Method for recycling fluorine in recovery process of retired lithium batteries
By adopting a two-stage acid leaching process and acid dissolution treatment in the lithium battery recycling process, the fluorine in the fluoride removal residue is converted into sodium fluoride, which solves the problem of waste of fluorine resources and achieves efficient fluorine recovery and purity improvement.
Patent Information
- Application Number
- PCT/CN2023/087942
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
During the recycling process of lithium batteries, the removal of fluorine elements produces a large amount of fluorine-containing waste residue. Existing technology cannot effectively recycle it, resulting in a waste of fluorine resources.
Using a two-stage acid leaching process, acid and sodium silicate are used for acid dissolution treatment to convert the fluorine in the fluorine removal residue into crude sodium fluorosilicate, and further processed to produce sodium fluoride, realizing the resource utilization of fluorine .
The recovery rate of fluorine is more than 90%, and the purity of the obtained sodium fluoride reaches more than 70%, which simplifies the process and is suitable for practical applications.
Smart Images

Figure CN2023087942_17102024_PF_FP_ABST
Abstract
Description
A method for fluorine resource utilization in the recycling process of retired lithium batteries Technical Field
[0001] The present application belongs to the field of lithium battery recycling technology, and in particular relates to a method for utilizing fluorine resources in the recycling process of retired lithium batteries. Background Art
[0002] With the looming goal of carbon neutrality, the new energy market is booming and holds immense promise. Lithium-ion batteries are a leading player in this market. However, lithium-ion batteries have a lifespan of only three to five years. As more and more lithium-ion batteries reach end-of-life, the efficient and effective disposal of retired batteries is essential for environmental protection and sustainable resource development.
[0003] When recovering valuable metals from retired lithium batteries, a hydrometallurgical process is generally used. The hydrometallurgical process is currently a relatively mature and widely used process method for recycling waste lithium-ion batteries. Generally, retired lithium batteries are subjected to processes such as discharge, crushing, screening, acid leaching, impurity removal, and extraction to recover nickel, cobalt, manganese, and lithium. Since the fluorine element in the electrolyte and binder will accompany the entire recovery process, and a large amount of calcium chloride, magnesium chloride, etc. will be consumed in the entire lithium recovery process, the existing fluorine element will not only corrode the production equipment, but also be brought into the lithium products, causing the products to be unqualified. Therefore, defluorination is required. However, a large amount of fluorine-containing waste residue, such as calcium fluoride, magnesium fluoride, etc., will be generated in the defluorination process. There is currently no effective way to recycle the large amount of fluorine-containing waste residue, namely defluorination residue, generated in the above-mentioned defluorination process, resulting in a waste of fluorine resources.
[0004] Summary of the Invention
[0005] The purpose of the present application is to overcome the deficiencies of the above-mentioned prior art and to provide a method for fluorine resource utilization in the recycling process of retired lithium batteries that can effectively recover fluorine in defluorination slag and improve the fluorine recovery rate.
[0006] To achieve the above objectives, the technical solution adopted in this application is: a method for fluorine resource utilization in the recycling process of retired lithium batteries, comprising the following steps:
[0007] (1) mixing the defluorination residue from the retired lithium battery recycling process with liquid A, a first inorganic acid, and sodium silicate, and then heating the mixture for reaction. After the reaction is completed, the solid and liquid are separated to obtain a first leaching residue and a first leaching liquid;
[0008] (2) mixing the first-stage leaching residue with water, a second inorganic acid, and sodium silicate, and then heating the mixture for reaction. After the reaction is completed, solid-liquid separation is performed to obtain the second-stage leaching residue and the second-stage leachate;
[0009] (3) mixing the second-stage leaching residue with a soda ash solution for reaction, and performing solid-liquid separation after the reaction to obtain sodium fluoride;
[0010] The liquid A is water or the second-stage leachate.
[0011] In a method for resource utilization of fluorine in the recycling process of retired lithium batteries provided in the present application, a two-stage acid leaching process is utilized, and an acid + sodium silicate process is used for acid dissolution treatment in each stage, so that the fluorine in the defluorination slag can be converted into crude sodium fluorosilicate to the greatest extent, and the crude sodium fluorosilicate is further made into sodium fluoride, thereby realizing resource utilization of fluorine; in addition, the inventors have found that the liquid A in step (1) can be water or a second-stage leachate. When the second-stage leachate is used, not only can the same effect as water be achieved, but the second-stage leachate can also be recycled.
[0012] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in the present application, before step (1) of the present application, the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag in the process of recycling retired lithium batteries are tested by atomic absorption spectrophotometry. At the same time, after steps (2) and (3), the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the first-stage leachate, the first-stage leachate slag, the second-stage leachate and the second-stage leachate slag are respectively tested by atomic absorption spectrophotometry.
[0013] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in the present application, in step (1), the sum of the molar amounts of calcium and magnesium elements in the defluorination slag and the H + The molar ratio of the nickel, cobalt and manganese in the defluorination slag is (0.4-0.8):1, the sum of the molar amounts of nickel, cobalt and manganese in the first inorganic acid + The molar ratio of sodium silicate to H in the first inorganic acid is (0.06-0.15):1. + The molar ratio is (0.1-0.7):1, and the liquid-solid ratio of liquid A to defluorination slag is (1.5-3) mL:1 g.
[0014] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, in the step (1), the temperature of the heating reaction is 60-150° C. and the time is 1-4 hours.
[0015] The inventors have found that when the molar ratio of the above substances, reaction temperature and time are used in a single-stage leaching, fluorine can be converted to sodium fluorosilicate to the greatest extent and exist in the form of a single-stage leaching residue.
[0016] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in the present application, in step (2), the sum of the molar amounts of calcium and magnesium elements in the first leaching residue and the H +The molar ratio of sodium silicate to H in the second inorganic acid is (0.2-0.7):1. + The molar ratio is (0.1-0.3):1, and the liquid-solid ratio of water to the first-stage leaching residue is (1-5)mL:1g.
[0017] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, in step (2), the temperature of the heating reaction is 60-150°C and the time is 3-6 hours.
[0018] The inventors have found that when the molar ratio of the above substances, reaction temperature and time are used in the second-stage leaching, fluorine can be converted into sodium fluorosilicate to the greatest extent and exist in the form of second-stage leaching residue.
[0019] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, in step (3), F in the second-stage leaching residue is + The ratio of the molar amount of HCl to the molar amount of soda ash is 1:(0.4-1.2).
[0020] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, in step (3), the concentration of soda ash is 150-300 g / L.
[0021] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, in step (3), the reaction temperature is 60-100°C and the reaction time is 1-5 hours.
[0022] The inventors have found that when a soda ash solution within the above concentration range and a corresponding reaction temperature and time are used in step (3), the purity of the subsequently obtained sodium fluoride can be ensured to be within an acceptable range. Specifically, the purity of the obtained sodium fluoride is above 70%, thereby avoiding the unnecessary process of further purification of the sodium fluoride.
[0023] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in the present application, the first inorganic acid and the second inorganic acid are each independently selected from any one of hydrochloric acid, nitric acid, and carbonic acid.
[0024] Preferably, the first inorganic acid and the second inorganic acid are both selected from hydrochloric acid.
[0025] As a preferred embodiment of the method for fluorine resource utilization in the process of recycling retired lithium batteries described in this application, the solid-liquid separation adopts a filter press method.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] The method for resource utilization of fluorine in the recycling process of retired lithium batteries provided in the present application utilizes a two-stage acid leaching process, in which an acid + sodium silicate process is used for acid dissolution treatment, so that the fluorine in the defluorination slag can be converted into crude sodium fluorosilicate to the greatest extent, and the crude sodium fluorosilicate is further prepared into sodium fluoride, thereby realizing resource utilization of fluorine; specifically, the recovery rate of fluorine in the defluorination slag is above 90%, and the purity of the obtained sodium fluoride is above 70%; and the method provided in the present application is simple to operate and suitable for practical application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG1 is a schematic flow chart of the method for fluorine resource utilization in the recycling process of retired lithium batteries in Example 1. DETAILED DESCRIPTION
[0029] In order to better illustrate the purpose, technical solutions and advantages of this application, this application will be further described below in conjunction with specific embodiments.
[0030] Unless otherwise specified, the reagents, methods and equipment used in this application are conventional reagents, methods and equipment in the art.
[0031] Example 1
[0032] The present invention provides a method for recycling fluorine in a decommissioned lithium battery recycling process. The method is shown in FIG1 , and includes the following steps:
[0033] (1) 1000 g of defluorination residue from a retired lithium battery recycling process was taken, and the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium were detected by atomic absorption spectrophotometry. The residue was then placed in a reaction tank, 1800 mL of water, 171 g of sodium silicate, and 1060 mL of 30% hydrochloric acid were added and mixed evenly. The mixture was then heated to 85° C. for 2 h. After the reaction was completed, the mixture was cooled to 25° C., and solid-liquid separation was performed by filter press to obtain 470 g of first-stage leaching residue and 2.8 L of first-stage leaching liquid.
[0034] (2) The contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium in the first-stage leaching residue obtained in step (1) were detected by atomic absorption spectrophotometry. 470 g of the first-stage leaching residue was uniformly mixed with 1800 mL of water, 41 g of sodium silicate, and 200 mL of 30% hydrochloric acid, and then heated to 85° C. for reaction for 4 h. After the reaction was completed, the mixture was cooled to 25° C. and then solid-liquid separation was performed by filter press to obtain 394 g of the second-stage leaching residue and 1.9 L of the second-stage leachate.
[0035] (3) placing 394 g of the second-stage leaching residue in step (2) in a reaction tank, adding 3.64 L of a soda ash solution with a mass concentration of 300 g / L, reacting at 85° C. for 2 h, cooling to 25° C. after the reaction, and then performing solid-liquid separation by filter press to obtain sodium fluoride;
[0036] In the process of fluorine resource utilization during the recycling of retired lithium batteries, atomic absorption spectrophotometry was used to detect the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag, first-stage leaching slag, first-stage leaching liquid, second-stage leaching slag and second-stage leaching liquid, as shown in Table 1, where the unit of slag is %, and the unit of liquid is g / L.
[0037] Table 1
[0038] Example 2
[0039] The present invention provides a method for recycling fluorine in a decommissioned lithium battery recycling process, comprising the following steps:
[0040] (1) 1000 g of defluorination residue from a retired lithium battery recycling process was taken, and the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium were detected by atomic absorption spectrophotometry. The residue was then placed in a reaction tank, 1800 mL of water, 214 g of sodium silicate, and 1060 mL of 30% hydrochloric acid were added and mixed evenly. The mixture was then heated to 145 ° C for 1 h. After the reaction was completed, the mixture was cooled to 25 ° C, and solid-liquid separation was performed by filter press to obtain 465 g of first-stage leaching residue and 2.8 L of first-stage leaching liquid.
[0041] (2) The contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium in the first-stage leaching residue obtained in step (1) were detected by atomic absorption spectrophotometry. 465 g of the first-stage leaching residue was uniformly mixed with 1800 mL of water, 40 g of sodium silicate, and 200 mL of 30% hydrochloric acid, and then heated to 145° C. for reaction for 3 h. After the reaction was completed, the mixture was cooled to 25° C. and then solid-liquid separation was performed by filter press to obtain 401 g of the second-stage leaching residue and 1.9 L of the second-stage leachate.
[0042] (3) placing 401 g of the second-stage leaching residue in step (2) in a reaction tank, adding 3.64 L of a soda ash solution with a mass concentration of 300 g / L, reacting at 95° C. for 1 h, cooling to 25° C. after the reaction, and then performing solid-liquid separation by filter press to obtain sodium fluoride;
[0043] In the process of fluorine resource utilization during the recycling of retired lithium batteries, atomic absorption spectrophotometry was used to detect the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag, first-stage leaching slag, first-stage leaching liquid, second-stage leaching slag and second-stage leaching liquid, as shown in Table 2, where the unit of slag is %, and the unit of liquid is g / L.
[0044] Table 2
[0045] Example 3
[0046] The present invention provides a method for recycling fluorine in a decommissioned lithium battery recycling process, comprising the following steps:
[0047] (1) 1000 g of defluorination residue from a retired lithium battery recycling process was taken, and the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium were detected by atomic absorption spectrophotometry. The residue was then placed in a reaction tank, 1800 mL of water, 1082 g of sodium silicate, and 1770 mL of 30% hydrochloric acid were added and mixed evenly. The mixture was then heated to 60 ° C for 4 h. After the reaction was completed, the mixture was cooled to 25 ° C, and solid-liquid separation was performed by filter press to obtain 439 g of first-stage leaching residue and 3.5 L of first-stage leaching liquid.
[0048] (2) The contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium in the first-stage leaching residue obtained in step (1) were detected by atomic absorption spectrophotometry. 439 g of the first-stage leaching residue was uniformly mixed with 1800 mL of water, 72.3 g of sodium silicate, and 311 mL of 30% hydrochloric acid, and then heated to 60° C. for reaction for 6 h. After the reaction was completed, the mixture was cooled to 25° C. and then solid-liquid separation was performed by filter press to obtain 372 g of the second-stage leaching residue and 2.0 L of the second-stage leachate.
[0049] (3) placing 372 g of the second-stage leaching residue in step (2) in a reaction tank, adding 3.89 L of a soda ash solution with a mass concentration of 300 g / L, reacting at 80° C. for 5 h, cooling to 25° C. after the reaction, and then performing solid-liquid separation by filter press to obtain sodium fluoride;
[0050] In the process of fluorine resource utilization during the recycling of retired lithium batteries, atomic absorption spectrophotometry was used to detect the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag, first-stage leaching slag, first-stage leaching liquid, second-stage leaching slag and second-stage leaching liquid, as shown in Table 3, where the unit of slag is %, and the unit of liquid is g / L.
[0051] Table 3
[0052] Example 4
[0053] The present invention provides a method for recycling fluorine in a decommissioned lithium battery recycling process, comprising the following steps:
[0054] (1) 1000 g of defluorination residue from a retired lithium battery recycling process was taken, and the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium were detected by atomic absorption spectrophotometry. The residue was then placed in a reaction tank, 1800 mL of water, 362 g of sodium silicate, and 1515 mL of 30% hydrochloric acid were added and mixed evenly. The mixture was then heated to 110° C. for 1.5 h. After the reaction was completed, the mixture was cooled to 25° C., and solid-liquid separation was performed by filter press to obtain 425 g of first-stage leaching residue and 3.2 L of first-stage leaching liquid.
[0055] (2) The contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium in the first-stage leaching residue obtained in step (1) were detected by atomic absorption spectrophotometry. 425 g of the first-stage leaching residue was uniformly mixed with 1800 mL of water, 67 g of sodium silicate, and 312 mL of 30% hydrochloric acid, and then heated to 110° C. for reaction for 3.5 h. After the reaction was completed, the mixture was cooled to 25° C. and then solid-liquid separation was performed by filter press to obtain 380 g of the second-stage leaching residue and 2.1 L of the second-stage leachate.
[0056] (3) placing 380 g of the second-stage leaching residue in step (2) in a reaction tank, adding 7.86 L of a soda ash solution with a mass concentration of 150 g / L, reacting at 85 ° C for 2 h, cooling to 25 ° C after the reaction, and then performing solid-liquid separation by filter press to obtain sodium fluoride;
[0057] In the process of fluorine resource utilization during the recycling of retired lithium batteries, atomic absorption spectrophotometry was used to detect the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag, first-stage leaching slag, first-stage leaching liquid, second-stage leaching slag and second-stage leaching liquid, as shown in Table 4, where the unit of slag is %, and the unit of liquid is g / L.
[0058] Table 4
[0059] Example 5
[0060] The present embodiment provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The only difference from Example 1 is that the amount of sodium silicate added in step (1) is 135 g. The test data during the method are shown in Table 5.
[0061] Table 5
[0062] Example 6
[0063] The present embodiment provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The only difference from Example 1 is that the amount of sodium silicate added in step (2) is 20 g. The test data during the method are shown in Table 6.
[0064] Table 6
[0065] Example 7
[0066] The present embodiment provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that the reaction temperature in step (1) is 140° C. for 1 hour. The test data during the method are shown in Table 7.
[0067] Table 7
[0068] Example 8
[0069] The present embodiment provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that the reaction temperature in step (2) is 60° C. and the reaction time is 5 hours. The test data during the method are shown in Table 8.
[0070] Table 8
[0071] Comparative Example 1
[0072] The comparative example of the present application provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The difference from Example 1 is that a single-stage leaching is adopted, including the following steps:
[0073] (1) 1000 g of defluorination residue from a retired lithium battery recycling process was taken, and the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese, and sodium were detected by atomic absorption spectrophotometry. The residue was then placed in a reaction tank, 1800 mL of water, 171 g of sodium silicate, and 1060 mL of 30% hydrochloric acid were added and mixed evenly. The mixture was then heated to 85° C. for 2 h. After the reaction was completed, the mixture was cooled to 25° C., and solid-liquid separation was performed by filter press to obtain 950 g of first-stage leaching residue and 2.8 L of first-stage leaching liquid.
[0074] (2) placing 950 g of the first-stage leaching residue in step (1) in a reaction tank, adding 3.64 L of a soda ash solution with a mass concentration of 300 g / L, reacting at 85° C. for 2 h, cooling to 25° C. after the reaction, and then performing solid-liquid separation by filter press to obtain sodium fluoride;
[0075] In the process of fluorine resource utilization during the recycling of retired lithium batteries, the contents of calcium, magnesium, fluorine, nickel, cobalt, manganese and sodium in the defluorination slag, the first-stage leaching slag and the first-stage leaching liquid were detected by atomic absorption spectrophotometry as shown in Table 9, where the unit of slag is %, and the unit of liquid is g / L.
[0076] Table 9
[0077] Comparative Example 2
[0078] The comparative example of the present application provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The difference from Example 1 is that the reaction temperature in step (3) is 50°C.
[0079] Comparative Example 3
[0080] The comparative example of the present application provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that 480 mL of 30% hydrochloric acid is added in step (1). The test data during the method are shown in Table 10.
[0081] Table 10
[0082] Comparative Example 4
[0083] The comparative example of the present application provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that 80g of sodium silicate is added in step (1). The test data during the method are shown in Table 11.
[0084] Table 11
[0085] Comparative Example 5
[0086] The comparative example of the present application provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The only difference from Example 1 is that 100 mL of 30% hydrochloric acid is added in step (2). The test data during the method are shown in Table 12.
[0087] Table 12
[0088] Comparative Example 6
[0089] The comparative example of the present application provides a method for fluorine resource utilization in the process of recycling retired lithium batteries. The only difference from Example 1 is that 18g of sodium silicate is added in step (1). The test data during the method are shown in Table 13.
[0090] Table 13
[0091] Comparative Example 7
[0092] The comparative example of the present application provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that the reaction temperature in step (1) is 180° C. and the reaction time is 2 hours. The test data during the method are shown in Table 14.
[0093] Table 14
[0094] Comparative Example 8
[0095] The comparative example of the present application provides a method for fluorine resource utilization in the recycling process of retired lithium batteries. The only difference from Example 1 is that the reaction temperature in step (2) is 40° C. and the reaction time is 6 hours. The test data during the method are shown in Table 15.
[0096] Table 15
[0097] Effect Examples
[0098] The present application effect example verifies the recovery rate of fluorine element in the defluorination slag and the overall recovery rate of fluorine element in the leaching process in Examples 1-8 and Comparative Examples 2-8, wherein the recovery rate of fluorine element in the defluorination slag during the leaching process is represented by y1, and the recovery rate of the overall process is represented by y2; y1=(m 二段 浸出渣 × the percentage of fluorine in the second-stage leaching residue) / (m 除氟渣 × percentage of fluorine in the defluorination slag) × 100%, y2 = (m 氟化钠 × sodium fluoride purity × 19 / 42) / (m 除氟渣 × percentage of fluorine in the defluorination slag) × 100%; in Comparative Example 1, y1 = (m 一段浸出渣 × the percentage of fluorine in the first-stage leaching residue) / (m 除氟渣 × percentage of fluorine in the defluorination slag) × 100%, y2 = (m 氟化钠 × sodium fluoride purity × 19 / 42) / (m 除氟渣 × percentage of fluorine in defluorination slag) × 100%;
[0099] Table 16
[0100] Note: In Comparative Examples 3 and 5, due to insufficient acid, most of the fluorine still exists in the form of calcium magnesium fluoride, and no sodium fluorosilicate is generated. Therefore, the recovery rate of fluorine in the leaching process is not calculated and is represented by “ / ”.
[0101] As can be seen from Table 16, when the method for fluorine resource utilization in the recycling process of retired lithium batteries of the present application is adopted, the fluorine in the defluorination slag can be effectively recovered and utilized, wherein the recovery rate of the fluorine element after the leaching is above 95%, the overall recovery rate is above 90%, and the purity of the recycled product sodium fluoride is above 70%, which meets the basic utilization requirements and can be used without further purification steps.
[0102] As can be seen from the data of Example 1 and Comparative Example 1, if a single-stage leaching is used, the calcium in the defluorination residue cannot be completely leached, while a large amount of fluorine is dissolved, resulting in a reduced fluorine content in the leached residue and an inability to effectively recover the fluorine in the defluorination residue. As can be seen from Example 1 and Comparative Example 2, when the second-stage leaching residue is reacted with the soda ash solution, if the reaction temperature is too low, the conversion is incomplete, resulting in low purity of the resulting sodium fluoride.
[0103] It can be seen from Example 1 and Comparative Examples 2-8 that the parameters in the recovery process will affect the recovery rate of fluorine element in the defluorination slag and the overall recovery rate of fluorine element in the leaching process. When the selected parameters are not within the range given in this application, the recovery rate of fluorine element in the defluorination slag and the overall recovery rate of fluorine element both show a significant downward trend.
[0104] Finally, it should be noted that the above embodiments are intended to illustrate the technical solutions of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present application.
Claims
1. A method for fluorine resource utilization in the process of recycling retired lithium batteries, characterized in that: The following steps are involved: (1) mixing the defluorinated residue from the recycling process of retired lithium batteries with liquid A, a first inorganic acid, and sodium silicate, and heating them for reaction, and separating the solid and the liquid after the reaction is completed to obtain a first leaching residue and a first leaching liquid; (2) mixing the first-stage leaching residue with water, a second inorganic acid, and sodium silicate, and heating the mixture for reaction. After the reaction is completed, the solid and liquid are separated to obtain the second-stage leaching residue and the second-stage leaching liquid; (3) mixing the second-stage leaching residue with a soda ash solution for reaction, and separating the solid and liquid after the reaction is completed to obtain sodium fluoride; The liquid A is water or a second-stage leaching liquid.
2. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (1), the sum of the molar amounts of calcium and magnesium in the defluorinated slag and the H + The molar ratio of the nickel, cobalt and manganese in the defluorination slag is (0.4-0.8): 1, the sum of the molar amounts of nickel, cobalt and manganese in the defluorination slag and the molar amount of H in the first inorganic acid + The molar ratio is (0.06-0.15):
1.
3. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (1), the molar amount of sodium silicate and the H in the first inorganic acid are + The molar ratio is (0.1-0.7):
1.
4. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (1), the liquid-to-solid ratio of liquid A to defluorination slag is (1.5-3) mL: 1 g.
5. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (1), the heating reaction temperature is 60-150° C. and the time is 1-4 hours.
6. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (2), the sum of the molar amounts of calcium and magnesium in the first leaching residue and the H + The molar ratio is (0.2-0.7):
1.
7. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (2), the molar amount of sodium silicate and the H in the second inorganic acid are + The molar ratio is (0.1-0.3):
1.
8. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (2), the liquid-to-solid ratio of water to the first-stage leaching residue is (1-5) mL: 1 g.
9. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (2), the heating reaction temperature is 60-150° C. and the time is 3-6 hours.
10. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (3), F in the second-stage leaching residue + The ratio of the molar amount of sodium bicarbonate to the molar amount of soda ash is 1:(0.4-1.2).
11. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (3), the concentration of soda ash is 150-300 g / L.
12. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: In the step (3), the reaction temperature is 60-100° C. and the reaction time is 1-5 h.
13. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: The first inorganic acid and the second organic acid are each independently selected from at least one of hydrochloric acid, nitric acid, and carbonic acid.
14. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: The first inorganic acid and the second organic acid are both selected from hydrochloric acid.
15. The method for fluorine resource utilization in the process of recycling retired lithium batteries according to claim 1, characterized in that: The solid-liquid separation is carried out by filter pressing.
Citation Information
Patent Citations
Method for preparing sodium fluoride from defluorination residue generated in production of phosphoric acid by wet process
CN104386711A
Method for recycling fluorine resources in phosphate fertilizer production
CN105776221A
Method for recovering fluorine resource from fluorination residues of feed phosphate
CN105819452A
Method for purifying defluorination residue to prepare sodium fluosilicate
CN107381578A
Recovery method for removing fluorine from nickel-cobalt-manganese solution
CN112079371A