Ferrite particles, carrier core material for electrophotographic developer, carrier for electrophotographic developer, and electrophotographic developer

Ferrite particles with a size-specific Sr or Ca gradient and surface roughness are used in an electrophotographic developer to address charge distribution issues, enhancing the charge imparting ability and maintaining image quality over time by ensuring a sharp charge distribution and reducing toner scattering.

WO2024204645A1PCT designated stage expired Publication Date: 2024-10-03POWDERTECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012889
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing electrophotographic developers face challenges in maintaining consistent charge distribution and image quality over time due to wide charge amount variations, leading to issues like toner scattering and poor image density, especially with carriers having resin coating layers that wear off, affecting the charge imparting ability.

Method used

Ferrite particles with a specific composition and surface roughness are developed, featuring a gradient of Sr or Ca content based on particle size, which are used to create a carrier core material with a resin coating, ensuring a sharp charge amount distribution and improved charge imparting ability.

Benefits of technology

The solution provides a high charge imparting ability and sharp charge amount distribution, reducing toner scattering and maintaining good image quality even during long-term use, by optimizing the Sr or Ca content on the surface of ferrite particles and using them in an electrophotographic developer with a resin-coated carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present invention provides: ferrite particles that satisfy 1.10≤Y / X, where X represents the proportion (atom%) of Sr or Ca in the surface of particles having a particle size of at most 35 μm, and Y represents the proportion (atom%) of Sr or Ca in the surface of particles having a particle size of at least 40 μm; and a carrier core material that is for an electrophotographic developer and that contains the ferrite particles.
Need to check novelty before this filing date? Find Prior Art

Description

Ferrite particles, carrier core material for electrophotographic developer, carrier for electrophotographic developer, and electrophotographic developer

[0001] The present invention relates to ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer.

[0002] The electrophotographic development method is a method of developing an electrostatic latent image formed on a photoreceptor by adhering toner particles in a developer, and the developers used in this method are divided into two-component developers consisting of toner particles and carrier particles, and one-component developers using only toner particles. Of these developers, the magnetic brush method using a magnet roll is the mainstream development method using two-component developers consisting of toner particles and carrier particles.

[0003] In two-component developers, carrier particles are a carrier material that imparts a desired charge to the toner particles by being stirred together with the toner particles in a developer box filled with the developer, and then transports the charged toner particles to the surface of a photoreceptor to form a toner image on the photoreceptor. The carrier particles remaining on the developer roll holding the magnet return from the developer roll to the developer box, where they are mixed and stirred with new toner particles and are used repeatedly for a certain period of time.

[0004] Unlike single-component developers, two-component developers have carrier particles that are mixed and stirred with toner particles, charge the toner particles, and transport them, allowing for good controllability when designing the developer. Therefore, two-component developers are suitable for full-color development devices that require high image quality and high-speed printing devices that require reliable image maintenance and durability.

[0005] Thus, carrier particles must triboelectrically charge toner particles to the desired polarity and a sufficient charge amount during long-term use. However, if the toner charge distribution is wide, toner scattering due to low charge toner and poor image density due to high charge toner are likely to occur. In other words, carrier particles are required not only to have the ability to charge toner, but also to be able to control the charge distribution more narrowly.

[0006] Patent Document 1 proposes ferrite particles that have excellent toner charge build-up and high charge stability by locally providing large protrusions on the surface of the ferrite particles that serve as carrier particles. X Fe 3 - X O 4 (wherein M is at least one metal selected from the group consisting of Mg, Mn, Ca, Ti, Cu, Zn, and Ni, and 0<X<1), and characterized in that the maximum particle height Rz is greater than 2.2 μm and the average particle length RSm is greater than 19 μm and less than 26 μm.

[0007] Patent Document 2 proposes a carrier having a sharp charge distribution by providing appropriate irregularities in the resin coating layer of a resin-coated carrier. Specifically, Patent Document 2 discloses an electrostatic image developing carrier having a coating film made of at least a binder resin and fine particles, characterized in that the particle diameter (D) and the binder resin film thickness (h) are 1<[D / h]<10, and the magnetization of the carrier at 1 kOe is in the range of 40 to 80 emu / g.

[0008] Japanese Patent Publication No. 2015-151287 Japanese Patent Publication No. 2004-198663

[0009] However, in the techniques described in Patent Documents 1 and 2, the charge amount distribution taking into consideration the particle size distribution of the carrier is not necessarily sufficiently considered, and the charge amount distribution is not sufficiently sharp. In particular, in a carrier having a resin coating layer on its surface, the resin coating layer may wear and peel off over a long period of use in a developer tank, exposing the carrier core material. This increases the influence of the charge imparting ability and charge amount distribution of the carrier core material, making it difficult to control the charge of the toner, and making it more likely to cause poor image density and toner scattering.

[0010] Therefore, an object of the present invention is to provide a carrier core material for an electrophotographic developer which has high charge-imparting ability and a sharp charge distribution, and therefore is less likely to cause poor image density or toner scattering, and which can provide good image quality even when used as a developer over a long period of time; a carrier for an electrophotographic developer obtained by coating the surface of the carrier core material for an electrophotographic developer with a resin; and ferrite particles which become an electrophotographic developer using the carrier for an electrophotographic developer.

[0011] As a result of intensive research to solve the above-mentioned problems, the inventors have discovered that when the proportion of Sr or Ca on the surface of particles with a relatively small particle size and the proportion of Sr or Ca on the surface of particles with a relatively large particle size satisfy certain conditions, ferrite particles can be obtained that provide a carrier core material for electrophotographic developers with the desired charge-imparting ability and a sharp charge amount distribution.

[0012] That is, the present invention provides ferrite particles that satisfy the following formula: 1.10≦Y / X, where X (atomic %) is the proportion of Sr or Ca on the surface of particles having a particle diameter of 35 μm or less, and Y (atomic %) is the proportion of Sr or Ca on the surface of particles having a particle diameter of 40 μm or more.

[0013] The ferrite particles according to the present invention preferably satisfy the following formulae: 0.30≦X≦0.80, 0.36≦Y≦1.55, and 1.20≦Y / X≦2.00.

[0014] In the ferrite particles according to the present invention, the cumulative 50% particle diameter D50 in the particle size distribution based on volume is 30 μm or more and 50 μm or less, and the proportion P of particles with a particle diameter of 40 μm or more in the particle size distribution based on number is +40 is preferably 5% by number or more and 40% by number or less.

[0015] In the ferrite particles according to the present invention, it is preferable that the surface roughness Rz is 2.5 μm or more and 4.5 μm or less, and the standard deviation Rzσ of the surface roughness Rz is 0.2 μm or more and 1.0 μm or less.

[0016] The ferrite particles according to the present invention preferably contain 0.3% by weight or more and 1.2% by weight or less of Sr or Ca, and more preferably contain 15% by weight or more and 30% by weight or less of Mn and 45% by weight or more and 65% by weight or less of Fe.

[0017] In the ferrite particles according to the present invention, the residual magnetization σr is 3.0 Am 2 It is preferable that the amount is less than 1 / kg.

[0018] The present invention also provides a carrier core material for an electrophotographic developer, which contains the above-mentioned ferrite particles.

[0019] The present invention also provides a carrier for an electrophotographic developer, comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles.

[0020] The present invention also provides an electrophotographic developer comprising the above-mentioned carrier for electrophotographic developer and a toner. The electrophotographic developer according to the present invention is preferably used as a replenishment developer.

[0021] According to the present invention, it is possible to provide a carrier core material for an electrophotographic developer which has high charge-imparting ability and a sharp charge distribution, and therefore is less likely to cause poor image density or toner scattering, and which can provide good image quality even when used as a developer over a long period of time; a carrier for an electrophotographic developer obtained by coating the surface of the carrier core material for an electrophotographic developer with a resin; and ferrite particles which become an electrophotographic developer using the carrier for an electrophotographic developer.

[0022] In the present invention, a combination of two or more preferred aspects is a more preferred aspect. Hereinafter, embodiments of the ferrite particles, the carrier core material for an electrophotographic developer, the carrier for an electrophotographic developer, and the electrophotographic developer according to the present invention will be described. In this specification, the ferrite particles, the carrier core material for an electrophotographic developer, the carrier for an electrophotographic developer, and the electrophotographic developer each refer to an aggregate of individual particles, i.e., powder, unless otherwise specified.

[0023] 1. Ferrite Particles and Carrier Core Material for Electrophotographic Developer The ferrite particles according to the present invention satisfy the following formula: 1.10≦Y / X, where X (atomic %) is the proportion of Sr or Ca on the surface of particles having a particle diameter of 35 μm or less, and Y (atomic %) is the proportion of Sr or Ca on the surface of particles having a particle diameter of 40 μm or more. First, an embodiment of the ferrite particles according to the present invention will be described. Hereinafter, the ferrite particles according to the present invention will be described as being primarily used as a carrier core material for electrophotographic developers. However, the ferrite particles according to the present invention can be used in a variety of applications, such as magnetic inks, magnetic fluids, magnetic fillers, fillers for bonded magnets, and various functional fillers such as fillers for electromagnetic wave shielding materials, electronic component materials, and the like, and the applications of the ferrite particles are not limited to carrier core materials for electrophotographic developers.

[0024] (1) Constituent Components The ferrite particles according to the present invention are composed of MO·Fe 2 O 3 (M: divalent metal element), and usually contains Fe as the main metal component, and is preferably composed of one or two components selected from Mn and Mg. These main metal components exist as a solid solution in the spinel structure. The ferrite particles according to the present invention preferably contain at least Fe and Mn as the main metal components, and are preferably composed of Fe, Mn, and Mg as the main metal components.

[0025] In the ferrite particles according to the present invention, the Fe content is preferably 45% by weight or more and 65% by weight or less. When the Fe content is within this range, it becomes easier to adjust the magnetization and resistance to the desired levels. The Fe content is more preferably 47% by weight or more, and even more preferably 48% by weight or more. Furthermore, the Fe content is more preferably 60% by weight or less, and even more preferably 55% by weight or less. In a preferred embodiment, the Fe content in the ferrite particles is preferably 45% by weight or more and 60% by weight or less, and even more preferably 45% by weight or more and 55% by weight or less. In a preferred embodiment, the Fe content in the ferrite particles is preferably 47% by weight or more and 65% by weight or less, more preferably 47% by weight or more and 60% by weight or less, and even more preferably 47% by weight or more and 55% by weight or less. In one preferred embodiment, the Fe content in the ferrite particles is preferably 48% by weight or more and 65% by weight or less, more preferably 48% by weight or more and 60% by weight or less, and even more preferably 48% by weight or more and 55% by weight or less.

[0026] In the ferrite particles according to the present invention, the Mn content is preferably 15% by weight or more and 30% by weight or less. A Mn content within this range makes it easier to adjust the magnetization and resistance to desired levels. The Mn content is more preferably 16% by weight or more, and even more preferably 17% by weight or more. Furthermore, the Mn content is more preferably 25% by weight or less, and even more preferably 22% by weight or less. In a preferred embodiment, the Mn content in the ferrite particles is preferably 15% by weight or more and 25% by weight or less, and even more preferably 15% by weight or more and 22% by weight or less. In a preferred embodiment, the Mn content in the ferrite particles is preferably 16% by weight or more and 30% by weight or less, more preferably 16% by weight or more and 25% by weight or less, and even more preferably 16% by weight or more and 22% by weight or less. In one preferred embodiment, the Mn content in the ferrite particles is preferably 17% by weight or more and 30% by weight or less, more preferably 17% by weight or more and 25% by weight or less, and even more preferably 17% by weight or more and 22% by weight or less.

[0027] The ferrite particles according to the present invention preferably contain 15% by weight or more and 30% by weight or less of Mn and 45% by weight or more and 65% by weight or less of Fe.

[0028] In the ferrite particles according to the present invention, the Mg content is preferably 0.5 wt% or more and 10 wt% or less. A Mg content within this range facilitates adjustment of magnetization and resistance to desired levels. The Mg content is more preferably 1.0 wt% or more, and even more preferably 1.5 wt% or more. Furthermore, the Mg content is more preferably 5.0 wt% or less, and even more preferably 3.0 wt% or less. In a preferred embodiment, the Mg content in the ferrite particles is preferably 0.5 wt% or more and 5.0 wt% or less, and even more preferably 0.5 wt% or more and 3.0 wt% or less. In a preferred embodiment, the Mg content in the ferrite particles is preferably 1.0 wt% or more and 10 wt% or less, more preferably 1.0 wt% or more and 5.0 wt% or less, and even more preferably 1.0 wt% or more and 3.0 wt% or less. In a preferred embodiment, the Mg content in the ferrite particles is preferably 1.5% by weight or more and 10% by weight or less, more preferably 1.5% by weight or more and 5.0% by weight or less, and even more preferably 1.5% by weight or more and 3.0% by weight or less.

[0029] It is also important that the ferrite particles according to the present invention contain Sr or Ca as a trace component. The Sr or Ca content in the ferrite particles according to the present invention is preferably 0.3% by weight or more and 1.2% by weight or less. By setting the Sr or Ca content to 0.3% by weight or more, the electrophotographic developer carrier's ability to impart charge to the toner is enhanced. By setting the Sr or Ca content to 1.2% by weight or less, the carrier is less susceptible to environmental influences such as high temperature and high humidity, improving the environmental dependency of the charge amount. The Sr or Ca content is more preferably 0.4% by weight or more, and even more preferably 0.5% by weight or more. The Sr or Ca content is more preferably 0.9% by weight or less, and even more preferably 0.8% by weight or less. The ferrite particles according to the present invention may contain either Sr or Ca, or may contain both Sr and Ca. When both Sr and Ca are included, the above content refers to the total content of Sr and Ca. In a preferred embodiment, the Sr or Ca content in the ferrite particles is preferably 0.3 wt% to 0.9 wt%, more preferably 0.3 wt% to 0.8 wt%. In a preferred embodiment, the Sr or Ca content in the ferrite particles is preferably 0.4 wt% to 1.2 wt%, more preferably 0.4 wt% to 0.9 wt%, and even more preferably 0.4 wt% to 0.8 wt%. In a preferred embodiment, the Sr or Ca content in the ferrite particles is preferably 0.5 wt% to 1.2 wt%, more preferably 0.5 wt% to 0.9 wt%, and even more preferably 0.5 wt% to 0.8 wt%.

[0030] (2) Sr or Ca Ratio According to Particle Size Here, the ability to impart charge to the toner is achieved by frictional charging between the electrophotographic developer carrier and the toner, so it is greatly affected by the particle size and specific surface area of ​​the electrophotographic developer carrier (ferrite particles). In general, there is a strong correlation between the particle size and specific surface area of ​​particles, and the larger the particle size, the smaller the specific surface area. Therefore, electrophotographic developer carriers with larger particle sizes have relatively weaker charge imparting ability than electrophotographic developer carriers with smaller particle sizes. In other words, it is thought that the particle size distribution causes variations in the ability of the electrophotographic developer carrier to impart charge to the toner, resulting in a wide charge distribution of the toner.

[0031] On the other hand, if the particle size distribution of the carrier for electrophotographic developer is too sharp, the amount of toner that enters the interparticle voids increases relatively, which reduces the frequency of contact with the toner, and this can result in a decrease in charge amount and a wide charge amount distribution, and can also significantly reduce production yield.

[0032] Therefore, in the present invention, when Sr or Ca, which is known to enhance the ability to impart charge to toner, is added to the ferrite particles, a gradient in the composition (particularly the proportion of Sr or Ca) according to the particle size of the ferrite particles is provided, thereby reducing the variation in the charge imparting ability due to particle size and making the charge amount distribution sharp. In other words, it is important to set the proportion of Sr or Ca on the surface of particles with a relatively large particle size higher than the proportion of Sr or Ca on the surface of particles with a relatively small particle size.

[0033] More specifically, in the present invention, when the proportion of Sr or Ca on the surface of particles having a particle diameter of 35 μm or less is X (atomic %) and the proportion of Sr or Ca on the surface of particles having a particle diameter of 40 μm or more is Y (atomic %), it is important to satisfy the following formula: 1.10≦Y / X. If Y / X is less than 1.10, the variation in the ability to impart charge to the toner increases and the charge distribution becomes broad, making toner scattering and insufficient image density more likely to occur. Y / X is preferably 1.20 or more, and more preferably 1.25 or more. However, if Y / X is too large, the variation in the ability to impart charge to the toner is more likely to occur, so Y / X is preferably 2.50 or less, more preferably 2.00 or less, and even more preferably 1.75 or less. In a preferred embodiment, it is preferable that 1.10≦Y / X≦2.50 is satisfied, more preferably that 1.10≦Y / X≦2.00 is satisfied, and even more preferably that 1.10≦Y / X≦1.75 is satisfied. In a preferred embodiment, it is preferable that 1.20≦Y / X≦2.50 is satisfied, more preferably that 1.20≦Y / X≦2.00 is satisfied, and even more preferably that 1.20≦Y / X≦1.75 is satisfied. In a preferred embodiment, it is preferable that 1.25≦Y / X≦2.50 is satisfied, more preferably that 1.25≦Y / X≦2.00 is satisfied, and even more preferably that 1.25≦Y / X≦1.75 is satisfied.

[0034] The proportion X (atomic %) of Sr or Ca on the surface of particles having a particle diameter of 35 μm or less preferably satisfies the following formula: 0.30≦X≦0.80. By setting X to 0.30 or more, sufficient charge-imparting ability can be obtained. Furthermore, by setting X to 0.80 or less, the particles are less susceptible to environmental influences such as high temperature and high humidity, improving the environmental dependency of the charge amount. X is more preferably 0.35 or more, and even more preferably 0.40 or more. Furthermore, X is more preferably 0.70 or less, and even more preferably 0.65 or less. In a preferred embodiment, it is preferable to satisfy 0.30≦X≦0.70, and more preferably to satisfy 0.30≦X≦0.65. In a preferred embodiment, it is preferable to satisfy 0.35≦X≦0.80, more preferably to satisfy 0.35≦X≦0.70, and even more preferably to satisfy 0.35≦X≦0.65. In a preferred embodiment, it is preferable that 0.40≦X≦0.80 is satisfied, more preferably 0.40≦X≦0.70 is satisfied, and even more preferably 0.40≦X≦0.65 is satisfied, where X represents the proportion of Sr or Ca in elemental mapping of the surface of particles having a particle diameter of 35 μm or less.

[0035] The proportion Y (atomic %) of Sr or Ca on the surface of particles having a particle diameter of 40 μm or more preferably satisfies the following formula: 0.36≦Y≦1.55. By setting Y to 0.36 or more, sufficient charge-imparting ability can be obtained. Furthermore, by setting Y to 1.55 or less, the particles are less susceptible to environmental influences such as high temperature and high humidity, and the environmental dependency of the charge amount is improved. Y is more preferably 0.45 or more, and even more preferably 0.60 or more. Furthermore, Y is more preferably 1.15 or less, and even more preferably 0.95 or less. In a preferred embodiment, it is preferable to satisfy 0.36≦Y≦1.15, and more preferably to satisfy 0.36≦Y≦0.95. In a preferred embodiment, it is preferable to satisfy 0.45≦Y≦1.55, more preferably to satisfy 0.45≦Y≦1.15, and even more preferably to satisfy 0.45≦Y≦0.95. In a preferred embodiment, it is preferable that 0.60≦Y≦1.55 is satisfied, more preferably 0.60≦Y≦1.15 is satisfied, and even more preferably 0.60≦Y≦0.95 is satisfied, where Y represents the proportion of Sr or Ca in elemental mapping of the surface of particles having a particle diameter of 40 μm or more.

[0036] The ferrite particles according to the present invention more preferably satisfy the following formulae: 0.30≦X≦0.80, 0.36≦Y≦1.55, and 1.20≦Y / X≦2.00.

[0037] The proportion of Sr or Ca in elemental mapping of the particle surface can be measured by energy dispersive X-ray analysis (EDX analysis). EDX analysis can measure the element content at a depth of about several μm in the ferrite particle. Specific measurement methods will be described in the examples below.

[0038] (3) Particle Size Distribution In the ferrite particles according to the present invention, the 50% volume cumulative particle diameter D50 in the volume-based particle size distribution is preferably 30 μm or more and 50 μm or less. By setting D50 to 30 μm or more, adhesion of the carrier for electrophotographic developer is less likely to occur. Furthermore, by setting D50 to 50 μm or less, the particle size becomes appropriate for the toner, thereby improving the charging ability. D50 is more preferably 33 μm or more. Furthermore, D50 is more preferably 45 μm or less, and even more preferably 42 μm or less. In a preferred embodiment, D50 is more preferably 30 μm or more and 45 μm or less, and even more preferably 30 μm or more and 42 μm or less. In a preferred embodiment, D50 is more preferably 33 μm or more and 50 μm or less, more preferably 33 μm or more and 45 μm or less, and even more preferably 33 μm or more and 42 μm or less.

[0039] In the ferrite particles according to the present invention, the ratio D of particles having a particle diameter of 62 μm or more in the particle size distribution based on volume +62 is preferably 12% by volume or less, and more preferably 10% by volume or less. +62 By setting the ratio D of particles having a particle diameter of 22 μm or less in the particle size distribution based on volume to 12% or less, a sharp distribution with few large particles is obtained, thereby increasing the toner transport ability and improving image quality. -22 is preferably 3% by volume or less, and more preferably 1.5% by volume or less. -22 By setting the content to 3% by volume or less, a sharp distribution with few small particles is obtained, so that carrier adhesion is less likely to occur.

[0040] In addition, in the ferrite particles according to the present invention, the ratio P of particles having a particle diameter of 40 μm or more in the particle size distribution based on the number +40 is preferably 5% by number or more and 40% by number or less. +40 If the particle size is within this range, the inter-particle voids are appropriately filled without reducing the yield, and therefore the charge imparting property of the toner can be easily adjusted to a desired value. +40is more preferably 8% by number or more. +40 is more preferably 20% by number or less. +40 is more preferably 5% by number or more and 20% by number or less. +40 is more preferably 8% by number or more and 40% by number or less, and even more preferably 8% by number or more and 20% by number or less.

[0041] The ferrite particles according to the present invention have a cumulative 50% particle diameter D50 in a particle size distribution based on volume of 30 μm or more and 50 μm or less, and a ratio P of particles with a particle diameter of 40 μm or more in a particle size distribution based on number of particles. +40 is more preferably 5% by number or more and 40% by number or less.

[0042] (4) Surface Properties In the ferrite particles according to the present invention, the surface roughness Rz is preferably 2.5 μm or more and 4.5 μm or less. By setting Rz to 2.5 μm or more, the charge imparting ability tends to be enhanced due to the moderately present unevenness. By setting Rz to 4.5 μm or less, the decrease in fluidity due to excessive unevenness is suppressed, and the frequency of contact with the toner is increased, thereby improving the charge imparting ability of the toner. Rz is more preferably 2.8 μm or more. Furthermore, Rz is more preferably 4.0 μm or less. In one preferred embodiment, Rz is more preferably 2.5 μm or more and 4.0 μm or less. In one preferred embodiment, Rz is more preferably 2.8 μm or more and 4.5 μm or less, and even more preferably 2.8 μm or more and 4.0 μm or less.

[0043] Furthermore, in the ferrite particles according to the present invention, the standard deviation Rzσ of the surface roughness Rz is preferably 0.2 μm or more and 1.0 μm or less. By setting Rzσ to 0.2 μm or more, it becomes easier to manufacture the particles using a method including sintering by solid-phase reaction. By setting Rzσ to 1.0 μm or less, when used with a resin coating, exposure of the core material due to variations in the resin coating is less likely to occur, and carrier adhesion due to charge injection is less likely to occur. Rzσ is more preferably 0.3 μm or more. Furthermore, Rzσ is more preferably 0.8 μm or less. In a preferred embodiment, Rzσ is more preferably 0.2 μm or more and 0.8 μm or less. In a preferred embodiment, Rzσ is more preferably 0.3 μm or more and 1.0 μm or less, and even more preferably 0.3 μm or more and 0.8 μm or less.

[0044] The ferrite particles according to the present invention preferably have a surface roughness Rz of 2.5 μm or more and 4.5 μm or less, and a standard deviation Rzσ of the surface roughness Rz of 0.2 μm or more and 1.0 μm or less.

[0045] (5) Magnetization In the ferrite particles according to the present invention, the residual magnetization σr is 3.0 Am 2 / kg. 2 If the σr is less than 2.5 Am / kg, aggregation due to residual magnetization is unlikely to occur, and the ability to impart charge to the toner is unlikely to decrease and the charge distribution is unlikely to vary. 2 / kg or less. 2 / kg or more.

[0046] (6) Manufacturing Method The method for manufacturing the ferrite particles according to the present invention is not particularly limited, but it is preferable to manufacture them by the following method.

[0047] First, the raw materials for producing the ferrite particles according to the present invention are weighed in appropriate amounts, and then pulverized and mixed for 0.5 hours or more (preferably 1 to 20 hours) using a ball mill or a vibration mill to obtain a pulverized product. The raw materials are not particularly limited, but are preferably selected so as to have a composition containing the above-mentioned elements. The raw material for Fe is preferably Fe, 2 O3 As a raw material for Mn, Mn 3 O 4 and MnO 2 It is preferable to use one or more compounds selected from the following: Mg(OH) 2 , MgO, and MgCO 3 It is preferable to use one or more compounds selected from the following: 3 As a raw material for Ca, it is preferable to use CaCO 3 It is preferable to use

[0048] The ferrite particles according to the present invention need to have a gradient in composition (particularly the proportion of Sr or Ca) depending on the particle size, and this gradient can be adjusted by mixing and firing granules of different compositions and particle sizes. Specifically, two types of blended raw materials having a desired composition ratio are prepared, and in the granulation stage, the particle size of the granules is adjusted by changing the granulation conditions (e.g., atomizer rotation speed, etc.), thereby preparing two types of granules with different particle sizes, and then mixing and firing the sintered product so that the D50 of the sintered product becomes the desired particle size.

[0049] In addition, the composition gradient according to particle size can also be adjusted by changing the particle size of the Sr or Ca raw material used. Specifically, there are methods such as preparing raw materials with different particle sizes and pulverizing only the Sr or Ca raw material using a bead mill. The finer the particle size of the raw material, the more likely it is that a solid-phase reaction will occur and precipitate on the particle surface. Therefore, for example, in the granulation stage, a raw material of a metal that is the main component, such as Fe, Mn, or Mg, is pulverized to a desired particle size, and then the Sr or Ca raw material is added and mixed, thereby producing a slurry in which only the Sr or Ca in the raw material has a different particle size.

[0050] Although increasing the firing temperature can facilitate the precipitation of Sr or Ca on the particle surface, it is difficult to create a gradient in the particle size distribution. Furthermore, the method of mixing fired materials fired at different temperatures results in mixing two types of particles with different surface properties or shapes, which may result in the inability to achieve a sharp charge distribution.

[0051] The pulverized material obtained in this manner is pelletized using a pressure molding machine or the like, and then pre-fired at a temperature of 700 to 1100°C in the atmosphere. Alternatively, instead of using a pressure molding machine, water may be added to the pulverized material to form a slurry, which may then be granulated using a spray dryer. After pre-fired, the material is further pulverized using a ball mill or a vibration mill, and then water and, if necessary, a dispersant or a binder are added to adjust the viscosity, followed by granulation and granulation using a spray dryer. When pulverizing after pre-fired, water may be added and the material may be pulverized using a wet ball mill or a wet vibration mill, etc.

[0052] The grinding machine, such as a ball mill or a vibration mill, is not particularly limited. However, in order to effectively and uniformly disperse the raw materials, it is preferable to use fine beads having a particle size of 1 mm or less as the media used. Furthermore, the degree of grinding can be controlled by adjusting the diameter, composition, and grinding time of the beads used. In order to uniformly disperse the raw materials, it is preferable to grind the material so that the volume average particle size (D50) of the ground product is 5 μm or less, more preferably 3.0 μm or less, and even more preferably 2.5 μm or less.

[0053] Next, in order to obtain ferrite powder with a uniform particle size, it is preferable to classify the granulated material before firing to remove fine particles contained in the granulated material. The classification of the granulated material can be carried out using a known air classification or a sieve.

[0054] The classified granules are then fired. The granules are preferably subjected to primary firing in a firing furnace, such as a rotary kiln, in which the granules (material to be fired) are passed through a hot section while flowing, followed by main firing. By performing primary firing in a firing furnace, such as a rotary kiln, in which the granules are passed through a hot section while flowing, organic substances such as binders used during granulation can be removed uniformly from the granules in a relatively short time, compared to performing primary firing while the granules are left stationary in a kiln or the like. At the same time, the ferrite reaction can be partially promoted during the primary firing, thereby suppressing variations in the surface Rz during the subsequent main firing.

[0055] When primary firing is performed using the above-described type of firing furnace, the temperature is preferably 750°C or higher and 1050°C or lower. By performing primary firing within this temperature range, organic matter removal and ferrite reaction are efficiently performed while abnormal grain growth is suppressed, making it easier to suppress the occurrence of variations in surface roughness Rz as described above. Furthermore, in order to efficiently remove organic matter and perform ferrite reaction, the primary firing temperature is more preferably 800°C or higher, and even more preferably 850°C or higher. Furthermore, in order to suppress abnormal grain growth, the primary firing temperature is more preferably 1000°C or lower, and even more preferably 980°C or lower. In a preferred embodiment, the primary firing temperature is more preferably 750°C or higher and 1000°C or lower, and even more preferably 750°C or higher and 980°C or lower. In a preferred embodiment, the primary firing temperature is more preferably 800° C. or higher and 1050° C. or lower, more preferably 800° C. or higher and 1000° C. or lower, and even more preferably 800° C. or higher and 980° C. In a preferred embodiment, the primary firing temperature is more preferably 850° C. or higher and 1050° C. or lower, more preferably 850° C. or higher and 1000° C. or lower, and even more preferably 850° C. or higher and 980° C. or lower.

[0056] The firing is preferably carried out in an inert atmosphere or a weakly oxidizing atmosphere by holding the material at a temperature of 1050°C to 1300°C for 3 to 24 hours, more preferably at a temperature of 1050°C to 1300°C for 4 to 24 hours, and even more preferably at 1100°C to 1250°C. Note that an inert atmosphere or a weakly oxidizing atmosphere refers to a nitrogen and oxygen mixed gas atmosphere in which the oxygen concentration is 0.1% by volume (1000 ppm) to 5% by volume (50,000 ppm). The atmospheric oxygen concentration is more preferably 0.1% by volume (1000 ppm) to 3.5% by volume (35,000 ppm), and even more preferably 0.1% by volume (1000 ppm) to 2.5% by volume (25,000 ppm). By firing within the above temperature and oxygen concentration ranges, the ferritization reaction proceeds, and the desired saturation magnetization and remanence can be obtained.

[0057] The fired product is then crushed and classified to obtain ferrite particles. The particle size is adjusted to the desired particle size using conventional classification methods such as air classification, mesh filtration, and sedimentation. When dry recovery is performed, recovery can also be performed using a cyclone or the like. When adjusting the particle size, two or more of the above-mentioned classification methods may be selected and carried out, or one classification method may be used with different conditions to remove coarse particles and fine particles. Thereafter, if necessary, the surfaces of the ferrite particles may be subjected to a surface oxidation treatment by low-temperature heating, for example, at 300°C to 700°C, to adjust the surface resistance of the ferrite particles.

[0058] The present invention also relates to a carrier core material for an electrophotographic developer, which contains the above-mentioned ferrite particles.

[0059] 2. Carrier for Electrophotographic Developer Next, the carrier for electrophotographic developer according to the present invention will be described. The carrier for electrophotographic developer according to the present invention is characterized by comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles. That is, the ferrite particles are used as a core material of the carrier for electrophotographic developer. As the ferrite particles have been described above, the resin coating layer will be mainly described here.

[0060] (1) Coating Resin The type of resin (coating resin) constituting the resin coating layer is not particularly limited. For example, fluororesin, acrylic resin, epoxy resin, polyamide resin, polyamideimide resin, polyester resin, unsaturated polyester resin, urea resin, melamine resin, alkyd resin, phenolic resin, fluoroacrylic resin, acrylic-styrene resin, silicone resin, etc. may be used. In addition, modified silicone resins obtained by modifying silicone resins with resins such as acrylic resin, polyester resin, epoxy resin, polyamide resin, polyamideimide resin, alkyd resin, urethane resin, fluororesin, etc. may also be used.

[0061] Furthermore, from the viewpoint of suppressing resin peeling due to mechanical stress received during stirring and mixing with the toner, the coating resin is preferably a thermosetting resin. Suitable thermosetting resins for the coating resin include epoxy resins, phenolic resins, silicone resins, unsaturated polyester resins, urea resins, melamine resins, alkyd resins, and resins containing these. However, as mentioned above, the type of coating resin is not particularly limited, and an appropriate one can be selected depending on the type of toner to be combined, the usage environment, etc.

[0062] The resin coating layer may be formed using one type of resin, or may be formed using two or more types of resin. When two or more types of resins are used, two or more types of resins may be mixed to form one resin coating layer, or multiple resin coating layers. For example, it is preferable to provide a first resin coating layer having good adhesion to the ferrite particles on the surface of the ferrite particles, and then provide a second resin coating layer on the surface of the first resin coating layer to impart the desired charging performance to the carrier.

[0063] (2) Resin Coating Amount The amount of resin coating the surface of the ferrite particles (resin coating amount) is preferably 0.1% by weight or more and 10% by weight or less relative to the ferrite particles used as a carrier core material for electrophotographic developers. By setting the resin coating amount to 0.1% by weight or more, the surface of the ferrite particles can be sufficiently coated with resin, making it possible to obtain the desired charging ability. Furthermore, by setting the resin coating amount to 10% by weight or less, aggregation of carrier particles during production is less likely to occur, thereby suppressing decreases in productivity such as a decrease in yield and fluctuations in developer properties such as developer fluidity in actual machines or charging ability to toner.

[0064] (3) Additives The resin coating layer may contain additives such as conductive agents and charge control agents for the purpose of controlling the electrical resistance, charge amount, and charge speed of the carrier.

[0065] Examples of conductive agents include conductive carbon, oxides such as titanium oxide and tin oxide, and various organic conductive agents. However, because the electrical resistance of conductive agents is low, adding too much conductive agent can easily cause charge leakage. Therefore, the content of the conductive agent is preferably 0.25 wt % to 20.0 wt % of the solid content of the coating resin, more preferably 0.5 wt % to 15.0 wt %, and even more preferably 1.0 wt % to 10.0 wt %.

[0066] Examples of charge control agents include various charge control agents commonly used for toners and silane coupling agents. While the types of these charge control agents and coupling agents are not particularly limited, preferred examples include nigrosine dyes, quaternary ammonium salts, organometallic complexes, and metal-containing monoazo dyes, as well as aminosilane coupling agents and fluorine-based silane coupling agents. The content of the charge control agent is preferably 0.25% by weight or more and 20.0% by weight or less, more preferably 0.5% by weight or more and 15.0% by weight or less, and even more preferably 1.0% by weight or more and 10.0% by weight or less, based on the solid content of the coating resin.

[0067] 3. Electrophotographic Developer Next, an embodiment of the electrophotographic developer according to the present invention will be described. The electrophotographic developer contains the above-described carrier for electrophotographic developer and toner. The electrophotographic developer is also preferably used as a replenishment developer.

[0068] (1) Toner As the toner constituting the electrophotographic developer, for example, either a polymerized toner produced by a polymerization method or a pulverized toner produced by a pulverization method can be preferably used. These toners may contain various additives and may be any toner as long as they can be used as an electrophotographic developer in combination with the above-mentioned carrier.

[0069] The volume average particle diameter (cumulative 50% particle diameter D50) of the toner is preferably 2 μm or more and 15 μm or less, and more preferably 3 μm or more and 10 μm or less. When the volume average particle diameter (cumulative 50% particle diameter D50) of the toner is within the above range, an electrophotographic developer that enables high-quality electrophotographic printing can be obtained.

[0070] Regarding the mixture ratio of the carrier and the toner, the toner concentration is preferably 3% by weight or more and 15% by weight or less. An electrophotographic developer containing the toner at the above concentration can easily obtain a desired image density and can more effectively suppress fogging and toner scattering. On the other hand, when the electrophotographic developer is used as a replenishment developer, the toner content is preferably 2 parts by weight or more and 50 parts by weight or less per 1 part by weight of the carrier.

[0071] (2) Application to Electrophotographic Devices The electrophotographic developer according to the present invention can be suitably used in various electrophotographic developing devices that employ a magnetic brush development method in which a carrier is attracted and attached to a magnetic drum or the like by magnetic force to form a brush-like toner, and a visible image is formed by attaching the toner to an electrostatic latent image formed on a photosensitive member or the like while applying a bias electric field. The electrophotographic developer according to the present invention can be used not only in electrophotographic developing devices that use a DC bias electric field when applying a bias electric field, but also in electrophotographic developing devices that use an AC bias electric field in which an AC bias electric field is superimposed on a DC bias electric field.

[0072] Example 1: MnO raw material, MgO raw material, and Fe as main component raw materials 2 O 3 The raw materials were MnO:MgO:Fe 2 O 3 The SrO raw material was weighed so that the molar ratio of the main component raw material to SrO was 100:0.8. The Mn raw material was trimanganese tetroxide, the MgO raw material was magnesium oxide, and the Fe raw material was 2 O 3 Ferric oxide was used as the raw material, and strontium carbonate was used as the SrO raw material.

[0073] Next, the weighed raw materials were pulverized for 5 hours using a dry media mill (vibration mill, 1 / 8-inch diameter stainless steel beads), and the resulting pulverized material was converted into pellets of approximately 1 mm square using a roller compactor. The resulting pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then passed through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then placed in a continuous electric furnace and heated at 900 ° C for 3 hours, thereby carrying out pre-firing. Next, using a dry media mill (vibration mill, 1 / 8-inch diameter stainless steel beads), the material was pulverized for 6 hours until the average particle size (D50) was approximately 5 μm.

[0074] Water was added to the resulting pulverized material and pulverized for 6 hours using a wet media mill (horizontal bead mill, 1 mm diameter zirconia beads). The particle size (primary particle size of the pulverized material) of the resulting slurry was measured using a laser diffraction particle size distribution analyzer (LA-950, manufactured by Horiba, Ltd.), and the average particle size (D50) was approximately 2.3 μm. Furthermore, an appropriate amount of dispersant was added to the resulting slurry, and 0.5 wt% of PVA (polyvinyl alcohol) was added as a binder relative to the solid content (amount of pre-calcined material in the slurry). The mixture was then granulated and dried using a spray dryer. The particle size of the resulting granulated material was adjusted to obtain granulated material A with an average particle size (D50) of approximately 42 μm.

[0075] Granulated product B having an average particle size (D50) of about 55 μm was obtained in the same manner as granulated product A, except that the SrO raw material was weighed so that the molar ratio of main component raw material:SrO was 100:1.2. The particle size of the granulated product was adjusted by adjusting the atomizer rotation speed during granulation in a spray dryer, and the particle size was also adjusted.

[0076] The granulated material obtained above was mixed with granulated material A and granulated material B in a ratio of 2:1, and the resulting granulated material was heated in an air atmosphere at 950°C for 2 hours in a rotary electric furnace for primary firing. The granulated material was then fired in a tunnel electric furnace at a firing temperature (holding temperature) of 1200°C in an atmosphere with an oxygen concentration of 0.3% by volume for 3 hours, at a heating rate of 200°C / hour and a cooling rate of 150°C / hour. The resulting fired material was crushed using a hammer crusher, and further classified using a gyrosifter (vibrating sieve) and a turbo classifier (air classifier) ​​to adjust the particle size. Ferrite particles were then obtained by separating low-magnetic-force products using magnetic separation.

[0077] Examples 2 to 9 and Comparative Examples 1 to 3 Ferrite particles were obtained in the same manner as in Example 1, except that the blending amounts of the raw materials used in producing granulated material A and granulated material B and the average particle sizes (D50) of granulated material A and granulated material B were changed as shown in Table 1. In Example 8, calcium carbonate was used as the CaO raw material instead of the SrO raw material.

[0078]

[0079] The ferrite particles obtained in Examples 1 to 9 and Comparative Examples 1 to 3 were evaluated for the following points. The results are shown in Table 2.

[0080] <Elemental Analysis> The content of metal components in the ferrite particles was measured by chemical analysis (ICP). Specifically, 0.2 g of ferrite particles was weighed, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added to the weighed ferrite particles. The mixture was heated to prepare an aqueous solution in which the ferrite particles were completely dissolved. The obtained aqueous solution was placed in an ICP analyzer (ICPS-1000IV, manufactured by Shimadzu Corporation), and the content of the metal components Fe, Mn, Mg, Sr, and Ca was measured.

[0081] <Particle Size Distribution> The particle size distribution of the ferrite particles was measured by a laser diffraction scattering method. Specifically, 10 g of ferrite particles and 80 ml of water were first placed in a 100 ml beaker, and 2 to 3 drops of a dispersant (sodium hexametaphosphate) were added. Next, an ultrasonic homogenizer (UH-150 type, manufactured by SMT) was used to set the output level to 4, disperse the particles for 20 seconds, and then remove bubbles formed on the surface of the beaker to prepare a measurement sample. Then, a Microtrac particle size analyzer (Model MT3300II, manufactured by Nikkiso) was used to measure the particle size distribution of the ferrite particles in the measurement sample under a refractive index of 2.42, and the cumulative 50% particle diameter D50 (μm) in the volume-based particle size distribution and the proportion D of particles with a particle diameter of 22 μm or less were measured. -22 (volume %), and the proportion D of particles with a particle diameter of 62 μm or more +62 The percentage of particles with a particle diameter of 40 μm or more in the particle size distribution based on the number of particles (P) was calculated. +40 The percentage (number %) was calculated.

[0082] <Magnetization> The remanent magnetization of the ferrite particles was measured using a vibrating sample magnetometer (VSM-C7-10A, manufactured by Toei Kogyo Co., Ltd.). Specifically, the ferrite particles were first filled into a cell with an inner diameter of 5 mm and a height of 2 mm, and the cell was set in the above-mentioned apparatus. A magnetic field was then applied and swept up to 1 K·1000 / 4π·A / m (=1 kOe). Next, the applied magnetic field was reduced, and a hysteresis curve was created on recording paper. The remanent magnetization was measured from the data of this curve.

[0083] <Surface Properties> To evaluate the surface properties of ferrite particles, the surface roughness Rz (μm) and the standard deviation Rzσ (μm) of the surface roughness Rz were measured. Specifically, a hybrid laser microscope (mc2000, manufactured by Lasertec) was used to obtain the three-dimensional shape of the surface of the ferrite particles to be measured (measurement target particles). As a pretreatment, double-sided tape was attached to a glass slide, and ferrite particles were sprinkled on the adhesive surface to fix the ferrite particles to the glass slide. A xenon lamp was used as the light source, the magnification of the objective lens was set to 100x, and the measurement target particles were selected, and the three-dimensional shape of the surface was obtained using the automatic photography function of the software LMeye7 included with the device.

[0084] Twenty-one 15.0 μm line segments were drawn at 0.75 μm intervals on the three-dimensional image of the target particle obtained as described above, and a measured profile curve on each line segment was extracted. Each of the obtained measured profile curves was corrected using a profile filter to extract a roughness curve. The cutoff values ​​of the profile filter were λs, which separates the roughness component from a shorter wavelength component, and λc, which separates the roughness component from a waviness component. The respective cutoff values ​​were set to λs = 0.0025 mm and λc = 0.0800 mm, and the surface roughness Rz (μm) was calculated from the obtained roughness curve. In this way, the average value of the surface roughness Rz (μm) obtained based on the 21 line segments was taken as the Rz (μm) of each target particle. Using the same procedure, the average value of the surface roughness Rz values ​​of 30 target particles was taken as the surface roughness Rz (μm) of each ferrite particle, and its standard deviation Rzσ (μm) was also calculated.

[0085] <EDX> The proportion (atomic %) of Sr or Ca on the particle surface was measured by energy dispersive X-ray analysis (EDX analysis). EDX analysis can measure the element content at a depth of about several μm in ferrite particles. Specifically, first, images of ferrite particles were taken using a scanning electron microscope (SEM, SU8020, manufactured by Hitachi High-Technogies) under conditions of an acceleration voltage of 20 kV, a WD of 15 mm, and a magnification of 150x. The obtained images were then imported into an energy dispersive X-ray analyzer (EMax X-Max50, manufactured by Horiba, Ltd.), and particles with no particle overlap and a particle diameter of 35 μm or less were selected by region selection. Note that particles with a ratio of the minimum Feret diameter to the maximum Feret diameter of 1.0 or more and 1.2 or less were selected, and particles with agglomerates of two or more particles within this range were also selected. Mapping was then performed on constituent elements such as Fe, Mn, Mg, Sr, and Ca, and the proportion (atomic %) of Sr or Ca was calculated from the obtained X-ray spectrum peaks. The average of the proportions (atomic %) of Sr or Ca for 100 particles measured in this manner was taken as the proportion X (atomic %) of Sr or Ca in the elemental mapping of the particle surface of particles with a particle diameter of 35 μm or less. The same procedure was performed on particles with a particle diameter of 40 μm or more, and the proportion Y (atomic %) of Sr or Ca in the elemental mapping of the particle surface of particles with a particle diameter of 40 μm or more was calculated.

[0086] <Chargeability> The chargeability of ferrite particles (carrier core material) was evaluated by measuring the charge amount Q under normal temperature and humidity (N / N) conditions. N/N and its standard deviation Q N/Nσ The charge amount was measured. The charge amount measuring device used was a device consisting of a cylindrical aluminum tube (sleeve), a magnet roll placed inside the sleeve, and a cylindrical electrode placed around the outside of the sleeve. The sleeve had a diameter of 31 mm and a length of 76 mm. The magnet roll had a total of eight magnet poles (magnetic flux density 0.1 T) arranged with their north and south poles alternating. The cylindrical sleeve and the cylindrical electrode were set so that the gap between them was 5.0 mm.

[0087] Measurement of charge amount and charge amount distribution under a normal temperature and humidity (N / N) environment was performed as follows. First, ferrite particles (carrier core material) and a commercially available negative toner (cyan toner, manufactured by Fuji Xerox, for DocuPrint C3530) used in full-color printers were weighed out so that the toner concentration was 7.5% by weight and the total weight was 50 g. The weighed ferrite particles and toner were exposed to a normal temperature and humidity environment of 20°C and 55% relative humidity for 12 hours or more. The ferrite particles and toner were then placed in a 50 ml glass bottle and stirred at 120 rpm for 30 minutes to prepare a developer.

[0088] 0.5 g of the resulting developer was uniformly applied to the sleeve of a charge amount measuring device. Next, with the sleeve fixed, the inner magnetic roll was rotated at 100 rpm, and in this state, a DC voltage of 2000 V was applied between the outer electrode and the sleeve for 60 seconds. The applied voltage caused the toner in the developer to migrate to the outer electrode. At this time, an electrometer (insulation resistance meter model 6517A, manufactured by KEITHLEY) was connected to the cylindrical electrode to measure the charge amount of the migrated toner. After 60 seconds, the applied voltage was turned off, the rotation of the magnetic roll was stopped, the outer electrode was removed, and the toner that had migrated to the electrode was recovered and its weight was measured. The charge amount Q was then calculated from the measured charge amount and weight of the toner. N/N (μC / g) was calculated.

[0089] The charge amount distribution of the developer obtained above was measured using a charge amount / particle size distribution measuring device (E-SPART Analyzer EST-G, manufactured by Hosokawa Micron). The measurement was carried out by holding the developer with an electromagnet and spraying nitrogen gas at an appropriate pressure to separate only the toner from the developer, which was then introduced into the measuring section of the measuring device. Analysis was carried out on 3,000 toner particles, and the standard deviation Q of the charge amount per particle size was N/Nσ (μC / g) was calculated.

[0090]

[0091] From the above results, it is clear that the ferrite particles obtained in Examples 1 to 9 have a high charge-imparting ability and a sharp charge distribution.

[0092] According to the present invention, it is possible to provide a carrier core material for an electrophotographic developer which has high charge-imparting ability and a sharp charge distribution, and therefore is less likely to cause poor image density or toner scattering, and which can provide good image quality even when used as a developer over a long period of time; a carrier for an electrophotographic developer obtained by coating the surface of the carrier core material for an electrophotographic developer with a resin; and ferrite particles which become an electrophotographic developer using the carrier for an electrophotographic developer.

[0093] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-052502) filed on March 29, 2023, the contents of which are incorporated herein by reference.

Claims

1. Ferrite particles that satisfy the following formula: 1.10≦Y / X, where X (atomic %) is the percentage of Sr or Ca on the surface of a particle having a particle diameter of 35 μm or less, and Y (atomic %) is the percentage of Sr or Ca on the surface of a particle having a particle diameter of 40 μm or more.

2. The ferrite particles according to claim 1, which satisfy the following formulae: 0.30≦X≦0.80, 0.36≦Y≦1.55, and 1.20≦Y / X≦2.

00.

3. The cumulative 50% particle diameter D50 in the particle size distribution based on volume is 30 μm or more and 50 μm or less, and the proportion P of particles with a particle diameter of 40 μm or more in the particle size distribution based on number +40 The ferrite particles according to claim 1 , wherein the content of the ferrite particles is 5% by number or more and 40% by number or less.

4. The ferrite particles according to claim 1, wherein the surface roughness Rz is 2.5 μm or more and 4.5 μm or less, and the standard deviation Rzσ of the surface roughness Rz is 0.2 μm or more and 1.0 μm or less.

5. The ferrite particles according to claim 1, containing 0.3% by weight or more and 1.2% by weight or less of Sr or Ca.

6. The ferrite particles according to claim 5, containing 15% by weight or more and 30% by weight or less of Mn and 45% by weight or more and 65% by weight or less of Fe.

7. Residual magnetization σr is 3.0 Am 2 The ferrite particles according to claim 1 , wherein the molecular weight is less than 1 / kg.

8. A carrier core material for electrophotographic developer, comprising the ferrite particles according to any one of claims 1 to 7.

9. A carrier for electrophotographic developer comprising the ferrite particles according to any one of claims 1 to 7 and a resin coating layer provided on the surface of the ferrite particles.

10. An electrophotographic developer comprising the carrier for electrophotographic developer according to claim 9 and a toner.

11. The electrophotographic developer according to claim 10, which is used as a replenishment developer.

Citation Information

Patent Citations

  • Carrier for electrophotography, developer, vessel, and image forming method

    JP2004198663A

  • System and method for rapidly building, managing, and sharing machine learning models

    JP2023052502A

  • Ferrite powder, carrier core for electro-photography developing agent, carrier for electro-photography developing agent, and electro-photography developing agent

    CN110928152A

  • Ferrite particle, and carrier for electrophotographic development and electrophotographic developer using the same

    JP2015151287A

  • Ferrite particle, and carrier for electrophotographic development and electrophotographic developer using the same