Silica-alumina and production method therefor
By supporting alumina on silica-alumina and optimizing key properties, the method effectively increases Brønsted acid content in silica alumina, addressing the challenge of controlling acid amounts in conventional methods and enhancing its catalytic performance.
Patent Information
- Application Number
- PCT/JP2024/013102
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for producing silica alumina struggle to control the amount of Brønsted acid effectively, particularly in achieving a large amount of Brønsted acid content in silica alumina, which is essential for catalytic applications.
A method involving the support of alumina on the surface of silica-alumina, optimizing the isoelectric point, specific surface area, pore volume, and acid ratios to achieve silica alumina with a high Brønsted acid content, specifically more than 10 μmol/g, and a controlled Lewis acid content, while maintaining a suitable alumina and silica composition.
The method successfully produces silica alumina with a high Brønsted acid content, enhancing its catalytic activity and versatility as a catalyst material for reactions like hydrocracking and catalytic cracking, with improved reactant diffusivity and reactivity.
Smart Images

Figure JP2024013102_03102024_PF_FP_ABST
Abstract
Description
Silica alumina and its manufacturing method
[0001] The present invention relates to silica-alumina and a method for producing the same.
[0002] Silica-alumina is a material that has long been used in the field of catalyst technology. It has distinctive solid acidity and a fine pore structure, and these properties have been utilized to serve as catalyst supports and active components.
[0003] It is known that the properties of silica-alumina vary depending on the preparation method, and methods for preparing silica-alumina are well known in the art, with representative methods including the neutralization reaction method and the pH swing method.
[0004] Examples of the neutralization reaction (coprecipitation method, cogelation method) method include preparation methods such as those described in Patent Documents 1 to 4 and 7, in which a solution of silica hydrogel and a metal salt is mixed to produce amorphous silica-alumina containing the metal salt uniformly inside.
[0005] Furthermore, the pH swing method (immersion method) includes preparation methods such as those described in Patent Documents 5 and 6, in which the pH of a reaction mixture is changed, thereby precipitating silica and alumina, thereby enabling the production of amorphous silica-alumina in a single vessel.
[0006] Japanese Patent Publication No. 27-3989 Japanese Patent Publication No. 31-1862 Japanese Patent Publication No. 30-5963 Japanese Patent Publication No. 32-413 Special Publication No. 2010-537808 Special Publication No. 2016-502971 Japanese Patent Publication No. 2021-151942
[0007] Edited by Takayasu Shirasaki and Naoyuki Todo, “Catalyst Preparation”, Kodansha, published November 10, 1971, p. 22C. A. Emeis, J. Catal. , 141, 347-354 (1993)
[0008] However, in the prior art, the preparation methods described in Patent Documents 1 to 7 have problems in terms of controlling the solid acidity. In particular, there has been a demand for a preparation method for obtaining silica-alumina with a high Bronsted acidity.
[0009] In view of the above circumstances, an object of the present invention is to provide silica-alumina having a high Bronsted acidity and a method for producing the silica-alumina.
[0010] Under such technical background, the inventors have conducted extensive research to solve the above-mentioned problems, and have found that silica-alumina having a high Bronsted acidity can be obtained by using a manufacturing method in which alumina is further supported on the surface of silica-alumina, and have thus developed the present invention.
[0011] The present invention, which has been developed to solve the above problems and achieve the above objects, is as follows. That is, the present invention first provides silica-alumina having a Bronsted acid amount of more than 10 μmol / g and an isoelectric point in the range of 4.5 to 7.0. The silica-alumina according to the present invention has the following characteristics: (a) a Lewis acid amount of 300 μmol / g or less, (b) a ratio of the Bronsted acid amount to the Lewis acid amount of more than 0.035, and (c) a Bronsted acid density of 0.025 μmol / m 2 (d) in the pore distribution measured by the nitrogen adsorption method, the total pore volume is in the range of 1.00 mL / g or more and 2.20 mL / g or less; (e) in the pore distribution, the ratio of the volume of pores having a diameter of 10 nm or more to the total pore volume is 60% or more; (f) the specific surface area is 250 m 2 / g or more, 600m 2 / g or less, (g) the silica content is SiO 2 A more preferable solution is that the content is in the range of 30% by mass or more and 70% by mass or less in terms of converted amount.
[0012] Secondly, the present invention proposes a method for producing silica-alumina, comprising: an alumina slurry preparation step of preparing an alumina slurry; a silica slurry preparation step of preparing a silica slurry; a silica-alumina slurry preparation step of mixing the alumina slurry and the silica slurry to prepare a silica-alumina slurry; and a reaction step of reacting the silica-alumina slurry with an aluminum compound.
[0013] 1 is a graph showing the IR spectrum of silica-alumina according to the present invention. 2 is a graph showing the relationship between the difference in isoelectric point and the Bronsted acid amount of silica-alumina according to the present invention. 3 is a graph showing the IR spectrum (3500 cm) of silica-alumina according to Example 1 and Comparative Example 6. -1 ~4000cm -1 ) is a graph showing the IR spectrum (3750 cm) of the silica-alumina of Example 1 and Comparative Example 6. -1 ~3800cm -1 ) is a graph showing
[0014] Preferred embodiments of the present invention will be described in detail below. [Definitions] In this embodiment, "silica" is a general term for silicon oxides, and silicon dioxide is considered to be included in silica. In this embodiment, "alumina" is a general term for aluminum oxides, and aluminum oxide and alumina hydrate are considered to be included in alumina. Furthermore, pseudoboehmite, which is a type of alumina hydrate, is also considered to be included in alumina. In this embodiment, "silica-alumina" is a general term for a mixture of silica and alumina, and crystalline aluminosilicates such as zeolites are not considered to be included in silica-alumina.
[0015] [Silica-alumina] The silica-alumina having a high Bronsted acid amount (hereinafter also referred to as "acid amount B") according to this embodiment will be described. Specifically, the silica-alumina has a Bronsted acid amount of more than 10 μmol / g and an isoelectric point in the range of 4.5 to 7.0 (hereinafter also referred to as "the present silica-alumina"). A detailed description will be given below.
[0016] The isoelectric point of the present silica-alumina is in the range of 4.5 to 7.0, since the present silica-alumina has alumina supported on its surface, it exhibits such an isoelectric point.
[0017] The silica content of the silica-alumina (SiO 2 The alumina content (Al converted) of the silica-alumina of the present invention is preferably in the range of 30 mass % or more and 70 mass % or less, and more preferably in the range of 35 mass % or more and 65 mass % or less. 2 O 3The Brønsted acid content (calculated as Brønsted acid content) is preferably in the range of 30% by mass or more and 70% by mass or less, and more preferably in the range of 35% by mass or more and 65% by mass or less. It is generally known that the acid content of silica-alumina increases most when the alumina content is about 20% by mass. In contrast, the Brønsted acid content of the present silica-alumina is high even when the alumina content is within the above-mentioned range.
[0018] The specific surface area (hereinafter also referred to as "SSA") of this silica-alumina measured by the BET method is 250 m 2 / g or more, 600m 2 The specific surface area is preferably in the range of 300 m / g or less. 2 / g or more, 550m 2 / g or less, and more preferably 350m 2 / g or more, 500m 2 / g or less. When the specific surface area of the present silica-alumina is in the above-mentioned range, the Bronsted acid density becomes high. A high Bronsted acid density is preferable because it increases the probability of contact with the reactants in the catalytic reaction.
[0019] The pore volume (hereinafter also referred to as "PV") of this silica-alumina measured by the BJH method is preferably in the range of 1.00 mL / g or more and 2.20 mL / g or less. The pore volume is more preferably in the range of 1.20 mL / g or more and 2.00 mL / g or less, and particularly preferably in the range of 1.40 mL / g or more and 1.80 mL / g or less. When pores are used as reaction fields in catalytic reactions, the catalytic activity tends to increase as the pore volume increases. Furthermore, this silica-alumina has a ratio of the volume of pores with pore diameters of 10 nm or more measured by the BJH method to the total pore volume (hereinafter referred to as "PV"). 10 " is also referred to as ". ) is preferably 60% by volume or more, more preferably 65% by volume or more. Within this range, the diffusibility of reactants in catalytic reactions is improved, and their reactivity is likely to increase. In the present invention, the total volume of pores having a pore diameter in the range of 2.4 nm or more and 192.4 nm or less is defined as the pore volume of the present silica-alumina, and the proportion of the volume of pores having a pore diameter of 10 nm or more and 192.4 nm or less in this pore volume is defined as P 10It was calculated as:
[0020] The Bronsted acid amount of the present silica-alumina is more than 10 μmol / g, and preferably 15 μmol / g or more. The upper limit of the Bronsted acid amount is not particularly limited, but may be 100 μmol / g or less, 75 μmol / g or less, or 50 μmol / g or less. Silica-alumina with a high Bronsted acid amount is suitable as a catalyst material used in reactions using Bronsted acids.
[0021] The Lewis acid amount (hereinafter also referred to as "L acid amount") of the present silica-alumina is preferably 300 μmol / g or less, more preferably 280 μmol / g or less. The lower limit of the Lewis acid amount is not particularly limited, but may be 1 μmol / g or more, or may be 10 μmol / g or more. In catalytic reactions using Brønsted acids, Lewis acids may promote side reactions. Therefore, silica-alumina with a low Lewis acid amount is suitable as a catalyst material used in reactions using Brønsted acids. Furthermore, the molar ratio of Brønsted acid to Lewis acid (hereinafter also referred to as "B / L") is preferably greater than 0.035, preferably 0.040 or more, and particularly preferably 0.050 or more. The upper limit of this molar ratio is not particularly limited, but may be 10 or less, 1 or less, or 0.5 or less.
[0022] The Bronsted acid density (hereinafter also referred to as "B acid density") of this silica-alumina is 0.025 μmol / m 2 It is preferable that the concentration is 0.030 μmol / m or more. 2 The upper limit of the Bronsted acid density is not particularly limited, but is preferably 1.000 μmol / m 2 or less, and may be 0.500 μmol / m 2 It may be 0.100 μmol / m or less, 2 Silica-alumina having a high Bronsted acid density is suitable as a catalyst material for reactions utilizing Bronsted acids.
[0023] The alumina contained in the present silica-alumina is preferably pseudo-boehmite. Silica-alumina containing pseudo-boehmite tends to have a large pore volume and specific surface area. Whether the silica-alumina of the present invention contains pseudo-boehmite can be determined from its X-ray diffraction pattern. Specifically, in an X-ray diffraction pattern obtained by X-ray diffraction measurement of the silica-alumina of the present invention, if diffraction peaks are present near 2θ = 15°, 28°, 38°, and 49°, corresponding to the Miller indices (020), (021), (130), and (150) of the boehmite structure, and the half-widths of the Miller indices (130) and (150) are 1.0° or greater, it can be determined that pseudo-boehmite is contained. Furthermore, if the half-width is less than 1.0, it can be determined that crystalline boehmite is contained. Furthermore, if the X-ray diffraction pattern does not show any other diffraction peaks with half-widths less than 1.0° in the range of 5°≦2θ≦50°, it can be determined that zeolite is not contained.
[0024] Since the present silica-alumina has a high Bronsted acidity, when it is used as a catalyst material for hydrocracking or catalytic cracking, the decomposition of the raw material is facilitated. The present silica-alumina acts as a catalyst by itself, but it is preferable to use it as a material constituting a catalyst such as a carrier or co-catalyst.
[0025] [Method for Producing Silica Lumina] Generally, silica is known to contain Bronsted acids derived from silanols on the surface (for example, Non-Patent Document 1). Also, alumina contains coordinatively unsaturated Al groups present on the surface of dehydrated alumina. 3+ It is known that silica-alumina contains Lewis acids derived from the above. Therefore, by increasing the content of silica contained in silica-alumina, it is possible to increase the Bronsted acid amount to some extent. In contrast, by using the production method of this embodiment, silica-alumina with a high Bronsted acid amount can be obtained without increasing the silica content. Hereinafter, the production method of silica-alumina according to this embodiment will be described in detail.
[0026] [Alumina Slurry Preparation Step] The production method according to this embodiment includes an alumina slurry preparation step. In this step, a conventionally known alumina, such as hydrated alumina such as pseudoboehmite, boehmite, gibbsite, or bayerite, or aluminum oxide such as γ-alumina, χ-alumina, θ-alumina, or η-alumina, is dispersed in a solvent to prepare an alumina slurry. An alumina sol can also be used as the alumina slurry. The alumina used in this step is preferably hydrated alumina, and more preferably pseudoboehmite. These aluminas prepared using conventionally known preparation methods may be used. Alternatively, commercially available alumina may be purchased and dispersed in a solvent.
[0027] In the production method according to this embodiment, by using pseudo-boehmite alumina with a large pore volume in the alumina slurry preparation step, silica-alumina with a large pore volume and a large Bronsted acid content can be obtained. Pseudo-boehmite with a large pore volume can be obtained by using a production method including a preparation step of neutralizing an aluminum aqueous solution in which at least one of an aluminum salt and an aluminate is dissolved with a neutralizing agent to obtain a pseudo-boehmite precursor slurry, and an aging step of aging the pseudo-boehmite precursor slurry to obtain a pseudo-boehmite slurry.
[0028] The aluminum salt used in this preparation step may be any compound such as aluminum sulfate, aluminum chloride, aluminum nitrate, etc. The aluminate may be any compound such as sodium aluminate, potassium aluminate, etc.
[0029] In this blending step, if the aluminum aqueous solution is acidic, a basic aqueous solution such as sodium hydroxide, potassium hydroxide, or aqueous ammonia can be used as the neutralizing agent. Furthermore, if the aluminum aqueous solution is basic, an acidic aqueous solution such as sulfuric acid, hydrochloric acid, or nitric acid can be used as the neutralizing agent. In this case, a basic aqueous solution containing an aluminate dissolved therein may be used as the basic aqueous solution, or an acidic aqueous solution containing an aluminum salt dissolved therein may be used as the acidic aqueous solution. From the viewpoint of production cost, a method of preparing a pseudo-boehmite precursor slurry by mixing an acidic aqueous solution containing an aluminum salt dissolved therein with a basic aqueous solution containing an aluminate dissolved therein is preferred.
[0030] In this blending step, the pH of the neutralized slurry obtained by mixing the aqueous solution and the neutralizing agent is adjusted to a range of 5.0 or more and 8.0 or less, thereby obtaining a pseudo-boehmite precursor slurry. At this time, the temperature of the neutralized slurry is preferably adjusted to a range of 30°C or more and 70°C or less, and more preferably adjusted to a range of 35°C or more and 65°C or less. Adjusting the temperature of the neutralized slurry within the above range increases the pore volume of the pseudo-boehmite obtained as a final product, and also increases the purity of the pseudo-boehmite. Furthermore, after adjusting the temperature and pH of the neutralized slurry to the above ranges, this state is preferably maintained for a range of 5 minutes or more and less than 60 minutes, and more preferably for a range of 5 minutes or more and 30 minutes or less. By shortening the maintenance time, the pore volume of the pseudo-boehmite obtained as a final product increases.
[0031] In this compounding step, the aqueous solution containing the aluminum salt or the aluminum ion is further added to the pseudo-boehmite precursor slurry, and the mixture is aged to obtain pseudo-boehmite alumina having a large specific surface area and a large pore volume with a pore diameter of 10 nm or more. 2 O 3The content of the cellulose acetate solution is preferably in the range of 10% by mass or more and 25% by mass or less in terms of the total mass of the cellulose acetate solution. The aging is preferably carried out at a temperature range of 40° C. or more and 95° C. or less, and more preferably at a temperature range of 50° C. or more and 80° C. or less. There are no particular restrictions on the aging time, but from the viewpoint of production efficiency, it is preferably 4 hours or less.
[0032] In this alumina slurry preparation step, the alumina concentration of the alumina slurry is adjusted to Al 2 O 3 The alumina concentration is preferably adjusted to a range of 1 mass % or more and 20 mass % or less, more preferably 1 mass % or more and 10 mass % or less, calculated as a converted value. By adjusting the alumina concentration to such a range, the handleability of the alumina slurry is improved, and the production efficiency of silica-alumina is also increased.
[0033] [Silica Slurry Preparation Step] The production method according to this embodiment includes a silica slurry preparation step. In this step, silica is dispersed in a solvent to prepare a silica slurry. For example, the silica slurry may be prepared by preparing a silica hydrogel using a conventionally known method and dispersing it in a solvent, or by dispersing commercially available silica powder in a solvent. At this time, the specific surface area of the silica contained in the silica slurry is 200 m 2 / g or more, 700m 2 / g or less, and 2 / g or more, 600m 2 / g or less is more preferable. When silica having a specific surface area in the above range is used, the specific surface area of the finally obtained silica-alumina will be in an appropriate range. Silica sol can also be used as the silica slurry.
[0034] In this step, the silica concentration of the silica slurry is adjusted to SiO 2 The silica concentration is preferably adjusted to a range of 10% by mass or more and 40% by mass or less, more preferably 15% by mass or more and 35% by mass or less, in terms of silica-alumina conversion. By adjusting the silica concentration to such a range, the handleability of the silica slurry is improved, and the production efficiency of silica-alumina is also increased.
[0035] [Silica-Alumina Slurry Preparation Step] The manufacturing method according to this embodiment includes a silica-alumina slurry preparation step. In this step, the alumina slurry obtained in the previous step is mixed with a silica slurry to prepare a silica-alumina slurry. At this time, the silica slurry may be added to the alumina slurry, the alumina slurry may be added to the silica slurry, or both may be added and mixed simultaneously.
[0036] In this step, it is preferable to age the silica-alumina slurry. By ageing the silica-alumina slurry, Bronsted acid is more likely to be expressed in the reaction step described below, and the Bronsted acid amount of the finally obtained silica-alumina is also likely to increase. The temperature of the silica-alumina slurry during aging is preferably in the range of 30°C or higher and 95°C or lower, more preferably in the range of 35°C or higher and 80°C or lower. Furthermore, the retention time during aging is preferably in the range of 0.1 hours or higher and 6 hours or lower, more preferably in the range of 0.5 hours or higher and 4 hours or lower.
[0037] [Reaction Step] The production method according to this embodiment includes a reaction step. In this step, the silica-alumina slurry obtained in the previous step is reacted with an aluminum compound. In this step, alumina is further supported on the surface of the silica-alumina, and this supported alumina reacts with the silica-alumina to generate a Brønsted acid, thereby obtaining silica-alumina with a high Brønsted acid content. In particular, the production method according to this embodiment can obtain silica-alumina with a high Brønsted acid content even if the amount of alumina supported in this step is small.
[0038] In this step, it is preferable to support alumina on silica-alumina so that the pH value is +0.3 or higher relative to the isoelectric point of the silica-alumina contained in the silica-alumina slurry obtained in the previous step. It is more preferable to support alumina so that the pH value is +0.5 or higher relative to the isoelectric point. Inorganic oxide particles have an isoelectric point at which the zeta potential changes significantly with changes in the pH value of the solution, and at a certain pH value, the surface potential becomes zero and no interfacial electrokinetic phenomena such as electrophoresis are exhibited. For example, it is known that the isoelectric point of silica is approximately pH 2.5, and the isoelectric point of alumina is approximately pH 9.5. Therefore, the isoelectric point of silica-alumina is in the pH range of 2.5 or higher and 9.5 or lower, and by supporting alumina on the surface of silica-alumina, the isoelectric point approaches pH 9.5. In this way, by supporting alumina on the surface of silica-alumina using the isoelectric point as an indicator, the Bronsted acidity can be efficiently increased.
[0039] In this step, any aluminum compound such as aluminum sulfate, aluminum chloride, or aluminum nitrate can be used. Furthermore, sodium aluminate, potassium aluminate, or the like can also be used as an aluminate. These compounds may be added directly to the silica-alumina slurry or may be added as an aqueous solution containing aluminum ions.
[0040] In this step, the silica-alumina slurry is preferably reacted with the aluminum compound after adjusting the temperature to a range of 30° C. or higher and 70° C. or lower, and more preferably reacted after adjusting to a range of 35° C. or higher and 65° C. or lower. By reacting the silica-alumina slurry with the aluminum compound under such conditions, silica-alumina having a large Bronsted acid amount is more likely to be obtained.
[0041] Silica alumina is obtained by removing the solvent from the silica alumina slurry obtained in this step. For example, silica alumina can be obtained by removing the solvent using a conventionally known method such as filtration or drying. In the case of filtration, silica alumina can be obtained by drying the silica alumina cake obtained by separating the solvent using a method such as vacuum filtration or filter press. Silica alumina can also be obtained by methods such as evaporation to dryness and spray drying. In the production method according to this embodiment, spray drying is preferably used. By using spray drying, powdered silica alumina with good flowability can be obtained. When spray drying is used, the inlet temperature of the spray dryer is preferably in the range of 150°C or higher and 350°C or lower. Furthermore, the outlet temperature of the spray dryer is preferably in the range of 80°C or higher and 150°C or lower.
[0042] The silica alumina obtained in this step may be washed as needed. For example, a method of suspending the silica alumina in a solvent, washing, and filtering may be repeated. Here, the efficiency of washing can be improved by adjusting the temperature of the solvent to a range of 40°C or higher and 70°C or lower. Furthermore, the efficiency of washing can be further improved by dissolving ammonium sulfate, ammonium nitrate, ammonium chloride, or the like in the solvent. Moreover, this washing may be performed after removing the solvent, or may be performed on the silica alumina slurry before removing the solvent.
[0043] The manufacturing method according to the present embodiment allows for fine adjustment of the Bronsted acidity, and therefore can provide silica-alumina having an optimum Bronsted acidity for various catalytic reactions. Therefore, the method is highly versatile as a method for manufacturing silica-alumina used as a catalyst material such as a carrier or a co-catalyst in catalytic reactions.
[0044] [Measurement and Evaluation Methods] Various measurements and evaluations were carried out as follows.
[0045] [1] Method for measuring composition 3 g of a measurement sample was placed in a 30 mL zirconia bowl with a lid, heated (200°C, 20 minutes), and baked (700°C, 5 minutes). 2 O 22 g of HCl and 1 g of NaOH were added and melted for 15 minutes. 2 SO 4 25 mL of HCl was added to 200 mL of water to dissolve the solution, and then diluted to 500 mL with pure water to prepare a sample. The obtained sample was measured for the content of each component on an oxide-equivalent mass basis using an inductively coupled plasma (ICP) optical emission spectrometer (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000). The silica content was determined by adding SiO 2 The alumina content is calculated by converting it into Al 2 O 3 was calculated by converting it into
[0046] [2] Isoelectric point measurement method: The isoelectric point was measured by pH titration using a Zetasizer Pro manufactured by Malvern Panalytical Co., Ltd. The measurement conditions were as follows: the solids concentration of the measurement sample was 0.1% by mass, the pH was adjusted using 0.1 mol / L HCl, 0.01 mol / L HCl, or 0.1 mol / L NaOH, and the measurement interval was set to pH value in 0.5 increments.
[0047] [3] Measurement method of specific surface area To measure the specific surface area, approximately 30 mL of the measurement sample was placed in a porcelain crucible (B-2 type), heated at 600°C for 2 hours, and then cooled to room temperature in a desiccator to obtain a measurement sample. Next, 1 g of this sample was taken and the specific surface area of the sample was measured by the BET single-point method using a fully automatic surface area measuring device (Multisorb 12 type, manufactured by Yuasa Ionics Co., Ltd.).
[0048] [4] Method for measuring pore volume and proportion of pores of 10 nm or more The pore distribution of the measurement sample was measured using BELSORP-mini Ver. 2.5.6 manufactured by Microtrac-Bell Corporation. Specifically, the measurement sample was heat-treated at 500°C for 2 hours while being evacuated to a vacuum, and nitrogen gas was adsorbed onto the measurement sample. 0 The pore size distribution was determined from the desorption isotherm (=0.99). From this pore size distribution, the total volume of pores having a pore size in the range of 2.4 nm or more and 192.4 nm or less was taken as the pore size of the measurement sample, and the ratio of the volume of pores having a pore size in the range of 10 nm or more and 192.4 nm or less to this pore size was calculated.
[0049] [5] Measurement of Solid Acidity Properties 50 mg of sample powder was molded into a 20 mm diameter disk, placed in an IR cell connected to a vacuum line, and evacuated at 500°C for one hour. After evacuating, the temperature was lowered to 150°C, and the IR (infrared absorption) spectrum of the sample disk was measured using a JASCO FT / IR-4600. Next, pyridine was introduced, and the sample was evacuated at 150°C for 10 minutes. The IR spectrum of the sample disk with pyridine adsorbed at 150°C was measured in the same manner as described above. The IR spectrum of the sample disk was then subtracted from the IR spectrum of the sample disk with pyridine adsorbed, yielding the graph shown in Figure 1. As shown in Figure 1, the areas of the absorption peaks assigned to the Brønsted acid site (B) and Lewis acid site (L) were calculated. Based on the calculated absorption peak areas, the Brønsted acid amount and Lewis acid amount were calculated using the method described in Non-Patent Document 2. The Brønsted acid density was calculated using the obtained Brønsted acid amount and specific surface area.
[0050] [6] X-ray diffraction measurement X-ray diffraction of silica alumina was measured using a MiniFlex manufactured by Rigaku Corporation. The measurement conditions were as follows: the operating axis was 2θ / θ, a CuKα source was used, and the measurement was performed continuously at a voltage of 40 kV and a current of 15 mA, from a start angle of 2θ = 5° to an end angle of 2θ = 50°, with a sampling width of 0.020° and a scan rate of 10,000° / min.
[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0052] [Example 1] <Alumina Slurry Preparation Step> A 200 L steam-jacketed stainless steel tank was charged with 120 kg of hot water at 60°C, and 48 g of a 25% by mass aqueous solution of sodium gluconate was added with stirring. 2 O 3 1.77 kg of a 22% by mass aqueous solution of sodium aluminate (manufactured by JGC Catalysts and Chemicals Co., Ltd.) was added and mixed for 5 minutes. 2 O 32.95 kg of an aluminum sulfate aqueous solution (manufactured by JGC Catalysts and Chemicals Co., Ltd.) with a converted concentration of 7% by mass was added and stirred at 60°C for 5 minutes to prepare an alumina slurry precursor. 16.10 kg of the sodium aluminate aqueous solution and 29.80 kg of the aluminum sulfate aqueous solution were simultaneously added to the alumina slurry precursor over 40 minutes and stirred for 5 minutes. Next, 3.85 kg of the sodium aluminate aqueous solution was added, and the mixture was aged at 60°C for 2 hours with stirring. 0.53 kg of 15% aqueous ammonia was added and stirred for 5 minutes. The mixture was then dehydrated using a flat filter, and the filtration residue was washed with warm water at 60°C to obtain a washed cake. The washed cake was slurried to an alumina concentration of 7.2% by mass to obtain an alumina slurry.
[0053] <Silica Slurry Preparation Step> Silica (average particle size = 12 μm, BET specific surface area = 480 m) was added to give a silica slurry concentration of 33 mass %. 2 / g) was suspended in water to obtain a silica slurry.
[0054] <Silica-alumina slurry preparation step> 0.16 kg of 15% ammonia water was added to 22.44 kg of the alumina slurry obtained in the previous step, and after stirring for 5 minutes, 3.27 kg of the silica slurry obtained in the previous step was added, and the mixture was aged at 40°C for 2 hours while stirring to obtain a silica-alumina slurry with a solid content of 10.4 mass%. At this time, the isoelectric point of the silica-alumina contained in the silica-alumina slurry was 5.3.
[0055] <Reaction Step> 10 kg of pure water was added to 10 kg of silica alumina slurry and heated to 40° C. Then, 0.29 kg of 25% by mass sulfuric acid was added to adjust the pH to 3, and the mixture was stirred for 5 minutes. 2 O 31.24 kg of an aqueous aluminum sulfate solution with a 7% by mass equivalent concentration was added. Then, 0.77 kg of 15% aqueous ammonia was added and stirred for 10 minutes. The solids obtained after dehydration using a flat filter were washed with warm water at 60°C to obtain a washed cake. This washed cake was reslurried to a solids concentration of 10.5% by mass, dispersed using a homogenizer, and dried in a spray dryer at an inlet temperature of 270°C and an outlet temperature of 130°C to obtain silica alumina 1. The production conditions are shown in Table 1 as Treatment No. 1. The obtained silica alumina 1 was subjected to the above-described measurements and analyses. The results are shown in Table 2 as Silica Alumina No. 1. Furthermore, in the evaluation described above in [5], the IR spectrum of the sample disk was subtracted from the IR spectrum of the sample disk with pyridine adsorbed thereon, and the areas of the absorption peaks assigned to the Bronsted acid sites and Lewis acid sites were calculated, as shown in Figure 1.
[0056] [Example 2] Silica alumina 2 was obtained in the same manner as in Example 1, except that in the silica alumina slurry preparation step, the amount of 15% aqueous ammonia added was changed from 0.16 kg to 0.27 kg, the aging temperature was changed from 40°C to 60°C, and in the reaction step, the amount of sulfuric acid added was changed from 0.29 kg to 0.24 kg, the amount of aluminum sulfate aqueous solution added was changed from 1.24 kg to 0.6 kg, and the amount of aqueous ammonia added was changed from 0.77 kg to 0.42 kg. The production conditions are shown in Table 1 as Treatment No. 2. The obtained silica alumina 2 was subjected to the above-mentioned measurements and analyses. The results are shown in Table 2 as Silica alumina No. 2.
[0057] [Example 3] Silica-alumina 3 was obtained in the same manner as in Example 2, except that in the reaction step, the amount of aluminum sulfate aqueous solution added was changed from 0.6 kg to 1.24 kg, and the amount of ammonia water added was changed from 0.42 kg to 0.73 kg. The production conditions are shown in Table 1 as Treatment No. 3. The obtained silica-alumina 3 was subjected to the above-mentioned measurements and analyses. The results are shown in Table 2 as Silica-alumina No. 3.
[0058] [Example 4] Silica-alumina 4 was obtained in the same manner as in Example 1, except that in the reaction step, the amount of aluminum sulfate aqueous solution added was changed from 1.24 kg to 0.6 kg, and the amount of ammonia water added was changed from 0.77 kg to 0.73 kg. The production conditions are shown in Table 1 as Treatment No. 4. The obtained silica-alumina 4 was subjected to the above-mentioned measurements and analyses. The results are shown in Table 2 as Silica-alumina No. 4.
[0059] Comparative Example 1: No reaction step of Example 2 The silica-alumina slurry of Example 2 was dispersed using a homogenizer and dried using a spray dryer at an inlet temperature of 270°C and an outlet temperature of 130°C to obtain silica-alumina 5. The production conditions are shown in Table 1 as Process No. 5. The obtained silica-alumina 5 was subjected to the above-mentioned measurements and analyses. The results are shown in Table 2 as Silica-alumina No. 5.
[0060] [Comparative Example 2: No reaction step of Example 1] The silica-alumina slurry of Example 1 was dispersed using a homogenizer and dried using a spray dryer at an inlet temperature of 270°C and an outlet temperature of 130°C to obtain silica-alumina 6. The production conditions are shown in Table 1 as Process No. 6. The obtained silica-alumina 6 was subjected to the above-mentioned measurements and analyses. The results are shown in Table 2 as Silica-alumina No. 6.
[0061]
[0062]
[0063] Silica-alumina 1 and 4 of Process Nos. 1 and 4, in which alumina was supported on silica-alumina 6 of Process No. 6, had a higher isoelectric point than silica-alumina 6, resulting in an increased Bronsted acid content (● in Figure 2). Furthermore, silica-alumina 2 and 3 of Process Nos. 2 and 3, in which alumina was supported on silica-alumina 5 of Process No. 5, also had a higher isoelectric point than silica-alumina 5, resulting in an increased Bronsted acid content (▲ in Figure 2). These results demonstrate the effectiveness of the manufacturing method of supporting alumina on silica-alumina. Furthermore, it was discovered that by controlling the isoelectric point of silica-alumina within a specific range, the Bronsted acid content can be increased without significantly changing the composition.
[0064] FT-IR (Fourier transform infrared absorption) measurements were carried out under the following conditions for silica-alumina 1 carrying alumina and silica-alumina 6 not carrying alumina. The results are shown in Figures 3 and 4.
[0065] <Conditions> 25 mg of sample powder was molded into a 20 mm diameter disk, then placed in an IR cell connected to a vacuum line and subjected to evacuation at 500°C for one hour. After evacuation, the disk was allowed to cool to room temperature, and the IR (infrared absorption) spectrum of the sample disk was measured using a JASCO FT / IR-6100. To remove water vapor and carbon dioxide from the measurement optical path and perform highly accurate measurements, high-purity nitrogen gas was supplied to the interference chamber, sample chamber, and detector chamber of the FT-IR. The obtained spectrum was subjected to baseline correction and weight correction based on 20 mg, and the spectra shown in Figures 3 and 4 were obtained.
[0066] The absorption band (3740 cm-1) derived from Si-OH is smaller in silica-alumina 1, which supports alumina, compared to silica-alumina 6, which does not support alumina. Furthermore, the absorption band (3780 cm-1) derived from Al-OH is larger in silica-alumina 1. This proves that alumina is supported on the surface of the silica-alumina. Furthermore, this alumina supported on the surface produces a Bronsted acid, which is not present in conventional silica-alumina.
[0067] In this specification, the unit of volume "L" is 10 -3m 3 Represents.
Claims
1. Silica alumina having a Bronsted acidity of more than 10 μmol / g and an isoelectric point in the range of 4.5 to 7.
0.
2. The silica-alumina according to claim 1, having a Lewis acid amount of 300 μmol / g or less.
3. The silica-alumina according to claim 2, wherein the ratio of Bronsted acidity to Lewis acidity is greater than 0.
035.
4. Bronsted acid density is 0.025 μmol / m 2 The silica-alumina according to claim 3, wherein 5. The silica-alumina according to claim 4, wherein the total pore volume is in the range of 1.00 mL / g or more and 2.20 mL / g or less in the pore distribution measured by a nitrogen adsorption method.
6. The silica-alumina according to claim 5, wherein in the pore distribution, the ratio of pore volume of pores having a diameter of 10 nm or more to the total pore volume is 60% or more.
7. Specific surface area is 250 m 2 / g or more, 600m 2 The silica-alumina according to claim 6, wherein the silica-alumina has a molecular weight of 1000 or less.
8. The silica content is SiO 2 The silica-alumina according to any one of claims 1 to 7, wherein the silica-alumina content is in the range of 30 mass% or more and 70 mass% or less in terms of the total mass.
9. A method for producing silica-alumina, comprising: an alumina slurry preparation step of preparing an alumina slurry; a silica slurry preparation step of preparing a silica slurry; a silica-alumina slurry preparation step of mixing the alumina slurry and the silica slurry to prepare a silica-alumina slurry; and a reaction step of reacting the silica-alumina slurry with an aluminum compound.
Citation Information
Patent Citations
Production of lubricating oil by mixed catalyst system
JP2002503756A
Catalyst composition comprising small sized molecular sieve crystals deposited on porous material
JP2016527076A
Silica alumina and manufacturing method therefor
JP2018083723A
Silica-alumina compositions having improved stability and methods for making same
JP2022510847A
Silica-alumina powder, method for producing silica-alumina powder, fluid catalytic cracking catalyst and method for producing same
WO2022196025A1
Cited By
Inorganic compounds and methods for producing the same
JP7945609B2
Inorganic compound and method for producing same
JPWO2026088649A1
Inorganic compound and method for producing same
WO2026088649A1