Calcified roasted clinker acid leaching process control method

By dividing the leaching agent into two parts for use in the acid leaching process of calcified roasted clinker, the problem of vanadium loss caused by excessive local acidity during the acid leaching process of vanadium slag is solved, and the rapid leaching of vanadium and the stability of the vanadium extraction tailings are achieved Improved performance and reduced risk of sulfuric acid consumption and high temperatures.

WO2024212986A1PCT designated stage expired Publication Date: 2024-10-17PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/086953
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

During the acid leaching process of calcified roasting clinker, the local acidity of vanadium slag is too high, which causes vanadium to easily hydrolyze and precipitate, resulting in losses and large fluctuations in the TV content of vanadium extraction tailings.

Method used

Divide the leaching agent into two parts, one part is used to mix with the calcified roasted clinker to prepare clinker slurry, and the other part is used to dilute the concentrated sulfuric acid, and perform the leaching reaction by controlling the pH value between 2.5 and 3.5 to avoid excessive local acidity. problem.

Benefits of technology

It achieves rapid leaching of vanadium, reduces sulfuric acid consumption, improves the stability of vanadium extraction tailings and the vanadium concentration of the leachate, and avoids the problems of high local acidity and high temperature caused by directly adding concentrated sulfuric acid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086953_17102024_PF_FP_ABST
    Figure CN2024086953_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention is a calcified roasted clinker acid leaching process control method. A leaching agent is divided into two parts, wherein one part is used for mixing with a calcified roasted clinker to prepare a clinker slurry, and the other part is used for diluting concentrated sulfuric acid. The calcified roasted clinker acid leaching process control method provided in the present invention is low cost, and is easy and convenient to operate. The leaching agent is divided into two parts for use, wherein one part is used for clinker pulping, and the other part is used for diluting concentrated sulfuric acid used for leaching; and the leaching agent containing sulfuric acid is then added to the clinker slurry, such that the liquid-solid ratio of the slurry is increased, and vanadium is also rapidly leached, thereby avoiding the problems of high local acidity, high temperature, high impurity content, etc. caused by the direct addition of concentrated sulfuric acid.
Need to check novelty before this filing date? Find Prior Art

Description

A method for controlling the acid leaching process of calcined roasted clinker Technical Field

[0001] The invention relates to the technical field of vanadium hydrometallurgy, and in particular to a method for controlling a calcified roasted clinker acid leaching process. Background Art

[0002] Vanadium, a key microalloying element, is widely used in metallurgy, chemical engineering, aerospace, and other fields. It significantly improves the strength, toughness, and ductility of steel, providing crucial support for ensuring the quality of key national projects. Vanadium-titanium magnetite is treated in a blast furnace or electric furnace at high temperatures to produce vanadium-containing molten iron. This molten iron is selectively oxidized to produce vanadium slag, which is then used as a raw material for vanadium extraction. In the vanadium oxide production process, calcination, roasting, and acid leaching of vanadium-containing materials is a typical vanadium extraction process.

[0003] After calcination and roasting, vanadium exists as pentavalent vanadium in vanadium slag. By adding sulfuric acid to control the leaching pH to 2.8-3.5, vanadium can be dissolved into the solution. Approximately 80% or more of the vanadium leaching reaction occurs within the first 15 minutes, requiring significant sulfuric acid consumption. In actual production, excessive acidity often occurs locally due to rapid or uneven addition of sulfuric acid. Due to the vanadium's existing form, when the leachate pH is low and the pentavalent vanadium concentration is high, the solution system is unstable, and vanadium is easily hydrolyzed and precipitated, resulting in losses. Consequently, the TV content of industrially produced vanadium tailings fluctuates widely, ranging from 1.0% to 1.7%.

[0004] In summary, the problem of excessive local acidity and easy loss of vanadium during the acid leaching of calcined roasted clinker has become a technical problem that needs to be urgently solved by those skilled in the art.

[0005] Based on this, the existing technology still needs to be improved.

[0006] Summary of the Invention

[0007] To solve the above technical problems, an embodiment of the present invention provides a method for controlling the acid leaching process of calcined roasted clinker, so as to solve the technical problem caused by excessive local acidity in the acid leaching process of calcined roasted clinker in the prior art.

[0008] To solve the above technical problems, some embodiments of the present invention disclose a method for controlling the acid leaching process of calcined roasted clinker, in which the leaching agent is divided into two parts, one part is used to mix with the calcined roasted clinker to prepare clinker slurry, and the other part is used to dilute concentrated sulfuric acid.

[0009] Further, including:

[0010] Step 1: mixing the calcified roasted clinker with a first leaching agent to obtain a clinker slurry;

[0011] Step 2: Mixing concentrated sulfuric acid with a second leaching agent to obtain a first solution;

[0012] Step 3: uniformly adding the first solution to the clinker slurry to obtain a third solution;

[0013] Step 4: Controlling the pH value of the third solution to be between 2.5 and 3.5, performing a leaching reaction, and then performing solid-liquid separation to obtain a vanadium-containing leaching solution and vanadium-extracting tailings.

[0014] Furthermore, in step 2, the amount of concentrated sulfuric acid used is 0.6-0.8 times the total amount of concentrated sulfuric acid consumed in the calcification roasted clinker leaching process.

[0015] Furthermore, in step 1, the mass ratio of the calcified roasted clinker to the first leaching agent is 1:1-2.

[0016] Furthermore, in step 1, the first leaching agent is water, recycled water from wastewater treatment or a vanadium-containing solution.

[0017] Furthermore, in step 2, the second leaching agent is water or recycled water from wastewater treatment.

[0018] Furthermore, in step three, the time for adding the first solution into the clinker slurry at a uniform speed is more than 15 minutes.

[0019] Furthermore, the first solution is added to the clinker slurry at a uniform speed for 15 to 25 minutes.

[0020] Furthermore, the liquid-solid mass ratio of the third solution is (2-10):1;

[0021] Preferably, the liquid-to-solid mass ratio of the third solution is (2-4):1.

[0022] Furthermore, the vanadium-containing solution includes a washing solution of vanadium-extracting tailings.

[0023] By adopting the above technical solution, the present invention has at least the following beneficial effects:

[0024] The present invention provides a method for controlling the acid leaching process of calcined roasted clinker, which is low in cost and easy to operate. The method divides a leaching agent into two parts, one for clinker beating and the other for diluting with concentrated sulfuric acid for leaching. The leaching agent containing sulfuric acid is then added to the clinker slurry, thereby increasing the liquid-to-solid ratio of the slurry and achieving rapid leaching of vanadium. The method avoids problems such as high local acidity, high temperature, and high impurity content caused by directly adding concentrated sulfuric acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] FIG1 is a flow chart of a method for controlling a calcified roasted clinker acid leaching process according to some embodiments of the present invention. DETAILED DESCRIPTION

[0027] The following embodiments of the present disclosure are further described in detail with reference to the accompanying drawings and examples. The detailed description of the following examples and the accompanying drawings are intended to illustrate the principles of the present disclosure, but are not intended to limit the scope of the present disclosure. The present disclosure can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but rather includes all technical solutions within the scope of the claims.

[0028] The present disclosure provides these embodiments in order to make this disclosure thorough and complete, and to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that: unless otherwise specifically stated, the relative arrangement of parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as merely exemplary, and not as limiting.

[0029] It should be noted that, in the description of this disclosure, unless otherwise specified, "plurality" means greater than or equal to two; terms such as "upper," "lower," "left," "right," "inner," and "outer" indicating directions or positional relationships are intended solely to facilitate and simplify the description of this disclosure, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on this disclosure. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0030] In addition, the terms "first," "second," and similar terms used in this disclosure do not denote any order, quantity, or importance, but are merely used to distinguish different parts. "Perpendicular" does not mean perpendicular in the strict sense, but rather means within the tolerance range. "Parallel" does not mean parallel in the strict sense, but rather means within the tolerance range. "Include" or "comprising" and similar terms mean that the elements preceding the term include the elements listed after the term, and do not exclude the possibility of also including other elements.

[0031] It should also be noted that, in the description of this disclosure, unless otherwise expressly specified or limited, the terms "installed," "connected," and "connected" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to direct connections or indirect connections through an intermediary. Those skilled in the art will understand the specific meanings of the above terms in this disclosure depending on the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intervening device between the specific device and the first or second device.

[0032] All terms used in this disclosure have the same meaning as understood by one of ordinary skill in the art to which this disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in, for example, common dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and should not be interpreted in an idealized or highly formal sense, unless explicitly defined as such herein.

[0033] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0034] As shown in Figure 1, some embodiments of the present invention disclose a method for controlling the acid leaching process of calcined roasted clinker. The method divides the leaching agent into two parts: one part is used to mix with the calcined roasted clinker to prepare a clinker slurry, and the other part is used to dilute concentrated sulfuric acid. Specifically, the control process may include the following steps:

[0035] Step 1: Mixing the calcified roasted clinker with a first leaching agent to obtain a clinker slurry; wherein the mass ratio of the calcified roasted clinker to the first leaching agent is preferably 1:1-2. The first leaching agent can be water, wastewater treatment recycled water or a vanadium-containing solution. The vanadium-containing solution can include but is not limited to the washing liquid of vanadium extraction tailings, or it can be a vanadium-containing leaching solvent, that is, a washing filtrate obtained after filtration and washing after acid leaching. The leaching solvent during the first acid leaching can be industrial water. After filtration and washing, a vanadium-containing leaching solvent can be obtained for use in the next leaching cycle. The washing filtrate can be used as a vanadium-containing leaching solvent.

[0036] Step 2: Mixing concentrated sulfuric acid with a second leaching agent to obtain a first solution; wherein the amount of concentrated sulfuric acid used is preferably 0.6-0.8 times the total amount of concentrated sulfuric acid consumed in the calcined roasted clinker leaching process. The second leaching agent can be water or recycled water from wastewater treatment.

[0037] Step 3: Under stirring, the first solution is uniformly added to the clinker slurry to obtain a third solution; wherein, the time for uniformly adding the first solution to the clinker slurry is preferably controlled to be more than 15 minutes. If the time is too short, it is easy to cause excessive local acidity, thereby causing the solution system to be unstable, and vanadium is easily hydrolyzed and precipitated to cause loss. Furthermore, the time for uniformly adding the first solution to the clinker slurry can be controlled to be 15 to 25 minutes. The liquid-to-solid mass ratio of the third solution is preferably (2 to 10): 1, preferably (2-4): 1.

[0038] Step 4: Control the pH of the third solution to between 2.5 and 3.5, perform a leaching reaction, and then perform solid-liquid separation to obtain a vanadium-containing leachate and vanadium-extracted tailings. In this step, the pH value can be controlled using dilute sulfuric acid, the concentration of which can be controlled to be approximately 50%.

[0039] In the embodiment of the present invention, the leaching agent is divided into two parts for use: one part is used for clinker beating, and the other part is used for dilution with concentrated sulfuric acid for leaching. The leaching agent containing sulfuric acid is then added to the clinker slurry, thereby improving the liquid-to-solid ratio of the slurry and achieving rapid leaching of vanadium, avoiding problems such as high local acidity, high temperature, and high impurity content caused by directly adding concentrated sulfuric acid.

[0040] The technical solution of the present application is further described in detail below through examples.

[0041] Comparative Example 1:

[0042] 100g of calcified roasted clinker (V = 7.07%, P = 0.066%) was added to 250mL of water. The mixture was stirred and the pH was adjusted to 3.0 with 50% dilute sulfuric acid. The reaction was continued for 60 minutes, followed by solid-liquid separation. This yielded a leachate (V = 23.82g / L, P = 0.03g / L) and a vanadium-extraction tailing (V = 1.14%). The sulfuric acid consumption during the leaching process was equivalent to 5.5mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 84.84%.

[0043] Example 1:

[0044] (1) Take 100 g of calcinated roasted clinker (TV = 7.07%, P = 0.066%), add 100 mL of water, and stir evenly to obtain clinker slurry A;

[0045] (2) Take 3.3 mL of concentrated sulfuric acid, add it to 150 mL of water, and stir evenly to obtain solution B;

[0046] (3) Solution B was added to the clinker slurry A at a uniform rate over a 15-min period to obtain slurry C, where the liquid-to-solid ratio of slurry C was 2.53:1.

[0047] (4) The pH of slurry C was controlled to 3.0 using 50% by mass dilute sulfuric acid. After leaching for 40 minutes, solid-liquid separation was performed to obtain a vanadium-containing leachate (V = 24.22 g / L, P = 0.018 g / L) and vanadium-extracting tailings (TV = 1.05%).

[0048] The sulfuric acid consumption during the leaching process was equivalent to 5.2 mL of concentrated sulfuric acid, and the vanadium dissolution rate was 86.03%.

[0049] Generally, the liquid-to-solid ratio of Slurry C should be controlled between 2:1 and 4:1, primarily to produce a vanadium-containing leachate with a high vanadium concentration (V > 20 g / L) to facilitate subsequent precipitation of vanadium oxide products. This liquid-to-solid ratio is an optimal value selected for practical production when the calcified clinker has a TV of 6-10%. Theoretically, this liquid-to-solid ratio can be increased to above 10:1, but the resulting vanadium concentration will be less than 10 g / L.

[0050] Comparative Example 2:

[0051] 100g of calcified roasted clinker (TV=8.54%, P=0.058%) was added to 300mL of a vanadium-containing solution (V=3.15g / L). The solution was stirred and the pH was adjusted to 2.8 with 50% dilute sulfuric acid. The reaction was continued for 80 minutes, followed by solid-liquid separation. This yielded a leachate (V=28.31g / L, P=0.028g / L) and a vanadium-extraction tailing (TV=1.08%). The sulfuric acid consumption during the leaching process was equivalent to 6.7mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 88.24%.

[0052] Example 2:

[0053] (1) 100 g of calcified roasted clinker (TV = 8.54%, P = 0.058%) was added with 100 mL of vanadium-containing solution (V = 3.15 g / L) and stirred evenly to obtain clinker slurry A;

[0054] (2) Take 5.4 mL of concentrated sulfuric acid, add it to 200 mL of water, and stir evenly to obtain solution B;

[0055] (3) Solution B was added to the clinker slurry A at a uniform rate over a period of 25 min to obtain slurry C, where the liquid-to-solid ratio of slurry C was 3.05:1.

[0056] (4) The pH of slurry C was controlled to 2.8 using 50% by mass dilute sulfuric acid, and the leaching reaction was carried out for 60 minutes. After solid-liquid separation, vanadium-containing leaching solution (V = 28.61 g / L, P = 0.020 g / L) and vanadium-extracting tailings (TV = 0.96%) were obtained.

[0057] The sulfuric acid consumption during the leaching process was equivalent to 6.6 mL of concentrated sulfuric acid, and the vanadium dissolution rate was 89.43%.

[0058] Comparative Example 3:

[0059] 100g of calcified roasted clinker (TV=8.54%, P=0.058%) was added to 400mL of recycled wastewater (V=0.1g / L). The mixture was stirred and the pH was adjusted to 2.5 with 50% dilute sulfuric acid. The reaction was continued for 80 minutes, followed by solid-liquid separation. This yielded a leachate (V=18.57g / L, P=0.035g / L) and a vanadium-extraction tailing (TV=1.21%). The sulfuric acid consumption during the leaching process was equivalent to 7.1mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 86.96%.

[0060] Example 3:

[0061] (1) 100 g of calcified roasted clinker (TV = 8.54%, P = 0.058%) was added to 200 mL of wastewater treatment recycled water (V = 0.1 g / L), and stirred evenly to obtain clinker slurry A;

[0062] (2) Take 5.5 mL of concentrated sulfuric acid, add it to 200 mL of water, and stir evenly to obtain solution B;

[0063] (3) Solution B was added to the clinker slurry A at a uniform rate over a period of 25 min to obtain slurry C, where the liquid-to-solid ratio of slurry C was 4.05:1.

[0064] (4) The pH of slurry C was controlled to 2.5 using 50% by mass dilute sulfuric acid, and the leaching reaction was carried out for 40 minutes. After solid-liquid separation, vanadium-containing leaching solution (V = 19.28 / L, P = 0.021 g / L) and vanadium-extracting tailings (TV = 0.91%) were obtained.

[0065] The sulfuric acid consumption during the leaching process was equivalent to 6.8 mL of concentrated sulfuric acid, and the vanadium dissolution rate was 90.19%.

[0066] Comparative Example 4:

[0067] 100g of calcified roasted clinker (TV=8.54%, P=0.058%) was added to 600mL of a vanadium-containing solution (V=3.15g / L). The solution was stirred and the pH was adjusted to 2.8 with 50% dilute sulfuric acid. The reaction was continued for 80 minutes, followed by solid-liquid separation. This yielded a leachate (V=15.70g / L, P=0.021g / L) and a vanadium-extraction tailing (TV=1.06%). The sulfuric acid consumption during the leaching process was equivalent to 7.2mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 88.52%.

[0068] Example 4:

[0069] (1) 100 g of calcified roasted clinker (TV = 8.54%, P = 0.058%) was added with 200 mL of vanadium-containing solution (V = 3.15 g / L) and stirred evenly to obtain clinker slurry A;

[0070] (2) Take 5.8 mL of concentrated sulfuric acid, add it to 400 mL of water, and stir evenly to obtain solution B;

[0071] (3) Solution B was added to the clinker slurry A at a uniform rate over a period of 25 min to obtain slurry C, where the liquid-to-solid ratio of slurry C was 6.06:1.

[0072] (4) The pH of slurry C was controlled to 2.8 using 50% by mass dilute sulfuric acid, and the leaching reaction was carried out for 60 minutes. After solid-liquid separation, vanadium-containing leaching solution (V = 15.17 g / L, P = 0.020 g / L) and vanadium-extracting tailings (TV = 0.93%) were obtained.

[0073] The sulfuric acid consumption during the leaching process was equivalent to 6.8 mL of concentrated sulfuric acid, and the vanadium dissolution rate was 89.82%.

[0074] Comparative Example 5:

[0075] 100g of calcified roasted clinker (TV=8.54%, P=0.058%) was added to 1200mL of recycled wastewater (V=0.1g / L). The mixture was stirred and the pH was adjusted to 2.8 with 50% dilute sulfuric acid. The reaction was continued for 80 minutes, followed by solid-liquid separation. This yielded a leachate (V=6.31g / L, P=0.022g / L) and a vanadium-extraction tailing (TV=1.04%). The sulfuric acid consumption during the leaching process was equivalent to 8.0mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 88.81%.

[0076] Example 5:

[0077] (1) 100 g of calcified roasted clinker (TV = 8.54%, P = 0.058%) was added to 200 mL of wastewater treatment recycled water (V = 0.1 g / L), and stirred evenly to obtain clinker slurry A;

[0078] (2) Take 6.0 mL of concentrated sulfuric acid, add it to 1000 mL of water, and stir evenly to obtain solution B;

[0079] (3) Solution B was added to the clinker slurry A at a uniform rate over a period of 25 min to obtain slurry C, where the liquid-to-solid ratio of slurry C was 12.06:1.

[0080] (4) The pH of slurry C was controlled to 2.8 using 50% by mass dilute sulfuric acid, and the leaching reaction was carried out for 40 minutes. After solid-liquid separation, vanadium-containing leaching solution (V = 6.58 / L, P = 0.021 g / L) and vanadium-extracting tailings (TV = 0.90%) were obtained.

[0081] The leaching process consumed 7.4 mL of concentrated sulfuric acid, resulting in a vanadium dissolution rate of 90.05%. In this case, the liquid-to-solid ratio of Slurry C was higher than 10:1, which improved the vanadium leaching rate. However, the resulting leachate had a vanadium concentration of less than 8 g / L, making it unsuitable for further vanadium extraction to produce vanadium oxide products.

[0082] Thus far, various embodiments of the present disclosure have been described in detail. To avoid obscuring the concept of the present disclosure, some details well known in the art have not been described. Based on the above description, those skilled in the art can fully understand how to implement the technical solutions disclosed herein.

[0083] Although some specific embodiments of the present disclosure have been described in detail through examples, those skilled in the art will understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the present disclosure. Those skilled in the art will understand that the above embodiments may be modified or some technical features may be replaced with equivalents without departing from the scope and spirit of the present disclosure. In particular, as long as there are no structural conflicts, the various technical features mentioned in the various embodiments may be combined in any manner.

Claims

1. A method for controlling the acid leaching process of calcined roasted clinker, characterized in that: The leaching agent is divided into two parts, one part is used to mix with the calcified roasted clinker to prepare clinker slurry, and the other part is used to dilute concentrated sulfuric acid.

2. The calcification roasted clinker acid leaching process control method according to claim 1, characterized in that: include: Step 1: mixing the calcified roasted clinker with a first leaching agent to obtain a clinker slurry; Step 2: Mixing concentrated sulfuric acid with a second leaching agent to obtain a first solution; Step 3: uniformly adding the first solution into the clinker slurry to obtain a third solution; Step 4: Controlling the pH value of the third solution to be between 2.5 and 3.5, performing a leaching reaction, and then performing solid-liquid separation to obtain a vanadium-containing leaching solution and vanadium-extracting tailings.

3. The calcification roasted clinker acid leaching process control method according to claim 2, characterized in that: In step 2, the amount of concentrated sulfuric acid used is 0.6-0.8 times the total amount of concentrated sulfuric acid consumed in the calcification roasted clinker leaching process.

4. The calcification roasted clinker acid leaching process control method according to claim 2, characterized in that: In step 1, the mass ratio of the calcified roasted clinker to the first leaching agent is 1:1-2.

5. The calcification roasted clinker acid leaching process control method according to claim 2, characterized in that: In step 1, the first leaching agent is water, recycled water from wastewater treatment or a vanadium-containing solution.

6. The calcification roasted clinker acid leaching process control method according to claim 2, characterized in that: In step 2, the second leaching agent is water or recycled water from wastewater treatment.

7. The calcification roasted clinker acid leaching process control method according to claim 2, characterized in that: In step three, the first solution is added to the clinker slurry at a uniform rate for more than 15 minutes.

8. The method for controlling the acid leaching process of calcined roasted clinker according to claim 7, characterized in that: The time for uniformly adding the first solution into the clinker slurry is 15 to 25 minutes.

9. The method for controlling the acid leaching process of calcified roasted clinker according to claim 2, characterized in that: The liquid-to-solid mass ratio of the third solution is (2-10):1; Preferably, the liquid-to-solid mass ratio of the third solution is (2-4):

1.

10. The method for controlling the acid leaching process of calcified roasted clinker according to claim 5, characterized in that: The vanadium-containing solution includes a washing solution of vanadium-extracting tailings.

Citation Information

Patent Citations

  • Clean production process for vanadium oxide

    CN101412539A

  • Vanadium leaching method for high-chrome vanadium residues

    CN105734308A

  • Method for preparing vanadium pentoxide by using vanadium chromium slag and manganese carbonate

    CN109666789A

  • Method for improving concentration of vanadium in vanadium slag calcium roasting clinker leaching solution

    CN115386742A

  • Calcified roasting clinker acid leaching process control method

    CN116497239A