A method for conversion of recycled concrete into reactive supplementary cementitious material
The method of crushing, screening, and mechanochemical processing of recycled concrete fines and minerals transforms them into reactive SCMs, addressing the underutilization of FRCA by enhancing their reactivity and environmental sustainability.
Patent Information
- Application Number
- PCT/CA2024/050471
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
Recycled concrete fines (FRCA) from Construction and Demolition Waste (CDW) are underutilized due to their low mechanical strength, high water absorption, and presence of impurities, limiting their application in concrete production, and existing methods to convert them into reactive Supplementary Cementitious Materials (SCMs) are not industry-accepted.
A method involving crushing, screening, mechanochemical activation, and mechanochemical synthesis using energy-intensive grinding mills to convert FRCA, RCA, and inert minerals into reactive pozzolanic or hydraulic SCMs, enhancing their chemical reactivity and usability.
The method effectively converts inert FRCA and minerals into reactive SCMs, improving their reactivity and enabling their use in concrete production, while being environmentally friendly and optimizing energy input.
Smart Images

Figure CA2024050471_17102024_PF_FP_ABST
Abstract
Description
A METHOD FOR CONVERSION OF RECYCLED CONCRETE INTO REACTIVE SUPPLEMENTARY CEMENTITIOUS MATERIALTECHNICAL FIELD
[0001] The following generally relates to concrete recycling, and more particularly, to a method for conversion of recycled concrete aggregates (RCA) obtained from Construction and Demolition Waste (CDW) and / or returned concrete (RC) from ready mix concrete trucks and / or other inert minerals into reactive Supplementary Cementitious Materials (SCMs).BACKGROUND
[0002] Concrete recycling is the use of rubble from demolished concrete structures, and the recycling of concrete aggregates produced from crushed Construction and Demolition Waste (CDW), primarily consisting of concrete.
[0003] Generally, strength parameters from recycled-concrete aggregates are consistently somewhat lower than natural aggregates, recycled concrete aggregates (RCA) have played an important role in replacing natural aggregates in concrete production; thereby contributing to a reduction in the extraction of natural resources and the promotion of a circular economy.
[0004] One of the massive by-products of concrete recycling is the crushed concrete fines (0 mm to ~4 - 5 mm) reaching the amount of 30 to 50% of the whole mass of crushed concrete. While RCA (> ~4 - 5 mm) is a practical reality in concrete production, there is generally no high- quality application for fines, or fine recycled concrete aggregates (FRCA), due to their low density and mechanical strength, high water absorption, and the presence of impurities such as cement paste.
[0005] FRCA is typically considered as a two-phase material including aggregates, such as old sand, and binder, such as old mortar glued together. In particular, FRCA from conventional concrete consisting of coarse (gravel, crushed stone, etc.) and fine (sand) aggregates and cement are considered as two-phase materials. The old mortar attached to the fine particles builds a weak porous layer on their surface and subsequently creates a fragile interface transition zone preventing bonding between the cementitious concrete matrix and the fines, and overall reduces the strength of concrete. Also, it has been observed that RCA and FRCA made from high performance and various types of special concretes also includes glued together aggregates comprising silica fume, fly ash and other materials used in production of said special concretes.It has been further observed that upgradation or enrichment of FRCA for their use in concrete production requires the separation of the agglomerated (glued together) components included in the composition of the FRCA particles.
[0006] Taking into consideration the significant importance of preserving natural resources, reduction of CO2 emissions and considering FRCA as a valuable resource and not as a waste, some attempts have been made to recycle FRCA into valuable products like hardened cement and clean sand. However, none of said attempts have been deemed generally accepted by industry for generating clean FRCA to further produce products. Accordingly, there is a need for an approach for converting inert FRCA into reactive SCMs.SUMMARY OF THE INVENTION
[0007] In an aspect, a method of converting recycled concrete obtained from Construction and Demolition Waste (CDW) to Supplementary Cementitious Materials (SCMs), and more particularly to a process of converting fine recycled concrete aggregates (hereinafter referred to as FRCA) obtained in the process of preparing recycled concrete aggregates from CDW into reactive SCMs is disclosed.
[0008] In some examples, the method of converting CDW in the form of RCA to a reactive, in particular pozzolanic or hydraulic SCM comprises obtaining crushed CDW in the form of RCA by subjecting the CDW to a crushing treatment. The method further comprises screening FRCA from the obtained RCA, where the particle size of less than approximately 4 mm is screened as FRCA. Further, the method comprises subjecting the screened FRCA to a mechanochemical activation and then, in some cases, a mechanochemical synthesis to obtain reactive (pozzolanic or hydraulic) SCM.
[0009] In some examples, the screening is carried out with vibratory screens, the vibratory screens separate the finer grains FRCA from the larger, gravel-like RCA. For example, the particular sieve size can be selected to be anywhere between 3 millimeters and 7 millimeters. In a particular case, the particular sieve size can be selected to be between 4 millimeters and 5 millimeters. In this way, the screening can use industry standard sieve sizes of, for example, 3.36 mm, 4 mm, 4.76 mm, and 6.73 mm.
[0010] In some examples, the remaining larger RCA particles are either re-processed and crushed down, or used as it is for mechanochemical activation and then, in some cases, for a mechanochemical synthesis.
[0011] In another example, the method of converting CDW to a reactive, in particular pozzolanic or hydraulic SCM comprises obtaining crushed CDW in the form of RCA by subjecting the CDW to a crushing treatment, and subjecting the crushed CDW in the form of RCA to mechanochemical activation and then, in some cases, to a mechanochemical synthesis to obtain reactive (pozzolanic or hydraulic) SCM.
[0012] In another aspect, a method of converting returned concrete (RC) from ready mix concrete trucks to a reactive, in particular pozzolanic or hydraulic SCM, is disclosed. The composition of such RC, though it may vary in a certain range, can be practically almost identical to the composition of RCA, which may vary also in a certain range. The method can include subjecting RC to mechanochemical activation and then mechanochemical synthesis to obtain reactive SCM.
[0013] In another aspect, a method of converting inert minerals other than RCA / FRCA to a reactive, in particular pozzolanic or hydraulic SCM is disclosed. The method comprises subjecting inert minerals to a crushing treatment, and subjecting the crushed inert minerals to mechanochemical activation and then mechanochemical synthesis to obtain reactive SCM.
[0014] In various examples, the crushing treatment may be carried out, for example, via jaw crushers, impact crushers, twin-shaft crushers or any other type of crushers used in concrete recycling plants.
[0015] In a specific example, the inert mineral is Georgian Bay shale which is a multi-phase material containing siltstone / sandstone and limestone.
[0016] In some examples, the inert minerals are selected from clay minerals and shale comprising quartz, calcite, kaolinite, montmorillonite, chert, dolomite, ankerite, muscovite, illite, bentonite, pyrophyllite, chlorite, zeolite, feldspar, and other commonly available natural mineral materials.
[0017] In some examples, the mechanochemical activation and then, in some cases, a mechanochemical synthesis of FRCA, RCA, RC or the inert minerals other than RCA, FRCA, and RC is carried out using energy-intensive grinding mills.
[0018] In some examples, the energy-intensive grinding mills are selected from mills with loose grinding media, such as vibratory ball / rod mills, planetary ball mills and stirred media mills as well as high-peripheral-speed mill (high speed disintegrator).
[0019] In a specific example, the stirred media mills are used for mechanochemical activationand then, in some cases, mechanochemical synthesis of FRCA / RCA / RC and other inert minerals. Examples of stirred media mills may include, but are not limited to vertical mills, such as Attritor mills, Stirred Media Detritor, Tower mill, VertiMill, MaxxMill, and horizontal mills, such as IssaMill and other similar mills.
[0020] Examples of high-peripheral-speed mills (high speed disintegrators, high speed rotor mills) include pin mills with special wear resistant grinding tools and, preferably, turbo mills.
[0021] In some example experiments, the mills with loose grinding media for converting FRCA / RCA / RC or inert minerals other than RCA, FRCA and RC into reactive SCM have a power density ranging from 40 to 250 kW / m3. In some examples, the mills with loose grinding media have a power density ranging from 40 to 450 kW / m3. In some examples, the high-peripheral- speed mills for converting FRCA / RCA / RC or inert minerals other than FRCA / RCA / RC into reactive SCM have rotor speed ranging from 1,800 rpm up to 26,000 rpm. In various examples, a predetermined specific grinding energy required to be generated in the energy-intensive grinding mills for mechanochemical activation and then, in some cases, for a mechanochemical synthesis of FRCA / RCA / RC or inert minerals other than RCA, FRCA and RC for conversion into reactive (pozzolanic or hydraulic) SCM is above 10 kJ / kg, and preferably in the range from 100 to 40,000 kJ / kg for providing definitely high SCM reactivity.
[0022] Other aspects and features of the present application will become apparent to those ordinarily skilled in the art upon review of the following description of embodiments of the invention in conjunction with the accompanying figures.DESCRIPTION OF THE DRAWINGS
[0023] Reference will now be made to the accompanying drawings which show, by way of example only, embodiments of the invention, and how they may be carried into effect, and in which:
[0024] FIG. 1 is a flowchart illustrating a method of converting screened FRCA from crushed recycled concrete obtained from CDW into reactive SCM, in accordance with an embodiment of the present invention;
[0025] FIG. 2 is a flowchart illustrating a method of converting recycled concrete obtained from CDW into reactive SCMs, in accordance with another embodiment of the present invention;
[0026] FIG. 3 is a flowchart illustrating a method of converting RC into reactive SCMs, inaccordance with another embodiment of the present invention;
[0027] FIG. 4 is a flowchart illustrating a method of converting inert minerals other than RCA / FRCA into reactive SCMs, in accordance with another embodiment of the present invention;
[0028] FIG. 5 is a plot of chemical reactivity (pozzolanic or hydraulic) of the original and activated recycled concrete samples with different levels of activation;
[0029] FIG. 6 is a plot of functional dependency of the processed FRCA reactivity on amounts of specific grinding energy;
[0030] FIG. 7 is a plot of chemical reactivity (pozzolanic or hydraulic) of the original and activated shale samples with different levels of activation;
[0031] FIG. 8 is a plot of functional dependency of the processed shale reactivity on amounts of specific grinding energy;
[0032] FIG. 9 is a plot of compressive strength of mortars with various levels of substitution of cement by activated shale (sample SMM I #3S) in compare with original mortar without the activated shale additive (control);
[0033] FIG. 10 is a plot of compressive strength of mortars with various levels of substitution of cement activated recycled concrete (sample SMM / #3C) in compare with original mortar without the activated recycled concrete additive (control); and
[0034] FIG. 11 is a plot of compressive strength of mortars with various levels of substitution of cement by activated recycled concrete (sample SMM I #3C) to compare with original mortar without the activated recycled concrete additive (control).DETAILED DESCRIPTION
[0035] The disclosure is provided in order to enable a person having ordinary skill in the art to practice the invention. Exemplary embodiments herein are provided only for illustrative purposes and various modifications will be readily apparent to persons skilled in the art. The general principles defined herein may be applied to other embodiments and applications without departing from the scope described herein. The terminology and phraseology used herein is for the purpose of describing exemplary embodiments and should not be considered limiting. Thus, the present disclosure is to be accorded the widest scope encompassing numerous alternatives,modifications and equivalents consistent with the principles and features disclosed herein. For purposes of clarity, details relating to technical material that is known in the technical fields related to what is described herein have been briefly described or omitted so as not to unnecessarily obscure the present disclosure.
[0036] Various terms used throughout the present description may be read and understood as follows, unless the context indicates otherwise: singular articles and pronouns as used throughout include their plural forms, and vice versa; similarly, gendered pronouns include their counterpart pronouns so that pronouns should not be understood as limiting anything described herein to use, implementation, performance, etc. by a single gender; “exemplary” should be understood as “illustrative” or “exemplifying” and not necessarily as “preferred” over other embodiments. It is to be noted that, as used in the present description, by the term “substantially” it is meant that the recited characteristic, parameter, or value need not be achieved exactly, but that deviations or variations, including for example, tolerances, measurement error, measurement accuracy limitations and other factors known to those skilled in the art, may occur in amounts that do not preclude the effect the characteristic was intended to provide. Further definitions for terms may be set out herein; these may apply to prior and subsequent instances of those terms, as will be understood from a reading of the present description.
[0037] For simplicity and clarity of illustration, where considered appropriate, reference numerals may be repeated among the Figures to indicate corresponding or analogous steps of the process. In addition, numerous specific details are set forth in order to provide a thorough understanding of the embodiments described herein.
[0038] Various studies have been conducted for recycling of FRCA into valuable products, like hardened cement and clean sand, are described herein. These studies can be divided into three general groups: thermal, chemical, and mechanical, or a combination thereof.
[0039] In thermal excitation, FRCA are heated to a high temperature to dehydrate the hydration products so that more active components can be produced and added to mortar replacing part of cement [see, for example, Y. Sui, C. Ou, S. Liu, J. Zhang, Q. Tian, Study on properties of waste concrete powder by thermal treatment and application in mortar, Appl. Sci. 10 (2020) 998, https: / / doi.org / 10.3390 / app10030998] or, as per another option a new recycled Portland cement clinker can be produced from the FRCA by the thermal treatment [see, for example, S. Zhutovsky, A. Shishkin, Recycling of hydrated Portland cement paste into new clinker, Construction andBuilding Materials 280 (2021)] https: / / doi.Org / 10.1016 / j.conbuildmat.2021.122510], However, thermal processes are environmentally unfriendly since they inevitably release carbon dioxide.
[0040] The mechanical processes and combination of mechanical and thermal treatments [see, for example, Lotfi, S., & Rem, P. (2016) and recycling of End of Life Concrete Fines into Hardened Cement and Clean Sand. Journal of Environmental Protection, 7, 934-950. https: / / doi.org / 10.4236 / jep.2016.76083] are mainly aimed at grinding the FRCA so that it can be used as an inert additive to cement in concrete production. However, efficiency of the mechanical processes, even if it is sometimes called “activation”, is evaluated by specific area of grinded filler and its cleanness and not its reactivity.
[0041] Chemical treatment [see, for example, Z. Prosek, V. Nezerka, R. Hluzek, J. Trejbal, P. Tesarek, G. Karra’a, Role of lime, fly ash, and slag in cement pastes containing recycled concrete fines, Construction and Building Materials 201 (2019) 702-714. https: / / doi.Org / 10.1016 / j.conbuildmat.2018.12.227] uses conversion of inert FRCA into reactive SCM. However, these chemical treatment processes require additional, sometimes rather expensive, chemical materials and may be used only in the process of making concrete but not to manufacture reactive SCM in reserve for future use.
[0042] Advantageously, embodiments of the present invention, by optimizing energy input of energy-intensive grinding mills, enable preparation of reactive SCMs from recycled concrete aggregates (RCA) and preparation of reactive SCMs from returned concrete (RC) from ready mix concrete trucks and preparation of reactive SCMs from fine recycled concrete aggregates (FRCA).
[0043] The optimized energy input of the grinding mills causes mechanochemical activation of FRCA and / or RCA and / or RC by inducing structural disorder, amorphization and increased chemical reactivity in the mineral crystals of FRCA and / or RCA and / or RC. In some cases, preparation of reactive SCMs from inert minerals other than RCA / FRCA / RC is also provided. Embodiments of the present invention advantageously afford conversion of FRCA into a usable product by a simple mechanochemical activation which is environment friendly.
[0044] Referring to FIG. 1 , a flowchart illustrating a method for converting recycled concrete obtained from CDW into reactive SCMs is shown, in accordance with an embodiment of the present invention.
[0045] At block 102, crushed recycled concrete obtained from CDW in the form of RCA isobtained from CDW. In an example, the CDWis obtained and crushed recycled concrete obtained from CDW is obtained, in the form of RCA, by subjecting the CDW to a crushing treatment. The crushing treatment may be carried out via jaw crushers, impact crushers, twin-shaft crushers, or any other type of crushers used in concrete recycling. The crushed CDW generally comprises RCA and FRCA.
[0046] At block 104, FRCA is screened from the crushed recycled concrete obtained from CDW. In some examples, the screening is carried out with vibratory screens. In an illustrative example, particles that have a size of less than approximately 4 mm in the crushed recycled concrete obtained from CDW, in the form of RCA, are screened as FRCA. The vibratory screens separate the finer grains FRCA (for example, with particle size for example less than approximately 4 mm) from the larger, gravel-like RCA (for example, with particle size for example more than approximately 4 - 5 mm). In some cases, the remaining larger RCA particles can be either used as a final product or re-processed and crushed down, or used as is for mechanochemical activation and then, in some cases, for a mechanochemical synthesis, as described herein with reference to FIG. 2.
[0047] In cases, the above screening is carried out with vibratory screens, the vibratory screens separate the finer grains FRCA from the larger, gravel-like RCA. For example, the particular sieve size can be selected to be anywhere between 3 millimeters and 7 millimeters. In a particular case, the particular sieve size can be selected to be between 4 millimeters and 5 millimeters. In this way, the screening can use industry standard sieve sizes of, for example, 3.36 mm, 4 mm, 4.76 mm, and 6.73 mm.
[0048] At block 106, the screened FRCA is subjected to mechanochemical activation and then, in some cases, a mechanochemical synthesis to obtain reactive (pozzolanic or hydraulic) SCM. The mechanochemical activation and then, in some cases, a mechanochemical synthesis of FRCA can be carried out, for example, using energy-intensive grinding mills. In various examples, energy-intensive mills are operated at predetermined mill power for a predetermined time to produce predetermined energy. The produced predetermined specific grinding energy induces mechanochemical activation into the FRCA (which is inert) to convert into a reactive FRCA. In operation, the predetermined specific grinding energy released by operating energy-intensive mills at predetermined mill power for a predetermined time induces a series of strong impacts. These may be constrained impacts when material particles are caught between two grinding media (usually balls) and subjected to stroke between the grinding media or between grindingmedia and wall, or collision when materials particles are subjected to hits (free impact) by grinding tool moving at high speed. The produced impact causes generation of crystal lattice defects or other metastable forms in the whole mineral particle (i.e. , the FRCA particle), thereby converting inert FRCA into a reactive FRCA. The reactive FRCA can be further used as a reactive (pozzolanic or hydraulic) SCM.
[0049] In some examples, the energy-intensive grinding mills are selected from mills with loose grinding media, such as vibratory ball / rod mills, planetary ball mills and stirred media mills as well as high-peripheral-speed mill (high speed disintegrator). In some examples, the mills with loose grinding media have a power density ranging from 40 to 250 kW / m3. In a preferred example, the mills with loose grinding media have a power density ranging from 40 to 450 kW / m3.
[0050] In a specific example, the stirred media mills are used for mechanochemical activation and then, in some cases, for a mechanochemical synthesis of FRCA. Examples of stirred media mills may include, but are not limited to vertical mills, such as Attritor mills, Stirred Media Detritor, Tower mill, VertiMill, MaxxMill, and horizontal mills, such as IssaMill and other similar mills.
[0051] Examples of high-peripheral-speed mills, also referred to as high speed disintegrators or high speed rotor mills, include pin mills with special wear resistant grinding tools and, preferably, turbo mills. In some examples, the high-peripheral-speed mills have a rotor speed ranging from 1 ,800 rpm up to 26,000 rpm.
[0052] In various examples, the predetermined energy generated in the energy-intensive grinding mills for mechanochemical activation and then, in some cases, a mechanochemical synthesis of FRCA into reactive (pozzolanic or hydraulic) SCM is above 10 kJ / kg, and preferably in the range from 100 to 40,000 kJ / kg for providing definitely high SCM reactivity. However, as understood by a person skilled in the art, different mills will have different mill speeds and other various parameters.
[0053] Referring to FIG. 2, a flowchart of a method of converting recycled concrete obtained from CDW into reactive SCMs is shown, in accordance with another embodiment of the present invention.
[0054] At block 202, crushed recycled concrete obtained from CDW in the form of RCA is produced from recycled concrete obtained from CDW. The CDW is obtained to produce crushed recycled concrete obtained from CDW in the form of RCA by subjecting the CDW to a crushing treatment. The crushed recycled concrete obtained from CDW generally comprises RCA andFRCA. In an example, the FRCA can include particles having a particle size less than a particular screening size (for example, selected between 3 mm and 7 mm). RCA includes larger, gravellike particles with a particle size, in an example, larger than approximately 4 - 5 mm. The crushing treatment may be carried out via jaw crushers, impact crushers, twin-shaft crushers or any other type of crushers used in concrete recycling plants.
[0055] At block 204, the crushed recycled concrete obtained from CDW is subjected to a mechanochemical activation and then, in some cases, to a mechanochemical synthesis treatment to obtain reactive (pozzolanic or hydraulic) SCM. In particular, the crushed recycled concrete obtained from CDW comprising RCA and FRCA is subjected to mechanochemical activation and then, in some cases, a mechanochemical synthesis. The mechanochemical activation and then, in some cases, a mechanochemical synthesis of crushed recycled concrete obtained from CDW can be carried out using, for example, energy-intensive grinding mills, as described herein. In various examples, energy-intensive mills can be operated at predetermined mill power for a predetermined time to produce predetermined energy. The produced predetermined energy induces mechanochemical activation into the FRCA and RCA (which is inert) to convert into a reactive FRCA and RCA. In an example, the predetermined energy produced in the energy- intensive grinding mills for mechanochemical activation and then, in some cases, for a mechanochemical synthesis of FRCA and RCA into reactive (pozzolanic or hydraulic) SCM is above 10 kJ / kg, and preferably, in the range from 100 to 40,000 kJ / kg for providing definitely high SCM reactivity. In operation, the predetermined energy above 10 KJ / Kg released by operating energy-intensive mills at predetermined mill power for a predetermined time induces a series of strong impacts on the RCA and FRCA particles in the crushed CDW. These may be constrained impacts when material particles are caught between two grinding media (usually balls) and subjected to stroke between the grinding media or between grinding media and wall, or collision when materials particles are subjected to hits (free impact) by grinding tool moving at high speed. The produced impact causes generation of crystal lattice defects or other metastable forms in the whole mineral particle, i.e., the RCA and FRCA particles, thereby converting inert FRCA and RCA into a reactive FRCA and RCA respectively. In some cases, the reactive FRCA and RCA can be further used as a reactive (pozzolanic or hydraulic) SCM.
[0056] In some examples, the energy-intensive grinding mills are selected from mills with loose grinding media, such as vibratory ball / rod mills, planetary ball mills and stirred media mills as well as high-peripheral-speed mill (high speed disintegrator). In some examples, the mills with loose grinding media can have a power density ranging from 40 to 250 kW / m3. In a preferred example,the mills with loose grinding media can have a power density ranging from 40 to 450 kW / m3. In a specific example, stirred media mills are used for mechanochemical activation and then, in some cases, for a mechanochemical synthesis. Examples of stirred media mills may include, but are not limited to vertical mills, such as Attritor mills, Stirred Media Detritor, Tower mill, VertiMill, MaxxMill, and horizontal mills, such as IssaMill and other similar mills. Examples of high- peripheral-speed mills, also referred to as high speed disintegrators or high speed rotor mills, include pin mills with special wear resistant grinding tools and, preferably, turbo mills. In some examples, the high-peripheral-speed mills can have a rotor speed ranging from 1 ,800 rpm up to 26,000 rpm.
[0057] Referring to FIG. 3, a flowchart illustrating a method of converting returned concrete (RC) from ready mix concrete trucks is shown, in accordance with another embodiment of the present invention.
[0058] At block 302, returned concrete (RC) from ready mix concrete trucks are obtained. The RC may be hardened or in a plastic state.
[0059] At block 304, the RC is subjected to mechanochemical activation and then, in some cases, to a mechanochemical synthesis process to obtain reactive SCM. The mechanochemical activation and then, in some cases, a mechanochemical synthesis of crushed inert minerals can be carried out using, for example, energy-intensive grinding mills, as described herein. The energy-intensive mills can be operated at predetermined mill power for a predetermined time to produce predetermined energy. The produced predetermined energy induces mechanochemical activation into the inert minerals and convert into reactive inert minerals. The predetermined energy produced in the energy-intensive grinding mills for mechanochemical activation and then, in some cases, a mechanochemical synthesis of RC into reactive (pozzolanic or hydraulic) SCM is, for example, above 10 kJ / kg, and preferably in the range from 100 to 40,000 kJ / kg for providing definitely high SCM reactivity. In operation, the predetermined energy above 10 kJ / Kg released by operating energy-intensive mills at the predetermined mill power for a predetermined time induces a series of strong impacts on the crushed inert mineral particles. The impact may be constrained when material particles are caught between two grinding media (usually balls) and subjected to stroke between the grinding media or between grinding media and wall, or collision when materials particles are subjected to hits (free impact) by grinding tool moving at high speed. The produced impact causes generation of crystal lattice defects or other metastable forms in the whole inert mineral particle, thereby causing conversion of inert minerals into reactive minerals.In some cases, reactive minerals can be further used as a reactive (pozzolanic or hydraulic) SCM.
[0060] As described herein, the energy-intensive grinding mills can be selected from mills with loose grinding media, such as vibratory ball / rod mills, planetary ball mills and stirred media mills as well as high-peripheral-speed mill (high speed disintegrator). In some examples, the mills with loose grinding media can have a power density ranging from 40 to 250 kW / m3. In a preferred example, the mills with loose grinding media have a power density ranging from 40 to 450 kW / m3. In a specific example, stirred media mills are used for mechanochemical activation and then, in some cases, for a mechanochemical synthesis. Examples of stirred media mills may include, but are not limited to, vertical mills, such as Attritor mills, Stirred Media Detritor, Tower mill, VertiMill, MaxxMill, and horizontal mills, such as IssaMill, and other similar mills. Examples of high- peripheral-speed mills, also referred to as high speed disintegrators or high speed rotor mills, include pin mills with special wear resistant grinding tools and, preferably, turbo mills. In some examples, the high-peripheral-speed mills can have a rotor speed ranging from 1 ,800 rpm up to 26,000 rpm.
[0061] Referring to FIG. 4, a flowchart illustrating a method of converting reactive SCMs into inert minerals other than RCA and / or FRCA and / or RC is shown, in accordance with another embodiment of the present invention.
[0062] At block 402, crushed inert minerals are obtained. Inert minerals are subjected to a crushing treatment. In some examples, the inert minerals are selected from clay minerals and shale comprising quartz, calcite, kaolinite, montmorillonite, chert, dolomite, ankerite, muscovite, illite, bentonite, pyrophyllite, chlorite, zeolite, feldspar, and other commonly available natural mineral materials. In a specific example, the inert mineral is Georgian Bay shale which is a multiphase material containing siltstone / sandstone and limestone. The crushing treatment may be carried out via jaw crushers, impact crushers, twin-shaft crushers or any other type of crushers used in concrete recycling plants or in the mining industry. In other cases, instead of crushing the material, the crushed inert minerals can be received by the system.
[0063] At block 404, the crushed inert minerals are subjected to mechanochemical activation and then, in some cases, to a mechanochemical synthesis process to obtain reactive SCM. The mechanochemical activation and then, in some cases, a mechanochemical synthesis of crushed inert minerals can be carried out using, for example, energy-intensive grinding mills, as described herein. The energy-intensive mills can be operated at predetermined mill power for a predetermined time to produce predetermined energy. The produced predetermined energyinduces mechanochemical activation into the inert minerals and convert into reactive inert minerals. The predetermined energy produced in the energy-intensive grinding mills for mechanochemical activation and then, in some cases, a mechanochemical synthesis of inert minerals other than FRCA and RCA and RC into reactive (pozzolanic or hydraulic) SCM is, for example, above 10 kJ / kg, and preferably in the range from 100 to 40,000 kJ / kg for providing definitely high SCM reactivity. In operation, the predetermined energy above 10 kJ / Kg released by operating energy-intensive mills at the predetermined mill power for a predetermined time induces a series of strong impacts on the crushed inert mineral particles. The impact may be constrained when material particles are caught between two grinding media (usually balls) and subjected to stroke between the grinding media or between grinding media and wall, or collision when materials particles are subjected to hits (free impact) by grinding tool moving at high speed. The produced impact causes generation of crystal lattice defects or other metastable forms in the whole inert mineral particle, thereby causing conversion of inert minerals into reactive minerals. In some cases, reactive minerals can be further used as a reactive (pozzolanic or hydraulic) SCM.
[0064] As described herein, the energy-intensive grinding mills can be selected from mills with loose grinding media, such as vibratory ball / rod mills, planetary ball mills and stirred media mills as well as high-peripheral-speed mill (high speed disintegrator). In some examples, the mills with loose grinding media can have a power density ranging from 40 to 250 kW / m3. In a preferred example, the mills with loose grinding media have a power density ranging from 40 to 450 kW / m3. In a specific example, stirred media mills are used for mechanochemical activation and then, in some cases, for a mechanochemical synthesis. Examples of stirred media mills may include, but are not limited to, vertical mills, such as Attritor mills, Stirred Media Detritor, Tower mill, VertiMill, MaxxMill, and horizontal mills, such as IssaMill, and other similar mills. Examples of high- peripheral-speed mills, also referred to as high speed disintegrators or high speed rotor mills, include pin mills with special wear resistant grinding tools and, preferably, turbo mills. In some examples, the high-peripheral-speed mills can have a rotor speed ranging from 1 ,800 rpm up to 26,000 rpm.Experimental Analysis
[0065] An experimental analysis was performed to verify the substantial advantages of the present embodiments; in particular, the amount of energy required for mechanochemical activation of FRCA.
[0066] The example experiments first confirmed the possibility of converting the inert FRCA into a reactive material. After that, the example experiments determined the optimal process for FRCA activation; in particular the amount of energy needed to activate the FRCA material. Accordingly, the FRCA particles were subjected to a combined action of pressure and shear forces using a high shear mixer (HSM), which caused successful activation of the cementitious materials. The FRCA particles were processed in the mixer for different time periods from 30 minutes (sufficient for activation of the cementitious materials) up to 4 hours. Subsequent x-ray diffraction (XRD) analysis of the processed FRCA particles and measuring of its reactivity by isothermal calorimetry showed that the FRCA remained inert after any of the processing time period from 30 minutes to 4 hours in the HSM. Upon further review, it was observed that the combined action of shear and compression (for example, in HSM) resulted in accumulation of structural defects at the surface and in the near-surface layers of the processed FRCA particles, which was sufficient for increasing activity of already reactive cementitious material but not sufficient for converting an inert FRCA material into reactive one.
[0067] Accordingly, it was concluded that for conversion of the inert material into a reactive one, and particularly conversion of FRCA into a reactive cementitious material, the crystal structure of the entire mineral particle (FRCA particle) should become disordered. This requires inducing maximum amount of energy into the treated solid material (FRCA material) to enable the accumulation of the input energy as defects in the entire volume of the particles and increase the excess enthalpy of the solid particle. In particular, for generation of crystal lattice defects or other metastable forms in the entire mineral particle, i.e., the FRCA particle, the particle should be subjected to a strong impact, or rather a series of strong impacts. These can be constrained impacts when material particles are caught between two grinding media (usually balls) and subjected to stroke between the grinding media or between grinding media and wall, or collision when materials particles are subjected to hits (free impact) by grinding tool moving at high speed.
[0068] It was observed that the first type of impact, which is the constraint impact, can be realized in vibration, planetary and stirred media mills. The second type of impact can be realized in high-peripheral-speed mills (high speed disintegrator, high speed rotor mills), for example, with two wheels rotating at different speeds, usually in opposite directions.
[0069] Considering numerous advantages of a stirred media mill (SMM) in comparison with other impact energy-intensive mills, exemplified above, the example experiment was conducted using SMM in order to determine the amount of energy needed to activate the FRCA. The input factor in the experiment was amount of energy for grinding the FRCA to a specified response -reactivity of the processed FRCA measured by isothermal calorimetry (according to ASTM C1897- 2).
[0070] FRCA obtained in laboratory from crushing RCA were processed in a vertical SMM with various grinding media sizes and for various durations of time, and input factor (amount of grinding energy), and response (reactivity of the processed FRCA) were measured. Particularly, in these example experiments:• grinding media (steel balls) with sizes 5 mm, 10 mm and 20 mm were used;• the degree of filling of the mill volume by the grinding media (steel balls) was 25%, 50% and 75%;• the ratio weight between the processed material and grinding media was 1 : 5, 1 : 10 and 1 : 20;• the speed of the rotor was 350 rpm, 400 rpm and 500 rpm; and• the processing time was from 30 min to 180 min.
[0071] Quantification of the reactivity of the original RCA and various RCA samples processed with different specific grinding energies and measured by isothermal calorimetry (estimated by amount released heat of hydration) is shown in TABLE 1 and in FIG. 5.TABLE 1
[0072] Considering that the recommended threshold to distinguish between the inert and reactive material is 98 J / g of SCM (as per Report of RILEM TC 267-TRM phase 3: validation ofthe R3 reactivity test across a wide range of materials, Materials and Structures (2022) 55:142), it was concluded that all the FRCA samples treated in the stirred media mill became reactive material and can be used as reactive SCM.
[0073] Referring now to FIG. 6, functional dependency of the processed FRCA reactivity on amounts of specific grinding energy is shown in a graph. It can be observed that the reactivity of the processed FRCA (i.e. , FRCA subjected to grinding) increases with an increase in specific grinding energy.
[0074] Similar experiments were conducted with coarser RCA and with RC which showed similar reactivities of the processed material as a function of the grinding energy, which can be described by the same FIG. 5 and FIG. 6 mentioned above.
[0075] Extrapolating the graph in FIG. 6 it is possible to conclude that FRCA / RCA / RC can be converted to reactive SCM by applying grinding energy above 30 kJ / kg and preferably in the range of energies from 100 kJ / kg to 30,000 kJ / kg for providing definitely high reactivity.
[0076] It was further determined based on calculations that the optimization of mill parameters may reduce grinding energy consumption for converting FRCA / RCA / RC to reactive SCM down to 10 kJ / kg. Accordingly, it was concluded that FRCA / RCA / RC can be converted to reactive SCM by applying grinding energy above 10 kJ / kg and preferably in the range of energies from 100 kJ / kg to 30,000 kJ / kg for providing definitely high SCM reactivity using the energy-intensive mills with loose grinding media having power density in the range from 40 to 450 kW / m3or using high- peripheral-speed mills with rotor speed in the range from 1 ,800 rpm up to 26,000 rpm.
[0077] In view of successful conversion of mineral based RCA / FRCA / RC into reactive SCM by mechanochemical activation and then, in some cases, by a mechanochemical synthesis, further experiments were conducted to determine the possibility of converting inert mineral materials other than RCA / FRCA / RC into reactive SCM using the same method.
[0078] In the second experiment, abundantly available shale, namely North American Georgian Bay shale, was processed in proprietary high shear mixer (HSM) as well as the stirred media mill (SMM) with various grinding energies. Further, the response factor and reactivity of the processed materials (Inert minerals other than FRCA / RCA / RC) were measured. Quantification of the reactivity of the original shale and various shale samples processed in different apparatuses (HSM and SMM) with different specific grinding energies were determined and measured by isothermal calorimetry (estimated by amount released heat of hydration); as shown in TABLE 2 and with reference to FIG. 7.TABLE 2
[0079] Further, a functional dependency of the processed shale reactivity on amounts of specific grinding energy is shown in FIG. 8. In view of a comparative analysis of the energy used for processing the shale as shown in graph of FIG. 8, it was observed that with the same energy consumption in the high shear mixer (HSM) and in the stirred media mill (SMM), the material practically was not activated in the HSM but was quite strongly activated in the SMM. In view of the aforementioned observation, it was concluded that the degree of activation of the materials depends not only on the amount of energy introduced, but also primarily on the nature of the type processing of the material. The type of processing is representative of a series of strong impacts needed for the mechanochemical activation and then, in some cases, for a mechanochemical synthesis.
[0080] Upon extrapolating the graph in FIG. 8, it was concluded that the shale can be converted to a reactive SOM by applying grinding energy above 2,000 kJ / kg and preferably in the range of energies from 3,000 kJ / kg to 40,000 kJ / kg for providing definitely high SOM reactivity.
[0081] It was further determined based on calculations that the optimization of mill parameters may reduce grinding energy consumption for converting shale to reactive SOM down to 40 kJ / kg. The mill parameters that can be optimized can include, for example:• type of rotor position (vertical or horizontal);• rotor speed;• material of the grinding media;• size of the grinding media;• degree of filling the mill by grinding media;• weight ratio between the processed material and grinding media;• processing time; and• for high-peripheral-speed mills in particular:• rotor material;• rotor diameter;• rotor speed; and• processing time.
[0082] Accordingly, it was concluded that shale can be converted to reactive SCM by applying grinding energy above 40 kJ / kg and preferably in the range of energies from 3,000 kJ / kg to 40,000 kJ / kg for providing definitely high SCM reactivity using the energy-intensive mills with loose grinding media having power density in the range from 40 to 450 kW / m3or using high-peripheral- speed mills with rotor speed in the range from 1 ,800 rpm up to 26,000 rpm.Examples
[0083] The following examples are exemplary in nature and are not to be construed as promises as to the effectiveness of the claimed invention.Example 1 :
[0084] A first example illustrates the mix design and properties of fresh (air content and flow) and hardened (compressive strength) properties of mortar samples made with various levels of cement replacement with mechanochemically activated shale.
[0085] Georgian Bay shale sample SMM I #3S with activation level 5,616 kJ / kg was used in the tests. The preparation and tests were performed in accordance with ASTM 109. Standard Tests Method for Compressive Strength of Hydraulic Cement Mortars (Using 50-mm Cube Specimens). The mix design is detailed in TABLE 3.TABLE 3
[0086] The results of tests of properties of fresh mortars are detailed in TABLE 4.TABLE 4
[0087] Data in TABLE 4 shows that properties of fresh mortar are practically not affected by replacement cement with sample SMM I #3S at all replacement levels.
[0088] The results of tests of properties of hardened mortars are detailed in TABLE 5.TABLE 5
[0089] Data in TABLE 5 shows that there is no statistical difference between compressive strength of all mortars after 7 days; i.e., compressive strength of mortar after 7 days was not affected by replacement cement with SMM I #3S at replacement levels 20%, 30% and 40%.
[0090] Compressive strength after 28 days of the Control mortar and the mortar with cement replacement level 20% are statistically equal; i.e., compressive strength of mortar after 28 days is not affected by replacement cement with SMM / #3 at replacement level 20%.
[0091] Compressive strength after 28 days of the mortars with cement replacement levels 30% and 40% are higher than corresponding compressive of the Control mortar; i.e., replacement cement with SMM I #3S at levels 30% and 40% increases compressive strength of the mortar.
[0092] Accordingly, it can be concluded that the replacement of cement with processed shale sample SMM I #3S at replacement levels up to 40% practically does not affect the properties of fresh mortar and positively affects strength of the mortar.
[0093] Compressive strength of the mortars with various levels of cement replacement with SMM I #3S as listed in TABLE 5 is further represented in FIG. 9. As can be seen from FIG. 9, compressive strength of the mortars with various levels of cement replacement with SMM I #3S clearly demonstrates the benefits of cement replacement with processed shale sample SMM I #3S at the replacement levels 30% and 40%.Example 2:
[0094] A second example illustrates the mix design and properties of fresh (air content and flow) and hardened (compressive strength) properties of mortar samples made with various levels of cement replacement with mechanochemically activated RCA. RCA sample SMM I #3C with activation level 7,488 kJ / kg was used in the tests. The preparation and tests were performed in accordance with ASTM 109. Standard Tests Method for Compressive Strength of Hydraulic Cement Mortars (Using 50-mm Cube Specimens).
[0095] The mix design is detailed in TABLE 6.TABLE 6
[0096] The results of tests of properties of fresh mortars are detailed in TABLE 7.TABLE 7
[0097] Data in TABLE 7 shows that mortars containing processed RCA have well higher air content than the control. It is explained by the fact that the RCA made from concrete with originally high content of polycarboxylate superplasticizer, which contributes to the high air content. It is known that air entrainment will reduce concrete strength.
[0098] As a general rule, a 1 % increase in the concrete air content will decrease the 28-day compressive strength by about 3 to 5%. So, in order to compare compressive strength of the mortar samples in Table 7, it is necessary to make corrections considering the different air content in the sample.
[0099] For the purpose of correction, it was assumed that 1 % increase in the concrete air content will decrease compressive strength by 4%.
[0100] The results of tests of properties of hardened mortars including actual compressive strength and corrected (calculated) strength are detailed in TABLE 8.TABLE 8
[0101] Compressive strength of the control mortar and the mortars with various levels of cement replacement with RCA SMM I #3C are listed in TABLE 8 and represented in FIG. 10, which indicates that cement replacement with processed RCA sample SMM / #3C at thereplacement levels 20% and 30% statistically does not affect the mortars strength.Example 3:
[0102] A third example illustrates a mix design and properties of fresh (air content and flow) and hardened (compressive strength) properties of mortar samples made with various levels of cement replacement with mechanochemically activated RCA. RCA sample SMM I #5C with activation level 14,796 kJ / kg was used in the tests. The preparation and tests were performed in accordance with ASTM 109. Standard Tests Method for Compressive Strength of Hydraulic Cement Mortars (Using 50-mm Cube Specimens).
[0103] The mix design is detailed in Table 9.TABLE 9
[0104] The results of tests of properties of fresh mortars are detailed in TABLE 10.TABLE 10
[0105] Data in TABLE 10 shows that by replacing cement with sample SMM I #5C at replacement level 20%, slightly increased air content because the RCA made from concrete with originally high content of polycarboxylate superplasticizer, and increased flow; i.e., improved workability of the mortar.
[0106] The results of tests of properties of hardened mortars including actual compressive strength and corrected (calculated) strength are detailed in TABLE 11.TABLE 11
[0107] Compressive strength of the control and the mortar at level of cement replacement with RCA SMM / #5C 20% are listed in the TABLE 11 and represented in FIG. 11, which demonstrates that cement replacement with processed RCA sample SMM I #5C at the replacement level 20% practically does not affect the mortars strength.
[0108] Although the invention has been described with reference to certain specific embodiments, various other aspects, advantages and modifications thereof will be apparent to those skilled in the art without departing from the spirit and scope of the invention as outlined in the claims appended hereto.
Claims
AMENDED CLAIMS received by the International Bureau on 03 August 2024 (03.08.2024)We claim:1 . A method for converting recycled concrete obtained from construction and demolition waste (CDW) into reactive supplemental cementitious materials (SCM), the method comprising: subjecting the recycled concrete obtained from CDW to a crushing treatment to obtain crushed CDW in the form of recycled concrete aggregates (RCA); and subjecting the crushed recycled concrete obtained from CDW to a mechanochemical activation treatment to obtain reactive SCM.
2. The method of claim 1 , wherein subjecting the crushed recycled concrete obtained from CDW to a mechanochemical activation treatment to obtain reactive SCM further comprises screening crushed CDW to obtain fine recycled concrete aggregates (FRCA) subjected to mechanochemical activation and filtering out RCA, wherein a particle size of less than a particular sieve size is screened as FRCA.
3. The method of claim 2, wherein the screening is performed with vibratory screens, the vibratory screens separating finer grains of FRCA with a particle size of less than the particular sieve size from grains of RCA with a particle size of more than the particular sieve size.
4. The method of claim 3, wherein the particular sieve size is selected to be between 3 millimeters and 7 millimeters.
5. The method of claim 4, wherein the particular sieve size is selected to be between 4 millimeters and 5 millimeters.
6. A method of converting inert minerals into reactive supplemental cementitious materials (SCM), the method comprising: subjecting the inert minerals to a crushing treatment; and subjecting the crushed inert minerals to a mechanochemical activation treatment to obtain reactive SCM.
7. The method of claim 6, wherein the inert minerals comprise returned concrete (RC) from ready mix concrete trucks.
8. The method of claim 7, wherein RC may be in hardened or plastic state.
9. The method of claims 1 or 6, wherein the crushing treatment uses one or more of jaw26AMENDED SHEET (ARTICLE 19)crushers, impact crushers, and twin-shaft crushers.
10. The method of claim 6, wherein the inert mineral is Georgian Bay shale comprising siltstone or sandstone and limestone.
11. The method of claim 6, wherein the inert minerals are selected from a group comprising clay minerals and shale comprising quartz, calcite, kaolinite, montmorillonite, chert, dolomite, ankerite, muscovite, illite, bentonite, pyrophyllite, chlorite, zeolite, and feldspar.
12. The method of claim 1 or 6, wherein the mechanochemical activation uses energy- intensive grinding mills.
13. The method of claim 12, wherein the energy-intensive grinding mills comprise mills with loose grinding media.
14. The method of claim 13, wherein the mills with loose grinding media are selected from vibratory ball / rod mills, planetary ball mills, and stirred media mills.
15. The method of claim 12, wherein the energy-intensive grinding mill has a power density ranging from 40 to 250 kW / m3.
16. The method of claim 12, wherein the energy-intensive grinding mill has a power density ranging from 40 to 450 kW / m3.
17. The method of claim 12, wherein the energy-intensive grinding mills comprise high- peripheral-speed mills.
18. The method of claim 17, wherein the high-peripheral-speed mills have rotor speed ranging from 1 ,800 rpm up to 26,000 rpm.
19. The method of claims 1 or 6, wherein the mechanochemical activation treatment comprises operating an energy-intensive grinding mill at a predetermined mill power for a predetermined time to produce predetermined specific grinding energy, the predetermined specific grinding energy being above 10 kJ / kg.
20. The method of claims 1 or 6, wherein the mechanochemical activation treatment comprises operating an energy-intensive grinding mill at a predetermined mill power for a predetermined time to produce predetermined specific grinding energy, the predetermined specific grinding energy ranges from 100 to 40,000 kJ / kg.27AMENDED SHEET (ARTICLE 19)
Citation Information
Patent Citations
Recycled concrete and preparation method thereof
CN110255983A
Integrated device for preparing recycled cement paste powder by using waste premixed concrete
CN113135674A
Building mortar recycling method and system
CN113831073A
Process for separating the components of hardened concrete waste for producing recycled cement