Polymer used for black matrix, preparation method therefor, and application thereof
By developing an intrinsic resin-based polymer that combines dianhydride monomer and 1,8 dihydroxy-2,4,5,7 tetraamino-9,10-anthraquinone, the high cost and cost of black matrix photoresist are solved. Electrical insulation performance issues, high-resolution patterns and localization are achieved.
Patent Information
- Application Number
- PCT/CN2024/085781
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-17
AI Technical Summary
The existing black matrix photoresist has high cost, high chromium reflectivity and environmental pollution problems. The use of carbon materials and organic dyes reduces the electrical insulation performance, making it difficult to achieve high-resolution patterns and localization.
Develop an intrinsic resin polymer that combines diamine monomer and 1,8 dihydroxy-2,4,5,7 tetraamino-9 through the reaction of dianhydride monomer, esterification reagent and acid chloride reagent. 10-Anthraquinone forms a black matrix polymer with high resolution and excellent mechanical and thermal properties, and is a positive photoresist developed with alkaline water.
It achieves high-resolution pattern formation and a black matrix polymer with excellent mechanical and thermal properties, which reduces production costs, avoids environmental pollution, and improves the level of localization.
Smart Images

Figure CN2024085781_17102024_PF_FP_ABST
Abstract
Description
A polymer for black matrix, preparation method and application thereof Technical Field
[0001] The present invention relates to a polymer for a black matrix, in particular to an intrinsic resin-based black matrix polymer with a high OD value, good mechanical, thermal and photolithographic properties, and a preparation method and application thereof. Background Art
[0002] Liquid crystal display (LCD) photoresist is a technology-intensive industry with high technical barriers. Currently, only a small number of manufacturers in Japan, South Korea, and Taiwan have the capacity to mass-produce LCD photoresist, and only a few Japanese companies possess the key technologies. This significantly restricts the development of LCD photoresist in my country. LCD photoresist includes both color and black photoresist.
[0003] With the rapid development of liquid crystal display technology in recent years, demand for high contrast ratios has become increasingly high. A black matrix is placed between the color filters and the dot gaps. This matrix shields light and creates a framework for the subsequent application of red, green, and blue primary color resists. The quality of the black matrix directly impacts the color rendering performance of the color filters.
[0004] In order to improve the contrast of liquid crystal display devices, chromium is used in black matrix, mainly by chromium deposition on the surface of glass substrate, and then patterning is formed by etching method. Although this method makes black matrix have higher optical density and stronger mechanical property, it also has problems such as high cost, high reflectivity of chromium and environmental pollution caused by chromium-containing wastewater. Then, researchers proposed to prepare black matrix photoresist composition with pigment. Due to the pigment doped in photoresist, it is not dissolved by developer, the developing time is long, and the developing effect is not good, which causes the pattern of high resolution to be unable to be obtained. The introduction of carbon material and organic dye significantly reduces the electrical insulation performance of black matrix. Although researchers also use non-carbon black color pigment to prepare black matrix, due to the color pigment having poor light shielding, black matrix photoresist composition needs high mixing ratio. Cause the viscosity of composition to increase, the intensity of the film formed is reduced.
[0005] Therefore, a lot of research is needed to develop an intrinsic resin-based black matrix to circumvent the above shortcomings and further provide theoretical and technical support and promotion for the localization of black matrix photoresist.
[0006] Summary of the Invention
[0007] The present invention aims to overcome the above-mentioned deficiencies of the prior art and provide a polymer having good mechanical, thermal and photolithographic properties for use in black matrices. The present invention also provides a method for preparing the polymer and its application.
[0008] To achieve the above object, the technical solution adopted by the present invention is: a polymer having the structural formula:
[0009] Where R is H or At least one of; n is an integer from 8 to 40.
[0010] The polymer of the present invention has unique structural characteristics, can form high-resolution patterns, has excellent mechanical and thermal properties, and can be used as a positive photoresist for alkaline water development. When applied to a black matrix, the performance of the black matrix can be improved.
[0011] In addition, the present invention also provides a method for preparing the above-mentioned polymer with simple process steps and easy industrialization. To achieve this purpose, the technical solution adopted by the present invention is: a method for preparing the above-mentioned polymer, the method comprising the following steps:
[0012] (1) reacting a dianhydride monomer, an esterification agent, and an acyl chloride agent in a solvent 1 to obtain an intermediate;
[0013] (2) reacting the intermediate obtained in step (1) with a diamine monomer and 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone in solvent 2 to obtain the polymer.
[0014] The preparation method of the polymer provided by the present invention first uses a dianhydride monomer and an esterification reagent to react in a solvent 1 to obtain an intermediate, and then reacts the obtained intermediate with a diamine monomer and 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone. The polymer with unique structural characteristics as described above can be quickly and efficiently prepared, and the preparation method has simple process steps.
[0015] In the preparation method of the polymer of the present invention, the structural formula of the 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone is as follows:
[0016] In the preparation method of the polymer of the present invention, the 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone can be purchased directly or prepared using conventional techniques in the art. The preparation methods of the 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone include but are not limited to the following two methods:
[0017] (1) In the presence of concentrated sulfuric acid and concentrated nitric acid, 1,8-dihydroxy-9,10-anthraquinone is nitrated to 1,8-dihydroxy-2,4,5,7-tetranitro-9,10-anthraquinone, and then the nitro group is reduced to the amino group to obtain 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone.
[0018] (2) In the presence of concentrated sulfuric acid and concentrated nitric acid, 1,8-dihydroxy-4,5-dinitro-9,10-anthraquinone is nitrated to 1,8-dihydroxy-2,4,5,7-tetranitro-9,10-anthraquinone, and then the nitro group is reduced to the amino group to obtain 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone.
[0019] As a preferred embodiment of the polymer preparation method of the present invention, the step (1) is: reacting a dianhydride monomer and an esterification reagent in a solvent 1 to obtain a reaction liquid; and adding an acyl chloride reagent dropwise to the reaction liquid under a nitrogen atmosphere and an ice bath condition to obtain an intermediate after the addition is complete.
[0020] As a preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the dianhydride monomer to the esterification agent in step (1) is 1:1 to 1:2. As a more preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the dianhydride monomer to the esterification agent in step (1) is 1:2.
[0021] As a preferred embodiment of the polymer preparation method of the present invention, the reaction temperature of the dianhydride monomer and the esterification agent in the solvent 1 in step (1) is 30 to 90° C. As a more preferred embodiment of the polymer preparation method of the present invention, the reaction temperature of the dianhydride monomer and the esterification agent in the solvent 1 in step (1) is 60° C.
[0022] As a preferred embodiment of the polymer preparation method of the present invention, the reaction time of the dianhydride monomer and the esterification agent in the solvent 1 in step (1) is 6-24 hours. As a more preferred embodiment of the polymer preparation method of the present invention, the reaction time of the dianhydride monomer and the esterification agent in the solvent 1 in step (1) is 10 hours.
[0023] As a preferred embodiment of the polymer preparation method of the present invention, the temperature of the ice bath condition in step (1) is 5-10° C. As a more preferred embodiment of the polymer preparation method of the present invention, the temperature of the ice bath condition in step (1) is 5° C.
[0024] As a preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the acyl chloride reagent to the dianhydride monomer in step (1) is 2:1 to 2.5:1. As a more preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the acyl chloride reagent to the dianhydride monomer in step (1) is 2.2:1.
[0025] As a preferred embodiment of the polymer preparation method of the present invention, the dripping speed of the acyl chloride reagent in step (1) is 1 to 4 drops / second. As a more preferred embodiment of the polymer preparation method of the present invention, the dripping speed of the acyl chloride reagent in step (1) is 1 drop / second.
[0026] As a preferred embodiment of the polymer preparation method of the present invention, the solvent 1 in step (1) is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran. As a more preferred embodiment of the polymer preparation method of the present invention, the solvent 1 in step (1) is N-methylpyrrolidone.
[0027] As a preferred embodiment of the polymer preparation method of the present invention, the chlorination agent in step (1) is at least one of SOCl2, AlCl3, BF3, SbCl5, FeBr3, FeCl3, SnCl4, TiCl4, and ZnCl2. As a more preferred embodiment of the polymer preparation method of the present invention, the chlorination agent in step (1) is SOCl2.
[0028] As a preferred embodiment of the polymer preparation method of the present invention, the esterification agent in step (1) is at least one of n-butanol, ethanol, isopropanol, n-propanol, tert-butanol, and methanol. As a more preferred embodiment of the polymer preparation method of the present invention, the esterification agent in step (1) is n-butanol.
[0029] As a preferred embodiment of the polymer preparation method of the present invention, the dianhydride monomer in step (1) is at least one of 3,3',4,4'-diphenylether tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxylic)hexafluoropropane dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3,4,4-diphenylsulfone tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, diphenyl sulfide dianhydride, and bisphenol A diether dianhydride. As a more preferred embodiment of the polymer preparation method of the present invention, the dianhydride monomer in step (1) is 3,3',4,4'-diphenylether tetracarboxylic dianhydride.
[0030] As a preferred embodiment of the polymer preparation method of the present invention, the structural formula of the intermediate is:
[0031] Where R is H or At least one of .
[0032] As a preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the diamine monomer, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone, and the intermediate in step (2) is: diamine monomer: 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone: intermediate = 1:1:2 to 1:1:4. As a more preferred embodiment of the polymer preparation method of the present invention, the molar ratio of the diamine monomer, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone, and the intermediate in step (2) is: diamine monomer: 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone: intermediate = 1:1:2.
[0033] As a preferred embodiment of the polymer preparation method of the present invention, the diamine monomer in step (2) is m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diamino-2,2'-dimethylbiphenyl, 2-(4-aminophenyl)-5-aminobenzoxazine At least one of oxadiazole, 2-(4-aminophenyl)-5-aminobenzimidazole, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-hydroxy-4-aminophenoxy)benzene, 2-(4-aminophenyl)-6-aminobenzoxazole, 2,2-p-phenyl-bis(5-aminobenzoxazole), 2,2'-p-phenyl-bis(6-aminobenzoxazole), 2,2-bis(4-hydroxy-3-aminophenyl)propane, 3,3'-dihydroxybenzidine, and 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid. As a more preferred embodiment of the polymer preparation method of the present invention, the diamine monomer in step (2) is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.
[0034] As a preferred embodiment of the polymer preparation method of the present invention, the dianhydride monomer in step (1) is 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, and the diamine monomer in step (2) is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.
[0035] As a preferred embodiment of the polymer preparation method of the present invention, the solvent 2 in step (2) is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran. As a more preferred embodiment of the polymer preparation method of the present invention, the solvent 2 in step (2) is N-methylpyrrolidone.
[0036] As a preferred embodiment of the polymer preparation method of the present invention, the reaction temperature in step (2) is 15-35° C. As a more preferred embodiment of the polymer preparation method of the present invention, the reaction temperature in step (2) is 25° C.
[0037] As a preferred embodiment of the polymer preparation method of the present invention, the reaction time of step (2) is 3-8 hours. As a more preferred embodiment of the polymer preparation method of the present invention, the reaction time of step (2) is 6 hours.
[0038] Finally, the present invention also provides an application of the polymer having the structural characteristics described above in the preparation of a black matrix.
[0039] The polymer provided by the present invention, due to its unique structural characteristics, can form high-resolution patterns, has excellent mechanical and thermal properties, and can be used as a positive photoresist developable with alkaline water. When applied to a black matrix, it can improve the performance of the black matrix.
[0040] The preparation method of the polymer of the present invention has readily available raw materials, simple preparation steps and process conditions, and is convenient for industrial promotion and application.
[0041] The application of the polymer of the present invention in the preparation of a black matrix not only provides a new polymer option for the black matrix, but also can significantly improve the mechanical and thermal properties of the black matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] FIG1 is the structural formula of the polymer of the present invention;
[0043] FIG2 is a structural reaction formula of an embodiment of the method for preparing a polymer according to the present invention;
[0044] FIG3 is a gel permeation chromatography elution curve of the polymer described in Example 1 of the present invention;
[0045] FIG4 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 1 of the present invention by gel permeation chromatography;
[0046] FIG5 is a gel permeation chromatography elution curve of the polymer described in Example 2 of the present invention;
[0047] FIG6 is a graph showing the statistical results of molecular weight analysis by gel permeation chromatography of the polymer described in Example 2 of the present invention;
[0048] FIG7 is a gel permeation chromatography elution curve of the polymer described in Example 3 of the present invention;
[0049] FIG8 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 3 of the present invention by gel permeation chromatography;
[0050] FIG9 is a gel permeation chromatography elution curve of the polymer described in Example 4 of the present invention;
[0051] FIG10 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 4 of the present invention by gel permeation chromatography;
[0052] FIG11 is a gel permeation chromatography elution curve of the polymer described in Example 5 of the present invention;
[0053] FIG12 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 5 of the present invention by gel permeation chromatography;
[0054] FIG13 is a gel permeation chromatography elution curve of the polymer described in Example 6 of the present invention;
[0055] FIG14 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 6 of the present invention by gel permeation chromatography;
[0056] FIG15 is a gel permeation chromatography elution curve of the polymer described in Example 7 of the present invention;
[0057] FIG16 is a graph showing the statistical results of molecular weight analysis by gel permeation chromatography of the polymer described in Example 7 of the present invention;
[0058] FIG17 is a gel permeation chromatography elution curve of the polymer described in Example 8 of the present invention;
[0059] FIG18 is a graph showing the statistical results of molecular weight analysis of the polymer described in Example 8 of the present invention by gel permeation chromatography;
[0060] FIG19 is a gel permeation chromatography elution curve of the polymer described in Example 9 of the present invention;
[0061] FIG20 is a graph showing the statistical results of molecular weight analysis by gel permeation chromatography of the polymer described in Example 9 of the present invention;
[0062] FIG21 is a gel permeation chromatography elution curve of the polymer described in Example 10 of the present invention;
[0063] FIG22 is a graph showing the statistical results of molecular weight analysis by gel permeation chromatography of the polymer described in Example 10 of the present invention;
[0064] FIG23 is a graph showing the thermal properties test results of the polymer described in Example 1 of the present invention;
[0065] FIG24 is a graph showing the lithographic performance test of the polymer described in Example 1 of the present invention;
[0066] FIG25 is another photolithography performance test graph of the polymer described in Example 1 of the present invention;
[0067] FIG26 is another photolithography performance test graph of the polymer described in Example 1 of the present invention;
[0068] FIG27 is another photolithography performance test graph of the polymer described in Example 1 of the present invention;
[0069] FIG28 is an NMR spectrum of the polymer described in Example 8 of the present invention. DETAILED DESCRIPTION
[0070] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0071] The structural formula of 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone described in the following examples is:
[0072] The 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone is prepared by one of the following two methods:
[0073] (1) In the presence of concentrated sulfuric acid and concentrated nitric acid, 1,8-dihydroxy-9,10-anthraquinone is nitrated to 1,8-dihydroxy-2,4,5,7-tetranitro-9,10-anthraquinone, and then the nitro group is reduced to the amino group to obtain 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone.
[0074] (2) In the presence of concentrated sulfuric acid and concentrated nitric acid, 1,8-dihydroxy-4,5-dinitro-9,10-anthraquinone is nitrated to 1,8-dihydroxy-2,4,5,7-tetranitro-9,10-anthraquinone, and then the nitro group is reduced to the amino group to obtain 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone.
[0075] In the above two methods, any one of them can be used to prepare the 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone described in this application. For details, please refer to the content disclosed in CN202110708909.2. At the same time, the acquisition of the 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone includes but is not limited to the preparation by the above two methods. Those skilled in the art can prepare it by other conventional preparation methods in the prior art or other conventional routes.
[0076] The present invention provides a polymer that can be used for a black matrix, and the structural formula of the polymer is shown in FIG1 .
[0077] The synthesis route of one embodiment of the polymer of the present invention is shown in FIG2 . The preparation method of the polymer specifically comprises the following steps:
[0078] (1) reacting a dianhydride monomer and an esterification reagent in a solvent 1 to obtain a reaction solution; adding an acyl chloride reagent dropwise to the reaction solution under a nitrogen atmosphere and an ice bath to obtain an intermediate after the addition is complete;
[0079] The molar ratio of the dianhydride monomer to the esterification reagent is 1:1 to 1:2;
[0080] The solvent 1 is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran;
[0081] The reaction temperature of the dianhydride monomer and the esterification agent in solvent 1 is 30 to 90° C.;
[0082] The reaction time of the dianhydride monomer and the esterification reagent in solvent 1 is 6-24 hours;
[0083] The temperature of the ice bath condition is 5 to 10°C;
[0084] The molar ratio of the acyl chloride reagent to the dianhydride monomer is 2:1 to 2.5:1;
[0085] The dropping speed of the acyl chloride reagent is 1 to 4 drops per second;
[0086] The acyl chloride reagent is at least one of SOCl2, AlCl3, BF3, SbCl5, FeBr3, FeCl3, SnCl4, TiCl4, and ZnCl2;
[0087] The dianhydride monomer is at least one of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, diphenyl sulfide dianhydride, and bisphenol A diether dianhydride;
[0088] The esterification agent is at least one of n-butanol, ethanol, isopropanol, n-propanol, tert-butanol, and methanol.
[0089] (2) reacting the intermediate obtained in step (1) with a diamine monomer and 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone in solvent 2 to obtain the polymer;
[0090] The molar ratio of the diamine monomer, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate is: diamine monomer: 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone: intermediate = 1:1:2 to 1:1:4;
[0091] The diamine monomers are m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diamino-2,2'-dimethylbiphenyl, 2-(4-aminophenyl)-5-aminobenzoxazole, 2-(4-aminophenyl)-5- At least one of aminobenzimidazole, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-hydroxy-4-aminophenoxy)benzene, 2-(4-aminophenyl)-6-aminobenzoxazole, 2,2-p-phenyl-bis(5-aminobenzoxazole), 2,2'-p-phenyl-bis(6-aminobenzoxazole), 2,2-bis(4-hydroxy-3-aminophenyl)propane, 3,3'-dihydroxybenzidine, and 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid;
[0092] The solvent 2 is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran.
[0093] The structural formula of the intermediate prepared in step (1) above is:
[0094] Where R is H or At least one of .
[0095] The reaction temperature of step (2) is 15-35°C;
[0096] The reaction time of step (2) is 3-8h.
[0097] Example 1
[0098] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0099] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0100] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:4 were added to N,N-dimethylformamide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand and decompose, the upper layer was removed, the resin was broken, replaced with deionized water for soaking, washing, filtering, repeating the process several times, and draining to obtain a solid resin, i.e., the polymer described in this embodiment was obtained.
[0101] The structural formula of the polymer obtained in this embodiment is:
[0102] Example 2
[0103] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0104] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 70°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 6°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0105] (2) 2,2-bis(4-hydroxy-3-aminophenyl)propane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:2 were added to N-methylpyrrolidone and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for soaking, washing, filtering, and the process was repeated several times, and then dried to obtain a solid resin, namely the polymer described in this embodiment.
[0106] The structural formula of the polymer obtained in this embodiment is:
[0107] Example 3
[0108] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0109] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:1 were added to N,N-dimethylacetamide, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 8 hours to obtain a reaction solution; SbCl5 was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of SbCl5 to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2.1:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0110] (2) 1,4-bis(4-aminophenoxy)benzene, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:2 were added to N-methylpyrrolidone and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for soaking, washing, filtering, and the process was repeated several times, and then dried to obtain a solid resin, namely the polymer described in this embodiment.
[0111] The structural formula of the polymer obtained in this embodiment is:
[0112] Example 4
[0113] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0114] (1) 3,3',4,4'-benzophenone tetracarboxylic dianhydride and ethanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 80°C under a nitrogen atmosphere for 8 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in an ice bath at 7°C under a nitrogen atmosphere, with the molar ratio of thionyl chloride to 3,3',4,4'-benzophenone tetracarboxylic dianhydride being 2:1, and the addition was completed at a rate of 1 drop / second to obtain an intermediate;
[0115] (2) 3,3'-dihydroxybenzidine, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:3 were added to dimethyl sulfoxide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and then dried to obtain a solid resin; the polymer described in this embodiment was obtained.
[0116] The structural formula of the polymer obtained in this embodiment is:
[0117] Example 5
[0118] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0119] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-propanol in a molar ratio of 1:2 are added to N,N-dimethylformamide, and reacted in an oil bath at 90°C under a nitrogen atmosphere for 10 hours to obtain a reaction solution; thionyl chloride is added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition is completed at 1 drop / second to obtain an intermediate;
[0120] (2) 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:4 were added to N-methyl-2-pyrrolidone and reacted at 15°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and dried to obtain a solid resin, namely, the polymer described in this embodiment.
[0121] The structural formula of the polymer obtained in this embodiment is:
[0122] Example 6
[0123] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0124] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and methanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 12 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 10°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 4 drops / second to obtain an intermediate.
[0125] (2) 1,4-bis(3-aminophenoxy)benzene, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:4 were added to N-methylpyrrolidone and reacted at 35°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for soaking, washing, filtering, and the process was repeated several times, and then dried to obtain a solid resin, namely the polymer described in this embodiment.
[0126] The structural formula of the polymer obtained in this embodiment is:
[0127] Example 7
[0128] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0129] (1) 3,3,4,4-diphenylsulfone tetracarboxylic acid anhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 70°C under a nitrogen atmosphere for 24 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution under a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3,4,4-diphenylsulfone tetracarboxylic acid anhydride being 2.5:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0130] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:3 were added to N-ethyl-2-pyrrolidone and reacted at 25° C. for 8 h to obtain a reaction product. The obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times. The solid resin was obtained by drying, and the polymer described in this embodiment was obtained.
[0131] The structural formula of the polymer obtained in this embodiment is:
[0132] Example 8
[0133] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0134] (1) 3,3,4,4-diphenylsulfone tetracarboxylic acid dianhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 12 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 6°C, with the molar ratio of thionyl chloride to 3,3,4,4-diphenylsulfone tetracarboxylic acid dianhydride being 2:1, and the addition was completed at a rate of 3 drops / second to obtain an intermediate;
[0135] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:2 were added to N-methylpyrrolidone and reacted at 15° C. for 8 h to obtain a reaction product. The obtained reaction product was uniformly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times. The solid resin was obtained by drying, and the polymer described in this embodiment was obtained.
[0136] The structural formula of the polymer obtained in this embodiment is:
[0137] Example 9
[0138] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0139] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and isopropyl alcohol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 30°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 10°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0140] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:2 were added to N,N-dimethylformamide and reacted at 25°C for 3 hours to obtain a reaction product. The obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times. The solid resin was obtained by drying, and the polymer described in this embodiment was obtained.
[0141] The structural formula of the polymer obtained in this embodiment is:
[0142] Example 10
[0143] An embodiment of the polymer of the present invention, the preparation method of the polymer of this embodiment comprises the following steps:
[0144] (1) Diphenyl sulfide dianhydride and n-butanol in a molar ratio of 1:1 are added to N-methylpyrrolidone, and the mixture is reacted in an oil bath at 80°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride is added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 8°C, with the molar ratio of thionyl chloride to diphenyl sulfide dianhydride being 2:1, at a rate of 1 drop / second, to obtain an intermediate;
[0145] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate in a molar ratio of 1:1:4 were added to N-methylpyrrolidone and reacted at 25° C. for 6 h to obtain a reaction product. The obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times. The solid resin was obtained by drying, and the polymer described in this embodiment was obtained.
[0146] The structural formula of the polymer obtained in this embodiment is:
[0147] Example 11
[0148] Gel Permeation Chromatography (GPC) Test of the Polymer of the Present Invention
[0149] The polymers described in Examples 1 to 10 were used as test subjects, and gel permeation chromatography (GPC) data for each group of polymers was measured. The testing method was as follows: During the experiment, a chromatographic column was filled with a solvent of the sample to be tested, so that it occupied all the spaces between the carrier particles and the cavities within the particles. Then, a sample solution prepared with the same solvent was added from the column head and eluted with the same solvent. The eluate was collected at the micro-end of the chromatographic column, and the volume and concentration of the eluate were calculated. The total volume of the eluate received is called the elution volume. The elution volume of the solute is related to its molecular weight. The larger the molecular weight, the smaller the elution volume. If the sample is polydisperse, a series of fractions with decreasing molecular weight can be collected according to the order of elution.
[0150] The elution curve of the polymer described in Example 1 is shown in FIG3 , and the statistical results of the molecular weight of the polymer are shown in FIG4 .
[0151] The elution curve of the polymer described in Example 2 is shown in FIG5 , and the statistical results of the molecular weight of the polymer are shown in FIG6 .
[0152] The elution curve of the polymer described in Example 3 is shown in FIG7 , and the statistical results of the molecular weight of the polymer are shown in FIG8 .
[0153] The elution curve of the polymer described in Example 4 is shown in FIG9 , and the statistical results of the molecular weight of the polymer are shown in FIG10 .
[0154] The elution curve of the polymer described in Example 5 is shown in FIG11 , and the statistical results of the molecular weight of the polymer are shown in FIG12 .
[0155] The elution curve of the polymer described in Example 6 is shown in FIG13 , and the statistical results of the molecular weight of the polymer are shown in FIG14 .
[0156] The elution curve of the polymer described in Example 7 is shown in FIG15 , and the statistical results of the molecular weight of the polymer are shown in FIG16 .
[0157] The elution curve of the polymer described in Example 8 is shown in FIG17 , and the statistical results of the molecular weight of the polymer are shown in FIG18 .
[0158] The elution curve of the polymer described in Example 9 is shown in FIG19 , and the statistical results of the molecular weight of the polymer are shown in FIG20 .
[0159] The elution curve of the polymer described in Example 10 is shown in FIG21 , and the statistical results of the molecular weight of the polymer are shown in FIG22 .
[0160] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution index (PDI) of the polymers described in Examples 1 to 10 are shown in Table 1 below:
[0161] Table 1 Mw, Mn and PDI test results of the polymers obtained in Examples 1 to 10
[0162] Example 12
[0163] Mechanical and thermal properties test of the polymer described in the present invention
[0164] 1. Mechanical properties of the polymers described in the present invention
[0165] The polymers described in Examples 1 to 10 and the polymers described in Comparative Examples 1 to 4 were used as test objects to test the mechanical properties of the polymers obtained in each group. The polymers described in Comparative Examples 1 to 4 are as follows:
[0166] The preparation method of the polymer described in Comparative Example 1 comprises the following steps:
[0167] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0168] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,4'-diaminodiphenyl ether and the intermediate obtained in step (1) in a molar ratio of 1:1:4 were added to N,N-dimethylformamide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and dried to obtain a solid resin, namely, the polymer described in this comparative example.
[0169] The polymer structural formula of Comparative Example 1 is:
[0170] The preparation method of the polymer described in Comparative Example 2 comprises the following steps:
[0171] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0172] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,4'-diaminodiphenyl ether and the intermediate obtained in step (1) in a molar ratio of 1:1:4 were added to N,N-dimethylformamide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and dried to obtain a solid resin, namely, the polymer described in this comparative example.
[0173] The structural formula of the polymer described in Comparative Example 2 is:
[0174] The preparation method of the polymer described in Comparative Example 3 comprises the following steps:
[0175] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:1.2 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0176] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate obtained in step (1) in a molar ratio of 1:1:4 were added to N,N-dimethylformamide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and dried to obtain a solid resin, namely, the polymer described in this comparative example.
[0177] The structural formula of the polymer described in Comparative Example 3 is:
[0178] The preparation method of the polymer described in Comparative Example 4 comprises the following steps:
[0179] (1) 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride and n-butanol in a molar ratio of 1:1.5 were added to N-methylpyrrolidone, and the mixture was reacted in an oil bath at 60°C under a nitrogen atmosphere for 6 hours to obtain a reaction solution; thionyl chloride was added dropwise to the reaction solution in a nitrogen atmosphere and an ice bath at 5°C, with the molar ratio of thionyl chloride to 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride being 2:1, and the addition was completed at 1 drop / second to obtain an intermediate;
[0180] (2) 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate obtained in step (1) in a molar ratio of 1:1:4 were added to N,N-dimethylformamide and reacted at 25°C for 6 hours to obtain a reaction product; the obtained reaction product was evenly introduced into deionized water, allowed to stand for stratification, the upper layer was removed, the resin was broken, replaced with deionized water for immersion washing, filtered, and the process was repeated several times, and dried to obtain a solid resin, namely, the polymer described in the comparative example.
[0181] The structural formula of the polymer described in Comparative Example 4 is:
[0182] The polymers of Examples 1 to 10 and Comparative Examples 1 to 4 were stirred and mixed with carbon black particles to obtain photoresist solutions. The mechanical properties of each group were then tested. The specific test method was as follows:
[0183] OD value test: Place the black sample under the optical densitometer, adjust to zero first and then measure the OD value. Move the position of the photoresist coating, measure four times and take the average value.
[0184] Tensile properties test:
[0185] CTE Test:
[0186] DMA test:
[0187] The test results are shown in Table 2.
[0188] Table 2 Mechanical test results of the polymers described in Examples 1 to 10
[0189] It can be seen from the results in Table 2 that, compared with Comparative Examples 1 to 4, the polymers described in Examples 1 to 10 of the present invention all have high OD values and good mechanical properties.
[0190] 2. Thermal properties of the polymers described in the present invention
[0191] The polymer described in Example 1 was used as a test object to test its thermal properties. The specific test method is as follows:
[0192] Td test:
[0193] The test results are shown in Figure 23.
[0194] As shown in FIG23 , the polymer of the present invention has good thermal properties.
[0195] The polymers of Examples 2 to 10 have similar thermal properties, which will not be described in detail here.
[0196] Example 12
[0197] Lithographic properties of the polymers of the present invention
[0198] The polymer described in Example 1 was used as the test object to test the lithographic performance of the polymer described in the present invention. The specific testing method is as follows:
[0199] The resulting polymer, dissolution inhibitor, crosslinker, coupling agent, and solvent were stirred and mixed. The completely dissolved mixed solution was filtered to remove insoluble matter and degassed under vacuum to obtain a photoresist solution. The solution was then exposed on a contact lithography machine (Shenzhen Lanxingyu Electronic Technology Co., Ltd., URE-2000 / 35) and developed with alkaline water.
[0200] The test results are shown in Figures 24 to 27.
[0201] As shown in Figures 24 to 27 , the polymer of the present invention has a high-resolution pattern (5 μm).
[0202] The polymers of Examples 2 to 10 have similar lithographic properties, which will not be described in detail here.
[0203] Example 13
[0204] NMR spectrum of the polymer of the present invention
[0205] The polymer described in Example 8 was used as the test object to test the NMR spectrum of the polymer described in the present invention. The specific testing method is: clean the NMR tube, dry the sample and the NMR tube, transfer the sample into the NMR tube (the solution needs to be dissolved before transfer), and test on the machine.
[0206] The test results are shown in Figure 28.
[0207] As shown in FIG28 , the polymer was successfully synthesized.
[0208] Examples 2 to 10 have similar NMR spectra, which will not be described in detail here.
[0209] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A polymer, characterized in that The structural formula of the polymer is: Where R is H or At least one of; n is an integer of 8-40. The method for preparing a polymer according to claim 1, characterized in that the method comprises the following steps: (1) reacting a dianhydride monomer, an esterification agent and an acyl chloride agent in a solvent 1 to obtain an intermediate; (2) reacting the intermediate obtained in step (1) with a diamine monomer and 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone in solvent 2 to obtain the polymer.
2. The method for preparing a polymer according to claim 2, characterized in that: The step (1) comprises: reacting a dianhydride monomer and an esterification agent in a solvent 1 to obtain a reaction solution; and dripping an acyl chloride agent into the reaction solution under a nitrogen atmosphere and an ice bath condition to obtain an intermediate after the dripping is completed.
3. The method for preparing a polymer according to claim 2 or 3, characterized in that: The step (1) satisfies at least one of the following conditions: (1a) the molar ratio of the dianhydride monomer to the esterification agent is 1:1 to 1:2; (1b) the reaction temperature of the dianhydride monomer and the esterification agent in the solvent 1 is 30 to 90° C.; (1c) the reaction time of the dianhydride monomer and the esterification agent in the solvent 1 is 6 to 24 hours; (1d) The temperature of the ice bath condition is 5 to 10°C; (1e) the molar ratio of the acyl chloride reagent to the dianhydride monomer is 2:1 to 2.5:1; (1f) the dropping speed of the acyl chloride reagent is 1 to 4 drops / second; (1g) the solvent 1 is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran; (1h) The acyl chloride reagent is SOCl2, AlCl3, BF3, SbCl5, FeBr3, FeCl3, SnCl4, TiCl4, ZnCl2 At least one of . (1i) The esterification agent is at least one of n-butanol, ethanol, isopropanol, n-propanol, tert-butanol and methanol.
4. The method for preparing a polymer according to claim 2 or 3, characterized in that: The dianhydride monomer is at least one of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, diphenyl sulfide dianhydride, and bisphenol A diether dianhydride.
5. The method for preparing a polymer according to claim 2 or 3, characterized in that: The structural formula of the intermediate is: Where R is H or At least one of .
6. The method for preparing a polymer according to claim 2, characterized in that: In the step (2), the molar ratio of the diamine monomer, 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone and the intermediate is: diamine monomer: 1,8-dihydroxy-2,4,5,7-tetraamino-9,10-anthraquinone: intermediate = 1:1:2 to 1:1:
4.
7. The method for preparing a polymer according to claim 2 or 7, characterized in that: The diamine monomer in step (2) is m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diamino-2,2'-dimethylbiphenyl, 2-(4-aminophenyl)-5-aminobenzoxazole, 2-(4-aminophenyl)-5-aminobenzoxazole, )-5-aminobenzimidazole, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-hydroxy-4-aminophenoxy)benzene, 2-(4-aminophenyl)-6-aminobenzoxazole, 2,2-p-phenyl-bis(5-aminobenzoxazole), 2,2'-p-phenyl-bis(6-aminobenzoxazole), 2,2-bis(4-hydroxy-3-aminophenyl)propane, 3,3'-dihydroxybenzidine, and at least one of 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid.
8. The method for preparing a polymer according to claim 2, characterized in that: The step (2) satisfies at least one of the following conditions: (2a) the solvent 2 is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and tetrahydrofuran; (2b) The reaction temperature of step (2) is 15-35°C; (2c) The reaction time of step (2) is 3-8h.
9. Use of the polymer prepared by the method of claim 1 or any one of claims 2 to 9 in preparing a black matrix.
Citation Information
Patent Citations
Black polyimide film as well as preparation method and application thereof
CN109867786A
Polymer for black matrix, and preparation method and application thereof
CN115232303A
Polymer for black matrix, and preparation method and application thereof
CN116836384A
Photosensitive resin composition and method for preparing heat-resistant resin film
CN1656427A