Preparation method of aqueous flow battery based on bionic amino acid quinone molecules

By attaching biomimetic amino acid modification groups to quinone molecules, the problem of conflicting solubility and ionic conductivity of quinone compounds in aqueous flow batteries is solved, significantly improving the energy density and cycle stability of the battery, and achieving more efficient of energy storage.

CN118782851APending Publication Date: 2024-10-15NANJING UNIV TIANCHANG NEW MATERIALS & ENERGY TECH R&D CENT +6
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411169891.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Quinone compounds have low solubility and conflicting ionic conductivity properties in aqueous flow batteries, which affect the energy density, energy storage capacity, cycle stability and power performance of the battery.

Method used

By attaching artificial bionic amino acid modification groups to quinone molecules to improve their solubility and ionic conductivity, efficient electrolytes are prepared, such as naphthoquinone alanine and anthraquinone cysteine ​​bionic molecules for use in aqueous solutions flow battery.

Benefits of technology

It significantly improves the solubility and ion conductivity of quinone molecules, enhances the energy density, energy storage capacity and cycle stability of the battery, optimizes the ion transmission rate and power performance, and has good biocompatibility and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782851A_ABST
    Figure CN118782851A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aqueous flow battery based on bionic amino acid quinone molecules, and belongs to the technical field of electrochemical energy storage. An artificial bionic amino acid modified group is used as a solubilizing group to be connected to a quinone molecule to form an electrolyte, the electrolyte is used for preparing the aqueous flow battery, the electrolyte of the aqueous flow battery is a naphthoquinone alanine bionic molecule, the electrolyte of the aqueous flow battery is an anthraquinone cysteine bionic molecule, and the electrolyte of the aqueous flow battery is used for preparing the aqueous flow battery. And the electrolyte adopts a 1M KOH aqueous solution as a supporting electrolyte. The amino acid can be used as a solubilizing group to be connected to quinone molecules, so that the solubility and ionic conductivity of the quinone molecules are improved, a new way is provided for technical progress and commercial application in the field of aqueous flow batteries, and sustainable development in the field of energy storage is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical energy storage, and in particular relates to a method for preparing an aqueous liquid flow battery based on bionic amino acid quinone molecules. Background Art

[0002] With the rapid development of renewable energy and the growing demand for energy storage, flow batteries, as an efficient and sustainable energy storage technology, are receiving more and more attention. Among them, aqueous flow batteries stand out for their excellent reliability, safety and environmental friendliness. However, there are still many challenges in the development of aqueous flow batteries, especially the selection and performance optimization of electrolytes, which have become key issues that need to be solved urgently. At present, quinone compounds have been widely studied as electrolytes for aqueous flow batteries. Because quinone compounds have many excellent properties such as high electrochemical activity and structural adjustability, they are regarded as ideal candidates for electrolyte materials. Therefore, in-depth research on quinone compounds and optimization of their performance are expected to open up new paths for the development of aqueous flow batteries.

[0003] However, there are some technical defects and deficiencies in quinone compounds in aqueous flow batteries, which limit their performance in practical applications. First, the solubility of quinone compounds is relatively low, which leads to limited concentration in the electrolyte, which in turn affects the energy density and energy storage capacity of the battery. In addition, due to the limitation of solubility, quinone compounds are prone to solid precipitation or precipitation in the electrolyte, which in turn affects the cycle stability and life of the battery. Secondly, there is a certain contradiction between the solubility of quinone compounds and their ionic conductivity. Generally, increasing the solubility of quinone compounds will reduce their ionic conductivity, thereby affecting the ion transfer rate of the electrolyte and the power performance of the battery. Therefore, how to balance the solubility and ionic conductivity of quinone compounds has become an important issue in aqueous flow batteries;

[0004] In view of these technical defects and shortcomings, a new method is urgently needed to improve the performance of quinone compounds as electrolytes for aqueous flow batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an aqueous liquid flow battery based on bionic amino acid quinone molecules, which can connect amino acids as solubilizing groups to quinone molecules to improve their solubility and ionic conductivity, provide a new way for technological progress and commercial application in the field of aqueous liquid flow batteries, and promote sustainable development in the field of energy storage.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules comprises: attaching artificial biomimetic amino acid modification groups as solubilizing groups to quinone molecules to prepare an electrolyte, and using the electrolyte to prepare an aqueous liquid flow battery.

[0008] Furthermore, the electrolyte of the aqueous liquid flow battery is naphthoquinone alanine biomimetic molecules.

[0009] Furthermore, the preparation steps of the naphthoquinone alanine biomimetic molecule are as follows:

[0010] A1: In a glove box filled with nitrogen, add xylene into a round-bottom flask;

[0011] A2: adding 2,3-dicyanoquinoxaline and 3-aminopropionitrile into the round-bottom flask and dissolving them in the xylene;

[0012] A3: adding potassium tert-butoxide to the round-bottom flask and simultaneously adding a catalyst to obtain a mixture;

[0013] A4: reflux the mixture in step A3 at 100° C. and stir for at least 12 hours to obtain a residual solvent;

[0014] A5: distilling the residual solvent in step A4 to obtain a residue, and purifying the residue by column chromatography to obtain an intermediate product;

[0015] A6: adding the intermediate product in step A5 to a KOH solution, hydrolyzing at 80° C. for 6 hours to obtain a novel solution A, adjusting the pH value of the novel solution A to 6, and then precipitating to obtain a precipitate;

[0016] A7: The precipitate in step A6 is filtered by vacuum filtration, washed with deionized water for several times, and dried under vacuum at 60° C. overnight to obtain the final product to form an electrolyte.

[0017] Furthermore, the water molecule concentration in the glove box is less than 0.1 ppm.

[0018] Furthermore, the electrolyte of the aqueous liquid flow battery is anthraquinone cysteine ​​biomimetic molecule.

[0019] Furthermore, it is characterized in that: the preparation steps of the anthraquinone cysteine ​​biomimetic molecule are:

[0020] B1: Mix carbon tetrachloride and aloe-emodin and add them into a round-bottom flask to obtain a solution;

[0021] B2: heating the solution in step B1 to 65° C., and then dropping phosphorus tribromide into the solution to obtain a mixture;

[0022] B3: The mixture obtained in step B2 was heated at 65° C. for 48 hours and evaporated to obtain a dark yellow solid;

[0023] B4: subjecting the dark yellow solid in step B3 to rapid column chromatography on silica gel, and purifying the dark yellow solid using a mixture of dichloromethane and petroleum ether to obtain an intermediate product of 3-(bromomethyl)-1,8-dihydroxyanthraquinone-9,10-dione;

[0024] B5: mixing the intermediate product in step B4 with cysteine ​​in a NaOH solution to obtain a novel solution B;

[0025] B6: The novel solution B in step B5 is stirred and reacted at 50° C. for 12 hours, and acidified, and the final anthraquinone cysteine ​​derivative is obtained by filtration to form an electrolyte.

[0026] Furthermore, the novel solution B in B6 is acidified by hydrochloric acid.

[0027] Furthermore, the electrolyte solution uses 1M KOH aqueous solution as a supporting electrolyte.

[0028] Beneficial effects of the present invention:

[0029] The present invention connects amino acids as solubilizing groups to quinone molecules, thereby improving their solubility and ion conductivity. This innovative method will provide a new way for technological progress and commercial applications in the field of aqueous flow batteries, and promote sustainable development in the field of energy storage. In the present invention, we use aromatic quinone molecules modified by artificial bionic amino acids as flow battery electrolytes. First, they can significantly improve the solubility of quinone molecules, increase the energy density and energy storage capacity of the battery, and improve the cycle stability. Secondly, by adjusting the balance between solubility and ion conductivity, amino acid-modified quinone molecules can optimize the performance of the electrolyte, improve the ion transfer rate and power performance. In addition, they have good biocompatibility and environmental friendliness, and meet the requirements of green energy storage. Finally, the diversity and adjustability of amino acid-modified aromatic quinone molecules enable them to be customized according to specific needs and adapt to different battery systems. In summary, amino acid bionic quinone molecules provide potential electrolyte materials for the development of flow battery technology and have broad application prospects in the field of energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings are used to provide further explanation of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0031] Figure 1The naphthoquinone alanine derivative of the present invention 1 H NMR spectra;

[0032] Figure 2 The anthraquinone cysteine ​​derivative of the present invention 1 H NMR spectra;

[0033] Figure 3 This is a graph showing the first test result in Example 4 of the present invention;

[0034] Figure 4 This is a graph showing the results of the second test experiment in Example 4 of the present invention;

[0035] Figure 5 This is a graph showing the first test result in Example 5 of the present invention;

[0036] Figure 6 This is a diagram showing the results of the second test experiment in Example 5 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.

[0038] Example 1

[0039] A method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules, comprising an electrolyte, a positive electrode, a negative electrode, an electrolytic cell and a diaphragm. The structure and principle of this part are mature existing technologies and will not be described in detail in this technical solution.

[0040] The core of this technical solution is to attach artificial biomimetic amino acid modification groups as solubilizing groups to quinone molecules to form an electrolyte, and use the electrolyte to prepare aqueous liquid flow batteries. They can significantly improve the solubility of quinone molecules, increase the energy density and energy storage capacity of the battery, and improve the cycle stability; secondly, by adjusting the balance between solubility and ion conductivity, amino acid-modified quinone molecules can optimize the performance of the electrolyte and improve the ion transfer rate and power performance;

[0041] In addition, they have good biocompatibility and environmental friendliness, meeting the requirements of green energy storage. Finally, the diversity and adjustability of amino acid-modified aromatic quinone molecules enable them to be customized according to specific needs and adapt to different battery systems.

[0042] Among them, the electrolyte of the aqueous flow battery is naphthoquinone alanine biomimetic molecule;

[0043] The preparation steps of the naphthoquinone alanine biomimetic molecule are as follows:

[0044] A1: In a glove box filled with nitrogen, the water molecule concentration in the glove box is less than 0.1 ppm to reduce the impact on the preparation, 50 mL of xylene is placed in a 100 mL round-bottom flask;

[0045] A2: 2.27 g, 10 mmol, of 2,3-dicyanoquinoxaline and 1.40 g, 20 mmol, of 3-aminopropionitrile were added to a round-bottom flask and dissolved in xylene which was pre-dried by passing through a molecular sieve;

[0046] A3: Add 2.24 g (20 mmol) of potassium tert-butoxide to a round-bottom flask and simultaneously add a catalyst to obtain a mixture;

[0047] The catalyst may be selected from 183.2 mg, 0.2 mmol of Pd2(dba)3 and 231 mg, 0.4 mmol of 4,5-bis(diphenylphosphine)-9,9-dimethylxanthene ligand;

[0048] A4: reflux the mixture in step A3 at 100° C. and stir for at least 12 hours to obtain a residual solvent;

[0049] A5: distilling the residual solvent in step A4 to obtain a residue, and purifying the residue by column chromatography to obtain an intermediate product;

[0050] Wherein, during purification, a mixture of 5% ethyl acetate / dichloromethane can be used;

[0051] A6: adding the intermediate product in step A5 to 100 mL of 1.0 M KOH solution, hydrolyzing at 80° C. for 6 hours to obtain a novel solution A, adjusting the pH value of the novel solution A to 6, and then precipitating to obtain a precipitate;

[0052] A7: The precipitate in step A6 is filtered by vacuum filtration, washed several times with deionized water, and dried overnight under vacuum at 60° C. to obtain a final product to form an electrolyte;

[0053] The naphthoquinone alanine biomimetic molecule synthesized in this application has a kinetic energy of 23.70 Ah L at a concentration of 0.5 M. -1 (1.0M transferable electrons) capacity, 264mW cm -2 High output power density at 80mA cm -2 The capacity retention rate after more than 500 cycles is 94.3% (the corresponding capacity decay rate is 0.39% day -1 ), which is highly competitive in aqueous flow batteries based on naphthoquinone derivatives.

[0054] like Figure 1 As shown, the 1H NMR spectrum (400 MHz, 1 M KOH heavy aqueous solution) of the naphthoquinone alanine derivative can prove that alanine is successfully grafted onto the naphthoquinone compound through nuclear magnetic hydrogen spectrum.

[0055] Embodiment 2:

[0056] The difference between this embodiment and embodiment 1 is only the different selection of quinone molecules, as follows:

[0057] The electrolyte of the aqueous flow battery is anthraquinone cysteine ​​biomimetic molecule;

[0058] The preparation steps of the anthraquinone cysteine ​​biomimetic molecule are as follows:

[0059] B1: 150 mL of carbon tetrachloride and 1.35 g, 5 mmol of aloe-emodin were mixed and added into a round-bottom flask to obtain a solution;

[0060] B2: Heat the solution in step B1 to 65° C., and then drop 5 mL of phosphorus tribromide into the solution to obtain a mixture;

[0061] B3: The mixture obtained in step B2 was heated at 65° C. for 48 hours and evaporated to obtain a dark yellow solid;

[0062] B4: The dark yellow solid in step B3 is subjected to flash column chromatography on silica gel, and the dark yellow solid is purified using a mixture of dichloromethane and petroleum ether to obtain an intermediate product of 3-bromomethyl-1,8-dihydroxyanthraquinone-9,10-dione;

[0063] The volume ratio of dichloromethane to petroleum ether is 2:1, and the obtained 3-bromomethyl-1,8-dihydroxyanthraquinone-9,10-dione is 1.23 g, accounting for 72% of the total mass;

[0064] B5: mixing the intermediate product in step B4 with cysteine ​​in a 1.0 M NaOH solution to obtain a novel solution B;

[0065] B6: stirring the novel solution B in step B5 at 50° C. for 12 hours, acidifying with hydrochloric acid, filtering to obtain the final anthraquinone cysteine ​​derivative, and preparing an electrolyte;

[0066] The initial capacity of the anthraquinone cysteine ​​biomimetic molecule synthesized in this application at a concentration of 0.5 M is 23.78 Ah L -1 (88.73% of theoretical capacity), after 800 cycles (19.1 days), the capacity loss was about 0.252% (remaining capacity was 23.72Ah L-1 ), the decay rate per cycle is about 0.00031% (equivalent to a decay rate of 0.013% per day), which indicates that the anthraquinone cysteine ​​derivative has good electrochemical stability;

[0067] like Figure 2 As shown, the 1HNMR spectrum (400 MHz, 1 M KOH heavy aqueous solution) of the anthraquinone cysteine ​​derivative proves that cysteine ​​is successfully grafted onto the anthraquinone compound through hydrogen nuclear magnetic spectrum.

[0068] Embodiment 3:

[0069] In order to ensure the accuracy and effect of the technical solution, in the technical solution, all electrolytes use 1M KOH aqueous solution as the supporting electrolyte, the electrolyte concentration of the low-concentration battery system is 0.1M, and the electrolyte concentration of the high-concentration battery system is 0.5M.

[0070] Embodiment 4:

[0071] This example is based on Example 1 and Example 2, and tests are performed on the physical and chemical properties of the electrolyte. Please refer to the attached Figure 3-4 As shown, the details are as follows:

[0072] Test 1: Redox performance test, using a standard three-electrode device to perform cyclic voltammetric analysis on the redox properties of the electrolyte, in which a 50 mm diameter glassy carbon electrode was selected as the working electrode, a platinum wire electrode as the counter electrode, and a saturated Ag / AgCl electrode as the reference electrode.

[0073] Test 2: Transmembrane permeation test of electrolyte. The static diffusion method is used to test the transmembrane permeation degree of electrolyte. The test device is divided into two equal-volume electrode chambers (raw material side and receiving side), separated by a cation exchange membrane. During the test, the solutions in the two electrode chambers are continuously stirred to make the concentration of the solutions inside each electrode chamber the same. The raw material side solution is 0.5M electrolyte dissolved in 1M KOH aqueous solution, and the receiving side is the same volume of 1M KOH aqueous solution. After one month, the concentration of the electrolyte in the receiving side solution is tested, and the characteristic peak intensity is tested using a UV-visible spectrophotometer.

[0074] Test three: Solubility test of quinone amino acid derivatives. At room temperature, the quinone amino acid derivatives were dissolved in 1M KOH solution, stirred and ultrasonically treated, and electrolytes were continuously added to the solution until a precipitate was formed in the solution to obtain a saturated solution of the electrolyte. The saturated solution was diluted a certain multiple, and the concentration of the electrolyte in the diluted solution was tested by an ultraviolet spectrophotometer, and then the solubility of the corresponding quinone amino acid derivative was calculated based on the dilution multiple.

[0075] Test 4: Diffusion coefficient test: a standard three-electrode apparatus was used to perform cyclic voltammetry tests on the electrolyte at different scan rates, and the Randles-Sevcik equation was used to calculate its diffusion coefficient.

[0076] Please see attached Figure 3 , a) CV curves of 1.0 mM naphthoquinone amino acid biomimetic molecules (3-AFNQ) and K4Fe(CN)6 dissolved in 1.0 M KOH solution respectively; b) SPEEK membrane permeability test of 3-AFNQ solution; c) UV-visible absorption curves of 3-AFNQ solutions with different concentrations in 1 M KOH; d) Absorbance and concentration fitting diagram of the corresponding 3-AFNQ solution at λ468 nm wavelength; e) CV curves of 1 mM 3-AFNQ at different scan rates in 1.0 M KOH solution; f) Corresponding oxidation and reduction peak currents (mA cm -2 ) and (V s -1 ) 1 / 2 relationship;

[0077] In 1.0 M KOH solution, cyclic voltammetry (CV) analysis revealed that the potential of 3-AFNQ was -0.41 V (relative to the standard hydrogen electrode), the difference between the oxidation peak and the reduction peak was 113 mV, and its permeability to the SPEEK membrane was 1.34 × 10 -11 cm 2 s -1 , solubility is 0.53M, diffusion coefficient is 2.32×10 -6 cm 2 s -1 The current density is linearly related to the square root of the scan rate. When combined with K4Fe(CN)6, the system can produce a cell voltage of 0.92V.

[0078] Please see attached Figure 4 , a) CV curves of 1.0 mM anthraquinone cysteine ​​biomimetic molecule (Cys-AQ) and Aloe emodin dissolved in 1.0 M KOH solution respectively; b) Permeability test of Nafion 212 membrane to Cys-AQ solution; c) UV-visible absorption curves of Cys-AQ solutions with different concentrations in 1 M KOH; d) Absorbance and concentration fitting diagram of the corresponding Cys-AQ solution at λ504 nm wavelength; e) CV curves of 1 mM Cys-AQ at different scan rates in 1.0 M KOH solution; f) Corresponding oxidation and reduction peak currents (mA cm -2 ) and (V s -1 ) 1 / 2 relationship.

[0079] Under alkaline conditions (pH 14), Cys-AE exhibited a redox potential of -0.51 V, and the difference between the oxidation peak and the reduction peak was 69 mV, which was 60 mV higher than that of aloe-emodin, indicating that the electron-donating ability of the cysteine ​​side chain was weak. The solubility of Cys-AE was 0.78 M, and the permeability through the Nafion-212 membrane was extremely low. Cyclic voltammetry analysis at different scan rates showed that the diffusion coefficient of Cys-AE was 2.78 × 10-6 cm 2 s -1 , which is similar to most anthraquinone derivatives, proving that it has good electrochemical properties and stability.

[0080] Embodiment 5:

[0081] This example tests the energy storage performance of aqueous flow batteries based on Example 1 and Example 2. Figure 5-6 As shown, the details are as follows:

[0082] The battery performance test was carried out using the LAND CT2001A battery test system and a standard flow battery module. 2 The cation exchange membrane separates the cathode and anode electrolytes. The reaction area is based on the area of ​​the graphite felt electrode (5 cm 2 The electrolyte was pumped through a peristaltic pump (BT100-2J) at a rate of 70 mL min -1 The flow rate circulates between the battery and the tank.

[0083] Test 1: Battery constant current charge and discharge test, using LAND CT2001A battery test system to test different batteries at 50 and 80 mA cm -2 Constant current charge and discharge test under current density;

[0084] Test 1: Battery rate performance test, using LAND CT2001A battery test system to test the battery at 20, 50, 80, and 120 mA cm -2 Constant current charge and discharge rate test under current density;

[0085] Test 1: Battery constant current charge and discharge stability test, using LAND CT2001A battery test system to test different batteries at 50 and 80 mA cm -2 Constant current charge and discharge test at current density.

[0086] Please see attached Figure 5 , a) 0.1 M 3-AFNQ||K4Fe(CN)6 aqueous flow battery at current densities of 20, 50, 80 and 120 mA cm -2Electrostatic charge-discharge curves at different current densities; b) Discharge capacity, Coulomb efficiency, and energy efficiency of 0.1M 3-AFNQ||K4Fe(CN)6 aqueous flow battery at different current densities; c) Discharge capacity, Coulomb efficiency, and energy efficiency of 0.1M 3-AFNQ||K4Fe(CN)6 aqueous flow battery at a current density of 80 mA cm -2 Cycling performance of 0.5M 3-AFNQ||K4Fe(CN)6 aqueous flow battery at a current density of 80 mA cm -2 Cycle performance when

[0087] At 0.1 M 3-AFNQ concentration, 3-AFNQ||K4Fe(CN)6 aqueous organic flow battery has a high conductivity at 20 mA cm -2 The discharge capacity at the current density is 5.32Ah L -1 , close to 99.2% of the theoretical capacity. The coulombic efficiency at different current densities is close to 100%, and the capacity retention rate is 98.24% after 1300 cycles, showing excellent cycle stability. Although the capacity decay of each cycle of the high concentration (0.5M) battery is slightly higher, its overall decay rate is lower, indicating that the cycle life of 3-AFNQ is greatly affected by the concentration and number of cycles, while the test duration has little effect on it.

[0088] Please see attached Figure 6 a) Polarization curves of 0.1M Cys-AQ||K4Fe(CN)6 aqueous flow battery at different charge states; b) Discharge capacity, Coulomb efficiency and energy efficiency of 0.1M Cys-AQ||K4Fe(CN)6 aqueous flow battery at different current densities; c) Discharge capacity, Coulomb efficiency and energy efficiency of 0.1M Cys-AQ||K4Fe(CN)6 aqueous flow battery at a current density of 80 mA cm -2 Cycling performance of 0.5 M Cys-AQ||K4Fe(CN)6 aqueous flow battery at a current density of 80 mA cm -2 Cycle performance.

[0089] At 100% charge and discharge state, the power density of 0.1 M Cys-AE||K4Fe(CN)6AORFB is 113 mW cm -2 , discharge capacity at 20 and 100 mA cm -2 The following are 5.21 and 4.82Ah L -1, and the capacity utilization rates were 97.0% and 89.9%, respectively. After 1090 cycles, the capacity retention rate was 99.8%, the Coulombic efficiency was close to 100%, and the average energy efficiency was 78%. Further testing showed that Cys-AE had excellent electrochemical stability at 100% SOC conditions and extremely low capacity decay rate. 0.5M Cys-AE||K4Fe(CN)6AORFB showed an extremely low capacity decay rate of only 0.00031% / cycle in 800 cycles, showing excellent long-term cycle performance.

[0090] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.

Claims

1. A method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules, characterized in that: Artificial biomimetic amino acid modification groups are connected to quinone molecules as solubilizing groups to form an electrolyte, and an aqueous liquid flow battery is prepared using the electrolyte.

2. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 1, characterized in that: The electrolyte of the aqueous liquid flow battery is naphthoquinone alanine biomimetic molecule.

3. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 2, characterized in that: The preparation steps of the naphthoquinone alanine biomimetic molecule are as follows: A1: In a glove box filled with nitrogen, add xylene into a round-bottom flask; A2: adding 2,3-dicyanoquinoxaline and 3-aminopropionitrile into the round-bottom flask and dissolving them in the xylene; A3: adding potassium tert-butoxide to the round-bottom flask and simultaneously adding a catalyst to obtain a mixture; A4: reflux the mixture in step A3 at 100° C. and stir for at least 12 hours to obtain a residual solvent; A5: distilling the residual solvent in step A4 to obtain a residue, and purifying the residue by column chromatography to obtain an intermediate product; A6: adding the intermediate product in step A5 to a KOH solution, hydrolyzing at 80° C. for 6 hours to obtain a novel solution A, adjusting the pH value of the novel solution A to 6, and then precipitating to obtain a precipitate; A7: The precipitate in step A6 is filtered by vacuum filtration, washed with deionized water for several times, and dried under vacuum at 60° C. overnight to obtain the final product to form an electrolyte.

4. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 3, characterized in that: The water molecule concentration in the glove box is less than 0.1 ppm.

5. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 1, characterized in that: The electrolyte of the aqueous liquid flow battery is anthraquinone cysteine ​​biomimetic molecule.

6. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 5, characterized in that: The preparation steps of the anthraquinone cysteine ​​biomimetic molecule are as follows: B1: Mix carbon tetrachloride and aloe-emodin and add them into a round-bottom flask to obtain a solution; B2: heating the solution in step B1 to 65° C., and then dropping phosphorus tribromide into the solution to obtain a mixture; B3: The mixture obtained in step B2 was heated at 65° C. for 48 hours and evaporated to obtain a dark yellow solid; B4: subjecting the dark yellow solid in step B3 to rapid column chromatography on silica gel, and purifying the dark yellow solid using a mixture of dichloromethane and petroleum ether to obtain an intermediate product of 3-bromomethyl-1,8-dihydroxyanthraquinone-9,10-dione; B5: mixing the intermediate product in step B4 with cysteine ​​in a NaOH solution to obtain a novel solution B; B6: The novel solution B in step B5 is stirred and reacted at 50° C. for 12 hours, and acidified, and the final anthraquinone cysteine ​​derivative is obtained by filtration to form an electrolyte.

7. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 6, characterized in that: The novel solution B in B6 is acidified by hydrochloric acid.

8. The method for preparing an aqueous liquid flow battery based on biomimetic amino acid quinone molecules according to claim 1, characterized in that: The electrolyte uses 1M KOH aqueous solution as a supporting electrolyte.

Citation Information

Cited By

  • Device and method for measuring solubility of carbon dioxide in formation water

    CN116482159A

  • An apparatus and method for determining the solubility of carbon dioxide in formation water

    CN116482159B