, even more preferably 40% or more, particularly preferably 50% or more, and most preferably 60% or more. The upper limit is 100%. If the biomass degree is low, the reduction in the burden on the global environment tends to be insufficient.
[0137] Here, the biomass degree of the polyester (A) refers to the mass ratio of the plant-derived raw materials used in producing the polyester (A) incorporated into the resin relative to the total mass of the polyester (A), and is calculated as follows: The biomass degrees of the polycarboxylic acid (α) and the polyhydric alcohol (β) are determined from the weighted average of their respective biomass degrees. Any of the following calculation methods may be used as long as the value obtained falls within the above-mentioned range. (Calculation Method) Biomass Degree (%) = [(Number of moles of carbon of plant-derived monomers calculated from the molar ratio of the polycarboxylic acid (α) and the polyhydric alcohol (β) in the polyester (A)) / (Number of moles of carbon of all constituent monomers in the polyester (A))] × 100
[0138] The biomass ratio can also be determined by analyzing the composition ratio by NMR and calculating the carbon number of the plant-derived monomer / the total carbon number.
[0139] Furthermore, the biomass degree can also be measured by the method described in "Technology for Determining the Origin of Biofuels Using Natural Radioactive Carbon C-14," Tokyo Metropolitan Industrial Technology Research Center Research Report, No. 4, 2009.
[0140] <Compound (B) Having a Photoreactive Group> The present composition 1 may contain the above-mentioned compound (B) having a photoreactive group in order to increase the crosslinking efficiency of the polyester (A) by active energy rays. The present composition 2 also contains the compound (B) having a photoreactive group. By containing the compound (B) having a photoreactive group, the present composition 2 can have excellent active energy ray curability even without containing an unsaturated group or a crosslinking agent.
[0141] The compound (B) having a photoreactive group contained in the composition functions as a photopolymerization initiator. Examples of the compound (B) having a photoreactive group that functions as a photopolymerization initiator include the aforementioned compound (b1) having a hydrogen abstraction reactive group (hydrogen abstraction photopolymerization initiator) and compound (b2) having a cleavage photoreactive group (cleavage photopolymerization initiator). These may be used alone or in combination of two or more. Among these, the compound (b1) having a hydrogen abstraction reactive group (hydrogen abstraction photopolymerization initiator) is preferred in terms of excellent active energy ray curability. Furthermore, the compound (B) having a photoreactive group is preferably a compound (b1) having a hydrogen abstraction photoreactive group and / or a compound (b2) having a cleavage photoreactive group. It is more preferred to have at least one of the compound (b1) having a hydrogen abstraction reactive group and the compound (b2) having a cleavage photoreactive group in terms of excellent active energy ray curability.
[0142] When the compound (B) having a photoreactive group is used as a photopolymerization initiator, it is preferable that the compound (B) having a photoreactive group is not incorporated into the structure of the polyester (A) by a chemical bond and is contained therein independently in the composition, since this results in excellent optical properties after active energy ray curing, easy control of the degree of crosslinking, and excellent stability. Therefore, when the compound (B) having a photoreactive group is also used as a photopolymerization initiator, it is preferable that the compound (B) does not have an active hydrogen group such as a carboxy group or a hydroxy group, in terms of excellent active energy ray curability.
[0143] Examples of the compound (b1) having a hydrogen abstraction reactive group [hydrogen abstraction photopolymerization initiator] include the above-mentioned benzophenones (b1-1), thioxanthones (b1-2), anthraquinones (b1-3), ketocoumarins, and camphorquinones. These may be used alone or in combination of two or more. Among these, benzophenones (b1-1) are preferred because of their excellent active energy ray curability.
[0144] The benzophenones (b1-1) that can be used as a photopolymerization initiator are not particularly limited, and examples thereof include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, methyl o-benzoylbenzoate, 3,3'-dimethyl-4-methoxybenzophenone, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 4-morpholinobenzophenone, 4,4'-diphenoxybenzophenone, 4-hydroxybenzophenone, 2-carboxybenzophenone, etc. Among these, benzophenone and 4-methylbenzophenone are preferred because of their excellent active energy ray curability.
[0145] Examples of commercially available benzophenones (b1-1) that can be used as such photopolymerization initiators include those under the trade names "Omnirad BP Flakes," "Omnirad 4MBZ Flakes," "Omnipol PB," "Esacure TZT," "Esacure TZM," "Omnirad 4PBZ," "Omnirad 81," "Omnirad BMF," and "Omnirad OMBB" (all manufactured by IGM REJINS).
[0146] The thioxanthone (b1-2) that can be used as a photopolymerization initiator is not particularly limited, but examples thereof include 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone.
[0147] The anthraquinones (b1-3) that can be used as the photopolymerization initiator are not particularly limited, but examples thereof include 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 2-aminoanthraquinone.
[0148] Furthermore, examples of the compound (b2) having a cleavable photoreactive group that can be used as a photopolymerization initiator [cleavable photopolymerization initiator] include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}phenyl]-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), phenylglyoxylic acid methyl ester, and the like. methyl, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof.
[0149] Examples of commercially available products of the compound (b2) having a cleavable photoreactive group that can be used as such a photopolymerization initiator include products under the trade names "Omnirad 651," "Omnirad 184," "Omnirad 1173," "Omnirad 2959," "Omnirad 127," "Omnirad 907," "Omnirad 369," and "Omnirad TPO H" (all manufactured by IGM REJINS).
[0150] When the compound (B) having a photoreactive group is used as a photopolymerization initiator, the content thereof is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 0.3 to 8 parts by mass, particularly preferably 0.5 to 7 parts by mass or less, particularly preferably 1 to 6 parts by mass, and most preferably 1.5 to 5.5 parts by mass, relative to 100 parts by mass of the polyester (A). If the content is too high, the cohesive strength of the adhesive layer after active energy ray curing tends to become too high, resulting in a decrease in adhesive strength, whereas if the content is too low, the active energy ray curability tends to decrease, resulting in insufficient adhesive strength and cohesive strength.
[0151] Furthermore, when the compound (b1) having a hydrogen abstraction reactive group is used as a photopolymerization initiator, the content thereof is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 0.3 to 8 parts by mass, particularly preferably 0.5 to 7 parts by mass or less, particularly preferably 1 to 6 parts by mass, and most preferably 1.5 to 5.5 parts by mass, relative to 100 parts by mass of the polyester (A). If the content is too high, the cohesive strength of the pressure-sensitive adhesive after active energy ray curing tends to become too high, resulting in a decrease in adhesive strength, whereas if the content is too low, the active energy ray curability tends to decrease, resulting in insufficient adhesive strength and cohesive strength.
[0152] In addition, as an auxiliary agent for enhancing the reactivity of the compound (B) having a photoreactive group, triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, etc. may be used in combination. These auxiliary agents may be used alone or in combination of two or more.
[0153] <Unsaturated Group-Containing Compound (C)> The present composition may contain an unsaturated group-containing compound (C), which is a component that is cured by active energy rays in order to enhance cohesive strength. Examples of the unsaturated group-containing compound include a urethane (meth)acrylate compound and an ethylenically unsaturated monomer having an ethylenically unsaturated group.
[0154] The urethane (meth)acrylate compound is a (meth)acrylate compound having a urethane bond in the molecule, and can be produced by reacting a hydroxyl group-containing (meth)acrylic compound with a polyvalent isocyanate compound, and further, if necessary, with a polyol.
[0155] Examples of the hydroxyl group-containing (meth)acrylic compound include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate. Examples of suitable acrylates include pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified dipentaerythritol penta(meth)acrylate, and ethylene oxide-modified pentaerythritol tri(meth)acrylate. Among these, hydroxyl group-containing (meth)acrylic compounds having three or more acryloyl groups are preferred. These may be used singly or in combination of two or more.
[0156] The polyisocyanate compound is not particularly limited, and examples thereof include aromatic, aliphatic, and alicyclic polyisocyanates, among which tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate. Examples of the polyisocyanate include polyisocyanates such as tetramethylxylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, phenylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and naphthalene diisocyanate, as well as trimer compounds or polymer compounds of these polyisocyanates, biuret-type polyisocyanates, and reaction products of these polyisocyanates with polyols.
[0157] Such polyols are not particularly limited, and examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, butylene glycol, polybutylene glycol, 1,6-hexanediol, neopentyl glycol, cyclohexanedimethanol, hydrogenated bisphenol A, polycaprolactone, trimethylolethane, trimethylolpropane, polytrimethylolpropane, pentaerythritol, polypentaerythritol, sorbitol, mannitol, glycerin, and polyglycerin. and polytetramethylene glycol; polyether polyols having at least one structure of polyethylene oxide, polypropylene oxide, or block or random copolymerization of ethylene oxide / propylene oxide; polyester polyols which are condensates of such polyhydric alcohols or polyether polyols with polybasic acids such as maleic anhydride, maleic acid, fumaric acid, itaconic anhydride, itaconic acid, adipic acid, and isophthalic acid; caprolactone-modified polyols such as caprolactone-modified polytetramethylene polyol; polyolefin polyols; and polybutadiene polyols such as hydrogenated polybutadiene polyols.
[0158] Further examples of such polyols include carboxy group-containing polyols such as 2,2-bis(hydroxymethyl)butyric acid, tartaric acid, 2,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxyethyl)propionic acid, 2,2-bis(hydroxypropyl)propionic acid, dihydroxymethylacetic acid, bis(4-hydroxyphenyl)acetic acid, 4,4-bis(4-hydroxyphenyl)pentanoic acid, and homogentisic acid; and sulfonic acid group- or sulfonate salt group-containing polyols such as 1,4-butanediol sodium sulfonate.
[0159] The method for producing the urethane (meth)acrylate compound is not particularly limited, and examples thereof include a method in which a hydroxyl group-containing (meth)acrylic compound and a polyvalent isocyanate compound are mixed in an inert gas atmosphere and reacted for 2 to 10 hours, typically at 30 to 80° C. In this reaction, it is preferable to use a urethane catalyst such as tin octenoate, di-n-butyltin dilaurate, lead octoate, potassium octoate, potassium acetate, stannous octoate, or triethylenediamine.
[0160] When a reaction product with a polyol is used as the urethane (meth)acrylate compound, for example, the reaction product obtained by reacting the polyol with the polyvalent isocyanate compound may be reacted with a hydroxyl group-containing (meth)acrylic compound. In the reaction between the polyvalent isocyanate compound and the polyol, it is also preferable to use a metal catalyst such as dibutyltin dilaurate or an amine catalyst such as 1,8-diazabicyclo[5.4.0]undecene-7 to promote the reaction.
[0161] The weight-average molecular weight of the urethane (meth)acrylate compound is preferably 300 to 10,000, more preferably 500 to 5,000, particularly preferably 750 to 4,000, particularly preferably 1,000 to 3,500, and most preferably 1,250 to 3,000. The method for measuring the weight-average molecular weight is the same as described above.
[0162] Examples of the ethylenically unsaturated monomer having an ethylenically unsaturated group include a monofunctional monomer having one ethylenically unsaturated group in one molecule, a bifunctional monomer having two ethylenically unsaturated groups in one molecule, and a trifunctional or higher functional monomer having three or more ethylenically unsaturated groups in one molecule.
[0163] Examples of the monofunctional monomer include styrene, vinyltoluene, chlorostyrene, α-methylstyrene, methyl (meth)acrylate, ethyl (meth)acrylate, acrylonitrile, vinyl acetate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-phenoxy-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, glycerin mono(meth)acrylate, glycidyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, Examples of the acrylate include acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, n-stearyl (meth)acrylate, benzyl (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, nonylphenol propylene oxide-modified (meth)acrylate, half ester (meth)acrylate of a phthalic acid derivative such as 2-(meth)acryloyloxy-2-hydroxypropyl phthalate, furfuryl (meth)acrylate, carbitol (meth)acrylate, benzyl (meth)acrylate, butoxyethyl (meth)acrylate, allyl (meth)acrylate, acryloylmorpholine, 2-hydroxyethyl acrylamide, N-methylol (meth)acrylamide, N-vinylpyrrolidone, 2-vinylpyridine, and 2-(meth)acryloyloxyethyl acid phosphate monoester.
[0164] Examples of the bifunctional monomer include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide-modified bisphenol A di(meth)acrylate, propylene oxide-modified bisphenol A di(meth)acrylate, 1, Examples of suitable di(meth)acrylates include 6-hexanediol di(meth)acrylate, 1,6-hexanediol ethylene oxide-modified di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, hydroxypivalic acid-modified neopentyl glycol di(meth)acrylate, isocyanuric acid ethylene oxide-modified diacrylate, and 2-(meth)acryloyloxyethyl acid phosphate diester.
[0165] Examples of the tri- or higher functional monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(meth)acryloyloxyethoxytrimethylolpropane, and glycerin polyglycerol. Examples of the poly(meth)acrylate include ricidyl ether poly(meth)acrylate, ethylene oxide-modified isocyanuric acid tri(meth)acrylate, ethylene oxide-modified dipentaerythritol penta(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified pentaerythritol tetra(meth)acrylate, and succinic acid-modified pentaerythritol tri(meth)acrylate.
[0166] In addition to the above, the ethylenically unsaturated monomer also includes a Michael adduct of (meth)acrylic acid or a 2-(meth)acryloyloxyethyl dicarboxylic acid monoester. Examples of the Michael adduct of (meth)acrylic acid include (meth)acrylic acid dimer, (meth)acrylic acid trimer, and (meth)acrylic acid tetramer. Examples of 2-(meth)acryloyloxyethyl dicarboxylic acid monoester, which is a carboxylic acid having a specific substituent, include 2-(meth)acryloyloxyethyl succinic acid monoester, 2-(meth)acryloyloxyethyl phthalic acid monoester, and 2-(meth)acryloyloxyethyl hexahydrophthalic acid monoester. Further, oligoester acrylates are also included.
[0167] These unsaturated group-containing compounds (C), such as urethane (meth)acrylate compounds and ethylenically unsaturated monomers, may be used alone or in combination of two or more.
[0168] When the present composition 1 contains the unsaturated group-containing compound (C), the content thereof is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, especially preferably 1 part by mass or less, and most preferably 0 part by mass, relative to 100 parts by mass of the polyester (A). That is, the present composition 1 preferably does not contain the unsaturated group-containing compound (C). If the content is too high, the cohesive strength of the adhesive layer after curing with active energy rays becomes too high, resulting in insufficient elongation and adhesive strength, or the unsaturated groups react with heat, causing an increase in viscosity or gelation, and the heat resistance tends to be insufficient.
[0169] Furthermore, when the present composition 2 contains an unsaturated group-containing compound (C), the content thereof is less than 15 parts by mass, preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, especially preferably 1 part by mass or less, and most preferably 0 part by mass, relative to 100 parts by mass of the polyester (A). That is, the present composition 2 preferably does not contain an unsaturated group-containing compound (C). If the content is too high, the cohesive strength of the adhesive layer after curing with active energy rays becomes too high, resulting in insufficient elongation and adhesive strength, and the unsaturated groups react with heat, causing an increase in viscosity and gelation, resulting in insufficient thermal stability.
[0170] <Crosslinking Agent (D)> The present composition may contain a crosslinking agent (D) for the purpose of increasing cohesive strength. The crosslinking agent (D) may be any compound having a functional group that reacts with a functional group, such as a hydroxyl group or a carboxyl group, contained in the polyester (A). Examples of the crosslinking agent (D) include epoxy compounds such as bisphenol A-epichlorohydrin epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, and diglycerol polyglycidyl ether; tetramethylolmethane-tri-β-aziridinyl propionate, trimethylolpropane-tri-β-aziridinyl propionate, N,N'-diphenyl ether, and the like. aziridine compounds such as N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, hexahexyloxymethylmelamine, and melamine resins; 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, hexamethylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, tetramethylxylylene diisocyanate, 1,Examples of the polyisocyanate include 5-naphthalene diisocyanate, triphenylmethane triisocyanate, and adducts of these polyisocyanate compounds with polyol compounds such as trimethylolpropane; isocyanate compounds such as biuret compounds and isocyanurates of these polyisocyanate compounds; aldehyde compounds such as glyoxal, malondialdehyde, succindialdehyde, maleic dialdehyde, glutaric dialdehyde, formaldehyde, acetaldehyde, and benzaldehyde; amine compounds such as hexamethylenediamine, triethyldiamine, polyethyleneimine, hexamethylenetetraamine, diethylenetriamine, triethyltetraamine, isophoronediamine, amino resins, and polyamides; and metal chelate compounds such as acetylacetone and acetoacetyl ester coordination compounds of polymetals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium. Among these, polyisocyanate compounds are preferably used in terms of reactivity with the polyester (A). These crosslinking agents (D) may be used alone or in combination of two or more. However, the crosslinking agent (D) does not include the hydrolysis inhibitor (E) described below.
[0171] The polyisocyanate compound is not particularly limited, and examples thereof include aromatic, aliphatic, and alicyclic polyisocyanates, among which tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylxylylene diisocyanate, and isophorone diisocyanate. Examples of suitable isocyanates include polyisocyanates such as methylisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, phenylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and naphthalene diisocyanate, as well as trimer compounds or polymer compounds of these polyisocyanates, biuret-type polyisocyanates, and reaction products of these polyisocyanates with polyols. Among these, tolylene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate are preferred because of their excellent reactivity. These can be used alone or in combination of two or more.
[0172] When a crosslinking agent (D) is used, its content can be appropriately selected depending on the amount of functional groups contained in the polyester (A), the molecular weight of the polyester (A), and the purpose of controlling the adhesive strength after irradiation with active energy rays, but it is usually preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 2 parts by mass or less, particularly preferably 1 part by mass or less, especially preferably 0.5 parts by mass or less, and most preferably 0 part by mass, per 100 parts by mass of the polyester (A). If the content of such crosslinking agent (D) is too high, the polyester (A) and the crosslinking agent (D) will react during hot-melt coating, increasing the melt viscosity and resulting in insufficient pot life, or gelation will tend to impair the appearance of the coating film.
[0173] <Hydrolysis inhibitor (E)> The present composition preferably contains a hydrolysis inhibitor (E) from the viewpoint of improving the hydrolysis resistance and moist heat resistance of the polyester (A). The hydrolysis inhibitor (E) is not particularly limited, and conventionally known compounds can be used, for example, compounds that react with the carboxyl end group of the polyester (A) to bond, specifically compounds having a functional group such as a carbodiimide group or an oxazoline group. Among these, carbodiimide group-containing compounds are preferred because of their excellent reactivity with the carboxyl group.
[0174] The carbodiimide group-containing compound may generally be a known carbodiimide having one or more carbodiimide groups (—N═C═N—) in the molecule, and examples thereof include a monomeric carbodiimide compound (E1) having one carbodiimide group in the molecule and a polymeric carbodiimide compound (E2) having at least two carbodiimide groups in the molecule. Among these, a monomeric carbodiimide compound having one carbodiimide group in the molecule is preferred, in that it suppresses an increase in viscosity at high temperatures, has excellent heat resistance, and further has excellent moist heat resistance.
[0175] Examples of the monomeric carbodiimide compound (E1) include dicyclohexylcarbodiimide, diisopropylcarbodiimide, diphenylcarbodiimide, bis(methylphenyl)carbodiimide, bis(methoxyphenyl)carbodiimide, bis(nitrophenyl)carbodiimide, bis(dimethylphenyl)carbodiimide, bis(diisopropylphenyl)carbodiimide, bis(di-t-butylphenyl)carbodiimide, N-ethyl-N'-(3-dimethylaminopropyl)carbodiimide, bis(triphenylsilyl)carbodiimide, and cyclic carbodiimides. Among these, diisopropylcarbodiimide, bis(methoxyphenyl)carbodiimide, bis(diisopropylphenyl)carbodiimide, N-ethyl-N'-(3-dimethylaminopropyl)carbodiimide, and bis(triphenylsilyl)carbodiimide are preferred, and bis(diisopropylphenyl)carbodiimide is preferred in terms of excellent reactivity and compatibility with the carboxy group of the polyester (A) and excellent heat and humidity durability. These may be used alone or in combination of two or more.
[0176] Examples of the polymeric carbodiimide compound (E2) include those obtained by a decarboxylation condensation reaction of the following diisocyanates. Examples of such diisocyanates include 4,4'-diphenylmethane diisocyanate, 3,3'-dimethoxy-4,4'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 3,3'-dimethyl-4,4'-diphenylether diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1-methoxyphenyl-2,4-diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate. These may be used alone or in combination of two or more.
[0177] When the hydrolysis inhibitor (E) is used, the content thereof is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, even more preferably 0.2 to 3 parts by mass, particularly preferably 0.3 to 2 parts by mass, especially preferably 0.4 to 1.5 parts by mass, and most preferably 0.5 to 1 part by mass, relative to 100 parts by mass of the polyester (A). If the content of such a hydrolysis inhibitor is too high, the active energy ray curability and adhesive strength tend to decrease, and the coating film appearance tends to be unsatisfactory due to poor compatibility with the polyester. If the content is too low, the hydrolysis resistance tends to decrease and the moist heat durability tends to be insufficient.
[0178] The content of the hydrolysis inhibitor (E) is preferably optimized depending on the acid value of the polyester (A). The molar ratio ((ii) / (i)) of the total number of carboxy groups (i), determined from the acid value of the polyester (A), to the total number of functional groups (ii) in the hydrolysis inhibitor (E) is preferably 0.5≦(ii) / (i), more preferably 1≦(ii) / (i)≦1000, even more preferably 1.5≦(ii) / (i)≦500, particularly preferably 2≦(ii) / (i)≦250, especially preferably 2.5≦(ii) / (i)≦100, and most preferably 3≦(ii) / (i)≦50. If the content ratio of (ii) relative to (i) is too high, the coating film appearance tends to be insufficient due to poor compatibility with the polyester (A), and the active energy ray curability, adhesive strength, cohesive strength, and hydrolysis resistance tend to decrease. On the other hand, if the content ratio of (ii) relative to (i) is low, the hydrolysis resistance and moist heat durability tend to decrease.
[0179] <Antioxidant (F)> The present composition preferably contains an antioxidant (F) in that it provides excellent heat resistance to the polyester (A) and stability to the pressure-sensitive adhesive sheet, and can suppress viscosity changes under conditions involving thermal history, such as hot-melt coating.
[0180] Examples of the antioxidant (F) include phenol-based antioxidants, hindered phenol-based antioxidants, amine-based antioxidants, hindered amine-based antioxidants, sulfur-based antioxidants, and phosphoric acid-based antioxidants. Among these, at least one selected from the group consisting of hindered phenol-based antioxidants, hindered amine-based antioxidants, and phosphoric acid-based antioxidants is preferred, and antioxidant (F) consisting of a hindered phenol-based compound is particularly preferred. Examples of the hindered phenol-based antioxidant include antioxidants having a hindered phenol structure in which a group with large steric hindrance, such as a tertiary butyl group, is bonded to at least one of the carbon atoms adjacent to the carbon atom on the aromatic ring to which the phenolic hydroxyl group is bonded.
[0181] When the antioxidant (F) is used, the content thereof is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, even more preferably 0.05 to 3 parts by mass, particularly preferably 0.1 to 2 parts by mass, and especially preferably 0.3 to 1.0 part by mass, relative to 100 parts by mass of the polyester (A). If the content is too small, heat resistance tends to be insufficient, and if the content is too large, active energy ray curability tends to be insufficient.
[0182] <Tackifying Resin (G)> The present composition may contain a tackifying resin (G) in order to improve adhesive properties such as adhesive strength and tackiness, and coatability.
[0183] The tackifier resin (G) is not particularly limited, and conventionally known resins can be used. Examples of the tackifier resin (G) include hydrocarbon resins, terpene resins, phenolic resins, rosin resins, xylene resins, epoxy resins, polyamide resins, ketone resins, and elastomer resins. These may be used alone or in combination of two or more. Among these, hydrocarbon resins and terpene resins are preferred in terms of compatibility with the polyester (A) and excellent heat resistance, and hydrocarbon resins are more preferred in terms of excellent active energy ray curability.
[0184] Examples of the hydrocarbon resin include various hydrocarbon resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated aromatic hydrocarbon resins, hydrogenated aliphatic hydrocarbon resins, coumarone resins, and coumarone-indene resins. Of these, aromatic hydrocarbon resins and hydrogenated aromatic hydrocarbon resins are preferred because of their excellent tackiness and heat resistance.
[0185] Examples of the terpene resin include terpene resins, terpene phenol resins, and aromatic-modified terpene resins. Specifically, α-pinene polymers, β-pinene polymers, dipentene polymers, and terpene resins obtained by modifying these polymers with phenol, aromatics, hydrogenation, or hydrocarbons can be used. Furthermore, terpene phenol resins are preferred because of their excellent compatibility with the polyester (A) and excellent tackiness.
[0186] Examples of the phenolic resin that can be used include condensates of formaldehyde with various phenols such as phenol, m-cresol, 3,5-xylenol, p-alkylphenol, and resorcinol.Furthermore, resol obtained by subjecting the phenols and formaldehyde to an addition reaction in the presence of an alkali catalyst, novolak obtained by subjecting the phenols and formaldehyde to a condensation reaction in the presence of an acid catalyst, and rosin-modified phenolic resin obtained by adding phenol to rosins such as unmodified or modified rosin or derivatives thereof in the presence of an acid catalyst, followed by thermal polymerization.
[0187] Examples of the rosin-based resin include rosin resin, polymerized rosin resin, hydrogenated rosin resin, rosin ester resin, hydrogenated rosin ester resin, rosin phenol resin, and polymerized rosin ester. Specific examples of the rosin resin that can be used include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin, modified rosins obtained by hydrogenating, disproportionating, polymerizing, or otherwise chemically modifying these, and derivatives of these.
[0188] From the viewpoint of moist heat resistance, the tackifier resin (G) preferably has an acid value of 30 mgKOH / g or less, particularly 15 mgKOH / g or less, further 10 mgKOH / g or less, particularly 6 mgKOH / g or less, and most preferably 3 mgKOH / g. When multiple types of tackifier resins are used in combination, the average of their acid values is preferably within the above range.
[0189] The softening point of the tackifier resin (G) (measured, for example, by the ring and ball method) is preferably 60 to 170° C., more preferably 80 to 160° C., even more preferably 90 to 150° C., and particularly preferably 100 to 140° C. If the softening point is within the above range, tackiness and adhesive strength can be improved, which is preferable.
[0190] In the present invention, the tackifier resin (G) is preferably a plant-derived resin from the viewpoint of global environmental conservation. Examples of plant-derived tackifier resins include terpene-based resins and rosin-based resins.
[0191] When a tackifier resin (G) is used, its content is preferably 50 parts by mass or less, more preferably 0.1 to 30 parts by mass, even more preferably 1 to 20 parts by mass, particularly preferably 2 to 15 parts by mass, and especially preferably 3 to 10 parts by mass, relative to 100 parts by mass of the polyester (A). A content within the above range is preferred because tackiness and adhesive strength can be improved, while a too high content tends to increase the glass transition temperature of the adhesive layer, resulting in insufficient tackiness and adhesive strength and reduced active energy ray curability.
[0192] <Active Energy Ray-Curable Composition> In addition to the polyester (A), the compound (B) having a photoreactive group, the unsaturated group-containing compound (C), the crosslinking agent (D), the hydrolysis inhibitor (E), the antioxidant (F), and the tackifier resin (G), other components may be blended in the composition, as long as they do not impair the effects of the present invention. These may include additives such as catalysts, plasticizers, UV absorbers, antistatic agents, silane coupling agents, fluxes, flame retardants, dispersants, emulsifiers, antifoaming agents, leveling agents, and ion trapping agents, as well as inorganic or organic fillers, powders, and particulate additives such as metal powders and pigments. Furthermore, the composition may contain small amounts of impurities contained in the raw materials used to produce the adhesive components. These may be used alone or in combination of two or more.
[0193] When the present composition contains these other components, the content thereof is preferably 70% by mass or less, more preferably 0.001 to 50% by mass, particularly preferably 0.005 to 30% by mass, and even more preferably 0.01 to 10% by mass of the entire composition.
[0194] The present composition can be obtained, for example, by preparing the polyester (A) and necessary optional components, and blending them during the production of the polyester (A) and then heating, melting, and dispersing them, or by blending them into a solution of the polyester (A) dissolved in an organic solvent and then dispersing them using a mixing roller or the like.
[0195] The melt viscosity (160°C) of Composition 1 is preferably 200 Pa s or less, more preferably 1 to 150 Pa s, even more preferably 2 to 100 Pa s, particularly preferably 3 to 80 Pa s, especially preferably 4 to 60 Pa s, and most preferably 5 to 40 Pa s. If the melt viscosity is too low, the coating tends to have an orange peel appearance, resulting in poor coatability, and the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, while if the melt viscosity is too high, the coating tends to have streaks in the appearance, resulting in insufficient coatability.
[0196] The melt viscosity (130°C) of Composition 2 is preferably 500 Pa s or less, more preferably 1 to 400 Pa s, even more preferably 3 to 300 Pa s, particularly preferably 5 to 200 Pa s, especially preferably 10 to 150 Pa s, and most preferably 15 to 100 Pa s. If the melt viscosity is too low, the coating tends to have an orange peel appearance, resulting in poor coatability, and the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, while if the melt viscosity is too high, the coating tends to have streaks in the appearance, resulting in poor coatability.
[0197] Furthermore, from the viewpoint of thermal stability and coatability, it is preferable that the composition have a small rate of change in melt viscosity before and after a heat resistance test (temperature 200°C, 3 hours, under air conditions). The rate of change in melt viscosity is preferably 20 to 500%, more preferably 30 to 400%, even more preferably 40 to 300%, particularly preferably 50 to 250%, especially preferably 60 to 200%, and most preferably 70 to 150%. If the rate of change in melt viscosity before and after thermal history is outside the above range, the adhesive may gel or decompose, resulting in insufficient coatability, adhesive strength, and adhesion. The rate of change in melt viscosity (%) is calculated using the following formula: Rate of change in melt viscosity (%) = [(melt viscosity after heat resistance test) / (melt viscosity before heat resistance test)] × 100
[0198] The present composition has excellent heat resistance because it is active energy ray-curable even without having an unsaturated group, and further, when used as a pressure-sensitive adhesive composition, it forms a pressure-sensitive adhesive having excellent adhesive strength and holding power. In particular, the present composition is useful as a solventless active energy ray-curable pressure-sensitive adhesive composition for use in pressure-sensitive adhesive tapes for electronic components, pressure-sensitive adhesive tapes for labels, etc.
[0199] [Solvent] The present composition is preferably used as a solvent-free active energy ray-curable pressure-sensitive adhesive composition, but a solvent may be added to the composition in order to appropriately adjust the viscosity of the composition and to facilitate handling when forming a coating film.
[0200] Examples of solvents include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate; ethers such as ethylene glycol monomethyl ether; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; alcohols such as methanol and ethanol; alkanes such as hexane and cyclohexane; and aromatics such as toluene and xylene. Among these, ketone-based solvents and ester-based solvents are preferred from the viewpoint of VOC emission regulations, and methyl ethyl ketone, cyclohexanone, and ethyl acetate are particularly preferred, and methyl ethyl ketone and ethyl acetate are even more preferred because they have low boiling points and excellent drying efficiency. The above-mentioned solvents may be used alone, or two or more may be mixed in any combination and ratio.
[0201] The content of the solvent is preferably less than 10% by mass, more preferably 5% by mass or less, even more preferably 3% by mass or less, and particularly preferably 1% by mass or less, based on the composition (including the solvent). The lower limit is 0% by mass, and it is preferable that no solvent is contained. If the solvent content is too high, the amount of energy required to volatilize the solvent in the coating process increases, and the environmental load reduction effect tends to be insufficient.
[0202] <Active energy ray-curable composition> An active energy ray-curable composition according to one embodiment of the present invention is an active energy ray-curable composition containing a structural unit derived from a polycarboxylic acid (α) and a structural single polyester (A) derived from a polyhydric alcohol (β), wherein the polyester (A) is a polyester (A1) containing a photoreactive group having a structural unit derived from a compound (B) having a photoreactive group. As the polyester (A1), the same polyesters as those described for the polyester (A) can be used.
[0203]
[0023] An active energy ray-curable composition according to one embodiment of the present invention contains a polyester (A) having a structural unit derived from a polycarboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, and the content of the unsaturated group-containing compound (C) is less than 15 parts by mass per 100 parts by mass of the polyester (A). As the polyester (A), the same polyester as described for the polyester (A) can be used, and a polyester (A2) not containing a photoreactive group is particularly preferred.
[0204] Furthermore, the active energy ray-curable composition may contain the compound (B) having a photoreactive group, the unsaturated group-containing compound (C), the crosslinking agent (D), the hydrolysis inhibitor (E), the antioxidant (F), the tackifier resin (G), the additives, and the like, which are all described in the present composition, and the preferred physical properties and contents thereof are also the same.
[0205] <Adhesive> The adhesive according to one embodiment of the present invention can be obtained by curing (crosslinking) the present composition or the active energy ray-curable composition, and can provide an adhesive that exhibits excellent effects in terms of heat resistance, adhesive strength, and holding power. In the present invention, "crosslinking" means intentionally crosslinking the present composition by heat and / or light, etc., more preferably by light, and particularly preferably by active energy rays such as ultraviolet rays or electron beams. The degree of crosslinking can be controlled depending on the desired physical properties and applications.
[0206] The degree of crosslinking can be confirmed by the gel fraction of the pressure-sensitive adhesive, with the gel fraction preferably being 1 to 100%, more preferably 3 to 90%, even more preferably 5 to 80%, particularly preferably 10 to 70%, especially preferably 15 to 60%, most preferably 20 to 50%, and especially preferably 25 to 45%. If the gel fraction is too low, the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, while if the gel fraction is too high, the tackiness and adhesive strength tend to be insufficient. The gel fraction serves as a measure of the degree of crosslinking and is calculated, for example, by the following method. That is, a pressure-sensitive adhesive sheet (without a release sheet) comprising a pressure-sensitive adhesive layer formed on a polymer sheet (e.g., a PET film) as a substrate is wrapped in a 200-mesh SUS wire mesh and immersed in toluene or ethyl acetate at 23°C for 24 hours, and the gel fraction is calculated as the mass percentage of the insoluble pressure-sensitive adhesive component remaining in the wire mesh after immersion relative to the mass of the pressure-sensitive adhesive component before immersion. However, the mass of the substrate is subtracted.
[0207] The pressure-sensitive adhesive can be formed into a sheet-like pressure-sensitive adhesive layer to obtain a pressure-sensitive adhesive sheet. Such a pressure-sensitive adhesive layer is preferably formed on one or both sides of a supporting substrate. In the present invention, the term "sheet" is used to include "film" and "tape."
[0208] <Adhesive Sheet> The adhesive sheet can be produced, for example, as follows: The adhesive sheet can be produced according to a known general adhesive sheet production method, for example, by applying the present composition to a substrate, drying, laminating a release sheet to the opposite surface of the composition layer, and optionally curing, to obtain an adhesive sheet having an adhesive layer on a substrate.
[0209] Alternatively, a pressure-sensitive adhesive sheet can be obtained by coating the composition on a release sheet, drying it, laminating a substrate to the opposite side of the composition layer, and curing if necessary.
[0210] Alternatively, a substrate-less double-sided PSA sheet can be produced by forming a PSA layer on a release sheet and then laminating another release sheet to the opposite side of the PSA layer.
[0211] When using the obtained pressure-sensitive adhesive sheet or substrate-less double-sided pressure-sensitive adhesive sheet, the release sheet is peeled off from the pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is then attached to an adherend.
[0212] Examples of the substrate include polyester resins such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, polybutylene succinate, polylactic acid, polyethylene terephthalate / isophthalate copolymer, polybutylene adipate / terephthalate copolymer, hydroxybutyrate / hydroxyhexanoate copolymer, and polycaprolactone; polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; polyethylene fluoride resins such as polyvinyl fluoride, polyvinylidene fluoride, and polyethylene fluoride; polyamides such as nylon 6 and nylon 6,6; polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol. Examples of the substrate include vinyl polymers such as vinyl copolymers, polyvinyl alcohol, and vinylon; cellulose-based resins such as cellulose triacetate and cellophane; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; fluorine-based resins; polystyrene; polycarbonate; acrylonitrile-butadiene-styrene copolymers; acrylonitrile-styrene-acrylic acid ester copolymers; polyarylates; polyimides; cycloolefin polymers; urethane acrylate resins; sheets made of at least one synthetic resin selected from the group consisting of polyesters; metal foils of aluminum, copper, and iron; paper such as fine paper and glassine paper; woven fabrics and nonwoven fabrics made of glass fiber, natural fibers, synthetic fibers, etc. These substrates can be used as a single layer or as a multilayer structure in which two or more types are laminated.
[0213] Among these, substrates made of polyester, nonwoven fabric, and polyolefin resin are particularly preferred.
[0214] The substrate may be a foam substrate, such as a foam sheet made of a synthetic resin foam such as polyurethane foam, polyethylene foam, polyacrylate foam, etc. Among these, polyurethane foam and polyethylene foam are preferred because they have an excellent balance of heat resistance, conformability to the adherend, and adhesive strength.
[0215] The thickness of the substrate is, for example, preferably 1 to 1000 μm, particularly preferably 3 to 500 μm, further preferably 5 to 250 μm, and particularly preferably 10 to 100 μm.
[0216] As the release sheet, for example, a sheet made of any of the various synthetic resins exemplified above as the base material, paper, cloth, nonwoven fabric, etc. that has been subjected to a release treatment can be used. As the release sheet, it is preferable to use a silicone-based release sheet.
[0217] The composition may be applied using, for example, a gravure roll coater, reverse roll coater, kiss roll coater, dip roll coater, bar coater, knife coater, spray coater, comma coater, or the like.
[0218] As for drying conditions, the drying temperature is preferably 60 to 140° C., particularly preferably 80 to 120° C., and the drying time is preferably 0.5 to 30 minutes, particularly preferably 1 to 5 minutes.
[0219] The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet or substrate-less double-sided pressure-sensitive adhesive sheet is preferably 1 to 500 μm, particularly preferably 3 to 200 μm, further preferably 5 to 100 μm, and especially preferably 10 to 50 μm. If the thickness of the pressure-sensitive adhesive layer is too thin, the adhesive strength tends to decrease, while if it is too thick, the uniformity of the coating film tends to decrease, resulting in poor appearance, or air bubbles tend to enter the coating film, resulting in insufficient optical properties.
[0220] The thickness of the adhesive layer is determined by subtracting the measured thickness of the constituent members other than the adhesive layer from the measured thickness of the entire adhesive sheet using a Mitutoyo ID-C112B.
[0221] Furthermore, such a PSA sheet may be protected by providing a release sheet on the outer side of the PSA layer, if necessary. In a PSA sheet in which the PSA layer is formed on one side of a substrate, the PSA layer can be protected by applying a release treatment to the side of the substrate opposite the PSA layer, thereby utilizing the release-treated surface.
[0222] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by mass.
[0223] The glass transition temperature (°C), acid value (mg KOH / g), hydroxyl value (mg KOH / g), epoxy group concentration (mmol / g), ester bond concentration (mmol / g), unsaturated group concentration (mmol / g), heat of crystalline fusion (J / g), number average molecular weight (Mn), weight average molecular weight (Mw), peak top molecular weight (Mp), polydispersity, melt viscosity (Pa s), and biomass degree were measured according to the description in this specification.
[0224] <Production of Polyester (A)> The compositions shown in Table 1 below are the composition ratios of the finished product (resin composition ratios), and are the relative ratios (molar ratios) of the amounts of the constituent monomers of the obtained polyester and their mass %.
[0225] [Production of polyester (A1-1)] A thermometer, a stirrer, a rectification column, and a reaction vessel equipped with a nitrogen inlet tube were charged with 51.9 parts of isophthalic acid (IPA) as the polycarboxylic acid (α), 592.1 parts of sebacic acid (SebA), 4.2 parts of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 80.8 parts of ethylene glycol (EG) as the polyhydric alcohol (β), 67.0 parts of neopentyl glycol (NPG), and 0.1 parts of tetrabutyl titanate as a catalyst. The internal temperature was raised to 260 ° C. over 2.5 hours, and an esterification reaction was carried out at 260 ° C. for 1.5 hours. Next, 0.1 parts of tetrabutyl titanate was added as a catalyst, and the pressure in the system was reduced to 2.5 hPa, and the polymerization reaction was carried out over 2 hours to obtain polyester (A1-1).
[0226] [Production of Polyesters (A1-2, A1-3, A2-1)] Polyesters (A1-2, A1-3, A2-1) were obtained in the same manner as A1-1, except that the resin compositions were changed as shown in Table 1 below.
[0227] [Production of polyester (A2-2)] A reactor equipped with a thermometer, a stirrer, a rectifying column, and a nitrogen inlet tube was charged with 96.1 parts of isophthalic acid (IPA) as the polycarboxylic acid (α), 467.8 parts of sebacic acid (SebA), 130.3 parts of 1,4-butanediol (1,4BG) as the polyhydric alcohol (β), 271 parts of neopentyl glycol (NPG), 29.7 parts of 1,6-hexanediol (1,6HG), 5 parts of trimethylolpropane (TMP), and 0.1 parts of tetrabutyl titanate as a catalyst, and the internal temperature was raised to 260 ° C. over 2.5 hours, followed by an esterification reaction at 260 ° C. for 1.5 hours. Next, 0.1 parts of tetrabutyl titanate was added as a catalyst, the pressure in the system was reduced to 2.5 hPa, and the polymerization reaction was carried out over 2 hours to obtain polyester (A2-2).
[0228] [Production of Polyesters (A2-3, A2-4)] Polyesters (A2-3, A2-4) were obtained in the same manner as A2-2, except that the resin compositions were changed as shown in Table 2 below.
[0229] The resin composition (structural units derived from the components) of the obtained polyester (A) is shown in Tables 1 and 3, and its physical properties are shown in Tables 2 and 4. In Tables 1 and 3, the abbreviations are as follows: [Polycarboxylic acid (α)] [Aliphatic polycarboxylic acid (α1)] SebA: sebacic acid (derived from biomass) AdA: adipic acid SuA: succinic acid (derived from biomass) [Aromatic polycarboxylic acids (α2)] IPA: isophthalic acid BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride Note that BTDA is also a compound (b1) having a hydrogen abstraction type photoreactive group. [Polyhydric alcohol (β)] [Straight-chain aliphatic polyhydric alcohol (β1-1)] EG: Ethylene glycol (derived from biomass) 1,3PG: 1,3-propanediol (derived from biomass) 1,4BG: 1,4-butanediol (derived from biomass) 1,6HG: 1,6-hexanediol [Branched fatty acid polyhydric alcohol (β1-2) having a hydrocarbon group in at least one side chain] NPG: Neopentyl glycol TMP: Trimethylolpropane
[0230]
[0231]
[0232]
[0233]
[0234] <Compound (B) Having a Photoreactive Group> The following compounds were prepared as a compound (B) having a photoreactive group [photopolymerization initiator]: b1-1(1): Benzophenone (manufactured by IGM Rejins, benzophenone-based hydrogen abstraction photopolymerization initiator "Omnirad BP Flake") b1-1(2): 4-methylbenzophenone (manufactured by IGM Rejins, benzophenone-based hydrogen abstraction photopolymerization initiator "Omnirad 4MBZ Flakes")
[0235] <Hydrolysis inhibitor (E)> The following hydrolysis inhibitors were prepared: E-1: bis(diisopropylphenyl)carbodiimide (manufactured by Rhein Chemie, monomeric carbodiimide compound "Stabaxol I Powder")
[0236] <Acid Value Inhibitor (F)> The following antioxidants were prepared: F-1: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (manufactured by BASF Japan, hindered phenol-based antioxidant "Irganox 1010")
[0237] <Tackifying Resin (G)> The following tackifying resins were prepared: G-1: Aromatic hydrocarbon resin (softening point 100°C, "FTR8100" manufactured by Mitsui Chemicals, Inc.) G-2: Terpene phenol resin (softening point 100°C, "YS Polystar T100" manufactured by Yasuhara Chemical Co., Ltd.)
[0238] Example 1 One part of the hydrolysis inhibitor (E-1) and 0.1 parts of the antioxidant (F-1) were blended with 100 parts of the polyester (A1-1) obtained above, and the mixture was stirred and mixed at 130°C for 1 hour to obtain an active energy ray-curable composition.
[0239] Examples 2 to 8, Comparative Examples 1 and 2 Active energy ray-curable compositions were obtained in the same manner as in Example 1, except that the components shown in Table 5 were blended.
[0240] [PET-based adhesive sheet with one-sided release film] The active energy ray-curable compositions of Examples 1 to 8 and Comparative Examples 1 and 2 obtained above were applied to a polyethylene terephthalate (PET) film (Lumirror T60, manufactured by Toray Industries, Inc., thickness 38 μm) to a thickness of approximately 25 μm, and then irradiated with a high-pressure mercury UV irradiation device at a peak irradiance of 150 mW / cm 2 A pressure-sensitive adhesive layer was formed by irradiating the adhesive with ultraviolet light at an integrated light dose of 500 mJ or 2000 mJ. A release-treated PET film (release film) (manufactured by Mitsui Chemicals Tocello, Inc., SP-PET-01-BU, thickness 38 μm) was then attached to the pressure-sensitive adhesive layer to protect its surface, thereby obtaining a PET-based pressure-sensitive adhesive sheet with a single-sided release film.
[0241] The resulting PET-based pressure-sensitive adhesive sheets with a single-sided release film were evaluated as follows. The evaluation results are shown in Table 5 below.
[0242] [Active energy ray curability (gel fraction)] The PET pressure-sensitive adhesive sheet with one-sided release film obtained above was cut into a size of 4 cm x 4 cm, and the release film was peeled off. This was wrapped in a 200-mesh SUS wire netting and immersed in toluene at 23 ° C for 24 hours. The mass of the insoluble pressure-sensitive adhesive component remaining in the wire netting relative to the mass of the pressure-sensitive adhesive component before immersion, minus the mass of the PET substrate, was measured, and the mass percentage was calculated according to the following formula, which was defined as the gel fraction (%). Gel fraction (%) = mass of insoluble pressure-sensitive adhesive component remaining in the wire netting after immersion / mass of pressure-sensitive adhesive component before immersion × 100
[0243] [Adhesive strength (peel strength) (against SUS-BA)] A SUS-BA plate was prepared as an adherend. The PET pressure-sensitive adhesive sheet with a release film on one side obtained above was cut to 25 mm x 200 mm in an environment of 23°C and 50% RH, and the release film was then peeled off. The pressure-sensitive adhesive layer side was then pressed and attached to the SUS-BA plate by rolling a 2 kg roller back and forth twice. After leaving the sheet to stand for 30 minutes in the same atmosphere, the 180-degree peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min using an autograph (Shimadzu Corporation, Autograph AG-X 50N). (Evaluation criteria) ◎ (excellent): Adhesive strength of 5N / 25mm or more, with no adhesive residue on the adherend ○ (very good): Adhesive strength of 3N / 25mm or more and less than 5N / 25mm, with no adhesive residue on the adherend △ (good): Adhesive strength of 1N / 25mm or more and less than 3N / 25mm, with no adhesive residue on the adherend × (poor): Adhesive strength less than 1N, or adhesive residue on the adherend
[0244] [Holding Power] The PET substrate pressure-sensitive adhesive sheet with a single-sided release film obtained above was cut to a size of 25 mm x 50 mm in an environment of 23°C and 50% RH, and then the release film was peeled off. The sheet was pressed and attached to a stainless steel plate (SUS304) by rolling a 2 kg roller back and forth twice (attached area 25 mm x 25 mm), and the holding power was measured using a creep tester (Tester Sangyo Co., Ltd., Holding Power Tester BE-501 with Constant Temperature and Humidity Chamber) under a load of 1 kg in an atmosphere of 40°C for 24 hours. The evaluation criteria are as follows. (Evaluation Criteria) ◯ (very good): no slippage △ (good): slippage of 1.0 mm or less × (poor): slippage of more than 1.0 mm, or drop
[0245] [Tackiness] The PET substrate pressure-sensitive adhesive sheet with a release film on one side obtained above was cut into a size of 12 mm x 12 mm under an environment of 23°C and 50% RH, the release film was peeled off, and the sheet was subjected to tackiness test using a Probe Tack (TE-6001, manufactured by Tester Sangyo Co., Ltd.) with a probe diameter of 5 mmΦ, a push-in speed of 10 mm / sec, a pull-up speed of 10 mm / sec, a pressure time of 5 seconds, and an application pressure of 1000 gf / cm. 2 The probe tack was measured using the following criteria: (Evaluation criteria) ⊚ (excellent) ... 5N or more ◯ (very good) ... 3N or more but less than 5N × (poor) ... 3N
[0246] [Environmental Load Reduction (Biomass Degree)] The biomass degree of the polyester resin (A) was calculated and evaluated using the following formula: Biomass degree (%) = [(number of moles of carbon of plant-derived monomer calculated from the molar ratio of polycarboxylic acid (α) and polyhydric alcohol (β) in polyester (A)) / (number of moles of carbon of all constituent monomers in polyester (A))] × 100 (Evaluation Criteria) ◎ (Excellent) ... 70% or more ○ (Very good) ... 50% or more and less than 70% △ (Good) ... 30% or more and less than 50% × (Poor) ... Less than 30%
[0247] [Thermal Stability] The active energy ray-curable compositions obtained in Examples 1 to 8 and Comparative Examples 1 and 2 were subjected to a heat resistance test (temperature 200°C, 3 hours, under air conditions), and the melt viscosity at 160°C before and after the heat resistance test was measured using a flow tester "CFT-500EX" (manufactured by Shimadzu Corporation), and the rate of change in melt viscosity was calculated and evaluated using the following formula. Melt viscosity change rate (%) = [(160°C melt viscosity after heat resistance test) / (160°C melt viscosity before heat resistance test)] x 100 (Evaluation criteria) ◎ (excellent) ... more than 30% and not more than 300% ○ (very good) ... more than 20% and not more than 30%, or more than 300% and not more than 500% △ (good) ... more than 10% and not more than 20%, or more than 500% and not more than 1000% × (poor) ... not more than 10% or more than 1000%
[0248]
[0249]
[0062] From the results in Table 5, the active energy ray-curable compositions and pressure-sensitive adhesive sheets of Examples 1 to 8 were excellent in active energy ray curability despite not containing an unsaturated group, and further excellent in adhesive strength, holding power, tackiness, environmental load reduction effect, and thermal stability. In contrast, the active energy ray-curable compositions and pressure-sensitive adhesive sheets of Comparative Examples 1 and 2 were inferior in active energy ray curability and did not satisfy the object of the present invention.
[0250] Example 9 5 parts of a compound having a photoreactive group (b1-1(1)), 1 part of a hydrolysis inhibitor (E-1), and 0.1 parts of an antioxidant (F-1) were blended with 100 parts of the polyester resin (A2-2) obtained above, and the mixture was stirred and mixed at 130°C for 1 hour to obtain an active energy ray-curable composition.
[0251] Examples 10 to 12, Comparative Example 3 Active energy ray-curable compositions were obtained in the same manner as in Example 9, except that the components shown in Table 6 were blended.
[0252] [PET-based pressure-sensitive adhesive sheet with one-sided release film] The active energy ray-curable compositions of Examples 9 to 12 and Comparative Example 3 obtained above were applied to a polyethylene terephthalate (PET) film (Lumirror T60, manufactured by Toray Industries, Inc., thickness 38 μm) to a thickness of approximately 25 μm, and then a release-treated PET film (release film) (SP-PET-01-BU, manufactured by Mitsui Chemicals Tocello, Inc., thickness 38 μm) was attached to the pressure-sensitive adhesive layer to protect its surface, and the sheet was then exposed to a high-pressure mercury UV irradiation device at a peak irradiance of 150 mW / cm. 2 The sheet was then irradiated with ultraviolet light at an integrated light intensity of 3000 mJ to obtain a PET substrate pressure-sensitive adhesive sheet with a release film on one side.
[0253] The resulting PET-based pressure-sensitive adhesive sheets with a single-sided release film were evaluated as follows. The evaluation results are shown in Table 6 below.
[0254] [Gel Fraction] The PET pressure-sensitive adhesive sheet with one-sided release film obtained above was cut into a size of 4 cm x 4 cm, and the release film was peeled off. This was wrapped in a 200-mesh SUS wire netting and immersed in toluene at 23°C for 24 hours. The mass of the insoluble pressure-sensitive adhesive component remaining in the wire netting relative to the mass of the pressure-sensitive adhesive component before immersion, minus the mass of the PET substrate, was measured, and the mass percentage was calculated according to the following formula, which was defined as the gel fraction (%). Gel fraction (%) = mass of insoluble pressure-sensitive adhesive component remaining in the wire netting after immersion / mass of pressure-sensitive adhesive component before immersion x 100
[0255] [Adhesive Strength (Peel Strength) (Against SUS-BA)] A SUS-BA plate was prepared as the adherend. The PET pressure-sensitive adhesive sheet with a release film on one side obtained above was cut to 25 mm x 200 mm in an environment of 23°C and 50% RH, and the release film was then peeled off. The pressure-sensitive adhesive layer side was then pressed and attached to the SUS-BA plate by rolling a 2 kg roller back and forth twice. After leaving the sheet to stand for 30 minutes in the same atmosphere, the 180-degree peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min using an autograph (Shimadzu Corporation, Autograph AG-X 50N), and evaluated according to the following evaluation criteria. (Evaluation criteria) ◎ (excellent): Adhesive strength of 5N / 25mm or more, with no adhesive residue on the adherend ○ (very good): Adhesive strength of 3N / 25mm or more and less than 5N / 25mm, with no adhesive residue on the adherend △ (good): Adhesive strength of 1N / 25mm or more and less than 3N / 25mm, with no adhesive residue on the adherend × (poor): Adhesive strength less than 1N, or adhesive residue on the adherend
[0256] [Holding Power] The PET substrate pressure-sensitive adhesive sheet with a single-sided release film obtained above was cut to a size of 25 mm x 50 mm in an environment of 23°C and 50% RH, and then the release film was peeled off. The sheet was pressed and attached to a stainless steel plate (SUS304) by rolling a 2 kg roller back and forth twice (attached area 25 mm x 25 mm), and the holding power was measured using a creep tester (Tester Sangyo Co., Ltd., Holding Power Tester BE-501 with High Temperature and Humidity Chamber) under a load of 1 kg in an atmosphere of 40°C for 24 hours. The evaluation criteria are as follows. (Evaluation Criteria) ◯ (Very good)...No slippage △ (Good)...Slippage is 1.0 mm or less × (Poor)...Slippage is more than 1.0 mm, or the sheet fell off
[0257] [Thermal stability] A heat resistance test (temperature 200°C, 3 hours, under air conditions) was carried out using the PET substrate pressure-sensitive adhesive sheet with a single-sided release film that had not been subjected to ultraviolet irradiation, and the melt viscosity at 130°C before and after the heat resistance test was measured using a flow tester "CFT-500EX" (manufactured by Shimadzu Corporation). The rate of change in melt viscosity was calculated and evaluated using the following formula. Melt viscosity change rate (%) = [(130°C melt viscosity after heat resistance test) / (130°C melt viscosity before heat resistance test)] x 100 (Evaluation criteria) ◎ (excellent) ... more than 30% and not more than 300% ○ (very good) ... more than 20% and not more than 30%, or more than 300% and not more than 500% △ (good) ... more than 10% and not more than 20%, or more than 500% and not more than 1000% × (poor) ... not more than 10% or more than 1000%
[0258]
[0259] The results in Table 6 show that the active energy ray-curable compositions and pressure-sensitive adhesive sheets of Examples 9 to 12 were excellent in active energy ray curability, and further excellent in adhesive strength, holding power, and thermal stability, despite not containing an unsaturated group. In contrast, the active energy ray-curable composition and pressure-sensitive adhesive sheet of Comparative Example 3 were inferior in active energy ray curability, adhesive strength, and holding power, and did not satisfy the object of the present invention.
[0260] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0261] The present composition is active energy ray-curable even without an unsaturated group, and therefore forms a pressure-sensitive adhesive having excellent thermal stability, adhesive strength, and holding power. Such a composition is particularly useful as a solvent-free pressure-sensitive adhesive for electronic components, label tapes, and the like.
Claims
1. An active energy ray-curable composition containing a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), wherein the polyester (A) further contains a polyester (A1) having a structural unit derived from a compound (B) having a photoreactive group.
2. An active energy ray-curable composition comprising a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, wherein the content of the polymerizable unsaturated group-containing compound (C) contained in the active energy ray-curable composition is less than 15 parts by mass per 100 parts by mass of the polyester (A).
3. The active energy ray-curable composition according to claim 1, further comprising a polyester (A2) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and having no structural unit derived from a compound (B) having a photoreactive group.
4. The active energy ray-curable composition according to claim 1, wherein the compound (B) having a photoreactive group is a compound (b1) having a hydrogen abstraction type photoreactive group and / or a compound (b2) having a cleavage type photoreactive group.
5. The active energy ray-curable composition according to claim 1 or 4, wherein a structural unit derived from the compound (B) having a photoreactive group is incorporated into the main chain of the polyester (A1) via an ester bond.
6. The active energy ray-curable composition according to claim 1, wherein the compound (B) having a photoreactive group is a polyvalent carboxylic acid (α).
7. The active energy ray-curable composition according to claim 2, wherein the compound (B) having a photoreactive group is a hydrogen abstraction type photopolymerization initiator.
8. The active energy ray-curable composition according to claim 2, wherein the compound (B) having a photoreactive group does not have a carboxy group or a hydroxy group as a functional group.
9. The active energy ray-curable composition according to claim 1 or 2, wherein the glass transition temperature of the polyester (A) is -80 to 30°C.
10. The active energy ray-curable composition according to claim 1 or 2, wherein the weight average molecular weight of the polyester (A) is 5,000 to 500,000.
11. The active energy ray-curable composition according to claim 1 or 2, wherein the polyester (A) has an unsaturated group concentration of 1 mmol / g or less.
12. The active energy ray-curable composition according to claim 1 or 2, which has a melt viscosity change rate of 20 to 500% before and after heating at 200° C. for 3 hours.
13. The active energy ray-curable composition according to claim 1 or 2, wherein the content of the organic solvent in the active energy ray-curable composition is less than 10 mass %.
14. An adhesive which is a cured product of the active energy ray-curable composition according to claim 1 or 2.
15. The pressure-sensitive adhesive according to claim 14, wherein the gel fraction of the pressure-sensitive adhesive is 1 to 100%.
16. An adhesive sheet comprising the adhesive according to claim 14.
Citation Information
Patent Citations
Photo crosslinkable polyester adhesive composition
JP2009102476A
Pressure-sensitive adhesive for optical member and optical member, and photo- and / or heat-crosslinking pressure-sensitive adhesive composition for optical member
JP2009209279A
Radiation-curable, repeelable self-adhesive sheet
JP2010059336A
Pressure-sensitive adhesive made from UV-cured vegetable oil-based polyester
JP2022535379A
Ultraviolet ray-curable resin composition
JP1983091714A